An electromagnetic shielding film
By controlling the pressing pressure and adjusting the interlayer material, the relationship between the expansion and contraction value of the electromagnetic shielding film and the pressing pressure was optimized, solving the problem of excessive expansion and contraction of the electromagnetic shielding film under high temperature and high pressure conditions, and achieving precise hole matching with the circuit board and improving the yield rate.
Patent Information
- Application Number
- CN202510522456.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-24
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-04-24
AI Technical Summary
When existing electromagnetic shielding films are pressed under high temperature and high pressure conditions, they expand and contract excessively, failing to meet the matching requirements with the holes on the circuit board, resulting in a decrease in the yield rate of the circuit board.
By controlling the pressing pressure and adjusting the interlayer material, the relationship between the expansion/contraction value ΔL of the electromagnetic shielding film and the pressing pressure δ is satisfied: ΔL=A×δ/E+B. By combining the matching of the thermal expansion coefficients of the protective layer and the carrier layer, the dimensional stability of the electromagnetic shielding film is optimized.
This improved the accuracy of hole matching and processing performance of the electromagnetic shielding film, thereby enhancing the manufacturing quality of the circuit board.
Smart Images

Figure CN120417355B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of shielding film technology, and specifically to an electromagnetic shielding film. Background Technology
[0002] With the widespread adoption of electronic devices and the development of wireless communication technologies, electromagnetic interference (EMI) has become an increasingly prominent issue. Electromagnetic shielding films, as an effective solution, are widely used in electronic devices, communication systems, and aerospace to reduce EMI and improve device performance. From early simple metallic shielding materials to modern high-performance composite materials, the electromagnetic shielding effect of electromagnetic shielding films has continuously improved. The trend towards miniaturization and lightweighting of electronic devices has driven the demand for flexible shielding materials. Developing shielding films with higher conductivity, higher shielding effectiveness, and adaptability to the needs of flexible electronics is a crucial requirement at present.
[0003] However, when electromagnetic shielding films provided by existing technologies are pressed under high temperature and high pressure conditions, excessive expansion and contraction cannot meet the matching requirements of the holes on the circuit board, resulting in a decrease in the yield rate of the circuit board. Summary of the Invention
[0004] Therefore, to solve the above-mentioned technical problems, the present invention provides an electromagnetic shielding film in which, in the mechanical direction, the expansion / contraction value ΔL of the electromagnetic shielding film and the pressing pressure δ satisfy: ΔL=A×δ / E+B, where the unit of ΔL is 1 / 2. The unit of the pressing pressure δ is MPa, E represents the overall elastic modulus of the electromagnetic shielding film, and 0.5≤E≤2.5GPa, A<0, B>0, and the calculation is dimensionless. Electromagnetic shielding films that satisfy the above relationships exhibit good expansion and contraction performance, ensuring dimensional stability during use and improving processing performance.
[0005] During the research and development process, the inventors measured the expansion and contraction values of electromagnetic shielding films formed under different pressing pressures. They discovered that the pressing pressure and the overall elastic modulus of the electromagnetic shielding film have a regular influence on the overall expansion and contraction values of the electromagnetic shielding film. When the change pattern satisfies the above-mentioned specific functional relationship, it can achieve better hole matching accuracy. Therefore, by controlling the pressing pressure or adjusting the selection of interlayer materials, the elastic modulus can be changed, and the required expansion and contraction values of the electromagnetic shielding film can be obtained, thereby improving the manufacturing quality of the circuit board.
[0006] in, It represents one ten-thousandth.
[0007] To further improve the dimensional stability of the electromagnetic shielding film, the value of constant A ranges from -0.8 to -0.05, and the value of constant B ranges from 20 to 80. This embodiment of the invention sets upper and lower limits by limiting the correction factor. Electromagnetic shielding films whose test results fall within the range above and below the function curve exhibit good expansion and contraction values and good dimensional stability. For example, constant A is -0.8, -0.75, -0.6, -0.45, -0.3, -0.15, -0.1, -0.07, -0.05, or any two of these values; constant B is 20, 30, 35, 50, 60, 65, 70, 80, or any two of these values.
[0008] In some embodiments, the expansion / contraction value ΔE is calculated as follows: ΔE = expansion / contraction before and after pressing / initial size × 100%; in this embodiment, the expansion / contraction value of the carrier layer is the expansion / contraction value obtained after air pressing the carrier layer, while the expansion / contraction value test method of the shielding film body is to press the carrier layer and the shielding film body together on the flexible copper clad laminate (FCCL) substrate before they are separated, and after curing, separate the carrier layer and the shielding film body, and calculate the expansion / contraction value of each respectively.
[0009] In some embodiments, the method for determining the expansion and contraction value of the shielding film is as follows: An electromagnetic shielding film sample with dimensions of 250×300mm is cut, and holes are drilled at the four corners of the sample, labeled A, B, C, and D respectively. The distances between the drilled points AB, CD, AC, and BD are measured using an image measuring instrument and denoted as L. A-B L C-D L A-C L B-D The structure consists of a laminated electromagnetic shielding film and an FCCL (Fused Cellular Glass). The connecting layer side of the electromagnetic shielding film is brought into contact with the substrate side of the FCCL. The high-speed press is preheated for 10 seconds, and the pressing conditions are: pressing temperature of 80–300℃ and pressing pressure of 60–180 kg / cm². 2 The pressing time is 120–240 seconds. After pressing and curing under suitable conditions, the distances of the punched points AB, CD, AC, and BD on the test sample are measured again using an image measuring instrument and recorded as F. A-B F C-D F A-C F B-D The formulas for calculating the horizontal and vertical expansion / contraction values are as follows:
[0010] Horizontal expansion / contraction value = [(F A-B -L A-B ) / (2×L A-B )+(F C-D -L C-D ) / (2×L C-D )]×100%;
[0011] Vertical expansion / contraction value = [(F A-C -L A-C ) / (2×L A-C )+(F B-D -L B-D ) / (2×L B-D )]×100%.
[0012] Furthermore, since the lateral expansion / contraction value is much smaller than the longitudinal expansion / contraction value, the embodiments of the present invention use the longitudinal expansion / contraction value as the evaluation benchmark.
[0013] The electromagnetic shielding film includes a protective layer. In the mechanical direction, the expansion / contraction value ΔL of the electromagnetic shielding film and the pressing temperature T satisfy: ΔL=C×α×ΔT+D, where α represents the thermal expansion coefficient of the protective layer, ranging from 100 to 280, with units of ppm / ℃, and 0.0005≤C≤0.002, the constant D ranges from -10 to -2, and ΔT is the difference between the pressing temperature T and the room temperature, with units of ℃, and the calculation is dimensionless.
[0014] The expansion and contraction of a membrane typically refers to the dimensional changes that occur when environmental conditions (such as temperature and humidity) change. Both the thermal expansion coefficient and the hygroscopic expansion coefficient of the material affect these changes, specifically manifesting as expansion or contraction in the length, width, or thickness directions. Since there is no humidity influence during the pressing of the shielding film, the thermal expansion coefficient has a significant impact on the expansion and contraction of the shielding film, particularly in the length and width directions. To further control the expansion and contraction values of the electromagnetic shielding film within a certain range, the thermal expansion coefficient of the protective layer is controlled between 100-280 ppm / ℃. Simultaneously, to further improve the dimensional stability of the electromagnetic shielding film, the constant C ranges from 0.0005 to 0.002, and the constant D ranges from -10 to -2. This embodiment of the invention sets upper and lower limits by limiting correction factors. Electromagnetic shielding films whose test results fall within the range above and below the function curve exhibit good expansion and contraction values and good dimensional stability. For example, the constant C is 0.0005, 0.0008, 0.001, 0.0012, 0.0015, 0.0018 / 0.002 or any two values; the constant B is -10, -8, -5, -4, -2 or any two values.
[0015] To further reduce the expansion and contraction of the electromagnetic shielding film and improve the quality of the circuit board, under preset pressing conditions, the expansion and contraction value ΔE1 of the protective layer in the mechanical direction is less than... For example, the expansion / contraction value ΔE1 of the protective layer is Or an interval of any two values.
[0016] This invention provides insulation and protection for the shielding layer by setting a protective layer, while also preventing wear and tear on the shielding layer and extending the lifespan of the electromagnetic shielding film. The protective layer can be made of bisphenol A type epoxy resin, acrylic resin, polyester resin, etc. In addition, the resin used can be any one or a mixture of at least two of the following: epoxy resin, cyanate resin, polyphenylene ether resin, polybutadiene resin, styrene-butadiene resin, bismaleimide-triazine resin (BT), bismaleimide resin, polytetrafluoroethylene resin, polyimide resin, phenolic resin, acrylic resin, liquid crystal resin, benzoxazine resin, phenolic resin, nitrile rubber, carboxyl-terminated nitrile rubber, or hydroxyl-terminated nitrile rubber. However, it is not limited to these, and all resin materials disclosed in the prior art can be used. The mixture may be, for example, a mixture of epoxy resin and cyanate resin, a mixture of polyphenylene ether resin and polybutadiene resin, a mixture of styrene-butadiene resin and BT resin, a mixture of polytetrafluoroethylene resin and polyimide resin, a mixture of phenolic resin and acrylic resin, a mixture of epoxy resin, cyanate resin and polyphenylene ether resin, a mixture of polybutadiene resin, styrene-butadiene resin and BT resin, or a mixture of polytetrafluoroethylene resin, polyimide resin, phenolic resin and acrylic resin. That is, two or more resin mixtures may be used. In some embodiments, the thickness of the protective layer is 2-80 μm. Preferably, the average thickness of the shielding layer may be 2 μm, 5 μm, 8 μm, 10 μm, 20 μm, 25 μm, 32 μm, 45 μm, 60 μm, 70 μm and 80 μm or any range of two values.
[0017] In some embodiments, the electromagnetic shielding film further includes a shielding layer disposed on one side of the protective layer. The shielding layer includes one or more of a metal shielding layer, a carbon nanotube shielding layer, a ferrite shielding layer, and a graphene shielding layer. The metal shielding layer includes a single-metal shielding layer and / or an alloy shielding layer; wherein the single-metal shielding layer is made of any one of aluminum, titanium, zinc, iron, nickel, chromium, cobalt, copper, silver, and gold, and the alloy shielding layer is made of any two or more of aluminum, titanium, zinc, iron, nickel, chromium, cobalt, copper, silver, and gold.
[0018] In some embodiments, the thickness of the shielding layer is 0.5-15 μm. Preferably, the thickness of the shielding layer can be 0.5 μm, 1 μm, 2 μm, 5 μm, 10 μm, 15 μm, or any range of two values.
[0019] The electromagnetic shielding film further includes a carrier layer, which is disposed on the side of the protective layer facing away from the shielding layer. Optionally, to further improve the expansion and contraction value of the carrier layer, the carrier film is selected from materials with a suitable coefficient of thermal expansion. Specifically, it can be at least one of polytetrafluoroethylene, cellulose, polyetheretherketone, or liquid crystal polymers, or it can be polyolefins, polysulfones, polyamides, polyesters, polycarbonates, polyvinyl alcohol, silicone rubber, etc. For example, high coefficient of thermal expansion materials can be obtained by modifying polyimide (PI), polyethylene terephthalate (PET), polypropylene (PP), polyvinyl chloride (PVC), polyester, or other polymer materials. Alternatively, when applying the insulating layer to the carrier layer, the carrier layer can be pre-expanded and contracted. For example, under high temperature and stretching conditions, the insulating layer or subsequent layers are applied to the carrier film, so that the shielding film body and the carrier layer have pre-expansion and contraction. This is beneficial for the subsequent pressing of the electromagnetic shielding film onto the circuit board. The pre-expansion and contraction offsets the expansion and contraction caused by pressing, thereby stabilizing the size of the shielding film.
[0020] In some embodiments, the thickness of the carrier layer is 2-20 μm. Preferably, the thickness of the carrier layer can be 2 μm, 5 μm, 7 μm, 10 μm, 12 μm, 15 μm, 20 μm, or any range of two values.
[0021] To prevent delamination of the electromagnetic shielding film due to excessive stress, the thermal expansion coefficients α1 of the carrier layer and α2 of the protective layer satisfy the following conditions: 1 ≤ α1 / α2 ≤ 1.7; and |α1 - α2| ≤ 20 ppm / ℃. This invention reduces stress variations between the carrier and protective layers by limiting the relationship between their thermal expansion coefficients, thus preventing delamination of the electromagnetic shielding film and improving the quality of the circuit board.
[0022] Preferably, the ratio of the thermal expansion coefficient α1 of the carrier layer to the thermal expansion coefficient α2 of the protective layer is 1, 1.2, 1.4, 1.5, 1.6, 1.7, or any two of these values; the difference between the thermal expansion coefficient α1 of the carrier layer and the thermal expansion coefficient α2 of the protective layer is 0 ppm / ℃, 1 ppm / ℃, 2.5 ppm / ℃, 4 ppm / ℃, 5.5 ppm / ℃, 8 ppm / ℃, 10 ppm / ℃, 15 ppm / ℃, 20 ppm / ℃, or any two of these values.
[0023] In order to reduce grounding resistance, improve grounding effect and shielding efficiency, and reduce production costs, the shielding layer has a protrusion on the side opposite to the protective layer, and the protrusion is used to ground the circuit board.
[0024] To improve the dimensional stability and quality of the electromagnetic shielding film, the shielding film body further includes a connecting layer, which is disposed on the side of the shielding layer facing away from the protective layer. The connecting layer is made of at least one of the following resins: vinyl acetate, polyester, polyethylene, polyamide, rubber, acrylate, phenolic, epoxy, polyimide, urethane, melamine, alkyd, and ABF.
[0025] The thickness of the connecting layer is 2-20 μm. For example, the thickness of the connecting layer can be 2 μm, 3 μm, 4 μm, 5 μm, 8 μm, 12 μm, 20 μm or any range of two values.
[0026] In some embodiments, the connecting layer contains conductive particles, and the shielding layer can be grounded to the circuit board through these conductive particles. Preferably, the conductive particles and protrusions can be used in combination or independently. When there are no conductive particles in the connecting layer, grounding is achieved through the protrusions, which not only reduces grounding resistance but also reduces costs. When the connecting layer contains conductive particles, the conductive particles can enhance the grounding effect of the electromagnetic shielding film and improve shielding effectiveness. The conductive particles can be separate conductive particles or large, aggregated conductive particles. When the conductive particles are separate conductive particles, the grounding conductivity of the bonding layer can be further improved; while when the conductive particles are large, aggregated conductive particles, the puncture strength can be increased.
[0027] To further reduce the expansion and contraction of the electromagnetic shielding film, the thickness d1 of the carrier layer and the thickness d2 of the shielding film body satisfy the condition: 0.5 ≤ d1 / d2 ≤ 10. This invention improves the dimensional stability of the electromagnetic shielding film by reducing the thickness of the carrier layer, thus limiting the expansion and contraction of the electromagnetic shielding film. For example, the ratio of the thickness d1 of the carrier layer to the thickness d2 of the shielding film body is 0.5, 1, 2, 2.5, 5, 7, 8, 8.5, 9, 10, or any range of two values.
[0028] To further reduce the expansion and contraction of the electromagnetic shielding film, the electromagnetic shielding film also includes a buffer layer. The buffer layer is disposed between the carrier layer and the shielding film body. By placing the buffer layer between the carrier layer and the shielding film body, it plays a buffering role during the pressing process, reducing the expansion and contraction of the electromagnetic shielding film. The buffer layer can be made of inorganic or organic materials. For example, the buffer layer is at least one of polyurethane, silicone, polyimide, carbon nanotube aerogel, graphene aerogel, polyurethane foam, polyethylene foam, natural rubber, styrene-butadiene rubber, or polyurethane rubber. The thickness of the buffer layer is 2-20 μm. For example, the thickness of the buffer layer can be 2 μm, 3 μm, 4 μm, 5 μm, 8 μm, 12 μm, 20 μm, or any range of two values.
[0029] More specifically, in the embodiments of the present invention, the shielding film body is the structure of the shielding film excluding the carrier layer, and may include a shielding layer, a protective layer, a connecting layer or a buffer layer.
[0030] In some embodiments, the electromagnetic shielding film includes a carrier layer, a protective layer, a shielding layer, and a connecting layer stacked sequentially. The shielding layer is formed on the protective layer by methods such as pressing, laminating, vacuum sputtering, or electroplating. The side of the shielding layer facing away from the protective layer has uneven surfaces forming protrusions for grounding with the circuit board. The connecting layer is applied to the side of the shielding layer facing away from the protective layer by methods such as laminating or coating. After the electromagnetic shielding film is pressed onto the circuit board, the connecting layer cures and becomes tightly connected to the circuit board. The shielding layer is electrically connected to the grounding layer of the circuit board through a grounding window to form a ground, thus dissipating electromagnetic interference and achieving electromagnetic shielding. Attached Figure Description
[0031] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0032] Figure 1 This is a schematic diagram of the structure of the electromagnetic shielding film in Embodiment 1 of the present invention;
[0033] Figure 2 This is a schematic diagram of the structure of the electromagnetic shielding film in Embodiment 8 of the present invention;
[0034] Figure label:
[0035] 11-Shielding layer; 12-Protective layer; 13-Connecting layer; 14-Protrusion;
[0036] 15-Conductive particles; 2-Carrier layer; 3-Buffer layer. Detailed Implementation
[0037] The following embodiments are provided to better understand the present invention and are not limited to the preferred embodiments described. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention.
[0038] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.
[0039] Example 1
[0040] This embodiment provides an electromagnetic shielding film, the structural schematic of which is shown below. Figure 1 As shown, the electromagnetic shielding film includes a protective layer 12 and a shielding layer 11 stacked sequentially. The protective layer is a mixture of epoxy resin, cyanate resin, rubber and modified polyester filled with modified polyimide adhesive as the base. The thickness of the protective layer is 8 μm. The shielding layer is copper with a thickness of 1.5 μm.
[0041] At a pressing temperature of 185℃, the electromagnetic shielding film with carrier layer 2 was pressed onto the test plate at 12MPa for 180s (the press used was a Shenzhen Bioon fast press).
[0042] Measurements showed that the expansion / contraction value ΔL and the compression pressure δ of the electromagnetic shielding film satisfy ΔL=A×δ / E+B, where, δ=12MPa, E=1.2GPa, A=-0.5, B=20.
[0043] Example 2
[0044] The other technical features of this embodiment are the same as those of Embodiment 1, except that the protective layer is based on modified polytetrafluoroethylene and filled with a mixture of epoxy resin and nitrile rubber, and the thickness of the protective layer is 8 μm.
[0045] Measurements showed that the expansion / contraction value ΔL and the compression pressure δ of the electromagnetic shielding film satisfy ΔL=A×δ / E+B, where, δ=10MPa, E=1GPa, A=-0.8, B=33.
[0046] Example 3
[0047] Other technical features of this embodiment are the same as those of Embodiment 1, except that, through measurement, the expansion / contraction value ΔL of the electromagnetic shielding film and the pressing pressure satisfy ΔL=A×δ / E+B, and the expansion / contraction value ΔL of the electromagnetic shielding film and the pressing temperature satisfy ΔL=C×α×ΔT+D, where, α=200ppm / ℃, C=0.0015, ΔT=130℃-25℃=115, D=-5.
[0048] Example 4
[0049] The other technical features of this embodiment are the same as those of Embodiment 2, except that, by measurement, the expansion / contraction value ΔL of the electromagnetic shielding film and the pressing pressure satisfy ΔL=A×δ / E+B, and by measurement, the expansion / contraction value ΔL of the electromagnetic shielding film satisfies ΔL=C×α×ΔT+D, where, α=250ppm / ℃, C=0.002, ΔT=175℃-25℃=155, D=-10.
[0050] Example 5
[0051] The other technical features of this embodiment are the same as those of Embodiment 1, except that, by measurement, the expansion and contraction value ΔE1 of the protective layer in the longitudinal direction is...
[0052] Example 6
[0053] Other technical features of this embodiment are the same as those of Embodiment 2, except that, by measurement, the expansion and contraction value ΔE1 of the protective layer in the longitudinal direction is...
[0054] Example 7
[0055] This embodiment provides an electromagnetic shielding film. The shielding film body includes a protective layer 12 and a shielding layer 11 stacked sequentially. The protective layer is based on polyimide and filled with a mixture of epoxy resin and cyanate resin, with a thickness of 12 μm. The shielding layer is made of copper with a thickness of 1.5 μm. The carrier layer is made of polyetheretherketone with a thickness of 8 μm.
[0056] At the same time, the ratio of the thermal expansion coefficient α1 of the carrier layer to the thermal expansion coefficient α2 of the protective layer, α1 / α2, is 1.2.
[0057] At a pressing temperature of 300℃, the electromagnetic shielding film with carrier layer 2 is pressed onto the circuit board at a pressure of 16MPa. Specifically, the protective layer is connected to the carrier layer and the pressing is carried out for 180s (the press is a Shenzhen Bion fast press).
[0058] Measurements showed that the expansion / contraction value ΔL and the compression pressure δ of the electromagnetic shielding film satisfy ΔL=A×δ / E+B, where, δ=16MPa, E=2GPa, A=-0.05, B=35.
[0059] Example 8
[0060] This embodiment provides an electromagnetic shielding film, the structural schematic of which is shown below. Figure 2 As shown, the shielding film body includes a buffer layer 3, a protective layer 12, a shielding layer 11 and a connecting layer 13 stacked in sequence. The shielding layer has a protrusion 14 on the side opposite to the protective layer, and the connecting layer contains conductive particles 15.
[0061] The shielding layer in the shielding film body is made of copper with a thickness of 1.5 μm, the carrier layer is made of modified PET adhesive with a thickness of 5 μm, the protective layer is a mixture of polymethyl methacrylate and rubber with a thickness of 3 μm, the connecting layer is an acrylic adhesive with a thickness of 4 μm, and the buffer layer is polyurethane with a thickness of 7 μm. The thickness d1 of the carrier layer and the thickness d2 of the shielding film body satisfy d1 / d2 = 2.5, which meets the condition 0.5 ≤ d1 / d2 ≤ 10.
[0062] The thermal expansion coefficient α1 of the carrier layer and the thermal expansion coefficient α2 of the protective layer satisfy |α1-α2| = 15ppm / ℃;
[0063] At a pressing temperature of 300℃, the electromagnetic shielding film is pressed onto the carrier layer 2 with a pressure of 16MPa. Specifically, the buffer layer is connected to the carrier layer, and the pressing is carried out for 180s (the press is a Shenzhen Bion fast press).
[0064] Measurements showed that the expansion / contraction value ΔL of the electromagnetic shielding film satisfies ΔL=A×δ / E+B, where Δ δ=16MPa, E=2.5GPa, A=-0.8, B=40.12.
[0065] Example 9
[0066] The other technical features of this embodiment are the same as those of Embodiment 1, except that the pressing pressure is 61 kg / cm². 2 73kg / cm 2 91kg / cm 2 110kg / cm 2 120kg / cm 2 The measured expansion and contraction values of the electromagnetic shielding film were as follows:
[0067] The R² of the fitting curve between the pressing pressure and the measured expansion and contraction value of the electromagnetic shielding film is 0.9018, indicating that the pressing pressure and the expansion and contraction value of the electromagnetic shielding film are negatively correlated and the fitting degree is good.
[0068] Example 10
[0069] The other technical features of this embodiment are the same as those of Embodiment 1, except that the pressing temperatures are 80℃, 100℃, 120℃, 140℃, and 180℃, and the measured expansion and contraction values of the electromagnetic shielding film are as follows:
[0070] It can be seen that the pressing temperature is positively correlated with the expansion and contraction value of the electromagnetic shielding film.
[0071] Comparative Example 1
[0072] The other technical features of this comparative example are the same as those of Example 1, except that the thickness of the shielding layer is 15 μm. Measurements show that the expansion / contraction value ΔL and the compression pressure δ of the electromagnetic shielding film do not satisfy ΔL=A×δ / E+B. δ = 12 MPa, E = 2 GPa.
[0073] Comparative Example 2
[0074] The other technical features of this comparative example are the same as those of Example 1, except that the thickness of the protective layer is 1 μm. Measurements show that the expansion / contraction value ΔL and the compression pressure δ of the electromagnetic shielding film do not satisfy ΔL=A×δ / E+B. δ = 12 MPa, E = 1 GPa.
[0075] Experimental Example
[0076] The electromagnetic shielding films formed in Examples 1-8 and Comparative Examples 1-2 were pressed onto FPC test plates using a high-speed press. The pressing conditions were: temperature 185°C, pressing time 180s, and pressing pressure 120kg / cm². 2 The offset of the holes in the shielding films of the embodiments and comparative examples on the FPC circuit boards was measured and calculated, and the results are shown in Table 1.
[0077] Method for determining hole offset: An optical measurement method is employed, using a high-resolution electron microscope. Before the shielding film is laminated, the holes on the circuit board are precisely measured and marked, and the center coordinates of each hole are recorded. The microscope's built-in measurement software or image analysis software is used to determine the center position of the hole. After the shielding film is laminated, the center coordinates of the same hole positions are observed and measured again using the microscope. By comparing the changes in the coordinates of the hole positions before and after lamination, the offset of the hole positions in the X and Y axes is calculated, and the average value is taken to obtain the total hole offset.
[0078] Table 1. Test results of electromagnetic shielding film
[0079]
[0080] According to the data in Table 1, compared with the electromagnetic shielding films provided in Comparative Examples 1-2, the measured expansion / contraction value ΔL and pressing pressure δ do not satisfy the formula ΔL=A×δ / E+B, and their hole position offsets are 98.4mm and 122.4mm respectively. However, the electromagnetic shielding films provided in Examples 1-8 of this invention have measured expansion / contraction value ΔL and pressing pressure δ that satisfy the formula ΔL=A×δ / E+B, and their hole position offsets are between 2.1-12.7mm. This proves that the electromagnetic shielding films with expansion / contraction value ΔL and pressing pressure δ that satisfy the formula ΔL=A×δ / E+B have strong stability and good processing performance.
[0081] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. An electromagnetic shielding film, characterized in that, In the mechanical direction, the expansion / contraction value ΔL of the electromagnetic shielding film and the pressing pressure δ satisfy the following: ΔL = A × δ / E + B Wherein, the unit of the pressing pressure δ is MPa, E represents the overall elastic modulus of the electromagnetic shielding film, and 0.5≤E≤2.5GPa, the value range of constant A is -0.8~-0.05, the value range of constant B is 20~80, and the calculation is dimensionless.
2. The electromagnetic shielding film according to claim 1, characterized in that, The electromagnetic shielding film includes a protective layer, and in the mechanical direction, the expansion / contraction value ΔL of the electromagnetic shielding film satisfies the following relationship with the pressing temperature T: ΔL = C × α × ΔT + D, Where α represents the thermal expansion coefficient of the protective layer, ranging from 100 to 280, with units of ppm / ℃, and 0.0005≤C≤0.002, the constant D ranges from -10 to -2, and ΔT is the difference between the pressing temperature T and the room temperature, with units of ℃, and the calculation is dimensionless.
3. The electromagnetic shielding film according to claim 2, characterized in that, Under preset pressing conditions, the expansion / contraction value ΔE1 of the protective layer in the mechanical direction is less than 40. The preset pressing conditions are: pressing temperature of 80~300℃ and pressing pressure of 60~180kg / cm². 2 The pressing time is 120~240s.
4. The electromagnetic shielding film according to claim 2, characterized in that, The electromagnetic shielding film further includes a shielding layer, which is disposed on one side of the protective layer.
5. The electromagnetic shielding film according to claim 4, characterized in that, The electromagnetic shielding film also includes a carrier layer, which is disposed on one side of the protective layer opposite to the shielding layer.
6. The electromagnetic shielding film according to claim 5, characterized in that, The thermal expansion coefficient α1 of the carrier layer and the thermal expansion coefficient α2 of the protective layer satisfy: 1 ≤ α1 / α2 ≤ 1.
7. The thermal expansion coefficient α1 of the carrier layer and the thermal expansion coefficient α2 of the protective layer satisfy: |α1-α2|≤50ppm / ℃.
7. The electromagnetic shielding film according to claim 4, characterized in that, The shielding layer has a protrusion on the side opposite to the protective layer, and the protrusion is used to ground the circuit board.
8. The electromagnetic shielding film according to claim 4, characterized in that, The electromagnetic shielding film further includes a connecting layer, which is disposed on the side of the shielding layer opposite to the protective layer.
9. The electromagnetic shielding film according to claim 8, characterized in that, The connecting layer contains conductive particles.
10. The electromagnetic shielding film according to claim 5, characterized in that, The thickness d1 of the carrier layer and the thickness d2 of the shielding film body satisfy the following condition: 0.5≤d1 / d2≤10.
11. The electromagnetic shielding film according to claim 5, characterized in that, The electromagnetic shielding film further includes a buffer layer, which is disposed between the carrier layer and the protective layer, and / or, the buffer layer is disposed between the protective layer and the shielding layer.
Citation Information
Patent Citations
Rigidity and flexibility combination circuit board possessing electromagnetic shielding film and manufacturing method thereof
CN106061107A
Rigid-flex printed circuit board and electromagnetic shielding film shedding control method thereof