A carbon nanotube-reinforced aluminum matrix composite material and its preparation method
By combining surface modification of carbon nanotubes with a two-stage sintering process involving low-temperature and high-temperature mixing, the problems of dispersion and interfacial reaction in carbon nanotube-reinforced aluminum matrix composites were solved, achieving high strength and high thermal conductivity in the material.
Patent Information
- Application Number
- CN202611313643.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-10
AI Technical Summary
In existing technologies, it is difficult to synergistically improve the strength and thermal conductivity of carbon nanotube-reinforced aluminum matrix composites, mainly due to the poor dispersion of carbon nanotubes, their susceptibility to breakage, and structural damage and performance degradation caused by insufficient interfacial reactions.
Acidic solutions were used to modify the surface of carbon nanotubes, and a combination of low-temperature premixing and high-temperature ball milling was performed. The two-stage sintering process controlled the thickness of the interfacial reaction layer to ensure uniform dispersion and strong bonding of carbon nanotubes in the aluminum matrix.
The mechanical and thermal properties of carbon nanotube-reinforced aluminum matrix composites were synergistically improved, with significant increases in tensile strength and thermal conductivity, and optimization of interfacial bonding strength and thermal conductivity.
Smart Images

Figure CN123063646A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metallic materials, specifically relating to a carbon nanotube-reinforced aluminum-based composite material and its preparation method. Background Technology
[0002] Carbon nanotubes (CNTs) are considered ideal reinforcements for improving the properties of aluminum matrix composites due to their ultra-high strength, modulus, and thermal conductivity. Currently, the most common method for preparing CNTs / Al composites is powder metallurgy, whose core steps include: ball milling and dispersing CNTs, mixing them with aluminum powder, and finally cold pressing and sintering. However, CNTs have poor dispersibility, and the high-energy impact of traditional ball milling processes easily leads to CNT fracture, a decrease in aspect ratio, and an inability to effectively solve the problem of entanglement and agglomeration, forming stress concentration points and resulting in limited reinforcement in the composite. Conventional sintering processes struggle to balance the structural integrity of CNTs and the strength of interfacial reactions, easily leading to CNT structural damage and excessive reaction with the aluminum matrix, generating excessive brittle phases. Furthermore, while some intermediate phases generated during sintering may improve some bonding strength, they also severely impair the intrinsic thermal conductivity of CNTs, resulting in a decrease in the thermal conductivity of the composite. Therefore, due to these limitations, composites prepared by existing processes often fail to achieve a synergistic improvement in strength and thermal conductivity. Summary of the Invention
[0003] In view of the problems in the prior art where the strength and thermal conductivity of carbon nanotube-reinforced aluminum matrix composites are often difficult to improve simultaneously, the present invention will provide carbon nanotube-reinforced aluminum matrix composites and their preparation methods.
[0004] To achieve the above objectives, the following technical solutions are specifically included: On one hand, the present invention provides a method for preparing carbon nanotube-reinforced aluminum-based composite materials, comprising the following steps: S1. Carbon nanotubes are mixed with an acidic aqueous solution, ultrasonically treated, washed and dried sequentially to obtain surface-modified carbon nanotubes. S2. The surface-modified carbon nanotubes, aluminum-based metal powder, and optional interface modifier are stirred and mixed at 0℃-15℃ to obtain the first premix. S3. The premixed material is ball-milled at 60-100°C in an inert gas atmosphere to obtain a second premixed material; S4. Press the second premix into shape to obtain a green body; S5. The green blank is subjected to a first-stage sintering treatment and a second-stage sintering treatment in sequence to obtain the carbon nanotube reinforced aluminum matrix composite material; the temperature of the first-stage sintering treatment is 420-480℃, and the temperature of the second-stage sintering treatment is 520-580℃.
[0005] In the preparation method of this invention, carbon nanotubes (CNTs) undergo surface modification with an acidic solution to introduce functional groups such as carboxyl groups (-COOH) and hydroxyl groups (-OH) onto the CNT surface, significantly improving their dispersibility and surface chemical activity in combination with metal powder. When the modified carbon nanotubes are mixed with raw materials such as aluminum-based metal powder, they are premixed at low temperature and then ball-milled at relatively high temperature. The low-temperature environment of the former helps to suppress the stickiness of aluminum-based metal powder and the kinetic energy of carbon nanotubes, and initially deagglomerates through gentle shear force, achieving uniform physical adsorption between powders and preventing initial cold welding. The relatively high-temperature environment of the latter thermally activates the aluminum-based metal powder, making it easier to undergo plastic deformation. Under high-energy impact, the carbon nanotubes are effectively embedded and firmly anchored inside the aluminum-based metal powder, achieving mechanical interlocking and composite at the microscale, which can effectively improve the tensile strength and thermal conductivity of the composite material.
[0006] During the sintering process, the green body is sintered sequentially in two stages at different temperatures. In the first stage, the temperature is lower than that in the second stage. At this stage, the solid particles in the green body undergo preliminary solid-phase sintering and densification to establish a metal framework. Simultaneously, this temperature is below the critical point for the violent reaction between carbon nanotubes and aluminum, which can preserve the structural integrity of carbon nanotubes to the maximum extent. The temperature is then raised to the second stage of sintering. The sintering temperature in this stage is higher than the solidus line of the aluminum matrix, which can generate a small amount of liquid phase or greatly accelerate atomic diffusion. This condition is used to promote the interfacial reaction and interdiffusion of elements between aluminum atoms and the surface of carbon nanotubes, forming a strong and tough metallurgical bond. Through precise sintering conditions, the thickness of the interfacial reaction layer (such as Al4C3) is controlled within the ideal range of 5-20 nm, which is beneficial to improving the bonding between carbon nanotubes and aluminum-based metals, while avoiding excessive precipitation of the interfacial reaction layer that would damage the thermal conductivity of the material. This achieves the goal of simultaneously improving the tensile strength and thermal conductivity of the composite material to a greater extent. Therefore, the method of the present invention achieves highly uniform dispersion of carbon nanotubes (CNTs) in an aluminum matrix without damaging the intrinsic structure of CNTs, and forms a strong and tough interfacial bond that is conducive to thermal / charge conduction, thereby preparing a carbon nanotube-reinforced aluminum matrix composite material with synergistic improvement in mechanical and thermal properties.
[0007] Preferably, in step S1, the acid in the acidic solution includes at least one of nitric acid and sulfuric acid, and the total mass concentration of the acid in the acidic solution is 70%-90%. Carbon nanotubes (CNTs) are surface modified by acidic solution to introduce functional groups such as carboxyl groups (-COOH) and hydroxyl groups (-OH) on the surface of CNTs, which significantly improves their dispersibility and surface chemical activity in combination with metal powder.
[0008] More preferably, the acidic solution includes nitric acid and sulfuric acid, and the mass ratio of the mass concentrations of the nitric acid and sulfuric acid is (10-15):(70-80).
[0009] Preferably, in step S1, the temperature of the ultrasonic treatment is 40-60℃, the time of the ultrasonic treatment is 0.5-1h, and the temperature of the drying is 60-100℃.
[0010] Preferably, in step S2, based on the total mass of the surface-modified carbon nanotubes, aluminum-based metal powder, and interface regulator, the mass percentage of the surface-modified carbon nanotubes is 0.3%-2.5%, and the mass percentage of the interface regulator is 0-1.5%.
[0011] Carbon nanotubes, as a reinforcing phase in aluminum-based metal cores, have a low reinforcing effect when their content is too low, and a high content can lead to difficulties in dispersing carbon nanotubes in the aluminum matrix and the formation of defects. The inventors of this invention have discovered that a carbon nanotube content in the range of 0.3%-2.5% can simultaneously improve the thermal conductivity and strength of the composite material.
[0012] Preferably, the carbon nanotubes are multi-walled carbon nanotubes (MWCNTs).
[0013] Preferably, in step S2, the interface modifier includes at least one of titanium powder, magnesium powder, and aluminum nitride (AlN) powder.
[0014] More preferably, based on the total mass of surface-modified carbon nanotubes, aluminum-based metal powder, and interface regulator, the mass percentage of magnesium powder is 0.2% to 1%, and the magnesium powder can improve the wettability of aluminum liquid to CNTs.
[0015] More preferably, based on the total mass of surface-modified carbon nanotubes, aluminum-based metal powder, and interface regulator, the mass percentage of titanium powder is 0.5%~1.5%. The titanium powder will preferentially react with carbon to generate TiC, forming a gradient transition layer, which will suppress the excessive generation of Al4C3 phase and avoid the deterioration of material performance due to excessive Al4C3 phase.
[0016] More preferably, based on the total mass of surface-modified carbon nanotubes, aluminum-based metal powder, and interface regulator, the mass percentage of aluminum nitride powder is 0.5%~1.5%, which acts as a heterogeneous nucleation point to refine the aluminum matrix grains and achieve a fine-grain strengthening effect.
[0017] In step S2, the mixing time is 0.5-1h.
[0018] Preferably, in step S2, the aluminum-based metal powder includes at least one of aluminum powder and aluminum alloy powder. The aluminum powder has a purity ≥99.9%; the aluminum alloy powder includes 6061 type, 7075 type, etc., more specifically, such as 6061 type aluminum alloy powder, which mainly includes the following components by mass percentage: Mg 0.8%-1.2%, Si 0.4%-0.8%, Cu 0.15%-0.4%, Cr 0.04%-0.35%, with the balance being Al.
[0019] Preferably, in step S3, the ball milling time is 2-6 hours, the ball-to-material ratio is (10-20):1, and the ball milling speed is 200-400 rpm.
[0020] Preferably, in step S3, the inert gas includes at least one of argon, nitrogen, and helium.
[0021] Preferably, in step S4, the pressing pressure is 200-400 MPa.
[0022] Preferably, in step S5, the sintering time for the first stage is 10-60 min, and the sintering time for the second stage is 30-120 min. Under the above two-stage sintering temperatures and times, the degree of material sintering can be precisely controlled, avoiding weak interfacial bonding due to insufficient sintering or structural damage to CNTs due to over-sintering and excessive reaction with the aluminum matrix to generate excessive brittle phases that degrade material properties.
[0023] Preferably, the process further includes the following step S6: S6. The carbon nanotube reinforced aluminum matrix composite material is further subjected to post-treatment, which includes at least one of hot rolling, hot isostatic pressing, and annealing.
[0024] In step S6, the rolling temperature is 350-450℃ and the deformation is 30-60%; the hot isostatic pressing temperature is 500-550℃, the pressure is 100-150MPa, and the time is 1-2h.
[0025] On the other hand, the present invention also provides a carbon nanotube-reinforced aluminum matrix composite material, which is prepared by the method for preparing the carbon nanotube-reinforced aluminum matrix composite material.
[0026] Compared with existing technologies, this invention has the following advantages: In the preparation method of this invention, carbon nanotubes are first modified with an acidic solution; secondly, the modified carbon nanotubes and aluminum-based metal materials are mixed twice at different temperatures, and finally, the composite material of this invention is obtained through pressing and two-stage sintering. The method of this invention can achieve highly uniform dispersion of carbon nanotubes in an aluminum matrix without damaging the intrinsic structure of the carbon nanotubes, and form a strong and tough interfacial bond that facilitates thermal and load conduction, thereby obtaining a carbon nanotube-reinforced aluminum-based composite material with synergistically improved mechanical and thermal properties. Attached Figure Description
[0027] Figure 1 This is a microstructure diagram of the 6061 type aluminum alloy powder in Example 1.
[0028] Figure 2 This is a microstructure diagram of the second mixture after ball milling in step S3 of Example 1.
[0029] Figure 3 This is a microstructure diagram of the sintered green body after step S5 in Example 1.
[0030] Figure 4 The electron microscope images of the carbon nanotube-reinforced aluminum matrix composite material in Example 1 are shown in (a) and (b), respectively, at low magnification (scale bar 10 μm) and high magnification (scale bar 200 nm) to show the material interface positions. Detailed Implementation
[0031] To better illustrate the purpose, technical solution, and advantages of this invention, specific embodiments will be used to further explain the invention below. Unless otherwise specified, the test methods used in the embodiments and / or comparative examples are conventional methods; the materials and reagents used, unless otherwise specified, are commercially available.
[0032] Example 1 A method for preparing a carbon nanotube-reinforced aluminum-based composite material includes the following steps: S1. Carbon nanotubes are placed in a mixed acidic solution prepared by mixing concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:3, and then ultrasonically treated at 60°C for 1 hour. After the treatment, they are repeatedly washed with deionized water until neutral, and then dried in a vacuum oven at 80°C to obtain surface-modified carbon nanotubes. S2. Weigh out surface-modified carbon nanotubes, 6061 aluminum alloy powder, and titanium powder as raw materials according to mass percentages of 1.5%, 98.0%, and 0.5%, respectively, and mix the above raw materials at 0℃ and low speed for 0.5h to obtain the first premix; the composition of 6061 aluminum alloy powder is as follows: Mg 1%, Si 0.6%, Cu 0.28%, Cr 0.2%, with the balance being Al; S3. The first premix is then ball-milled at 80°C under argon protection for 3 hours to obtain the second premix; wherein the ball-to-material ratio in the ball mill is 15:1 and the rotation speed is 300 rpm. S4. The second premix is subjected to biaxial cold pressing at room temperature and 300MPa to obtain a green body. S5. Under vacuum, the green body is heated to 480°C for the first stage of sintering for 30 minutes, then heated to 560°C for the second stage of sintering for 60 minutes, and then cooled naturally to obtain the sintered green body. S6. The sintered billet is hot rolled at 400℃ to achieve a deformation of 50%, thus obtaining a carbon nanotube-reinforced aluminum matrix composite material.
[0033] Example 2 The difference between this embodiment and embodiment 1 is that in step S2 of this embodiment, the surface-modified carbon nanotubes, titanium powder and 7075 aluminum powder are weighed as raw materials in the following proportions: 2.2%, 0.3% and 97.5% by mass, respectively. The rest are the same.
[0034] Example 3 The difference between this embodiment and embodiment 1 is that in step S2 of this embodiment, there is no titanium powder, and aluminum alloy powder is used to make up the amount, while the rest are the same.
[0035] Example 4 The difference between this embodiment and embodiment 1 is that in step S2 of this embodiment, the mixing temperature is 5°C, while the rest are the same.
[0036] Example 5 The difference between this embodiment and embodiment 1 is that in step S2 of this embodiment, the mixing temperature is 10°C, while the rest are the same.
[0037] Example 6 The difference between this embodiment and embodiment 1 is that in step S3 of this embodiment, the ball milling temperature is 60°C, while the rest are the same.
[0038] Example 7 The difference between this embodiment and embodiment 1 is that in step S2 of this embodiment, the mixing temperature is 15°C, while the rest are the same.
[0039] Example 8 The difference between this embodiment and embodiment 1 is that in step S3 of this embodiment, the ball milling temperature is 90°C, while the rest are the same.
[0040] Example 9 The difference between this embodiment and embodiment 1 is that in step S3 of this embodiment, the ball milling temperature is 100°C, while the rest are the same.
[0041] Example 10 The difference between this embodiment and embodiment 1 is that in step S5 of this embodiment, the sintering temperature in the second stage is 520°C, while the rest are the same.
[0042] Example 11 The difference between this embodiment and embodiment 1 is that in step S5 of this embodiment, the sintering temperature in the second stage is 580°C, while the rest are the same.
[0043] Example 12 The difference between this embodiment and embodiment 1 is that this embodiment does not include the hot rolling process in step S6, but the rest are the same.
[0044] Comparative Example 1 The difference between this comparative example and Example 1 is that the 0°C in step S2 is set to 80°C, that is, the mixing temperature in steps S2-S3 is 80°C, and the other steps are the same.
[0045] Comparative Example 2 The difference between this comparative example and Example 1 is that in step S5 of this comparative example, the sintering temperature of both stages is set to 580°C, that is, the green body is sintered at 580°C for 90 minutes. The rest are the same.
[0046] Comparative Example 3 The difference between this comparative example and Example 1 is that the sintering temperature in the second stage of step S5 is 600°C, while the rest are the same.
[0047] The performance of carbon nanotube-reinforced aluminum matrix composites was tested, including phase microscopy (SEM), transmission electron microscopy (TEM), thermal conductivity, and tensile strength. Some test results are shown below. Figure 1-4 As shown in Table 1.
[0048] Table 1 Depend on Figure 1-4 It can be seen that in the material of Example 1, the CNTs are uniformly dispersed at the interface, the interface reaction layer is thin and continuous, and the interface morphology is relatively ideal. However, the SEM performance results of the material of Comparative Example 1 show that the CNT agglomerates are increased; the SEM of the material of Comparative Example 2 shows that some CNT structures are destroyed, and the interface reaction layer is uneven and too thick.
[0049] As can be seen from Example 1 and Comparative Examples 1-3 above, when carbon nanotubes and aluminum-based metal powder are mixed, they are first pre-mixed at low temperature and then ball-milled at relatively high temperature. The low temperature environment of the former helps to suppress the stickiness of aluminum-based metal powder and the kinetic energy of carbon nanotubes. Through gentle shear force, the agglomeration is initially de-agglomerated, and the powder particles are uniformly physically adsorbed to each other, preventing initial cold welding. The relatively high temperature environment of the latter thermally activates the aluminum-based metal powder, making it easier to undergo plastic deformation. Under high-energy impact, the carbon nanotubes are effectively embedded and firmly nailed into the interior of the aluminum-based metal powder, realizing mechanical interlocking and composite at the microscale. This can effectively improve the tensile strength and thermal conductivity of the composite material.
[0050] During the sintering process, sintering is carried out in two stages at different temperatures. In the first stage, the temperature is lower than that in the second stage. At this stage, the solid particles in the green body undergo preliminary solid-phase sintering and densification to establish a metal framework. At the same time, this temperature is below the critical point for the violent reaction between carbon nanotubes and aluminum, which can preserve the structural integrity of carbon nanotubes to the maximum extent. Then, the temperature is raised to the second stage of sintering. The sintering temperature in this stage is higher than the solidus line of the aluminum matrix, which can generate a small amount of liquid phase or greatly accelerate atomic diffusion. This condition is used to promote the interfacial reaction and element interdiffusion between aluminum atoms and the surface of carbon nanotubes, forming a strong and tough metallurgical bond. Through precise sintering conditions, the thickness of the interfacial reaction layer (such as Al4C3) is controlled within the ideal range of 5-20 nm, which is beneficial to improving the bonding between carbon nanotubes and aluminum-based metals, thereby achieving the goal of greatly improving the tensile strength and thermal conductivity of the composite material.
[0051] Furthermore, as can be seen from Examples 1-12, the amount of carbon nanotubes added, the interface modifier, the mixing temperature, the sintering temperature, and the post-treatment conditions have a certain influence on the tensile strength and thermal conductivity of the composite material.
[0052] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. A method for preparing a carbon nanotube-reinforced aluminum-based composite material, characterized in that, Includes the following steps: S1. Carbon nanotubes are mixed with an acidic aqueous solution, ultrasonically treated, washed and dried sequentially to obtain surface-modified carbon nanotubes. S2. The surface-modified carbon nanotubes, aluminum-based metal powder, and optional interface modifier are stirred and mixed at 0℃-15℃ to obtain the first premix. S3. The premixed material is ball-milled at 60-100°C in an inert gas atmosphere to obtain a second premixed material; S4. Press the second premix into shape to obtain a green body; S5. The green blank is subjected to a first-stage sintering treatment and a second-stage sintering treatment in sequence to obtain the carbon nanotube reinforced aluminum matrix composite material; the temperature of the first-stage sintering treatment is 420-480℃, and the temperature of the second-stage sintering treatment is 520-580℃.
2. The method for preparing carbon nanotube-reinforced aluminum-based composite materials as described in claim 1, characterized in that, In step S2, based on the total mass of the surface-modified carbon nanotubes, aluminum-based metal powder, and interface regulator, the mass percentage of the surface-modified carbon nanotubes is 0.3%-2.5%, and the mass percentage of the interface regulator is 0-1.5%.
3. The method for preparing carbon nanotube-reinforced aluminum-based composite materials as described in claim 1, characterized in that, In step S2, the interface modifier includes at least one of titanium powder, magnesium powder, and aluminum nitride powder.
4. The method for preparing carbon nanotube-reinforced aluminum-based composite materials as described in claim 1, characterized in that, It also includes the following step S6: S6. The carbon nanotube reinforced aluminum matrix composite material is further subjected to post-treatment, which includes at least one of hot rolling, hot isostatic pressing, and annealing.
5. The method for preparing carbon nanotube-reinforced aluminum-based composite materials as described in claim 4, characterized in that, In step S6, the rolling temperature is 350-450℃ and the deformation is 30-60%; the hot isostatic pressing temperature is 500-550℃, the pressure is 100-150MPa, and the time is 1-2h.
6. The method for preparing carbon nanotube-reinforced aluminum-based composite materials as described in claim 1, characterized in that, In step S3, the ball milling time is 2-6 hours, the ball-to-material ratio is (10-20):1, and the ball milling speed is 200-400 rpm.
7. The method for preparing carbon nanotube-reinforced aluminum-based composite materials as described in claim 1, characterized in that, In step S5, the sintering time for the first stage is 10-60 min, and the sintering time for the second stage is 30-120 min.
8. The method for preparing carbon nanotube-reinforced aluminum-based composite materials as described in claim 1, characterized in that, Includes at least one of the following ADs: A. In step S1, the acid in the acidic solution includes at least one of nitric acid and sulfuric acid, and the total mass concentration of the acid in the acidic solution is 70%-90%. B. In step S1, the temperature of the ultrasonic treatment is 40-60℃, the time of the ultrasonic treatment is 0.5-1h, and the temperature of the drying is 60-100℃. C. In step S2, the aluminum-based metal powder includes at least one of aluminum powder and aluminum alloy powder; D. In step S4, the pressure for pressing and molding is 200-400 MPa.
9. A carbon nanotube-reinforced aluminum-based composite material, characterized in that, The carbon nanotube-reinforced aluminum matrix composite material is prepared by the method described in any one of claims 1-8.