A low-cost, high-strength meta-aramid paper honeycomb core material and its preparation method

By applying an inorganic-organic composite coating to aramid paper, the problem of poor wettability of low-cost aramid paper was solved, and the node strength and mechanical properties of the honeycomb core material were improved. This enabled the preparation of low-cost, high-strength aramid paper honeycomb core material, which is suitable for high-end equipment manufacturing.

CN123064053APending Publication Date: 2026-11-10THE RES INST FOR SPECIAL STRUCTURES OF AERONAUTICAL COMPOSITE AVIC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611135030.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-29
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In existing technologies, low-cost aramid paper honeycomb core materials are difficult to penetrate evenly with resin during the impregnation process, resulting in low node strength and large dispersion of mechanical properties, which cannot meet the reliability requirements of high-end equipment.

Method used

An inorganic-organic composite coating solution is used to pretreat the surface of aramid paper to form a micro-rough structure to enhance resin bonding. Chemical cross-linking is then performed with silane coupling agent and water-soluble phenolic resin to form a strong and tough interfacial transition zone.

Benefits of technology

It significantly improves the node strength and mechanical properties of aramid paper honeycomb core material, reduces raw material costs, and enhances product consistency and performance stability, making it suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of composite material technology, specifically to a low-cost, high-strength meta-aramid paper honeycomb core material and its preparation method. The aramid paper in the meta-aramid paper honeycomb core material undergoes surface pretreatment with an inorganic-organic composite coating solution. The inorganic-organic composite coating solution, by mass parts, comprises: water-soluble phenolic resin: 20-40 parts, nano-silica sol: 5-15 parts, silane coupling agent: 0.5-2 parts, and deionized water: 50-70 parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of composite materials technology, specifically to a low-cost, high-strength meta-aramid paper honeycomb core material and its preparation method. Background Technology

[0002] Meta-aramid paper honeycomb cores are widely used in high-end equipment manufacturing fields such as aircraft cabin materials, radomes, and high-speed train bodies due to their excellent specific strength, specific modulus, flame retardancy, and high-temperature resistance. Traditional high-performance aramid paper honeycomb is usually prepared using high-specification aramid paper such as DuPont's Nomex® T series. This type of aramid paper is made from a finely proportioned blend of long fibers and precipitated fibers, which is expensive, resulting in high costs for the final honeycomb core material and limiting its wider application.

[0003] To reduce costs, the industry has attempted to use low-cost aramid paper with a higher chopped fiber content (such as domestically produced aramid paper or certain industrial-grade aramid paper). However, this type of paper has a smooth surface, few active functional groups, and poor wettability with phenolic resin. This makes it difficult for the resin to penetrate evenly during the impregnation process, resulting in honeycomb structures with low node strength, large dispersion in mechanical properties (especially planar compressive strength and shear strength), and low product yield. Simply using low-cost materials often comes at the cost of sacrificing key performance characteristics, failing to meet the reliability requirements of high-end equipment.

[0004] Therefore, developing a method that can effectively accommodate low-cost aramid paper and compensate for its performance shortcomings through process and material innovation to prepare aramid paper honeycomb core materials with both low cost and high strength has become a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0005] Purpose of the invention: This invention provides a low-cost, high-strength meta-aramid paper honeycomb core material and its preparation method, thereby producing an aramid paper honeycomb core material that combines low cost and high strength.

[0006] Technical solution: A low-cost, high-strength meta-aramid paper honeycomb core material, wherein the aramid paper of the meta-aramid paper honeycomb core material is surface pretreated with an inorganic-organic composite coating solution. The inorganic-organic composite coating solution, by mass parts, comprises: water-soluble phenolic resin: 20-40 parts, nano-silica sol: 5-15 parts, silane coupling agent: 0.5-2 parts, and deionized water: 50-70 parts.

[0007] Furthermore, the nano-silica sol has a particle size of 10-30 nm and a solid content of 20%-30%.

[0008] A method for preparing a low-cost, high-strength meta-aramid paper honeycomb core material, the method comprising: S1: Prepare an inorganic-organic composite coating solution and coat it evenly on the surface of meta-aramid paper; S2: Pre-curing and drying; S3: Apply adhesive; S4: Lamination and curing; S5: Cutting, stretching and shaping; S6: Impregnation and curing yield meta-aramid paper honeycomb core material.

[0009] Further, S2: Specifically includes: treating the coated aramid paper in an oven at 80-120°C for 1-3 minutes to pre-cur and dry the coating, forming a slightly rough, highly active surface layer.

[0010] Furthermore, S3 specifically refers to: Dilute the adhesive to a certain viscosity and apply it to the meta-aramid paper according to the specifications of the honeycomb core material. The width of the adhesive strip is 2mm to 4mm.

[0011] Furthermore, S4 specifically refers to: Meta-aramid fibers are laminated using a staggered lamination method and pressed under certain temperature and pressure to cure the adhesive strips and form strong nodes, thus producing bare honeycomb.

[0012] Furthermore, phenolic resin adhesive is used for impregnation in S6.

[0013] Furthermore, the solid content of the phenolic resin solution is 50%-60%, and the viscosity is 300-600 mPa·s.

[0014] Furthermore, in S6, the curing parameters are: the honeycomb curing temperature is 120℃ / 1h + 150℃ / 2h + 180℃ / 3h.

[0015] Beneficial effects: This invention employs a special "inorganic-organic composite coating" to pretreat low-cost meta-aramid paper, which significantly reduces raw material costs while ensuring that the honeycomb core material has excellent and stable mechanical properties, thus promoting its large-scale application in the industrial field.

[0016] (1) Significant cost advantage: The core of this invention is to use low-cost meta-aramid paper with high chopped fiber content and common low-cost phenolic resin. The raw material cost can be reduced by 20%-30% compared with the scheme of using imported high-specification aramid paper.

[0017] (2) Innovative interface enhancement technology: Aramid paper is pretreated using a unique "inorganic-organic composite coating". Among them, nano-silica particles form a rough structure at the micro-nano scale on the paper surface, which physically anchors the resin; silane coupling agent and water-soluble phenolic resin act as bridges, on the one hand combining with a small number of polar groups on the surface of aramid paper fibers, and on the other hand chemically cross-linking with the subsequently impregnated phenolic resin, forming a strong and tough interface transition zone of "fiber-pretreatment layer-resin", which fundamentally solves the problem of poor wettability of low-cost aramid paper.

[0018] (3) Excellent comprehensive performance: Thanks to the excellent interface bonding, the honeycomb core material prepared by this invention has high node strength and mechanical properties (planar compression and shear strength) that not only far exceed those of untreated low-cost honeycomb, but can even reach or approach the level of traditional high-cost solutions. Moreover, the performance dispersion coefficient is small and the product consistency is good.

[0019] (4) Strong process feasibility: The pretreatment process is simple and easy to integrate and implement on existing cellular production lines. It does not require expensive equipment and is suitable for large-scale industrial production. Detailed Implementation

[0020] To meet the corresponding mechanical performance requirements, the minimum density of aramid paper honeycomb used in aircraft is currently 48 kg / m3, which is not conducive to further weight reduction of aircraft.

[0021] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a low-cost, high-strength meta-aramid paper honeycomb core material and its preparation method. By pretreating the low-cost aramid paper with a special inorganic-organic composite coating, the interfacial bonding between the aramid paper and the resin is greatly improved, thereby significantly reducing raw material costs while ensuring the honeycomb core material possesses excellent and stable mechanical properties.

[0022] The present invention provides a low-cost, high-strength meta-aramid paper honeycomb core material. The aramid paper is surface pretreated with an inorganic-organic composite coating solution. The inorganic-organic composite coating solution, by mass parts, includes: water-soluble phenolic resin: 20-40 parts, nano-silica sol: 5-15 parts, silane coupling agent: 0.5-2 parts, and deionized water: 50-70 parts.

[0023] In one possible embodiment, the nano-silica sol has a particle size of 10-30 nm and a solid content of 20%-30%.

[0024] A method for preparing a low-cost, high-strength meta-aramid paper honeycomb core material includes: Step 1, Pretreatment of aramid paper: Prepare an inorganic-organic composite coating solution and coat it evenly on the surface of meta-aramid paper.

[0025] Step 2, Pre-curing and drying: The coated aramid paper is treated in an oven at 80-120℃ for 1-3 minutes to pre-cur and dry the coating, forming a slightly rough, highly active surface layer.

[0026] Step 3: Applying adhesive: Before applying adhesive, the adhesive solution needs to be diluted to a certain viscosity. According to the specifications of the honeycomb core material, apply adhesive to the composite paper base. The width of the adhesive strip is 2mm to 4mm.

[0027] Step four, lamination and curing: The honeycomb laminates are laminated using a staggered lamination method and pressed under certain temperature and pressure to cure the adhesive strips and form strong nodes, thus producing bare honeycomb. The hot pressing process of the laminates adopts a gradient temperature hot pressing process, with a hot pressing temperature range of 130-150℃ and a pressure of 5-15 MPa.

[0028] Step 5, slitting, stretching and shaping: According to the specifications of the honeycomb core material, a paper cutter is used to cut it to the required height. Then, it is stretched under the set stretching process conditions. After the grid size meets the requirements, it is fixed on the tooling for honeycomb shaping.

[0029] Step Six, Impregnation and Curing: The pretreated aramid paper honeycomb is impregnated in a low-cost phenolic resin solution using an impregnation machine. The technical specifications of the low-cost phenolic resin solution are: solid content 50%-60%, viscosity 300-600 mPa•s (25℃), and good water dilution. The honeycomb is then cured in a high-temperature oven with stepped temperature increases (honeycomb curing temperature is 120℃ / 1h + 150℃ / 2h + 180℃ / 3h) to finally obtain the low-cost, high-strength meta-aramid paper honeycomb core material.

[0030] Example 1: Step 1: Pretreatment of Aramid Paper: Domestic meta-aramid paper with a basis weight of 80 g / m² and a short-cut fiber content of approximately 60% was selected. Preparation of the composite coating solution: 30 parts water-soluble phenolic resin, 10 parts nano-silica sol (25nm, 25%), 1 part KH-550 silane coupling agent, and 59 parts deionized water were mixed and stirred at high speed for 30 minutes. Using a microgravure coating method, the above solution was uniformly coated onto the surface of the aramid paper, with the coating amount controlled at 5±1 g / m² (dry weight).

[0031] Step 2: Pre-curing and drying: Dry the coated aramid paper at 110°C for 2 minutes.

[0032] Step 3: Applying and curing the adhesive. Step 4: Impregnation and Curing: Using a common phenolic resin solution with a solid content of 55% and a viscosity of 450 mPa•s, the impregnation speed is controlled to ensure that the final resin content of the honeycomb (including the pretreatment layer) is 40±3%. After impregnation, a stepped post-curing process is performed (120℃ / 1h + 150℃ / 2h + 180℃ / 3h) to obtain an aramid paper honeycomb core material with a density of 48kg / m³.

[0033] Example 2: Step 1: Pretreatment of Aramid Paper: Domestic meta-aramid paper with a basis weight of 80 g / m² and a short-cut fiber content of approximately 60% was selected. Preparation of the composite coating solution: 30 parts water-soluble phenolic resin, 10 parts nano-silica sol (25 nm, 25%), 1 part KH-550 silane coupling agent, and 59 parts deionized water were mixed and stirred at high speed for 30 minutes. The above solution was uniformly coated onto the surface of the aramid paper using a microgravure coating method, with the coating amount controlled at 5 ± 1 g / m² (dry weight).

[0034] Step 2: Pre-curing and drying: Dry the coated aramid paper at 110°C for 2 minutes.

[0035] Step 3: Applying adhesive layers and curing Step 4: Impregnation and Curing: Using a common phenolic resin solution with a solid content of 55% and a viscosity of 450 mPa•s, the impregnation speed is controlled to ensure that the final resin content of the honeycomb (including the pretreatment layer) is 55±5%. After impregnation, a stepped post-curing process is performed (120℃ / 1h + 150℃ / 2h + 180℃ / 3h) to obtain an aramid paper honeycomb core material with a density of 64kg / m³.

[0036] Comparative example: Using the same low-cost aramid paper and phenolic resin as in Example 1, but skipping the pretreatment steps 1 and 2, and directly proceeding to steps 3 and 4, an aramid paper honeycomb core material with a density of 48 kg / m³ was obtained.

[0037] Performance testing: The performance of the honeycomb core materials obtained in the above embodiments and comparative examples was tested, and the results are shown in the table below: Table 1 Mechanical and dielectric properties of honeycomb core materials

[0038] Test results show that the honeycomb core material prepared by this invention has significantly better key mechanical properties (compressive strength and shear strength) than untreated aramid paper honeycomb at the same density, fully demonstrating the technical advantages of this invention.

[0039] The above detailed embodiments are a description of the present invention. It should not be considered that the specific embodiments of the present invention are limited to these descriptions. For those skilled in the art, several simple deductions and substitutions can be made without departing from the concept of the present invention, and all of these should be considered to fall within the protection scope of the present invention.

Claims

1. A low-cost, high-strength meta-aramid paper honeycomb core material, characterized in that, The aramid paper of the meta-aramid paper honeycomb core material is surface pretreated with an inorganic-organic composite coating solution. The inorganic-organic composite coating solution, by mass parts, includes: water-soluble phenolic resin: 20-40 parts, nano-silica sol: 5-15 parts, silane coupling agent: 0.5-2 parts, and deionized water: 50-70 parts.

2. The low-cost, high-strength meta-aramid paper honeycomb core material according to claim 1, characterized in that, The particle size of the nano silica sol is 10-30 nm, and the solid content is 20%-30%.

3. A method for preparing a low-cost, high-strength meta-aramid paper honeycomb core material, characterized in that, The method for preparing the low-cost, high-strength meta-aramid paper honeycomb core material according to claim 1 or 2 includes: S1: Prepare an inorganic-organic composite coating solution and coat it evenly on the surface of meta-aramid paper; S2: Pre-curing and drying; S3: Apply adhesive; S4: Lamination and curing; S5: Cutting, stretching and shaping; S6: Impregnation and curing yield meta-aramid paper honeycomb core material.

4. The preparation method according to claim 3, characterized in that, S2: Specifically, the coated aramid paper is treated in an oven at 80-120℃ for 1-3 minutes to pre-cur and dry the coating, forming a slightly rough, highly active surface layer.

5. The preparation method according to claim 3, characterized in that, S3, specifically: Dilute the adhesive to a certain viscosity and apply it to the meta-aramid paper according to the specifications of the honeycomb core material. The width of the adhesive strip is 2mm to 4mm.

6. The preparation method according to claim 3, characterized in that, S4, specifically: Meta-aramid fibers are laminated using a staggered lamination method and pressed under certain temperature and pressure to cure the adhesive strips and form strong nodes, thus producing bare honeycomb.

7. The preparation method according to claim 3, characterized in that, The S6 is impregnated with phenolic resin solution.

8. The preparation method according to claim 7, characterized in that, The solid content of the phenolic resin solution is 50%-60%, and the viscosity is 300-600 mPa·s.

9. The preparation method according to claim 3, characterized in that, In S6, the curing parameters are: the honeycomb curing temperature is 120℃ / 1h + 150℃ / 2h + 180℃ / 3h.