A molded inductor with partial inter-turn adhesive filling and its manufacturing method

By applying insulating adhesive locally to the outer circumference of a multi-turn coil to form an insulating filler, the problem of magnetic powder entering the gaps between coil turns is solved, the risk of interlayer short circuits is reduced, and the withstand voltage performance and molding yield of inductor products are improved.

CN123072928APending Publication Date: 2026-11-10ZHEJIANG CIDA ELECTRONIC TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611157588.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-31
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively prevent magnetic powder from entering the gaps between coil turns, especially on the outer circumference of the coil and in the lead transition area, while maintaining the particle size distribution, pressing density, and electrical performance of the magnetic powder. This results in a high risk of interlayer short circuits.

Method used

A fluid insulating adhesive is applied locally to the outer circumference of a multi-turn coil to form an insulating filler, which seals the path of magnetic powder entry. The adhesive is then cured before the magnetic powder is pressed to form an insulating filler to prevent magnetic powder from entering the inter-turn gap.

Benefits of technology

It significantly reduces the risk of inter-turn short circuits, improves the product's withstand voltage performance and molding yield, maintains inductance, DC resistance and saturation characteristics, and is low in cost, making it suitable for high inductance and multi-turn inductor products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123072928A_ABST
    Figure CN123072928A_ABST
Patent Text Reader

Abstract

This invention relates to the technical field of inductor fabrication, specifically to an integrally molded inductor with localized inter-turn filling and its manufacturing method. The method involves winding wires to form a multi-turn coil, creating inter-turn gaps between adjacent turns. Insulating adhesive is applied locally from the outer circumference of the multi-turn coil towards the corresponding inter-turn gap and then cured, forming an insulating filler between adjacent turns. This insulating filler extends from the outer circumference of the multi-turn coil into the inter-turn gap and covers the outer opening area. The multi-turn coil with the insulating filler is placed in a molding die, and magnetic powder is filled into the die. The magnetic powder is then pressed to form a magnetically pressed body covering the multi-turn coil. This invention's integrally molded inductor manufacturing process, which involves localized filling of transition areas, seals the magnetic powder entry path, reducing the probability of magnetic powder puncturing the insulation layer and causing interlayer short circuits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of inductor fabrication, specifically to an integrally molded inductor with partial inter-turn adhesive filling and its manufacturing method. Background Technology

[0002] Inductors, as one of the three major passive electronic components in electronic product circuit boards, are widely used in communications, industrial equipment, automobiles, new energy, and the Internet of Things (IoT). With rapid market changes and the large-scale construction of related industries such as IoT and smart cities, the inductor market is growing rapidly, and the market's quality requirements for inductors are becoming increasingly stringent. Molded inductors typically consist of a coil, terminals, and a magnetically pressed body covering the coil. During manufacturing, the wound coil is placed in a mold, filled with magnetic powder, and then pressed. Due to gaps between adjacent turns, magnetic powder particles may enter between the turns during powder filling and pressing. When large-diameter or angular magnetic powder particles are subjected to molding pressure, they can easily pierce the insulation layer of the enameled wire, forming a conductive path between the coil conductor, magnetic powder, and coil conductor between adjacent turns, causing interlayer short circuits. This problem is particularly pronounced in high-inductance inductors with a large number of turns, easily leading to a decrease in withstand voltage, abnormal electrical performance, non-converging test waveforms, and product scrap.

[0003] Publication No. CN1343996A discloses an inductor and a method for manufacturing an inductor, which involves pre-coating the surface of a metal wire with hot-melt resin, bonding adjacent turns by heating after winding, and then encapsulating the coil with a resin material containing magnetic powder. This method can maintain the coil shape and improve inter-turn insulation, but the resin is formed on the entire surface of the conductor, making it difficult to locally control the outer circumference of the coil and the lead transition area where magnetic powder can easily enter.

[0004] Publication No. CN112201463A discloses a method for preparing a molded inductor and the molded inductor itself. The method involves spraying a coating agent onto the surface of the coil and lead frame, followed by curing and then magnetic powder encapsulation to improve the coil's resistance to magnetic powder penetration. This approach is similar to addressing short-circuit problems in this field, but it primarily involves forming a coating layer across the entire coil surface. When the coating amount is small, the coating agent may not fully penetrate the gaps between turns; when the coating amount is large, it may increase the space occupied by non-magnetic materials, affecting the filling of magnetic powder and electrical performance.

[0005] Announcement No. CN109166717A describes a method for molding integral inductors, employing a staged molding process combining pre-pressing, heating, and hot-pressing curing to reduce the risk of coil deformation and magnetic powder puncturing the insulation layer. However, this method primarily controls the pressing pressure and the state of the binder, and cannot directly prevent magnetic powder particles from entering the gaps between coil layers; excessively reducing the molding pressure may also affect the density, strength, and magnetic properties of the magnetically pressed body.

[0006] In addition, existing technologies include reducing the particle size of magnetic powder, increasing the thickness of the magnetic powder insulation coating, increasing the thickness of the enameled wire insulation layer, and setting a protective sleeve outside the coil. However, reducing the particle size of magnetic powder may reduce the permeability, and increasing the insulation layer or protective structure will occupy magnetic circuit space, reduce the effective filling rate of magnetic materials, and increase manufacturing costs.

[0007] Therefore, existing technologies still struggle to effectively prevent magnetic powder from entering the gaps between coil turns while maintaining the original magnetic powder particle size distribution, pressing density, and electrical properties. Magnetic powder intrusion channels are particularly prone to form on the outer circumference of the coil and in the lead transition area. Summary of the Invention

[0008] Therefore, the purpose of this invention is to provide an integrally molded inductor with partial inter-turn filling and its manufacturing method. The manufacturing process of the integrally molded inductor with partial filling treatment of the transition area can block the magnetic powder entry path and reduce the probability of magnetic powder puncturing the insulation layer and inter-layer short circuit.

[0009] To achieve the above objectives, the present invention provides the following technical solution:

[0010] A method for manufacturing an integrally molded inductor with partial inter-turn adhesive filling includes the following steps:

[0011] S1. Coil preparation: A wire with an insulating layer is wound to form a multi-turn coil, and an inter-turn gap is formed between adjacent turns of the multi-turn coil, and at least part of the inter-turn gap forms an outer opening area on the outer circle side of the multi-turn coil;

[0012] S2, Local application of adhesive: Apply a fluid insulating adhesive from the outer circle side of the multi-turn coil to at least part of the outer opening area, so that the insulating adhesive enters the corresponding inter-turn gap through the outer opening area, and at least part of the inner circle side of the multi-turn coil remains uncoated.

[0013] S3. Adhesive curing: The insulating adhesive that enters the inter-turn gap is cured so that the cured insulating adhesive forms an insulating filling part between adjacent turns. The insulating filling part extends from the outer circle side of the multi-turn coil into the interior of the inter-turn gap and covers the outer opening area.

[0014] S4. Magnetic powder pressing: The multi-turn coil with the insulating filling part is placed in the molding mold, magnetic powder is filled into the molding mold, and the magnetic powder is pressed to form a magnetic pressed body covering the multi-turn coil.

[0015] The invention is further configured such that: the outer opening area is jointly defined by the outer peripheral arc surface of two adjacent turns of wire toward the outer circle side of the multi-turn coil; the insulating filling portion at least fills the magnetic powder jamming area surrounded by the outer peripheral arc surface, so as to prevent magnetic powder from entering the inter-turn gap from the outer circle side of the multi-turn coil.

[0016] The present invention is further configured such that: step S2 is performed while maintaining the inter-turn spacing after step S1 is completed, and the multi-turn coil is not subjected to axial stretching or radial expansion during the application of the insulating adhesive.

[0017] The present invention is further configured such that: the multi-turn coil has leads; step S1 further includes welding the leads to the terminal frame; step S2 is performed after the leads are welded to the terminal frame; and the area where the insulating adhesive is applied also includes a transition gap between the leads and the coil body of the multi-turn coil, so that the insulating adhesive entering the transition gap is cured in step S3 to form a lead insulation filling part.

[0018] The present invention is further configured such that step S2 includes moving the dispensing head relative to the multi-turn coil along the outer circumference of the multi-turn coil to form a continuous or intermittent dispensing trajectory on the multiple outer opening areas, and causing the insulating adhesive to flow from the outer opening areas into the inter-turn gap under its own gravity and / or inter-turn capillary action.

[0019] The present invention is further configured such that: the viscosity of the insulating adhesive used in step S2 is not greater than 50 mPa·s at a test rotation speed of 50 rpm, and the mass of the insulating adhesive applied to each multi-turn coil is 4.0 to 7.0 mg.

[0020] The present invention is further configured such that: in a radial section including the central axis of the multi-turn coil, the coverage depth A of the insulating filling portion extending from the outer circular contour of the multi-turn coil into the interior of the inter-turn gap is not less than 60 μm, and the maximum protrusion thickness B of the insulating filling portion beyond the outer circular contour of the multi-turn coil is not greater than 20 μm.

[0021] Wherein, the coverage depth A is the distance from the outer circular contour of the multi-turn coil radially inward to the inner boundary of the insulating filling portion, and the maximum protrusion thickness B is the maximum distance by which the insulating filling portion extends radially beyond the outer circular contour of the multi-turn coil.

[0022] An integrally molded inductor with partial inter-turn filling includes a multi-turn coil, a terminal frame connected to the leads of the multi-turn coil, and a magnetic pressing body covering the multi-turn coil. Inter-turn gaps are formed between adjacent turns of the multi-turn coil, and at least a portion of the inter-turn gaps form an outer opening region on the outer circumference side of the multi-turn coil.

[0023] An insulating filling part formed by cured insulating adhesive is provided in the outer opening area. The insulating filling part extends from the outer circle side of the multi-turn coil into the inside of the inter-turn gap and crosses the corresponding adjacent turns to prevent the magnetic powder in the magnetic pressing body from entering the inter-turn gap.

[0024] The inner circular side of the multi-turn coil has an uncoated area that is not covered by the cured insulating adhesive and is in direct contact with the magnetic pressing body.

[0025] The present invention is further configured such that: a transition gap is formed between the lead wire and the coil body of the multi-turn coil, and a lead wire insulation filling part formed by the cured insulating adhesive is provided in the transition gap, and the lead wire insulation filling part is continuously connected to at least one insulation filling part located in the outer opening area.

[0026] The present invention is further configured such that: in a radial section including the central axis of the multi-turn coil, the coverage depth A of the insulating filling portion extending from the outer circular contour of the multi-turn coil into the interior of the inter-turn gap is not less than 60 μm, and the maximum protrusion thickness B of the insulating filling portion beyond the outer circular contour of the multi-turn coil is not greater than 20 μm.

[0027] Wherein, the coverage depth A is the distance from the outer circular contour of the multi-turn coil radially inward to the inner boundary of the insulating filling portion, and the maximum protrusion thickness B is the maximum distance by which the insulating filling portion extends radially beyond the outer circular contour of the multi-turn coil.

[0028] Compared with the shortcomings of the prior art, the beneficial effects of the present invention are as follows:

[0029] This invention creates a localized insulating filling structure at locations between coil turns susceptible to magnetic powder intrusion. This effectively prevents magnetic powder particles from entering the turns and piercing the wire insulation layer during the pressing process, thus significantly reducing the risk of inter-turn short circuits in integrally molded inductors. Simultaneously, this localized filling method has minimal impact on the magnetic powder filling space and the overall magnetic circuit of the coil. It improves the product's withstand voltage performance, molding yield, and long-term reliability while essentially maintaining inductance, DC resistance, saturation characteristics, and equivalent series resistance. Furthermore, it requires minimal process modifications and has low implementation costs, making it suitable for integrally molded inductor products with high inductance, multiple turns, and high reliability requirements. Attached Figure Description

[0030] Figure 1 This is a process flow diagram of the present invention;

[0031] Figure 2A and Figure 2B The images show the product without adhesive and the product after adhesive application, respectively.

[0032] Figure 3AThis is a perspective view of the product after adhesive application according to the present invention;

[0033] Figure 3B This is a top view of the product after adhesive application according to the present invention;

[0034] Figure 4 A schematic diagram illustrating the determination of the insulation filling coverage depth A and the maximum protrusion thickness B, and their impact on performance. Detailed Implementation

[0035] Reference Figures 1 to 4 The embodiments of the present invention will be further described below.

[0036] Example 1: This example provides a method for manufacturing an integrally molded inductor with partial inter-turn filling. This method addresses the problem of magnetic powder entering between adjacent turns during the molding process of the integrally molded inductor and piercing the conductor insulation layer under the pressing load. Before magnetic powder molding, insulating adhesive is applied locally from the outer circumference of the multi-turn coil towards the inter-turn opening area, allowing the insulating adhesive to enter the inter-turn area where magnetic powder is easily stuck. After curing, an insulating filling part is formed, followed by magnetic powder filling and molding.

[0037] In this embodiment, the multi-turn coil has a central axis. The side of the coil away from the central axis is the outer circle side, and the side of the coil facing the central axis is the inner circle side. An inter-turn gap is formed between the outer circumferential arc surfaces of adjacent turns facing the outer circle side of the coil, which is recessed into the coil. The inter-turn gap forms an outer opening area on the outer circle side of the coil that communicates with the outside.

[0038] Within a radial section containing the central axis of the multi-turn coil, the outermost contours of each turn of wire facing outward from the coil collectively form the outer circular contour of the coil. A recessed space is formed between the outer circumferential arc surface of two adjacent turns of wire and the outer circular contour. This recessed space is a magnetic powder jamming area where magnetic powder particles can easily enter and be clamped by adjacent turns during the powder filling and pressing process.

[0039] The manufacturing method of this embodiment includes the following steps.

[0040] S1. Coil preparation: Select a wire with an electrically insulating layer on its outer surface, and wind the wire into a multi-turn coil that extends spirally along the central axis according to the design requirements of the inductor to be manufactured.

[0041] This embodiment uses enameled copper wire with a circular cross-section. The wire diameter, insulation thickness, number of turns, inner diameter of the coil, outer diameter of the coil, and axial height of the coil are determined based on the inductance, DC resistance, and size specifications of the integrally molded inductor to be manufactured.

[0042] During the winding process, each turn of wire is arranged sequentially along the coil axis. Because the outer circumferential surface of the wire is arc-shaped, even if adjacent turns are close to each other or in partial contact, an outer opening area that gradually narrows from the outside to the inside will still be formed between their outer circumferential arc surfaces facing the outer circle of the coil.

[0043] The outer opening area is connected to the inter-turn gap between adjacent turns. During the subsequent powder filling process, magnetic powder particles can enter the inter-turn gap through this outer opening area; when the magnetic powder particles entering the inter-turn gap are large in size, irregular in shape, or have sharp edges, the magnetic powder particles are prone to getting stuck between adjacent turns and forming local concentrated pressure on the conductor insulation layer under the action of compression load.

[0044] After the multi-turn coil is wound, the two ends of the conductor extend outward from the coil body to form leads. The two leads are respectively placed at the corresponding connection positions of the terminal frame, and the leads are fixedly connected to the terminal frame by welding, so that the leads and the terminal frame are mechanically and electrically connected.

[0045] In this embodiment, localized adhesive is applied after the lead wire and terminal frame are soldered together. By completing the soldering before applying the adhesive, damage to the already formed insulation filling structure can be avoided due to the high temperature, pressure, or position adjustment during the soldering process.

[0046] After the leads are connected to the terminal frame, the multi-turn coil retains its natural shape and original inter-turn spacing after winding. During subsequent adhesive application, no axial stretching, radial expansion, or other shaping operations are performed on the multi-turn coil to actively increase the inter-turn spacing.

[0047] By maintaining the natural winding state of the coil, fluctuations in the coil's outer diameter, axial height, turn pitch, or inductance can be avoided due to increased inter-turn spacing and subsequent coil reset. At the same time, it eliminates the need to add a dedicated mechanism for stretching and resetting the coil in the coil assembly.

[0048] The lead wire extends from the coil body towards the terminal frame, creating a transition gap between the lead wire and the coil body. The width and shape of the transition gap are usually uneven, and magnetic powder particles may be trapped during subsequent powder filling and pressing processes. Therefore, in this embodiment, the outer opening area on the outer circumference of the coil is used as the main adhesive application area, and the transition gap between the lead wire and the coil body is used as an additional adhesive application area.

[0049] S2. Localized Glue Application: Place the coil assembly with completed lead soldering into the glue dispensing positioning fixture. The glue dispensing positioning fixture supports and positions the terminal frame to limit the movement of the coil assembly during the glue application process, but does not apply a force to the multi-turn coil that changes its natural turn pitch.

[0050] This embodiment uses a peristaltic dispensing machine to apply insulating adhesive to the coil assembly. Specifically, a YTT-MT-410 peristaltic dispensing machine is used, equipped with a dispensing tube with an orifice diameter of 0.8mm. The equipment model is only used as a specific example in this embodiment; other dispensing equipment capable of stably controlling the dispensing volume and application trajectory can also be used to implement this invention.

[0051] This embodiment uses COT011 type insulating adhesive. Before curing, the insulating adhesive has a low viscosity, not exceeding 50 mPa·s at a test rotation speed of 50 rpm. Before curing, this insulating adhesive can wet the surface of the insulation layer of the enameled wire and can enter the inter-turn gap along the outer circumferential arc surface of adjacent turns; after curing, it can form an insulating filling structure with electrical insulation and heat resistance properties.

[0052] COT011 type insulating adhesive is only one specific adhesive material used in this embodiment. This invention does not limit the use of this model. As long as the insulating adhesive can enter the magnetic powder stuck area on the outer circle side of the coil before curing and withstand the subsequent magnetic powder hot pressing molding process after curing, it can be used to implement this invention.

[0053] When applying adhesive, position the dispensing head above or diagonally above the outer circumference of the multi-turn coil, so that the dispensing nozzle faces multiple outer opening areas, and allow the dispensing head and the multi-turn coil to move relative to each other along the coil axis.

[0054] This embodiment employs a glue application method that uses a fixed coil assembly and a movable dispensing head. The dispensing head performs a scribing dispensing along the outer circumference of the multi-turn coil, causing the insulating adhesive output from the dispensing head to form a glue application trajectory that sequentially passes through multiple outer opening areas.

[0055] The single-stroke stroke of the dispensing head is 5.7 mm, the moving speed of the dispensing head relative to the coil assembly is 3 mm / s, and the dispensing time for a single coil is 1.9 s. Under these dispensing conditions, the insulating adhesive forms a continuous line along the outer circumference of the coil, covering a predetermined number of outer opening areas.

[0056] The mass of insulating adhesive applied to each multi-turn coil is controlled at 5.5 ± 1.5 mg, meaning the mass of insulating adhesive applied to a single coil is 4.0–7.0 mg. The adhesive application mass includes the insulating adhesive applied to the inter-turn positions on the outer circumference of the coil, as well as the insulating adhesive applied to the transition gap between the leads and the coil body.

[0057] Before the actual dispensing, the dispensing equipment can be calibrated by timed dispensing and weighing. Specifically, perform multiple dispensing operations at the same dispensing time and dispensing level, weigh the total mass of the dispensing operations, and calculate the average mass of each dispensing operation. Then, adjust the dispensing time, dispensing head movement speed, or equipment dispensing level based on the calculation results to ensure that the actual dispensing mass of a single coil is stabilized within the range of 4.0 to 7.0 mg.

[0058] After the insulating adhesive is dispensed from the dispensing head and contacts the outer circumference of the multi-turn coil, it first adheres to the outer circumferential arc surface of the adjacent turns facing the outer circumference. Due to the fluidity of the insulating adhesive, it flows from the outer opening area into the gap between the turns under the influence of its own gravity, the wetting effect on the surface of the conductor insulation layer, and the capillary action generated in the narrow area between the turns.

[0059] The insulating adhesive penetrates inward along the outer circumferential arc of the adjacent turns and enters the magnetic powder stuck area enclosed by the adjacent turns, so that at least a portion of the magnetic powder stuck area is occupied by the insulating adhesive.

[0060] This embodiment does not require the insulating adhesive to completely fill the entire gap between adjacent turns, extending from the outer circle to the inner circle. The insulating adhesive only needs to enter from the outer circle and cover the area where magnetic powder particles are easily stuck, so that it can form a continuous insulating structure that prevents magnetic powder particles from entering after subsequent curing.

[0061] By controlling the viscosity of the insulating adhesive and the quality of each application, the adhesive is primarily allowed to penetrate into the inter-turn gaps, rather than accumulating excessively outside the outer contour of the coil. Simultaneously, at least a portion of the inner circle of the coil remains uncoated, allowing subsequent magnetic powder to enter the coil's inner bore and directly fill the inner circle.

[0062] For the transition gap between the lead wire and the coil body, the glue application trajectory of the dispensing head extends from the outer circle of the coil to the transition gap, or after completing the glue application on the outer circle of the coil, additional glue is applied to the transition gap.

[0063] In this embodiment, the dispensing head moves from the outer circle of the coil near the first lead, passes through multiple outer opening areas along the coil axis, and extends to a position near another lead, so that one dispensing trajectory simultaneously covers the main magnetic powder entry area on the outer circle of the coil and the transition area near the root of the lead.

[0064] For locations with relatively large transition gaps, the moving speed of the dispensing head at that location can be appropriately reduced or the local dispensing time can be extended to allow the insulating adhesive to enter the recessed space between the lead wire and the coil body.

[0065] After completing the localized adhesive application, the position and natural turn pitch of the coil assembly are kept unchanged, so that the insulating adhesive forms a stable wet distribution in the inter-turn gap and lead transition gap on the outer circle side of the coil. Then, the coil assembly is sent to the adhesive curing step.

[0066] S3. Adhesive Curing: After completing the localized adhesive application in step S2, the coil assembly is transferred to a curing device for heat curing. In this embodiment, a tunnel-type curing device is used. The coated coil assembly is placed in a curing environment at 130°C for 20 minutes to allow the insulating adhesive that has entered the inter-turn gap and lead wire transition gap to cure completely.

[0067] During the process of transferring the coil assembly from the dispensing station to the curing station, the relative position between the multi-turn coil and the terminal frame is kept unchanged to avoid collisions, flipping, or squeezing of the coil assembly, so as to reduce the loss of uncured insulating adhesive from the target application area.

[0068] During the curing process, the multi-turn coil is not subjected to axial stretching, radial expansion, or reshaping, allowing the insulating adhesive to cure under the natural turn spacing of the coil. Before curing, the insulating adhesive continues to wet the surface of the insulation layer of adjacent turns and flows into the gap between turns along the outer opening area; as the curing reaction proceeds, the fluidity of the insulating adhesive gradually decreases and it becomes fixed between adjacent turns.

[0069] After the insulating adhesive cures, an insulating filler is formed in at least a portion of the inter-turn gaps on the outer circumference of the multi-turn coil. The insulating filler is attached to the surface of the insulation layer of two adjacent turns of wire and spans between the two adjacent turns of wire, thereby closing or at least partially closing the outer opening area that was originally connected to the outside by the outer circumference of the coil.

[0070] The insulating filler extends from the outer circumference of the multi-turn coil into the inter-turn gap, and occupies at least the magnetic powder jamming area between adjacent turns. Therefore, during subsequent magnetic powder filling and pressing, the insulating filler can form a solid barrier structure along the magnetic powder entry path, reducing the probability of magnetic powder particles entering the inter-turn gap from the outer opening area.

[0071] In this embodiment, the insulating filling portion does not extend to the entire space between adjacent turns, nor does it form an integral cover over the entire surface of the multi-turn coil. At least a portion of the inner circular side of the multi-turn coil remains uncoated to allow subsequent magnetic powder to enter the coil's inner hole and directly fill the inner circular side of the coil.

[0072] When insulating adhesive is applied to the transition gap between the lead wire and the coil body in step S2, the insulating adhesive in the transition gap is simultaneously cured in this step and forms the lead wire insulation filling part.

[0073] The lead insulation filler is attached to the surface of the lead and the surface of the coil turns near the lead, and is used to seal the space between the lead root and the coil body that may contain magnetic powder particles. Preferably, the lead insulation filler is continuously connected to the insulation filler located adjacent to the outer circle side of the coil, thereby reducing the possibility that magnetic powder particles will bypass the insulation filler on the outer circle side of the coil from the lead transition area and enter the interior of the coil.

[0074] To characterize the distribution of the insulation filling portion in the radial direction of the coil, this embodiment uses the coverage depth A and the maximum protrusion thickness B for control.

[0075] Within a radial section encompassing the central axis of the multi-turn coil and passing through the position between the turns to be measured, the outer circular profile of the multi-turn coil is used as the measurement reference. The outer circular profile is the outer envelope formed by the outermost profile of the multiple turns pointing outwards from the coil.

[0076] Coverage depth A is the distance from the outer circumference of the multi-turn coil radially inward to the inner boundary of the insulation filler. Coverage depth A characterizes the extent to which the insulating adhesive penetrates from the outer circumference of the coil into the inter-turn gap.

[0077] The maximum protrusion thickness B is the maximum distance by which the insulating filler extends radially beyond the outer contour of the multi-turn coil. The maximum protrusion thickness B is used to characterize the degree of accumulation of the insulating adhesive outside the outer contour of the coil.

[0078] In this embodiment, the coverage depth A of the insulating filling part is controlled to be no less than 60 μm, and the maximum protrusion thickness B of the insulating filling part is controlled to be no more than 20 μm.

[0079] Based on the observation results of larger magnetic powder particles in the short-circuit failure sample and the geometric morphology between adjacent turns, controlling the coverage depth A to be no less than 60μm can improve the coverage of the magnetic powder stuck area by the insulation filling part and reduce the probability of larger magnetic powder particles entering between adjacent turns and being wedged.

[0080] By controlling the maximum protrusion thickness B to no more than 20μm, excessive accumulation of cured insulating adhesive on the outer circle of the coil can be limited, reducing the space occupied by non-magnetic insulating adhesive for magnetic powder filling, and reducing the risk of uneven local pressure distribution caused by the protruding adhesive during subsequent pressing.

[0081] The coverage depth A and the maximum protrusion thickness B are jointly controlled by the viscosity of the insulating adhesive, the quality of single application, the moving speed of the dispensing head, the local dispensing time, and the dispensing position of the dispensing head.

[0082] When the coverage depth A of the insulation filling part is insufficient, the amount of adhesive can be appropriately increased within the allowable range of single adhesive application quality, the dispensing head moving speed can be reduced, the dwell time of the dispensing head at the target inter-turn position can be extended, or the dispensing position can be moved closer to the recessed position of the outer opening area to increase the amount of insulating adhesive penetrating into the inter-turn gap.

[0083] When the maximum protrusion thickness B of the insulation filling part is too large, the amount of adhesive applied to a single piece can be reduced, the moving speed of the dispensing head can be increased, the dwell time of the dispensing head in a local position can be shortened, or the relative position between the dispensing head and the outer circle of the coil can be adjusted to reduce the accumulation of insulating adhesive outside the outer circle contour of the coil.

[0084] After curing, the coil assembly can be extracted for cross-sectional inspection. The coil assembly under test is cut along a radial plane containing the central axis of the coil, and the cut surfaces are inlaid, ground, and polished to expose the cross-sectional shape of adjacent turns and insulation filler.

[0085] The positional relationship between the insulation filler and adjacent turns was observed using a microscopic measuring device, and the coverage depth A and maximum protrusion thickness B were measured respectively. Measurements could be taken at multiple inter-turn locations on the outer circumference of the coil to evaluate the coverage of the insulation filler over the outer opening area and the degree of protrusion of the adhesive.

[0086] In addition to the coverage depth A and the maximum protrusion thickness B, you can also check whether the insulation filling part is connected to the corresponding adjacent turns, whether there is an unfilled channel that runs from the outer circle of the coil to the inside of the turn gap, whether the lead wire transition gap is covered by the lead wire insulation filling part, and whether there is an uncoated area on the inner circle of the coil.

[0087] S4. Magnetic Powder Pressing: After confirming that the insulating adhesive has cured, transfer the coil assembly with the insulating filling part to the magnetic powder molding station and place it into the corresponding cavity of the molding mold.

[0088] This embodiment uses a molding die with 40 molding cavities. During mold assembly, the terminal frame cooperates with the positioning structure in the molding die to position the multi-turn coil at a predetermined position in the cavity, and ensures that the part of the terminal frame that needs to form an external electrical connection is outside the molding range of the magnetic pressing body.

[0089] After the multi-turn coil is installed into the cavity, space is left for magnetic powder to be filled in its inner hole, outer circumference, and both axial ends. On the outer circumference of the coil, the cured insulation filling part remains located in the outer opening area formed by the adjacent turns.

[0090] Magnetic powder is filled into the cavity of the molding die, distributing it within the inner hole, outer circumference, and axial ends of the multi-turn coil. The magnetic powder includes metallic magnetic powder and a binder component that bonds the metallic magnetic powder together after pressing. An electrically insulating coating layer may be provided on the surface of the metallic magnetic powder.

[0091] The localized filling process of this invention does not require reducing the magnetic powder particle size or lowering the proportion of large magnetic powder particles as a necessary condition. Therefore, while meeting the requirements for inductance, saturation performance, and molding strength of the integrally molded inductor, a gradation system containing magnetic powder particles of different sizes can be used.

[0092] Because the inner circle of the multi-turn coil retains an uncoated area, the magnetic powder can enter the inner hole of the coil and directly fill the inner circle of the coil to maintain the amount of magnetic material filling in the inner hole area of ​​the coil.

[0093] On the outer circumference of the coil, magnetic powder fills the outer side of the insulating filler. Since the insulating filler has been cured before the magnetic powder filling and bridges adjacent turns and covers the outer opening area, the magnetic powder particles are blocked by the insulating filler and cannot continue to enter the inter-turn gap along the outer opening area.

[0094] After the magnetic powder is filled, the molding die is closed, and the magnetic powder is hot-pressed. In this embodiment, the molding equipment applies a total pressing force of 50T to the 40-cavity molding die, the pressing temperature is 180℃, and the holding time is 80s.

[0095] 50T refers to the total load on the equipment corresponding to a 40-cavity molding die, not the pressure or pressure per unit area borne by a single integrally molded inductor. When using different numbers of cavities, different product sizes, or different magnetic powder systems, the equipment load can be adjusted accordingly based on the projected area of ​​a single cavity, the compression characteristics of the magnetic powder, and the target molding density.

[0096] During the hot pressing process, the particles in the magnetic powder are rearranged and gradually densified. Under the action of temperature and pressure, the binder components cause the magnetic powder particles to combine with each other, forming a magnetic pressed body that covers multiple turns of coil.

[0097] For coils without insulation filling, magnetic powder particles may enter between adjacent turns from the outer opening area during the rearrangement process and become stuck in the inter-turn gap under compression load. In this embodiment, the cured insulation filling occupies the main magnetic powder stuck area, so that the magnetic powder particles first contact the insulation filling when moving towards the inter-turn gap, thereby reducing the probability of magnetic powder particles directly wedging into the inter-turn gap.

[0098] The insulating filler adheres to the surface of the insulation layer of adjacent turns, forming a continuous colloidal structure between adjacent turns. When the magnetic powder particles are subjected to a compressive load and act on the insulating filler, the insulating filler can expand the stress area between the magnetic powder particles and the coil, reducing the local stress concentration caused by the sharp edges of the magnetic powder particles directly acting on the wire insulation layer.

[0099] The lead insulation filling part in the lead transition gap forms a barrier to the magnetic powder particles that enter between the lead root and the coil end, reducing the risk of magnetic powder particles getting stuck between the lead and the adjacent turn and puncturing the insulation layer.

[0100] After the pressure holding is completed, the pressure is released from the molding die, and the molded inductor blank is cooled to a temperature suitable for stable demolding. Once the magnetically pressed body has achieved sufficient structural stability, the molding die is opened, and the integrally molded inductor blank is removed from the cavity.

[0101] According to product manufacturing requirements, the molded inductor blank after demolding can be deburred, terminal shaped, surface cleaned, electrode treated, visually inspected, and its electrical performance tested.

[0102] Molded Inductor Prepared in Example 1

[0103] The integrally molded inductor produced by the above method includes a multi-turn coil, a terminal frame, a magnetic pressing body, an insulating filling part, and a lead wire insulating filling part.

[0104] The two leads of the multi-turn coil are connected to the terminal frame respectively. The magnetic pressing body covers the multi-turn coil and fills the inner hole, outer circle side and axial ends of the multi-turn coil.

[0105] At least some adjacent turns are separated by an inter-turn gap, which forms an outer opening region on the outer circumference of the coil. An insulating filler formed of cured insulating adhesive is provided within the outer opening region.

[0106] The insulating filling part extends from the outer circle of the multi-turn coil into the gap between the turns and crosses the corresponding adjacent turns to prevent magnetic powder particles in the magnetic pressing body from entering the gap between the turns.

[0107] The inner circle of the multi-turn coil has an uncoated area that is not covered by cured insulating adhesive. The magnetic powder in the magnetic pressing body directly fills the uncoated area and contacts the inner circle of the coil.

[0108] A transition gap is formed between the lead wire and the coil body, and an insulation filling portion for the lead wire is provided within the transition gap. Preferably, the insulation filling portion for the lead wire is continuously connected to at least one insulation filling portion near the position of the lead wire, thereby forming a continuous local insulation barrier structure between the outer circle side of the coil and the transition area of ​​the lead wire.

[0109] Within a radial section containing the central axis of the multi-turn coil and passing through the insulating filler, the covering depth A of the insulating filler extending from the outer contour of the coil into the interior of the inter-turn gap is not less than 60 μm, and the maximum protrusion thickness B of the insulating filler beyond the outer contour of the coil is not greater than 20 μm.

[0110] Detection methods and test results

[0111] To verify whether the insulating filling portion formed in Example 1 can stably cover the magnetic powder stuck area, and to evaluate the impact of local filling on the electrical performance, inter-turn short circuit risk and long-term reliability of the integral molded inductor, the coil assembly and integral molded inductor prepared in Example 1 were subjected to cross-sectional dimension testing, electrical performance testing, short circuit statistics and reliability verification.

[0112] After the insulating adhesive has cured and before the magnetic powder has been pressed, test samples are taken from coil assemblies of the same production batch. The test samples are cut along a radial plane that includes the central axis of the multi-turn coil and passes through the insulation filling part. The cut surfaces are then inlaid, ground, and polished to expose the cross-sectional shape of adjacent turns, inter-turn gaps, and insulation filling parts.

[0113] The distribution of the insulation filler between adjacent turns was observed using a microscopic measuring device. During measurement, the outer envelope formed by the outermost contour of each turn of wire facing outwards from the coil was used as the outer circular contour of the multi-turn coil.

[0114] The distance measured radially inward from the outer circle contour along the coil to the inner boundary of the insulation filling part is taken as the coverage depth A; the maximum distance measured radially outward from the outer circle contour along the coil to the outermost boundary of the insulation filling part is taken as the maximum protrusion thickness B.

[0115] In the same test sample, multiple inter-turn locations with insulating fillers can be selected for measurement. During testing, it is also observed whether the insulating filler bridges two adjacent turns of wire, whether it covers the outer opening area, whether there is an unfilled channel extending from the outer circle of the coil into the inter-turn gap, and whether an uncoated area remains on the inner circle of the coil.

[0116] In the sampling results of the corresponding batch in Example 1, the average coverage depth A of the insulation filling was approximately 117 μm, and the process capability index Cpk was approximately 1.87. When the coverage depth A is not less than 60 μm as the control lower limit, the existing process can stably meet the coverage depth requirement.

[0117] The average maximum protrusion thickness B of the insulation filler is approximately 1.5 μm, and the process capability index Cpk is approximately 3.71. With a maximum protrusion thickness B not exceeding 20 μm as the control limit, the existing process can stably restrict the accumulation of the colloid outside the outer contour of the coil. The average values ​​of A and B and the process capability index recorded in the supplementary material are approximately 117 μm and 1.87, and approximately 1.5 μm and 3.71, respectively.

[0118] The above test results show that by controlling the viscosity of the insulating adhesive, the quality of a single application, the marking speed, and the curing conditions, the insulating adhesive can be made to mainly penetrate between adjacent turns, rather than forming a thicker adhesive layer on the outer circle of the coil, thereby obtaining a local insulation filling structure that is fully covered inward and protrudes only slightly outward.

[0119] To evaluate the impact of the degree to which the insulation filler protrudes beyond the outer contour of the coil on the performance and appearance of the finished product, coil assemblies with maximum protrusion thicknesses B of approximately 0 μm, 10 μm, 20 μm and 30 μm were prepared by adjusting the amount and conditions of adhesive application, and were molded using the same magnetic powder, mold and pressing conditions.

[0120] When the maximum protrusion thickness B is approximately 0 μm, the rate of change of the finished product's inductance relative to the reference product is approximately 0%, and the finished product's appearance and reliability tests are both qualified.

[0121] When the maximum protrusion thickness B is about 10μm, the inductance change rate of the finished product is about -1.5%, and the appearance and reliability of the finished product are qualified.

[0122] When the maximum protrusion thickness B is approximately 20 μm, the inductance change rate of the finished product is approximately -3.7%, and the appearance and reliability of the finished product still pass the tests.

[0123] When the maximum protrusion thickness B increases to approximately 30 μm, the inductance change rate of the finished product is approximately -5.5%, and about 3% of the products exhibit surface crack defects. According to existing test records, when B reaches 30 μm, the reduction in the effective filling space of the magnetic powder caused by the external protrusion of the colloid and the uneven local stress are already quite obvious. Therefore, the maximum protrusion thickness B is controlled to be no more than 20 μm.

[0124] The reason for these changes is that the cured insulating adhesive is a non-magnetic material. When the thickness of the insulation filler protrusion on the outer circumference of the coil increases, it occupies the space originally used for filling magnetic powder, reducing the magnetic material occupancy rate in the local area on the outer circumference of the coil.

[0125] In addition, the thicker protrusion of the cured colloid can create local support positions during hot pressing, causing the pressing load of the magnetic powder to be unevenly distributed on the outside of the coil or in the area near the electrode, thereby increasing the risk of cracks in the magnetic pressing body or electrode surface.

[0126] Therefore, a maximum protrusion thickness B of no more than 20 μm is used not only to limit the amount of colloid used, but also to take into account the inter-turn magnetic powder barrier effect, magnetic material filling rate, inductance retention and pressing appearance.

[0127] The integral molded inductor prepared using the partial glue filling process of Example 1 was selected as the test group, and the integral molded inductor with the same coil specifications, magnetic powder and magnetic powder pressing conditions but without partial glue filling was selected as the control group. The inductance, DC resistance, saturation rate of change and equivalent series resistance of the two groups of products were tested.

[0128] The average inductance of the control group product was approximately 31.08 μH, while the average inductance of the product in Example 1 was approximately 30.95 μH. The difference between the two was approximately 0.4%, which is within the allowable variation range of the products.

[0129] The average DC resistance of the control group product was approximately 111.79 mΩ, and the average DC resistance of the product in Example 1 was approximately 111.66 mΩ. No significant difference was observed between the two.

[0130] The saturation change rate of the control group product was approximately -20.38%, and the saturation change rate of the product in Example 1 was approximately -20.19%, with no significant difference between the two.

[0131] The average equivalent series resistance of the control group products was approximately 2.85Ω, while the average equivalent series resistance of the product in Example 1 was approximately 2.72Ω, with a variation of approximately 4.5%, which is within the normal range.

[0132] As can be seen from the above results, the insulating adhesive in Example 1 mainly enters the powder-laden area between the turns on the outer circle side of the coil, and the maximum protrusion thickness is limited. The inner circle side of the coil still retains an uncoated area, so a thick non-magnetic coating layer will not be formed around the entire coil.

[0133] Therefore, Example 1 can essentially maintain the inductance, DC resistance, saturation characteristics, and equivalent series resistance of the integrally molded inductor while forming an inter-turn magnetic powder barrier structure. The original mapping test results also indicate that there is no significant difference in the main electrical properties between the glued and unglueed products, and minor differences are within an acceptable range.

[0134] Short-circuit defects were statistically analyzed for products before and after the application of partial adhesive filling process. Short-circuit defects can be determined using the product's current electrical performance testing or waveform testing standards. Products that do not meet the corresponding withstand voltage or waveform requirements were reviewed, and cross-sectional observation was conducted to confirm whether magnetic powder particles entered between adjacent turns and formed a "wire-powder-wire" conductive path.

[0135] According to the applicant's existing production statistical records, before the implementation of the partial glue filling improvement, the inter-turn short circuit defect was about 1900 PPM; after the implementation of the improvement, the statistical values of short circuits in different time periods were significantly reduced, and the subsequent statistical points were mainly in the range of 0 to 69.48 PPM.

[0136] Wherein, part of the data points recorded by the existing statistical curve include about 45 PPM, 69.48 PPM, 7 PPM, 13 PPM, 0 PPM, 50 PPM, 0 PPM and 22 PPM. Although the values in different production periods fluctuate, the overall short circuit defect is significantly reduced compared with about 1900 PPM before the improvement.

[0137] Combined with the cross-sectional observation of failed samples, it can be confirmed that the short circuit defect is mainly related to the magnetic powder particles entering the inter-turn region on the outer circular side of the coil and piercing the insulating layer of adjacent turns during the high-pressure molding process. The original disclosure also identifies the short circuit failure as a wire-powder-wire conduction loop formed after the magnetic powder pierces the coil.

[0138] After the partial glue filling is implemented, the cured insulating glue pre-occupies the magnetic powder trapping area between adjacent turns, and blocks the path for magnetic powder particles to enter the inter-turn gap from the outer circular side of the coil, thereby reducing the probability that larger magnetic powder particles are clamped by adjacent turns and pierce the insulating layer.

[0139] It can be known from the electrical performance test and the short circuit statistical results that this embodiment does not reduce the short circuit by integrally increasing the insulation coating thickness of the coil or reducing the particle size of the magnetic powder, but realizes the short circuit improvement by partially blocking the magnetic powder entry path while basically maintaining the original electrical performance.

[0140] The integrally formed inductor prepared in Example 1 was subjected to waveform voltage detection. 3000 samples were tested under the detection condition of 140V, all samples completed the test, and the results were qualified.

[0141] 30 samples were subjected to tin immersion heat resistance verification at 260±5℃ for 10s, and the test results were qualified. This result indicates that the insulating filling part can withstand the short-term high temperature environment that may be experienced in the subsequent terminal welding or assembly process.

[0142] 80 samples were respectively subjected to 48-hour staged environmental verification under the conditions of 35℃, 85%RH and 60℃, 95%RH, and the test results were qualified.

[0143] The above results show that after the partial insulating filling structure completes the magnetic powder pressing, it can adapt to the product production and preliminary environmental verification process, and is not prone to obvious falling off or insulation failure due to short-term high temperature or damp heat conditions.

[0144] The product prepared in Example 1 was subjected to multiple reflow verification. A single cycle includes 3 times of reflow at 265°C and one time of 140V waveform voltage detection, for a total of 3 cycles, that is, a cumulative total of 9 times of reflow was performed.

[0145] After the reflow verification, the inductance, DC resistance, saturation characteristics, series resistance and cross-sectional state of the product were inspected, and all the test results were qualified.

[0146] This result shows that after experiencing multiple high-temperature reflows, the insulating filling portion can still remain between adjacent turns of the wire, will not undergo obvious softening and loss, shedding or cracking due to repeated heating, and will not cause a significant adverse effect on the main electrical properties of the integrally formed inductor.

[0147] The integrally formed inductor prepared in Example 1 was subjected to high-temperature storage, temperature cycling, moisture resistance, biased humidity-heat, operating life and low-temperature storage verification.

[0148] A 2000 h high-temperature storage test was carried out at the maximum storage temperature specified for the product. After the test, the inductance, DC resistance, self-resonant frequency, saturation characteristics, insulation resistance and pulse performance of the product were tested, and the test results were qualified.

[0149] 3000 temperature cycles were carried out between the minimum temperature and the maximum temperature specified for the product. The dwell time of each high-temperature stage and low-temperature stage is 30 min, and the temperature transition time is less than 10 s. After the test, the inductance, DC resistance, self-resonant frequency, saturation characteristics, insulation resistance and pulse performance of the product were tested, and the test results were qualified.

[0150] A 2000 h moisture resistance test was carried out under the conditions of 85°C and 85%RH, and the test results of electrical performance, insulation performance and pulse performance after the test were qualified.

[0151] A 2000 h biased humidity-heat test was carried out under the conditions of 85°C, 85%RH and rated current, and the appearance test result of the product after the test was qualified.

[0152] A 2000 h operating life test was carried out under the operating temperature and rated current conditions specified for the product, and the appearance test result of the product after the test was qualified.

[0153] A 2000 h low-temperature storage test was carried out under the minimum operating temperature condition specified for the product, and the appearance test result of the product after the test was qualified.

[0154] The above long-term reliability results show that the insulating filling portion can withstand the thermal stress and environmental stress generated during the storage, temperature change, humidity-heat and long-term energized use of the integrally formed inductor, and no obvious colloidal shedding, inter-turn insulation failure or abnormal product appearance is observed.

[0155] The cross-sectional test of Example 1 shows that the insulation filling part can form a stable local filling structure between adjacent turns, with an average coverage depth A of about 117 μm and an average maximum protrusion thickness B of about 1.5 μm, which can meet the control requirements of A not less than 60 μm and B not greater than 20 μm, respectively.

[0156] The comparison of electrical properties before and after dispensing shows that after using the local filling process in this embodiment, the inductance, DC resistance, saturation characteristics and equivalent series resistance of the product did not undergo significant adverse changes.

[0157] Short-circuit statistics show that the short-circuit PPM of the product significantly decreased after partial adhesive filling compared to before the improvement. The original technical specifications also clearly state that the short-circuit PPM decreased significantly before and after adhesive application, and that the product's withstand voltage performance could be improved at the same electrical performance level.

[0158] Maximum protrusion thickness verification shows that more colloid is not necessarily better. When B reaches about 30μm, the product inductance decreases more significantly and surface cracks appear; when B is controlled to be no more than 20μm, the inter-turn sealing effect, magnetic powder filling and molding appearance can be balanced.

[0159] Therefore, Example 1, through the process sequence of "partial application of adhesive from the outer circumference of the coil—adhesive entering the powder-trapping area between turns—forming an insulating filling part after curing—and then magnetic powder pressing," and through the coordinated control of viscosity, adhesive application quality, coverage depth A, and maximum protrusion thickness B, achieved the following effects:

[0160] Without completely covering the multi-turn coil, the main path for magnetic powder to enter between turns is sealed off; a space for magnetic powder to fill is retained on the inner circle side of the coil; the probability of large magnetic powder particles piercing the insulation layer of the conductor and forming a short circuit between turns is reduced; at the same time, the electrical performance, appearance and long-term reliability of the integrally molded inductor are basically maintained.

[0161] Example 1 continues to use the preferred production process that has been fully described above, that is, a peristaltic dispensing machine is used to apply adhesive locally on the outer circle side of the coil. The adhesive mass of a single coil is 5.5±1.5mg. The viscosity of the insulating adhesive solution under the test condition of 50rpm is not greater than 50mPa·s. After application, it is cured at 130℃ for 20min. Then, a 40-cavity mold is used for magnetic powder hot pressing. The total pressing force of the equipment is 50T, the pressing temperature is 180℃, and the holding time is 80s.

[0162] Cross-sectional testing was performed on the coil assembly cured in Example 1. The average coverage depth A of the insulation filling part was about 117 μm, and the average maximum protrusion thickness B was about 1.5 μm. The corresponding process capability indices Cpk were about 1.87 and 3.71, respectively, which can meet the process requirements of A not less than 60 μm and B not greater than 20 μm.

[0163] This embodiment is a preferred embodiment of this application and is used to fully illustrate the manufacturing process, dimensional control method, electrical performance, and reliability results of the present invention.

[0164] Example 2 was used to verify the product performance when the maximum protrusion thickness B of the insulating filler was approximately 10 μm. Except for the maximum protrusion thickness B explicitly stated in this example, the coil structure, insulating adhesive, application location, adhesive curing conditions, magnetic powder, and molding conditions were the same as in Example 1, and will not be repeated here.

[0165] In this embodiment, by appropriately increasing the amount of insulating adhesive applied, reducing the dispensing head moving speed, or extending the local dispensing time at the target position compared to Embodiment 1, the maximum protrusion thickness B of the insulating filling part formed after the insulating adhesive has cured beyond the outer circle contour of the coil is approximately 10 μm.

[0166] After the insulating adhesive has cured, the coil assembly is subjected to cross-sectional testing, and samples whose insulation filling has covered the outer opening area of ​​the adjacent turns are selected for subsequent magnetic powder pressing molding.

[0167] The test results show that the inductance of the product in this embodiment is reduced by about 1.5% compared with the test benchmark group where B is 0μm. The product appearance test result is qualified, and the reliability test result is qualified.

[0168] This embodiment illustrates that when the thickness of the insulating filler protruding beyond the outer contour of the coil is approximately 10 μm, although the non-magnetic colloid occupies a small amount of magnetic powder filling space, its impact on the product's inductance, molding appearance, and reliability is still within an acceptable range.

[0169] Example 3 was used to verify the product performance when the maximum protrusion thickness B of the insulating filler was approximately 20 μm. Except for the maximum protrusion thickness B explicitly stated in this example, the rest of the manufacturing process and process conditions were the same as in Example 1, and will not be repeated here.

[0170] In this embodiment, by further adjusting the amount of insulating adhesive applied and the local adhesive dispensing time, the maximum protrusion thickness B of the insulating filler portion formed after the insulating adhesive has cured is approximately 20 μm beyond the outer circle contour of the coil.

[0171] After the insulating adhesive has cured, the cross-section of the coil assembly is inspected, and samples covering the corresponding outer opening area of ​​the insulating filling part are selected for magnetic powder filling and pressing molding.

[0172] The test results show that the inductance of the product in this embodiment is reduced by about 3.7% compared with the test benchmark group where B is 0μm. The product appearance test result is qualified, and the reliability test result is qualified.

[0173] This embodiment illustrates that when the maximum protrusion thickness B reaches approximately 20 μm, the influence of the insulating filler on the effective filling space of the magnetic powder increases, but the product's inductance, pressed appearance, and reliability still meet the usage requirements. Therefore, 20 μm can be considered as the preferred upper limit for controlling the maximum protrusion thickness B.

[0174] Comparative Example 1 uses the same multi-turn coil, terminal frame, magnetic powder, and magnetic powder pressing conditions as Example 1. However, after the coil winding and lead wire welding are completed, insulating adhesive is not applied to the inter-turn opening area on the outer circumference of the coil; instead, magnetic powder is directly filled and pressed. Because the outer opening area between adjacent turns is not sealed by the insulating filling part, magnetic powder particles can enter the inter-turn gap during the powder filling and pressing process. Larger or angular magnetic powder particles, after becoming stuck between adjacent turns, may pierce the conductor insulation layer under the pressing load, forming a conductive path of coil conductor—magnetic powder particles—coil conductor. The average inductance of this comparative example product is approximately 31.08 μH, the average DC resistance is approximately 111.79 mΩ, the saturation rate of change is approximately -20.38%, and the average equivalent series resistance is approximately 2.85 Ω. Before the localized adhesive filling improvement, the short-circuit defect rate was approximately 1933 PPM. After implementing localized adhesive filling, the short-circuit defect rate decreased significantly in all production statistical stages. This indicates that localized adhesive filling primarily improved the short-circuit problem caused by magnetic powder entering between turns, rather than sacrificing product electrical performance for improvement. The original technical specifications also clearly state that the difference in electrical performance before and after localized adhesive filling was small, while the short-circuit PPM decreased significantly.

[0175] Comparative Example 2 was used to verify the effect of excessive accumulation of insulating adhesive on the outer circumference of the coil. Except for the maximum protrusion thickness B, the coil structure, insulating adhesive, adhesive curing, magnetic powder filling, and pressing conditions were the same as in Example 1. In this comparative example, by increasing the amount of insulating adhesive applied or extending the local adhesive dispensing time, the maximum protrusion thickness B of the cured insulating filling exceeding the outer circumference of the coil reached approximately 30 μm. The test results showed that the inductance of the product in this comparative example was reduced by approximately 5.5% compared to the test baseline group with B of 0 μm, and approximately 3% of the products showed electrode surface cracks. Due to the obvious appearance defects in the products, the original test data did not provide complete reliability test results for this group. This comparative example illustrates that when the maximum protrusion thickness B reaches approximately 30 μm, the excess adhesive will significantly occupy the space filled by the magnetic powder, and may also form local support points during pressing, causing uneven stress on the magnetic powder. Therefore, the maximum protrusion thickness B should not reach 30 μm.

[0176] Comparative Example 3 illustrates the effect when the insulating adhesive, although applied to the outer circumference of the coil, does not fully penetrate the magnetic powder jamming area. Except for the application location and the coverage depth A of the insulating filling portion, all other conditions are the same as in Example 1. This comparative example achieves this by reducing the amount of insulating adhesive applied, increasing the dispensing head's moving speed, or shifting the dispensing position away from the outer opening area formed by adjacent turns, so that the insulating adhesive mainly adheres to the outer circumference of the coil and does not fully penetrate the inter-turn gap. After the insulating adhesive cures, the coverage depth A of the insulating filling portion is less than 60 μm. In cross-sectional observation, unfilled channels extending from the outer circumference of the coil into the inter-turn gap can be seen in some of the outer opening areas. During subsequent magnetic powder filling and pressing processes, magnetic powder particles may still enter between adjacent turns along these unfilled channels, thus this structure cannot stably seal the magnetic powder entry path.

[0177] Table 1 compares the structural parameters and performance of Examples 1-3 and the comparative examples:

[0178]

[0179] Table 2 compares the impact of maximum protrusion thickness B on product performance:

[0180]

[0181] Table 3: Comparison of main electrical properties and short-circuit performance before and after partial adhesive filling:

[0182]

[0183] As can be seen from the comprehensive test results of Examples 1-3 and Comparative Examples 1-3 shown in Table 1, the risk of inter-turn short circuit in integral molded inductors does not depend solely on whether insulating adhesive is attached to the outer surface of the coil, but mainly on whether the insulating adhesive enters the magnetic powder stuck area between adjacent turns from the outer circle side of the multi-turn coil, and whether the cured insulating filling part can seal the entry path of magnetic powder particles without excessively occupying the magnetic powder filling space.

[0184] In Example 1, the average coverage depth A of the insulation filler is 117 μm, and the average maximum protrusion thickness B is 1.5 μm. The insulation filler can fully penetrate between adjacent turns and cover the outer opening area, while only forming a small adhesive protrusion outside the outer contour of the coil. The product of this example has an average inductance of 30.95 μH, an average DC resistance of 111.66 mΩ, a saturation rate of change of -20.19%, and an average equivalent series resistance of 2.72 Ω. Its main electrical performance is basically equivalent to that of Comparative Example 1 without local adhesive filling, while the short-circuit failure rate is reduced from 1933 PPM in Comparative Example 1 to approximately 21.66 PPM.

[0185] Therefore, it can be seen that the present invention does not reduce the short circuit rate by significantly reducing the inductance, increasing the conductor resistance, or changing the coil conductor structure. Instead, it reduces the probability that magnetic powder particles will enter the inter-turn gap and puncture the wire insulation layer during the subsequent high-voltage forming process by pre-forming a local insulation barrier structure on the path of magnetic powder entering the inter-turn gap.

[0186] The results of Examples 2 and 3 show that when the maximum protrusion thickness B of the insulation filler is approximately 10 μm and 20 μm, respectively, the inductance of the product decreases by approximately 1.5% and 3.7% compared to the baseline state where B is 0 μm, but the product appearance and reliability remain acceptable. This indicates that the insulation filler can extend beyond the outer contour of the coil to a certain extent, and its outer boundary is not required to be completely within the outer contour of the coil.

[0187] However, as the maximum protrusion thickness B increases, the space occupied by the non-magnetic insulating adhesive for the magnetic powder filling gradually increases, and the magnetic material occupancy rate in the local area on the outer circumference of the coil decreases accordingly. Therefore, the inductance of the product shows a gradual decreasing trend.

[0188] In Comparative Example 2, the maximum protrusion thickness B reached approximately 30 μm, the product inductance decreased by about 5.5%, and about 3% of the electrode surfaces showed cracks. This result indicates that when the insulating adhesive is excessively deposited on the outer circumference of the coil, it not only significantly reduces the effective filling space of the magnetic powder but may also form local support points during the magnetic powder pressing process, leading to uneven distribution of the pressing load and increasing the risk of cracks in the magnetic pressing body or the area adjacent to the electrodes.

[0189] Therefore, controlling the maximum protrusion thickness B to no more than 20μm is not an arbitrary choice based solely on product size, but rather a way to achieve a balance between the inter-turn magnetic powder barrier effect, magnetic material filling rate, inductance retention, and pressed appearance.

[0190] The results of Comparative Example 3 show that when the coverage depth A of the insulation filling is less than 60 μm, even if there is insulating adhesive on the outer circumference of the coil, the entry channel for magnetic powder particles may still be retained because the insulating adhesive does not fully enter the magnetic powder jamming area. Although the short-circuit failure rate of this group of products is lower than that of Comparative Example 1, which has no adhesive filling, it is significantly higher than that of Examples 1-3, which meet the coverage depth requirements.

[0191] The above results demonstrate that the presence of insulating adhesive is not the sole factor determining the effectiveness of short-circuit improvement. Only when the insulating filler extends from the outer circumference of the coil into the inter-turn gap sufficiently to cover the main magnetic powder jamming area can it reliably prevent larger magnetic powder particles from entering between adjacent turns. Therefore, controlling the coverage depth A to be no less than 60 μm is beneficial for ensuring the sealing effect of the localized adhesive filling structure on the magnetic powder entry path.

[0192] As shown in Table 2, the maximum protrusion thickness B gradient test further reveals that as B increases from 0 μm to 10 μm, 20 μm, and 30 μm, the product inductance change rate is 0%, -1.5%, -3.7%, and -5.5% respectively, showing a gradual downward trend. When B is no greater than 20 μm, the product appearance and reliability are still qualified, while when B reaches 30 μm, about 3% of the electrode surface cracks appear.

[0193] This trend further demonstrates that the amount of insulating adhesive applied is not necessarily better the more. The present invention requires that the insulating adhesive preferentially flow into the inter-turn gaps to form an insulating fill with sufficient coverage depth, rather than allowing a large amount of insulating adhesive to accumulate outside the outer contour of the coil.

[0194] As shown in Table 3, the performance comparison before and after partial filling shows that the inductance of Example 1 is reduced by only about 0.42% and the DC resistance is reduced by about 0.12% compared with Comparative Example 1. The saturation change rate is about 0.19 percentage points different. The equivalent series resistance does not show a significant adverse increase, while the short circuit failure rate decreases by an average of about 98.88%.

[0195] This demonstrates that the localized adhesive filling method employed in this invention differs from the existing method of overall thick-layer coating of the coil. Because the insulating adhesive is only applied to the magnetic powder stuck area on the outer circumference of the coil, while the inner circumference of the coil retains an uncoated area, the magnetic powder can continue to enter the inner hole of the coil and directly fill the inner circumference, thus reducing the overall impact of the non-magnetic insulating adhesive on the magnetic circuit and the occupancy rate of the magnetic material.

[0196] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any ordinary changes and substitutions made by those skilled in the art within the scope of the technical solution of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for manufacturing an integrally molded inductor with partial inter-turn adhesive filling, characterized in that, Includes the following steps: S1. Coil preparation: A wire with an insulating layer is wound to form a multi-turn coil, and an inter-turn gap is formed between adjacent turns of the multi-turn coil, and at least part of the inter-turn gap forms an outer opening area on the outer circle side of the multi-turn coil; S2, Local application of adhesive: Apply a fluid insulating adhesive from the outer circle side of the multi-turn coil to at least part of the outer opening area, so that the insulating adhesive enters the corresponding inter-turn gap through the outer opening area, and at least part of the inner circle side of the multi-turn coil remains uncoated. S3. Adhesive curing: The insulating adhesive that enters the inter-turn gap is cured so that the cured insulating adhesive forms an insulating filling part between adjacent turns. The insulating filling part extends from the outer circle side of the multi-turn coil into the interior of the inter-turn gap and covers the outer opening area. S4. Magnetic powder pressing: The multi-turn coil with the insulating filling part is placed in the molding mold, magnetic powder is filled into the molding mold, and the magnetic powder is pressed to form a magnetic pressed body covering the multi-turn coil.

2. The manufacturing method of an integrally molded inductor with partial inter-turn adhesive filling according to claim 1, characterized in that, The outer opening area is defined by the outer circumferential arc surface of two adjacent turns of wire facing the outer circle of the multi-turn coil. The insulating filling portion fills at least the magnetic powder jamming area surrounded by the outer circumferential arc surface to prevent magnetic powder from entering the inter-turn gap from the outer circle of the multi-turn coil.

3. The manufacturing method of an integrally molded inductor with partial inter-turn adhesive filling according to claim 1, characterized in that, Step S2 is performed while maintaining the inter-turn spacing after step S1 is completed, and the multi-turn coil is not subjected to axial stretching or radial expansion during the application of the insulating adhesive.

4. The manufacturing method of an integrally molded inductor with partial inter-turn adhesive filling according to claim 1, characterized in that, The multi-turn coil has leads, and step S1 further includes welding the leads to the terminal frame; step S2 is performed after the leads are welded to the terminal frame, and the area where the insulating adhesive is applied also includes a transition gap between the leads and the coil body of the multi-turn coil, so that the insulating adhesive entering the transition gap is cured in step S3 to form a lead insulation filling part.

5. The manufacturing method of an integrally molded inductor with partial inter-turn adhesive filling according to claim 1, characterized in that, Step S2 includes moving the dispensing head relative to the multi-turn coil along the outer circumference of the multi-turn coil to form a continuous or intermittent dispensing trajectory on the multiple outer opening areas, and causing the insulating adhesive to flow from the outer opening areas into the inter-turn gap under its own gravity and / or inter-turn capillary action.

6. The manufacturing method of an integrally molded inductor with partial inter-turn adhesive filling according to claim 1, characterized in that, The insulating adhesive used in step S2 has a viscosity of no more than 50 mPa·s at a test rotation speed of 50 rpm, and the mass of the insulating adhesive applied to each multi-turn coil is 4.0 to 7.0 mg.

7. The manufacturing method of an integrally molded inductor with partial inter-turn adhesive filling according to claim 1, characterized in that, Within a radial section containing the central axis of the multi-turn coil, the insulation filling portion extends from the outer circular contour of the multi-turn coil into the interior of the inter-turn gap with a coverage depth A of not less than 60 μm, and the maximum protrusion thickness B of the insulation filling portion beyond the outer circular contour of the multi-turn coil is not greater than 20 μm. Wherein, the coverage depth A is the distance from the outer circular contour of the multi-turn coil radially inward to the inner boundary of the insulating filling portion, and the maximum protrusion thickness B is the maximum distance by which the insulating filling portion extends radially beyond the outer circular contour of the multi-turn coil.

8. A one-piece molded inductor with partial inter-turn adhesive filling, comprising a multi-turn coil, a terminal frame connected to the leads of the multi-turn coil, and a magnetic pressing body covering the multi-turn coil, characterized in that: A turn gap is formed between adjacent turns of the multi-turn coil, and at least a portion of the turn gap forms an outer opening region on the outer circumference of the multi-turn coil; An insulating filling part formed by cured insulating adhesive is provided in the outer opening area. The insulating filling part extends from the outer circle side of the multi-turn coil into the inside of the inter-turn gap and crosses the corresponding adjacent turns to prevent the magnetic powder in the magnetic pressing body from entering the inter-turn gap. The inner circular side of the multi-turn coil has an uncoated area that is not covered by the cured insulating adhesive and is in direct contact with the magnetic pressing body.

9. The integrally molded inductor with partial inter-turn filling according to claim 8, characterized in that, A transition gap is formed between the lead wire and the coil body of the multi-turn coil. An insulating filler portion formed by the cured insulating adhesive is provided in the transition gap. The insulating filler portion of the lead wire is continuously connected to at least one insulating filler portion located in the outer opening area.

10. The integrally molded inductor with partial inter-turn filling according to claim 8, characterized in that, Within a radial section containing the central axis of the multi-turn coil, the insulation filling portion extends from the outer circular contour of the multi-turn coil into the interior of the inter-turn gap with a coverage depth A of not less than 60 μm, and the maximum protrusion thickness B of the insulation filling portion beyond the outer circular contour of the multi-turn coil is not greater than 20 μm. Wherein, the coverage depth A is the distance from the outer circular contour of the multi-turn coil radially inward to the inner boundary of the insulating filling portion, and the maximum protrusion thickness B is the maximum distance by which the insulating filling portion extends radially beyond the outer circular contour of the multi-turn coil.

Citation Information

Patent Citations

  • Integral-molding inductance molding method

    CN109166717A

  • Preparation method of integrally-formed inductor, and integrally-formed inductor

    CN112201463A

  • Inductor and method of mfg. same

    CN1343996A