A ceramic heater electrode and its welding method

By optimizing the structure of the ceramic heater electrode and using vacuum brazing technology, a one-time high-efficiency welding of the ceramic heater electrode was achieved, solving the problems of low welding strength and welding eccentricity, improving the welding bonding rate and welding surface strength, and ensuring the stability and uniformity of the CVD process.

CN123075746APending Publication Date: 2026-11-10KONFOONG MATERIALS INTERNATIONAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611526618.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The welding process of existing ceramic heater electrodes has problems such as low welding strength, welding eccentricity and high welding difficulty. In particular, it is easy to cause cracking of the ceramic matrix under high temperature conditions, which affects the uniformity and repeatability of the CVD process.

Method used

An optimized ceramic heater electrode structure is adopted, which connects the lead-out electrode to the ceramic substrate by thread, and a notch is set on the external thread structure. Kovar alloy is used as the transition layer alloy, and vacuum brazing technology is combined to achieve one-time welding. The problem of solder venting is solved by setting grooves and notches.

Benefits of technology

This technology enables efficient welding of ceramic heater electrodes, improving welding strength and achieving a welding bonding rate of over 92%. The welded surface can withstand shear stress of 480 MPa, preventing cracking of the ceramic matrix and ensuring the stability and uniformity of the CVD process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123075746A_ABST
    Figure CN123075746A_ABST
Patent Text Reader

Abstract

This application relates to a ceramic heater electrode and its welding method. The ceramic heater electrode includes a lead-out electrode, a welding layer, and a Kovar alloy connected in sequence. The ceramic heater electrode also includes a ceramic substrate and an electrode connector embedded within the ceramic substrate. The sidewall of the lead-out electrode has an external thread structure. The external thread structure has a first notch. The ceramic substrate has an internal thread structure. The lead-out electrode is threadedly connected to the ceramic substrate. The Kovar alloy in the ceramic heater electrode is located near the electrode connector. This application optimizes the structure of the ceramic heater electrode, allowing it to be welded in one step during assembly, increasing welding strength and weld bonding rate. Simultaneously, the first notch on the external thread structure facilitates solder venting, solving the problem of difficult solder venting during the welding process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of semiconductor manufacturing equipment technology, and in particular to a ceramic heater electrode and its welding method. Background Technology

[0002] Chemical vapor deposition (CVD) equipment is a core component of semiconductor chip manufacturing, and its key technology lies in ensuring the uniformity and repeatability of material growth. As a crucial component of the CVD reaction chamber, the chip heating plate (usually made of ceramic) bears the heavy responsibility of uniformly heating the silicon wafer and promoting gas ionization to form a uniform plasma deposition layer. Radio frequency electrodes and heating components are pre-embedded within the heating plate, which need to be welded to external nickel electrode rods to introduce power. However, this welding process faces significant challenges: the heating plate fabrication requires exposure to high temperatures of 1700-1900℃, and its internal electrodes must be made of high-temperature resistant tungsten or molybdenum materials with thermal expansion coefficients close to those of aluminum nitride ceramics. However, the thermal expansion coefficients of these two materials differ significantly from those of the external nickel electrode rods. Improper welding design or process can easily lead to cracking of the ceramic substrate near the connection point due to thermal stress, rendering the entire expensive heating plate unusable. Therefore, achieving reliable, low-stress welding between the tungsten / molybdenum electrodes and the nickel electrode rods is a decisive factor in determining the performance of the ceramic heating plate and even the success or failure of the fabrication process, thus affecting the uniformity and repeatability of the CVD process.

[0003] CN216982138U discloses a structure for a ceramic heating plate lead-out electrode, including a heating plate body, a connector embedded in a ceramic substrate, a lead-out electrode, and a connecting hole. The connector is a positive and negative connector pre-embedded in the heating plate. The lead-out electrode includes an electrode tube segment and an electrode rod segment. The electrode tube segment includes a light hole segment and a pre-fixed segment. A first gap is provided between the light hole segment and the light hole of the connecting hole, and a second gap is provided between the electrode rod segment and the electrode tube segment. The first gap and the second gap form an expansion buffer zone. This requires multiple welding operations, resulting in high welding difficulty and low weld strength.

[0004] Currently, the lead-out electrodes of ceramic heaters are all connected by vacuum brazing, which involves connecting nickel electrode rods, Kovar alloys, and tungsten (or molybdenum) materials together. The welding structure is complex and difficult, often resulting in low welding strength and weld misalignment, leading to problems such as weld failure during use. Therefore, it is necessary to optimize the structure of ceramic heater electrodes so that they can be welded in one go, increasing welding strength and weld bonding rate, and solving the problem of solder venting during the welding process. Summary of the Invention

[0005] To address the aforementioned technical problems, this application provides a ceramic heater electrode and its welding method. The structure of the ceramic heater electrode is optimized so that it can be welded in one go during assembly, increasing welding strength and welding bonding rate. At the same time, a first notch is provided on the external thread structure to allow for solder venting, solving the problem of difficult solder venting during the welding process.

[0006] To achieve this objective, the following technical solution is adopted in this application: In a first aspect, this application provides a ceramic heater electrode, the ceramic heater electrode comprising a lead-out electrode, a welding layer and a Kovar alloy connected in sequence; The ceramic heater electrode also includes a ceramic substrate and an electrode connector embedded inside the ceramic substrate; The sidewall of the lead-out electrode has an external thread structure; the external thread structure has a first notch; the ceramic substrate has an internal thread structure. The lead-out electrode in the ceramic heater electrode is threadedly connected to the ceramic substrate; Kovar alloy in the ceramic heater electrode is located near the electrode joint.

[0007] This application incorporates Kovar alloy between the lead-out electrode and the electrode connector because the difference in thermal expansion coefficients between them is significant. Using Kovar alloy as a transition layer alloy reduces the risk of cracking due to excessive thermal stress on the lead-out electrode and electrode connector. Simultaneously, the structure of the ceramic heater electrode is optimized. The lead-out electrode is connected to the ceramic substrate via a threaded structure, and the lead-out electrode is connected to the Kovar alloy via a weld layer. This allows the ceramic heater electrode to be welded in one step during assembly, increasing weld strength and weld bonding rate. Furthermore, a first notch is provided on the external threaded structure for solder venting, preventing tight assembly of the lead-out electrode and the ceramic substrate's threaded hole, which could lead to closure, making solder venting difficult and ultimately affecting the weld bonding rate.

[0008] In some embodiments, the lead-out electrode has a first groove on the side near the weld layer; the weld layer and Kovar alloy are located in the first groove of the lead-out electrode, and the weld layer covers the outside of the Kovar alloy.

[0009] In this application, the welding layer and Kovar alloy are placed in the first groove, which can directly increase the concentricity of the lead electrode and Kovar alloy, avoiding the need to adjust the concentricity of the lead electrode and Kovar alloy during assembly.

[0010] In some embodiments, the first notch is symmetrically arranged along the axial direction of the lead-out electrode.

[0011] In some implementations, the number of the first gaps is ≥2, for example, it can be 2, 4, 6 or 8, but it is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0012] In some implementations, the shape of the first notch includes an arc shape and / or a rectangle.

[0013] In some embodiments, the width of the first groove is larger than the width of the Kovar alloy.

[0014] In some embodiments, the first groove has a second notch on the sidewall that contacts the Kovar alloy.

[0015] In this application, a second notch is provided for solder venting to prevent the solder venting from pushing out the solder between the lead electrode and Kovar alloy, thereby reducing the solder bonding rate.

[0016] In some embodiments, the electrode connector is made of molybdenum and / or tungsten.

[0017] In some embodiments, the material of the lead-out electrode includes nickel.

[0018] In some embodiments, the Kovar alloy has a second groove on both the side near the lead-out electrode and the side away from the lead-out electrode.

[0019] In some embodiments, the width of the first groove is 0.04 to 0.4 mm larger than the width of the Kovar alloy, for example, it can be 0.04 mm, 0.1 mm, 0.2 mm, 0.3 mm or 0.4 mm, but is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0020] In this application, the width of the first groove is 0.04~0.4mm larger than the width of the Kovar alloy, that is, the gap between the lead-out electrode and the sidewall of the Kovar alloy is 0.02~0.2mm.

[0021] In some embodiments, the difference between the height of the Kovar alloy and the height of the first groove is 0 to 0.5 mm, for example, it can be 0 mm, 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm or 0.5 mm, but it is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0022] In some implementations, the number of the second gaps is ≥1, for example, it can be 1, 2, 3, 4 or 5, but is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0023] In some embodiments, the depth of the second groove is 0.02~0.2mm, for example, it can be 0.02mm, 0.05mm, 0.1mm, 0.15mm or 0.2mm, but is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0024] In this application, by limiting the depth of the second groove to 0.02~0.2mm, the welding strength and welding bonding rate can be increased. If the depth is too small, i.e. less than 0.02mm, the solder layer will be too thin and the solder layer thickness will be uneven, resulting in welding cavities and affecting the welding strength. If the depth is too large, i.e. greater than 0.2mm, the distance between Kovar alloy and lead electrode and electrode connector will be too far, and effective contact cannot be formed. More solder will be needed during welding and the welding strength will be extremely unstable. The lead electrode after welding will also be difficult to maintain excellent concentricity.

[0025] Secondly, this application provides a welding method for ceramic heater electrodes according to the first aspect, the welding method comprising the following steps: (1) The lead electrode, solder and Kovar alloy are assembled sequentially along the axial direction of the lead electrode to obtain an assembly; wherein the side wall of the lead electrode has an external thread structure and the external thread structure has a first notch; (2) The electrode connector is embedded inside the ceramic substrate to obtain a ceramic substrate containing the electrode connector; wherein the ceramic substrate has an internal thread structure; (3) The assembly is threaded to the ceramic substrate containing the electrode connector to obtain the assembly, wherein Kovar alloy is close to the electrode connector in the assembly, and the assembly is vacuum brazed to obtain the ceramic heater electrode; There is no order between steps (1) and (2).

[0026] The welding method provided in this application optimizes the structure of the ceramic heater electrode and uses vacuum brazing to connect the lead electrode, Kovar alloy and electrode connector together, achieving efficient welding of the ceramic heater electrode. The welding can be completed in one go, and the resulting ceramic heater electrode has good welding uniformity and welding strength, which helps to ensure the performance of the ceramic heater electrode and avoid cracking of the ceramic matrix during heating.

[0027] It should be noted that vacuum brazing (VB) is a technique that operates in a high vacuum environment (typically below 10°C). -2 Pa~10 -4A welding process that uses a filler metal (metal or alloy) with a melting point lower than that of the base metal to melt at a specific temperature and pressure. This filler metal then fills the gaps between tightly assembled parts through capillary action, thus joining the base metals together. The core principle is that in a high vacuum environment, reactive gases such as oxygen and water vapor in the air are effectively removed, preventing oxidation or nitriding of the metals to be welded during heating. This results in oxidation-free and pollution-free clean welding. The entire process requires no flux, resulting in a bright, clean joint with excellent performance.

[0028] In some embodiments, the welding method further includes pre-cleaning, pickling, washing and drying the lead-out electrodes and Kovar alloy sequentially before assembly.

[0029] The pre-cleaning process must satisfy at least one of the following conditions: The cleaning agents used in the pre-cleaning process include, in sequence, degreasing agent, rust remover, and organic solvent.

[0030] It should be noted that the degreasing agent and rust remover used in this application are commonly used reagents in the field, and will not be described in detail here.

[0031] In some embodiments, the organic solvent includes isopropanol.

[0032] In some embodiments, the pre-cleaning process includes ultrasonic cleaning.

[0033] The ultrasonic cleaning shall satisfy at least one of the following conditions: The power of the ultrasonic cleaning is 200~500W, for example, it can be 200W, 300W, 400W or 500W, but it is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0034] In some embodiments, the ultrasonic cleaning time is 15 to 30 minutes, for example, 15 minutes, 20 minutes, 25 minutes or 30 minutes, but is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0035] In some embodiments, the acid used in the pickling process includes a nitric acid solution; the mass fraction of the nitric acid solution is 10-30%, for example, it can be 10%, 15%, 20%, 25% or 30%, but is not limited to the listed values, and other unlisted values ​​within the above range are also applicable.

[0036] In some embodiments, the pickling time is 2 to 3 minutes, for example, 2 minutes, 2.2 minutes, 2.4 minutes, 2.6 minutes, 2.8 minutes or 3 minutes, but it is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0037] In some embodiments, the drying temperature is 50~100°C, for example, 50°C, 60°C, 70°C, 80°C, 90°C or 100°C, but is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0038] In some embodiments, the drying time is 1 to 1.5 hours, for example, 1 hour, 1.1 hours, 1.2 hours, 1.3 hours, 1.4 hours or 1.5 hours, but is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0039] In some embodiments, the solder includes any one or a combination of at least two of solder pads, solder paste, or solder wire, wherein typical but non-limiting combinations include: a combination of solder pads and solder paste, a combination of solder pads and solder wire, a combination of solder paste and solder wire, and a combination of solder pads, solder paste, and solder wire.

[0040] In some embodiments, the solder material includes any one or a combination of at least two of AuNi solder, AgCu solder, AgCuInTi solder, AgCuNi solder, or AgCuMn solder, wherein typical but non-limiting combinations include: a combination of AuNi solder and AgCuMn solder, a combination of AuNi solder and AgCu solder, a combination of AuNi solder and AgCuInTi solder, and a combination of AuNi solder, AgCuNi solder, and AgCuMn solder.

[0041] In some embodiments, the temperature of the vacuum brazing process is 500~1100℃, for example, it can be 500℃, 600℃, 700℃, 800℃, 900℃, 1000℃ or 1100℃, but is not limited to the listed values, and other unlisted values ​​within the above range are also applicable.

[0042] In some embodiments, the holding time for the vacuum brazing process is 30 to 60 minutes, for example, 30 minutes, 40 minutes, 50 minutes or 60 minutes, but it is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0043] In some embodiments, the vacuum brazing process is performed under pressure; the pressure during the vacuum brazing process is 2 to 10 MPa, for example, it can be 2 MPa, 4 MPa, 6 MPa, 8 MPa or 10 MPa, but is not limited to the listed values, and other unlisted values ​​within the above range are also applicable.

[0044] In some embodiments, the welding method includes the following steps: (1) The lead-out electrode and Kovar alloy are pre-cleaned, acid-washed, water-washed and dried in sequence. Then, the lead-out electrode, solder and Kovar alloy are assembled in sequence along the axial direction of the lead-out electrode to obtain an assembly. The sidewall of the lead-out electrode has an external thread structure and the external thread structure has a first notch. (2) The electrode connector is embedded inside the ceramic substrate to obtain a ceramic substrate containing the electrode connector; wherein the ceramic substrate has an internal thread structure; (3) The assembly is threaded to the ceramic substrate containing the electrode connector to obtain the assembly, wherein the Kovar alloy is close to the electrode connector in the assembly, and the assembly is subjected to vacuum brazing at a temperature of 500~1100℃ and a holding time of 30~60min under pressure to obtain the ceramic heater electrode. There is no order between steps (1) and (2).

[0045] Compared with the prior art, this application has at least the following beneficial effects: (1) This application optimizes the structure of the ceramic heater electrode so that the ceramic heater electrode can be welded in one go during assembly, increasing the welding strength and welding bonding rate, and solving the problem of solder venting during the welding process. Its welding surface can withstand shear stress of not less than 480MPa and the welding bonding rate can reach more than 92%. (2) This application optimizes the structure of the ceramic heater electrode and uses vacuum brazing to connect the lead electrode, Kovar alloy and electrode connector together, realizing efficient welding of the ceramic heater electrode and completing the welding in one go. The welded ceramic heater electrode has good welding uniformity and welding strength, which helps to ensure the use effect of the ceramic heater electrode and avoid cracking of the ceramic matrix during heating. Attached Figure Description

[0046] Figure 1 This is a schematic diagram of the structure of the ceramic heater electrode provided in Embodiment 1 of this application.

[0047] Figure 2 This is a top view of the first notch in the lead-out electrode provided in Embodiment 1 of this application.

[0048] Figure 3This is a front view of the first notch in the lead-out electrode provided in Embodiment 1 of this application.

[0049] Figure 4 This is a top view of the second notch in the lead-out electrode provided in Embodiment 1 of this application.

[0050] Figure 5 This is a front view of the second notch in the lead-out electrode provided in Embodiment 1 of this application.

[0051] Figure 6 This is a top view of the first notch in the lead-out electrode provided in Embodiment 2 of this application.

[0052] Figure 7 This is a front view of the first notch in the lead-out electrode provided in Embodiment 2 of this application.

[0053] Wherein, 1-lead electrode; 11-first notch; 12-second notch; 2-welding layer; 3-Kovar alloy; 4-electrode connector; 5-ceramic substrate. Detailed Implementation

[0054] The technical solution of this application will be further described below with reference to the accompanying drawings and specific embodiments. However, the examples below are merely simplified examples of this application and do not represent or limit the scope of protection of this application. The scope of protection of this application shall be determined by the claims.

[0055] Example 1 This embodiment provides a ceramic heater electrode, such as Figure 1 As shown, the ceramic heater electrode includes a lead-out electrode 1, a welding layer 2, and a Kovar alloy 3 connected in sequence; wherein, the lead-out electrode 1 is made of nickel, and the lead-out electrode 1 has a first groove on the side near the welding layer 2; the welding layer 2 and the Kovar alloy 3 are located within the first groove of the lead-out electrode 1, and the welding layer 2 covers the outside of the Kovar alloy 3; the width of the first groove is 0.2 mm larger than the width of the Kovar alloy 3, and the height of the Kovar alloy 3 is equal to the height of the first groove; Figure 4 and Figure 5 As shown, the first groove has two second notches 12 on the sidewall that contacts the Kovar alloy 3; the Kovar alloy 3 has a second groove with a depth of 0.1 mm on both the side near the lead electrode and the side away from the lead electrode. The ceramic heater electrode also includes a ceramic substrate 5 and an electrode connector 4 embedded inside the ceramic substrate 5; wherein the material of the electrode connector 4 is molybdenum. The sidewall of the lead-out electrode 1 has an external thread structure; such as Figure 2 and Figure 3As shown, the external thread structure has four arc-shaped first notches 11; the first notches 11 are symmetrically arranged along the axial direction of the lead-out electrode 1; the ceramic substrate 5 has an internal thread structure; the lead-out electrode 1 in the ceramic heater electrode is threadedly connected to the ceramic substrate 5; the Kovar alloy 3 in the ceramic heater electrode is close to the electrode connector 4.

[0056] This embodiment also provides a welding method for the ceramic heater electrode, the welding method comprising the following steps: (1) At a power of 300W, the lead electrode and Kovar alloy were ultrasonically cleaned for 10 minutes using a phosphorus-free degreasing agent (Kotek Metal Surface Technology Co., Ltd., electrolytic degreasing powder), a rust remover (citric acid) and isopropanol in sequence. Then, the lead electrode and Kovar alloy were pickled for 3 minutes using a 20% nitric acid solution and washed with water. Finally, they were dried at 80℃ for 1.2 hours. (2) The lead electrode, the solder pad and the Kovar alloy are assembled sequentially along the axial direction of the lead electrode to obtain an assembly; wherein the side wall of the lead electrode has an external thread structure and the external thread structure has a first notch; and the solder pad is placed in the second groove and side of the Kovar alloy; the material of the solder pad is AuNi solder. (3) The electrode connector is embedded inside the ceramic substrate to obtain a ceramic substrate containing the electrode connector; wherein the ceramic substrate has an internal thread structure; (4) The assembly is threaded to the ceramic substrate containing the electrode connector to obtain the assembly, wherein the Kovar alloy is close to the electrode connector in the assembly, and the assembly is subjected to vacuum brazing at a temperature of 1000℃ and a holding time of 60min under a pressure of 4MPa to obtain the ceramic heater electrode. There is no order between steps (2) and (3).

[0057] Example 2 This embodiment provides a ceramic heater electrode, which includes a lead-out electrode 1, a welding layer 2, and a Kovar alloy 3 connected in sequence. The lead-out electrode 1 is made of nickel and has a first groove on the side near the welding layer 2. The welding layer 2 and the Kovar alloy 3 are located within the first groove of the lead-out electrode 1, with the welding layer 2 covering the outside of the Kovar alloy 3. The width of the first groove is 0.04 mm larger than the width of the Kovar alloy 3, and the difference between the height of the Kovar alloy 3 and the height of the first groove is 0.1 mm. A second notch 12 is provided on the sidewall of the first groove that contacts the Kovar alloy 3. The Kovar alloy 3 has a second groove with a depth of 0.02 mm on both the side near and away from the lead-out electrode. The ceramic heater electrode also includes a ceramic substrate 5 and an electrode connector 4 embedded inside the ceramic substrate 5; wherein the electrode connector 4 is made of tungsten. The sidewall of the lead-out electrode 1 has an external thread structure; such as Figure 6 and Figure 7 As shown, the external thread structure has two rectangular first notches 11; the first notches 11 are symmetrically arranged along the axial direction of the lead-out electrode 1; the ceramic substrate 5 has an internal thread structure; the lead-out electrode 1 in the ceramic heater electrode is threadedly connected to the ceramic substrate 5; the Kovar alloy 3 in the ceramic heater electrode is close to the electrode connector 4.

[0058] This embodiment also provides a welding method for the ceramic heater electrode, the welding method comprising the following steps: (1) At a power of 200W, the lead-out electrode and Kovar alloy were ultrasonically cleaned for 8 minutes using a phosphorus-free degreasing agent (Kotek Metal Surface Technology Co., Ltd., electrolytic degreasing powder), a rust remover (citric acid) and isopropanol in sequence. Then, the lead-out electrode and Kovar alloy were pickled for 2 minutes using a 30% nitric acid solution and washed with water. Finally, they were dried at a temperature of 50℃ for 1.5 hours. (2) The lead electrode, solder paste and Kovar alloy are assembled sequentially along the axial direction of the lead electrode to obtain an assembly; wherein the side wall of the lead electrode has an external thread structure and the external thread structure has a first notch; and the solder paste is applied to the second groove and side of the Kovar alloy; the material of the solder sheet is AgCuMn solder. (3) The electrode connector is embedded inside the ceramic substrate to obtain a ceramic substrate containing the electrode connector; wherein the ceramic substrate has an internal thread structure; (4) The assembly is threaded to the ceramic substrate containing the electrode connector to obtain the assembly, wherein the Kovar alloy is close to the electrode connector in the assembly, and the assembly is subjected to vacuum brazing at a temperature of 800°C and a holding time of 60 min under a pressure of 4 MPa to obtain the ceramic heater electrode. There is no order between steps (2) and (3).

[0059] Example 3 This embodiment provides a ceramic heater electrode, which includes a lead-out electrode, a welding layer, and a Kovar alloy connected in sequence. The lead-out electrode is made of nickel and has a first groove on the side near the welding layer. The welding layer and the Kovar alloy are located within the first groove of the lead-out electrode, with the welding layer covering the outside of the Kovar alloy. The width of the first groove is 0.4 mm greater than the width of the Kovar alloy, and the difference between the height of the Kovar alloy and the height of the first groove is 0.5 mm. The sidewall of the first groove in contact with the Kovar alloy has four second notches. The Kovar alloy has second grooves with a depth of 0.2 mm on both the side near and away from the lead-out electrode. The ceramic heater electrode further includes a ceramic substrate and an electrode connector embedded inside the ceramic substrate; wherein the electrode connector is made of molybdenum. The sidewall of the lead-out electrode has an external thread structure; the external thread structure has six arc-shaped first notches; the first notches are symmetrically arranged along the axial direction of the lead-out electrode; the ceramic substrate has an internal thread structure; the lead-out electrode in the ceramic heater electrode is threadedly connected to the ceramic substrate; the Kovar alloy in the ceramic heater electrode is close to the electrode joint.

[0060] This embodiment also provides a welding method for the ceramic heater electrode, the welding method comprising the following steps: (1) At a power of 500W, the lead electrode and Kovar alloy were ultrasonically cleaned for 5 minutes using a phosphorus-free degreasing agent (Kotek Metal Surface Technology Co., Ltd., electrolytic degreasing powder), a rust remover (citric acid) and isopropanol in sequence. Then, the lead electrode and Kovar alloy were pickled for 3 minutes using a 10% nitric acid solution and washed with water. Finally, they were dried at 100℃ for 1 hour. (2) The lead electrode, the solder pad and the Kovar alloy are assembled sequentially along the axial direction of the lead electrode to obtain an assembly; wherein the side wall of the lead electrode has an external thread structure and the external thread structure has a first notch; and the solder pad is placed in the second groove and side of the Kovar alloy; the material of the solder pad is AgCuInTi solder. (3) The electrode connector is embedded inside the ceramic substrate to obtain a ceramic substrate containing the electrode connector; wherein the ceramic substrate has an internal thread structure; (4) The assembly is threaded to the ceramic substrate containing the electrode connector to obtain the assembly, wherein the Kovar alloy in the assembly is close to the electrode connector, and the assembly is subjected to vacuum brazing at a temperature of 1100℃ and a holding time of 30min under a pressure of 4MPa to obtain the ceramic heater electrode. There is no order between steps (2) and (3).

[0061] Example 4 This embodiment provides a ceramic heater electrode, which differs from Embodiment 1 only in that the second notch is not provided on the side wall of the first groove, but all other aspects are the same as in Embodiment 1.

[0062] Example 5 This embodiment provides a ceramic heater electrode, which differs from Embodiment 1 only in that the depth of the second groove is adjusted from 0.1 mm to 0.01 mm, while all other aspects are the same as in Embodiment 1.

[0063] Example 6 This embodiment provides a ceramic heater electrode, which differs from Embodiment 1 only in that the depth of the second groove is adjusted from 0.1 mm to 0.5 mm, while all other aspects are the same as in Embodiment 1.

[0064] Example 7 This embodiment provides a ceramic heater electrode, which differs from Embodiment 1 only in that the vacuum brazing process in step (4) is performed at 0.1 MPa, while the rest is the same as Embodiment 1.

[0065] Comparative Example 1 This comparative example provides a ceramic heater electrode, which differs from Example 1 only in that the external thread structure of the lead-out electrode does not have a first notch, but is otherwise the same as Example 1.

[0066] Comparative Example 2 This comparative example provides a ceramic heater electrode, which differs from Example 1 only in that the ceramic heater electrode does not include Kovar alloy and the lead-out electrode does not have a first groove, i.e., only a welding layer is provided between the lead-out electrode and the electrode connector. Otherwise, it is the same as Example 1.

[0067] The ceramic heater electrodes obtained in the above embodiments and comparative examples were subjected to welding bonding rate and welding bonding strength tests. The welding bonding rate test was conducted using ultrasonic testing technology. The welding interface was analyzed by ultrasonic waves to determine the proportion of unbonded defects such as pores on the welding interface. The welding bonding strength was tested according to GB / T39163-2020 "Test Method for Bond Strength of Target Material and Backing Plate". The results showed that the welding surface could withstand shear force. The test results are shown in Table 1.

[0068] Table 1 The test results show that: (1) As can be seen from Examples 1 to 3, this application cleans and dries each component of the ceramic heater electrode through a clean cleaning process to remove dirt and particulate matter from its surface; processes the first notch, the first and second grooves and uses appropriate brazing filler metal and brazing process, which can make the heater electrode welding success rate high and the welding strength high.

[0069] (2) As can be seen from Examples 1 and 4, the second notch processed in this application can keep Kovar alloy in good contact with the electrode, effectively improving the welding success rate and welding strength.

[0070] (3) As can be seen from Examples 1 and 5-6, this application can ensure that the lead-out electrode, the solder sheet, the Kovar alloy and the electrode connector are in close contact during assembly and welding by limiting the depth of the second groove, thus ensuring the welding success rate and welding strength.

[0071] (4) As can be seen from Examples 1 and 7, the application applies pressure during the brazing process, which enables the heater electrode components and the ceramic substrate to be more tightly bonded together during brazing, effectively improving the welding strength and welding success rate.

[0072] (5) As can be seen from Example 1 and Comparative Example 1, by processing the first notch of the electrode, the gas generated during brazing can be discharged in time, which effectively improves the welding success rate.

[0073] (6) As can be seen from Example 1 and Comparative Example 2, the present application uses Kovar alloy to connect the lead electrode and the electrode connector, which can reduce the risk of cracking of the lead electrode and the electrode connector due to excessive thermal stress, and realize the effective welding of the lead electrode and the ceramic substrate.

[0074] In summary, this application optimizes the structure of the ceramic heater electrode, enabling the ceramic heater electrode to be welded in one go during assembly, increasing the welding strength and welding bonding rate, and solving the problem of solder venting during the welding process. The welded surface can withstand shear force of over 480 MPa, and the welding bonding rate can reach over 92%.

[0075] The applicant declares that the above description is only a specific implementation of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. A ceramic heater electrode, characterized in that, The ceramic heater electrode includes a lead-out electrode, a welding layer, and a Kovar alloy connected in sequence. The ceramic heater electrode also includes a ceramic substrate and an electrode connector embedded inside the ceramic substrate; The sidewall of the lead-out electrode has an external thread structure; the external thread structure has a first notch; the ceramic substrate has an internal thread structure. The lead-out electrode in the ceramic heater electrode is threadedly connected to the ceramic substrate; Kovar alloy in the ceramic heater electrode is located near the electrode joint.

2. The ceramic heater electrode according to claim 1, characterized in that, The lead-out electrode has a first groove on the side near the welding layer; the welding layer and Kovar alloy are located in the first groove of the lead-out electrode, and the welding layer covers the outside of the Kovar alloy; And / or, the first notch is symmetrically arranged along the axial direction of the lead-out electrode; And / or, the number of the first gaps is ≥2; And / or, the shape of the first notch includes an arc shape and / or a rectangle.

3. The ceramic heater electrode according to claim 2, characterized in that, The width of the first groove is greater than the width of the Kovar alloy. And / or, the first groove has a second notch on the sidewall that contacts the Kovar alloy; And / or, the material of the electrode connector includes molybdenum and / or tungsten; And / or, the material of the lead-out electrode includes nickel; And / or, the Kovar alloy has a second groove on both the side near the lead-out electrode and the side away from the lead-out electrode.

4. The ceramic heater electrode according to claim 3, characterized in that, The width of the first groove is 0.04~0.4mm larger than the width of the Kovar alloy; And / or, the difference between the height of the Kovar alloy and the height of the first groove is 0~0.5mm; And / or, the number of the second gaps is ≥1; And / or, the depth of the second groove is 0.02~0.2mm.

5. A welding method for a ceramic heater electrode according to any one of claims 1-4, characterized in that, The welding method includes the following steps: (1) The lead electrode, solder and Kovar alloy are assembled sequentially along the axial direction of the lead electrode to obtain an assembly; wherein the side wall of the lead electrode has an external thread structure and the external thread structure has a first notch; (2) The electrode connector is embedded inside the ceramic substrate to obtain a ceramic substrate containing the electrode connector; wherein the ceramic substrate has an internal thread structure; (3) The assembly is threaded to the ceramic substrate containing the electrode connector to obtain the assembly, wherein Kovar alloy is close to the electrode connector in the assembly, and the assembly is vacuum brazed to obtain the ceramic heater electrode; There is no order between steps (1) and (2).

6. The welding method according to claim 5, characterized in that, The welding method further includes pre-cleaning, pickling, water washing and drying of the lead-out electrodes and Kovar alloy in sequence before assembly; The pre-cleaning process must satisfy at least one of the following conditions: The cleaning agents used in the pre-cleaning process include, in sequence, degreaser, rust remover, and organic solvent; And / or, the pre-cleaning process includes ultrasonic cleaning; The ultrasonic cleaning shall satisfy at least one of the following conditions: The power of the ultrasonic cleaning is 200~500W; And / or, the ultrasonic cleaning time is 15~30 min.

7. The welding method according to claim 6, characterized in that, The acid solution used in the pickling process includes a nitric acid solution; the nitric acid solution has a mass fraction of 10-30%. And / or, the pickling process takes 2 to 3 minutes; And / or, the drying temperature is 50~100℃; And / or, the drying process takes 1 to 1.5 hours.

8. The welding method according to any one of claims 5-7, characterized in that, The solder includes any one or a combination of at least two of the following: solder sheets, solder paste, or solder wire; And / or, the solder material includes any one or a combination of at least two of AuNi solder, AgCu solder, AgCuInTi solder, AgCuNi solder, or AgCuMn solder.

9. The welding method according to any one of claims 5-8, characterized in that, The temperature for the vacuum brazing process is 500~1100℃; And / or, the heat preservation time for the vacuum brazing treatment is 30~60 min; And / or, the vacuum brazing process is performed under pressure; the pressure during the vacuum brazing process is 2~10MPa.

10. The welding method according to any one of claims 5-9, characterized in that, The welding method includes the following steps: (1) The lead-out electrode and Kovar alloy are pre-cleaned, acid-washed, water-washed and dried in sequence. Then, the lead-out electrode, solder and Kovar alloy are assembled in sequence along the axial direction of the lead-out electrode to obtain an assembly. The sidewall of the lead-out electrode has an external thread structure and the external thread structure has a first notch. (2) The electrode connector is embedded inside the ceramic substrate to obtain a ceramic substrate containing the electrode connector; wherein the ceramic substrate has an internal thread structure; (3) The assembly is threaded to the ceramic substrate containing the electrode connector to obtain the assembly, wherein the Kovar alloy is close to the electrode connector in the assembly, and the assembly is subjected to vacuum brazing at a temperature of 500~1100℃ and a holding time of 30~60min under pressure to obtain the ceramic heater electrode. There is no order between steps (1) and (2).