Visible-light response type titanium dioxide composite de-aldehyde and odorless photocatalyst and preparation method thereof

By constructing an amorphous titanium dioxide isolation layer on the surface of the photocatalyst and regulating the nucleation sites of zeolite imidazole esters, the problems of insufficient visible light response and structural instability of the photocatalyst were solved, achieving efficient formaldehyde purification and long-term stability.

CN123102416APending Publication Date: 2026-11-17SHIYU NEW BUILDING MATERIALS (JINGZHOU) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611170584.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-04
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing photocatalysts suffer from insufficient visible light response and pseudo-deactivation of the catalytic layer in indoor formaldehyde purification. In particular, the stagnant gas concentration boundary layer formed on the surface of gypsum board veneer leads to low purification efficiency, and the skeleton material is structurally unstable in humid and hot environments.

Method used

By constructing an amorphous titanium dioxide isolation layer on the surface of a bismuth halide-titanium carbide heterojunction, the distribution of nucleation sites of the zeolite imidazole ester framework material is regulated, and the interfacial bonding strength is enhanced by the defect sites of trivalent titanium. By utilizing the electron transport capability of titanium carbide and the reversible adsorption and release of gas by zeolite imidazole ester, the formaldehyde diffusion pathway is opened.

Benefits of technology

It improves the visible light utilization rate and structural stability of the photocatalyst, ensuring effective mineralization of formaldehyde under low light conditions, solving the problems of pseudo-deactivation of the catalyst layer and hydrolysis and dissolution of the framework material, and achieving long-lasting purification effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102416A_ABST
    Figure CN123102416A_ABST
Patent Text Reader

Abstract

This invention discloses a visible light-responsive titanium dioxide composite photocatalyst for formaldehyde removal and odor elimination, and its preparation method, belonging to the field of environmental remediation materials technology. The method includes the following steps: etching titanium aluminum carbide powder in a lithium fluoride-containing hydrochloric acid etching solution, washing until neutral, and then ultrasonically exfoliating in an ice bath under a protective atmosphere to obtain titanium carbide nanosheets; dispersing the titanium carbide nanosheets in ethylene glycol and ultrasonically dispersing in an ice bath to obtain a titanium carbide dispersion; adding an organic solution of bismuth source and halogen source to the titanium carbide dispersion, stirring and mixing, and then performing a solvothermal reaction to obtain a bismuth halide-titanium carbide heterojunction; and passivating the in-plane region of the bismuth halide sheet layer by pre-constructing an amorphous titanium dioxide isolation layer on the surface of the bismuth halide-titanium carbide heterojunction using the steric hindrance effect of this isolation layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of environmental remediation materials technology, and in particular to a visible light responsive titanium dioxide composite photocatalyst for formaldehyde removal and odor elimination, and its preparation method. Background Technology

[0002] Indoor air quality is directly related to human health. Formaldehyde, as one of the main gaseous pollutants released from indoor decoration materials, has been listed as a Group 1 carcinogen by the World Health Organization. Free formaldehyde remaining in various adhesives used in the manufacturing process of building decoration boards will continue to be released into the indoor environment for several years, which is one of the important sources of long-term excessive indoor formaldehyde concentration. Photocatalytic oxidation technology can completely mineralize formaldehyde into carbon dioxide and water at normal temperature and pressure without secondary pollution, and the catalyst itself can be reused. It is considered to be one of the most promising technical routes to solve the problem of indoor formaldehyde pollution.

[0003] To address the aforementioned issue of insufficient visible light response, existing technologies primarily employ two approaches: heterostructure construction and surface functional layer modification. Heterostructure construction involves interfacially compositing two semiconductor materials with matching band structures. This utilizes the energy level difference to create a built-in electric field at the interface, driving photogenerated electrons to migrate from one material to the other, thereby suppressing electron-hole recombination. Simultaneously, narrow bandgap materials are used to extend the light response range into the visible light region; for example, titanium dioxide is composited with narrow bandgap semiconductors such as tungsten trioxide, tin oxide, or cadmium sulfide to construct a heterojunction. Surface functional layer modification involves introducing auxiliary layer materials with specific physical or chemical functions onto the surface of photocatalyst particles. This improves the catalyst's interfacial behavior in complex environments or endows it with additional functionality. Examples include loading porous adsorbent materials onto the photocatalyst surface to enhance its enrichment capacity for target pollutants, or loading noble metal nanoparticles to utilize their surface plasmon resonance effect to enhance visible light absorption.

[0004] Then, in the practical application of new building materials such as paper-faced gypsum board, decorative ceilings, and lightweight partition boards, the photocatalytic purification functional layer is usually loaded on the surface finishing layer of the board. In the quasi-static air environment with extremely low air exchange rate formed by the closure of doors and windows in the building, the carbon dioxide and water vapor generated by the slow release of formaldehyde from the core of the board and the adhesive through photocatalytic decomposition continuously accumulate on the surface of the finishing catalyst layer, forming a stagnant gas concentration boundary layer with a thickness of about 1-3mm. This boundary layer, like a sealed gas film covering the surface of the board finishing layer, severely blocks the diffusion mass transfer channels of free formaldehyde continuously emitted from the core gypsum matrix and the facing paper adhesive layer to the surface catalytic sites. As a result, the formaldehyde concentration in the indoor space is difficult to decrease further after dropping to a plateau of 100-200ppb, exhibiting a purification stagnation phenomenon of pseudo-deactivation of the surface catalyst layer. If mechanical ventilation is used indoors to forcibly disturb the boundary layer, the airflow shear force can easily damage the interfacial adhesion of the board finishing layer, leading to the problem of gypsum board surface layer powdering and peeling. Summary of the Invention

[0005] This invention overcomes the shortcomings of the prior art and provides a visible light responsive titanium dioxide composite photocatalyst for formaldehyde removal and odor elimination, and its preparation method.

[0006] To achieve the above objectives, the technical solution adopted by this invention is as follows: a method for preparing a visible light-responsive titanium dioxide composite photocatalyst for formaldehyde removal and odor elimination, comprising the following steps:

[0007] S1. Titanium aluminum carbide powder is etched in hydrochloric acid etching solution containing lithium fluoride, washed until neutral, and then ultrasonically exfoliated in an ice bath under a protective atmosphere to obtain titanium carbide nanosheets; wherein, the mass ratio of titanium aluminum carbide to lithium fluoride is 1:1-3.

[0008] S2. The titanium carbide nanosheets are dispersed in ethylene glycol and ultrasonically dispersed in an ice bath to obtain a titanium carbide dispersion; wherein the dispersion concentration of the titanium carbide nanosheets is 1-5 mg / mL.

[0009] S3. Add an organic solution of bismuth source and halogen source to the titanium carbide dispersion, stir and mix, and then perform a solvothermal reaction to obtain a bismuth halide-titanium carbide heterojunction; wherein, the molar ratio of titanium carbide to bismuth source in the titanium carbide dispersion is 0.005-0.05:1.

[0010] S4. The bismuth halide-titanium carbide heterojunction is dispersed in anhydrous ethanol, a titanium source is added, and water is added dropwise under ice bath stirring to hydrolyze the titanium source, forming an amorphous titanium dioxide layer. The layer is then calcined in an inert atmosphere to obtain an isolation layer coating the heterojunction.

[0011] S5. The isolation layer-coated heterojunction is dispersed in methanol and ultrasonically dispersed to obtain a heterojunction-coated dispersion; wherein the dispersion concentration of the isolation layer-coated heterojunction is 1-5 mg / mL.

[0012] S6. Under a protective atmosphere and with stirring, a metal salt solution and an organic ligand solution are simultaneously added dropwise to the coated heterojunction dispersion. The mixture is allowed to stand for reaction, washed, and activated under vacuum to obtain the final complex. The molar ratio of the metal salt to the organic ligand is 1:4-12.

[0013] In a preferred embodiment of the present invention, in step S1, the solid-liquid ratio of titanium aluminum carbide to the hydrochloric acid etching solution is 1:10-30, the etching temperature is 20-50℃, and the etching time is 18-36h; the thickness of the titanium carbide nanosheets is 2-10nm.

[0014] In a preferred embodiment of the present invention, in step S1, the concentration of hydrochloric acid is 8-10M, and the washing is water washing until pH 6.0-7.0.

[0015] In a preferred embodiment of the present invention, in step S3, the bismuth source is bismuth nitrate pentahydrate or bismuth chloride, the halogen source is potassium iodide or sodium iodide, and the molar ratio of the bismuth source to the halogen source is 1:1-3 based on the ratio of bismuth element to halogen element; the temperature of the solvothermal reaction is 120-200℃, and the time is 8-24h.

[0016] In a preferred embodiment of the present invention, in step S4, the titanium source is isopropyl titanate or tetrabutyl titanate; the mass ratio of the bismuth halide-titanium carbide heterojunction to the titanium source is 1:0.01-0.1.

[0017] In a preferred embodiment of the present invention, in step S4, the thickness of the amorphous titanium dioxide layer is 1-5 nm, and the isolation layer covering the heterojunction surface contains trivalent titanium self-doped defect sites.

[0018] In a preferred embodiment of the present invention, in step S4, the calcination temperature is 200-400℃ and the time is 0.5-3h.

[0019] In a preferred embodiment of the present invention, in step S6, the metal salt is zinc nitrate hexahydrate or zinc acetate, and the organic ligand is 2-methylimidazole or benzimidazole.

[0020] In a preferred embodiment of the present invention, in step S6, the static reaction time is 1-4 hours, and the vacuum activation temperature is 100-200°C for 1-6 hours.

[0021] Secondly, the present invention provides a visible light responsive titanium dioxide composite photocatalyst for formaldehyde removal and odor elimination, which is prepared by any of the above-described preparation methods.

[0022] This invention addresses the shortcomings of the prior art and has the following beneficial effects:

[0023] (1) By pre-constructing an amorphous titanium dioxide isolation layer on the surface of the bismuth oxyhalide-titanium carbide heterojunction, the steric hindrance effect of the isolation layer is used to passivate the in-plane region of the bismuth oxyhalide sheet, so that the zeolite imidazole ester framework material subsequently grown in situ can only be oriented to nucleate at edge sites with higher energy and more abundant surface defects. This spatial selectivity of nucleation sites avoids the problem of in-plane shading of the visible light absorption window of bismuth oxyhalide by the framework material from the root, while completely preserving the catalytic active centers on the surface of the sheet. Compared with the existing technology of indiscriminate deposition of framework material on the surface of the sheet, the visible light utilization efficiency and accessibility of active sites of bismuth oxyhalide in this invention are effectively guaranteed, thereby improving the actual light energy utilization rate of the photocatalyst in the gypsum board finishing coating.

[0024] (2) Trivalent titanium self-doped defect sites are formed through the amorphous titanium dioxide isolation layer during the subsequent inert atmosphere calcination process. These defect sites have a strong chemical anchoring effect on the subsequently introduced zinc ions. When the zeolite imidazole ester framework material nucleates and grows at the edge sites, the zinc ions are effectively captured by the trivalent titanium defect sites on the surface of the isolation layer, which significantly enhances the interfacial bonding strength between the framework material and the heterojunction substrate. In the weakly alkaline service environment of gypsum board accompanied by alternating heat and humidity, the hydrolysis and dissolution problem faced by the framework material due to local carbon dioxide concentration fluctuations is effectively suppressed. Compared with the traditional structure in which the framework material is directly loaded on the surface of bismuth halogen oxide, the ligand loss rate and crystal structure degradation rate of the framework material in this invention are significantly reduced, which endows the photocatalyst with structural stability and purification durability under long-term pulsed carbon dioxide release conditions.

[0025] (3) By using titanium carbide nanosheets as an electron transport medium, a built-in electric field is formed at the interface of the heterojunction constructed with bismuth oxyhalide. Photogenerated electrons are rapidly extracted from the conduction band of bismuth oxyhalide and migrate to the surface of titanium carbide, effectively suppressing the bulk recombination of electrons and holes. This carrier separation mechanism ensures that the photogenerated holes generated by bismuth oxyhalide under visible light excitation can fully participate in the formaldehyde oxidation reaction, and can maintain a high photon efficiency even in the low light environment indoors. Compared with the serious carrier recombination problem in pure bismuth oxyhalide materials, the introduction of titanium carbide in this invention improves the utilization rate of unit photons, ensures the mineralization ability of the photocatalyst under low light conditions, and thus solves the problem of low purification efficiency caused by insufficient light energy in the actual indoor lighting environment of gypsum board cladding catalyst layer. Attached Figure Description

[0026] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0027] Figure 1 This is a flowchart of a preferred embodiment of the present invention. Detailed Implementation

[0028] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0029] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein. Therefore, the scope of protection of the invention is not limited to the specific embodiments disclosed below.

[0030] Application Overview:

[0031] During the loading of zeolite imidazole ester framework nanoparticles onto the surface of bismuth halide sheets, some particles uncontrollably deposit in the in-plane region of the bismuth halide sheets. This in-plane deposition directly blocks the visible light absorption window of bismuth halide and covers its catalytic active centers, resulting in a 10-15% decrease in the actual light utilization efficiency of the photocatalyst in gypsum board finishing coatings. In addition, during long-term pulsed carbon dioxide release, the local carbonic acid concentration fluctuates with the release cycle, inducing ligand exchange reactions in the framework, causing its crystal structure to slowly hydrolyze and dissolve. In the weakly alkaline service environment of gypsum board accompanied by alternating heat and humidity, its long-term structural stability faces severe challenges.

[0032] The applicant discovered that pre-constructing an amorphous titanium dioxide isolation layer on the surface of a bismuth oxyhalide-titanium carbide heterojunction can effectively regulate the distribution of nucleation sites for subsequent zeolite imidazole ester framework materials. This isolation layer passivates the in-plane region of the bismuth oxyhalide sheet through steric hindrance, allowing the subsequently grown zeolite imidazole ester framework material to nucleate only at edge sites with higher energy and more abundant surface defects, thus fundamentally avoiding the loss of visible light utilization caused by in-plane shading. More importantly, the amorphous titanium dioxide isolation layer forms trivalent titanium self-doped defect sites during calcination. These defect sites have a strong anchoring effect on zinc ions, which can significantly delay the hydrolysis rate and ligand loss rate of the zeolite imidazole ester framework material under alternating carbonic acid and water vapor erosion conditions.

[0033] The applicant proposes to obtain titanium carbide nanosheets by stripping titanium aluminum carbide with a lithium fluoride-containing hydrochloric acid etching solution, and then to construct a bismuth halide-titanium carbide heterojunction by solvothermal reaction of the nanosheets with bismuth and halogen sources. A titanium source is then introduced for hydrolysis and calcination to form a titanium dioxide isolation layer containing trivalent titanium defects. A solution of metal salts and organic ligands is added dropwise to grow zeolite imidazole ester framework materials in situ. The rapid extraction of photogenerated electrons by titanium carbide inhibits carrier recombination, ensuring low-light mineralization efficiency. The titanium dioxide isolation layer forces the framework material to nucleate only at the edges, eliminating in-plane shading, while the trivalent titanium defects anchor zinc ions, delaying hydrolysis. The edge-loaded framework material is released through reversible adsorption of carbon dioxide, generating gas micro-perturbations on the surface of the catalytic layer, tearing apart the stagnant boundary layer, and forcibly pumping formaldehyde from deep within the board to the catalytic site, giving the board long-term stable formaldehyde removal performance.

[0034] like Figure 1 As shown, a method for preparing a visible light-responsive titanium dioxide composite photocatalyst for formaldehyde removal and odor elimination includes the following steps:

[0035] S1. Titanium aluminum carbide powder is etched in hydrochloric acid etching solution containing lithium fluoride, washed until neutral, and then ultrasonically exfoliated in an ice bath under a protective atmosphere to obtain titanium carbide nanosheets; wherein, the mass ratio of titanium aluminum carbide to lithium fluoride is 1:1-3.

[0036] S2. The titanium carbide nanosheets are dispersed in ethylene glycol and ultrasonically dispersed in an ice bath to obtain a titanium carbide dispersion; wherein the dispersion concentration of the titanium carbide nanosheets is 1-5 mg / mL.

[0037] S3. Add an organic solution of bismuth source and halogen source to the titanium carbide dispersion, stir and mix, and then perform a solvothermal reaction to obtain a bismuth halide-titanium carbide heterojunction; wherein, the molar ratio of titanium carbide to bismuth source in the titanium carbide dispersion is 0.005-0.05:1.

[0038] S4. The bismuth halide-titanium carbide heterojunction is dispersed in anhydrous ethanol, a titanium source is added, and water is added dropwise under ice bath stirring to hydrolyze the titanium source, forming an amorphous titanium dioxide layer. The layer is then calcined in an inert atmosphere to obtain an isolation layer coating the heterojunction.

[0039] S5. The isolation layer-coated heterojunction is dispersed in methanol and ultrasonically dispersed to obtain a heterojunction-coated dispersion; wherein the dispersion concentration of the isolation layer-coated heterojunction is 1-5 mg / mL.

[0040] S6. Under a protective atmosphere and with stirring, a metal salt solution and an organic ligand solution are simultaneously added dropwise to the coated heterojunction dispersion. The mixture is allowed to stand for reaction, washed, and activated under vacuum to obtain the final complex. The molar ratio of the metal salt to the organic ligand is 1:4-12.

[0041] The core innovation of this invention lies in: by pre-constructing a titanium dioxide isolation layer containing trivalent titanium self-doped defects on the surface of a bismuth halide-titanium carbide heterojunction, the steric hindrance effect of the titanium dioxide isolate layer is used to regulate the zeolite imidazole ester framework material to nucleate only at the edges, eliminating in-plane shading to ensure light absorption and accessibility of active sites. At the same time, the anchoring effect of defects on zinc ions delays the hydrolysis of the framework material to enhance service stability. Furthermore, the reversible adsorption and release of carbon dioxide by the edge-loaded framework material generates gas perturbations, tearing the stagnant gas concentration boundary layer of the gypsum board finish layer to open up the formaldehyde diffusion mass transfer pathway. Thus, while ensuring efficient utilization of visible light and long-term structural stability, the problem of purification stagnation caused by the pseudo-deactivation of the surface catalyst layer in a quasi-static air environment is solved.

[0042] Each step will be explained in detail below.

[0043] In step S1, titanium aluminum carbide powder is placed in a hydrochloric acid etching solution containing lithium fluoride for etching. Hydrofluoric acid generated in situ by lithium fluoride and hydrochloric acid is used to selectively etch the aluminum atom layer in titanium aluminum carbide to obtain multilayer titanium carbide.

[0044] The mass ratio of titanium aluminum carbide to lithium fluoride is 1:1-3, the solid-liquid ratio of titanium aluminum carbide to hydrochloric acid etching solution is 1:10-30, the concentration of hydrochloric acid is 8-10M, the etching temperature is 20-50℃, and the etching time is 18-36h.

[0045] After etching, the product is washed with deionized water to remove residual acid and etching byproducts; the washing is carried out until the pH reaches 6.0-7.0.

[0046] Subsequently, ultrasonic exfoliation in an ice bath was performed under an argon or nitrogen protective atmosphere to suppress the oxidation of titanium carbide nanosheets during the ultrasonic process, resulting in titanium carbide nanosheets with a thickness of 2-10 nm; wherein the ultrasonic power was 100-300 W and the ultrasonic time was 1-3 h.

[0047] Titanium carbide nanosheets have excellent electronic conductivity and can serve as an electron transport medium in the subsequently constructed heterostructures. They can rapidly extract photogenerated electrons and effectively suppress carrier recombination.

[0048] In step S2, titanium carbide nanosheets are dispersed in ethylene glycol and ultrasonically dispersed under ice bath conditions. The low temperature environment prevents the nanosheets from oxidizing or agglomerating due to local overheating during the ultrasonic process, resulting in a titanium carbide dispersion in which titanium carbide nanosheets are uniformly dispersed.

[0049] The dispersion concentration of titanium carbide nanosheets is 1-5 mg / mL, the ultrasonic power is 100-300 W, and the ultrasonic time is 30-90 min.

[0050] Ethylene glycol, as a dispersion medium, also has reducing properties, which can protect the surface of titanium carbide nanosheets during dispersion and maintain their electronic conductivity.

[0051] In step S3, organic solutions of bismuth source and halogen source are added to the titanium carbide dispersion. After stirring and mixing evenly, the mixture is transferred to a reaction vessel for solvothermal reaction. Bismuth halide nanosheets are grown in situ on the surface of titanium carbide nanosheets, forming a heterojunction interface in close contact between the two, thus obtaining a bismuth halide-titanium carbide heterojunction.

[0052] The organic solvent used is ethanol. The molar ratio of titanium carbide to bismuth source in the titanium carbide dispersion is 0.005-0.05:1. The bismuth source is bismuth nitrate pentahydrate or bismuth chloride. The halogen source is potassium iodide or sodium iodide. The molar ratio of bismuth source to halogen source is 1:1-3 based on bismuth element to halogen element. The solvothermal reaction temperature is 120-200℃ and the time is 8-24h.

[0053] During the solvothermal reaction, titanium carbide nanosheets serve as a nucleation substrate, guiding the growth of bismuth halide nanosheets along their surface to form a tight heterojunction interface.

[0054] At the heterojunction interface, due to the difference in band structure between bismuth halide and titanium carbide, a built-in electric field is formed. This electric field drives the photogenerated electrons generated by bismuth halide under visible light to migrate rapidly to the surface of titanium carbide, thereby effectively suppressing the bulk recombination of electrons and holes and ensuring that photogenerated holes can fully participate in the formaldehyde oxidation reaction.

[0055] In step S4, the bismuth halide-titanium carbide heterojunction is dispersed in anhydrous ethanol, a titanium source is added, and water is slowly added dropwise under ice bath stirring conditions to cause the titanium source to undergo a hydrolysis reaction, and an amorphous titanium dioxide layer is uniformly deposited on the surface of the heterojunction.

[0056] The titanium source is either isopropyl titanate or tetrabutyl titanate. The mass ratio of the bismuth halide-titanium carbide heterojunction to the titanium source is 1:0.01-0.1. The volume of water added is 1-3 times the volume of the titanium source. The dropping rate is 0.5-2 mL / min. The hydrolysis reaction time is 2-6 h.

[0057] When the titanium source comes into contact with water, it undergoes a hydrolysis and condensation reaction, forming a continuous amorphous titanium dioxide coating layer on the surface of the heterojunction, with a coating layer thickness of 1-5 nm.

[0058] Subsequently, calcination is carried out in an inert atmosphere of argon or nitrogen to obtain a heterojunction coated with an isolation layer; wherein the calcination temperature is 200-400℃ and the calcination time is 0.5-3h.

[0059] During the calcination process, the heat treatment under an inert atmosphere reduces some of the tetravalent titanium in the amorphous titanium dioxide layer to trivalent titanium, forming trivalent titanium self-doping defect sites. These defect sites have a strong chemical anchoring effect on the subsequently introduced zinc ions.

[0060] In step S5, the isolation layer-coated heterojunction is dispersed in methanol and ultrasonically dispersed to ensure that the isolation layer-coated heterojunction is uniformly dispersed in methanol, thereby obtaining a heterojunction-coated dispersion.

[0061] The dispersion concentration of the heterojunction coated by the isolation layer is 1-5 mg / mL, the ultrasonic power is 100-300 W, and the ultrasonic time is 30-60 min.

[0062] Methanol, as a dispersion medium, is well miscible with the subsequently added organic ligand solution, which is beneficial for the uniform nucleation and growth of zeolite imidazole ester framework materials on the surface of the coated heterojunction.

[0063] In step S6, under the protective atmosphere of argon or nitrogen and with stirring, metal salt solution and organic ligand solution are simultaneously added dropwise to the heterojunction dispersion. After the addition is complete, the mixture is allowed to stand and react, so that the zeolite imidazole ester framework material grows in situ on the surface of the heterojunction coated by the isolation layer.

[0064] The metal salt is zinc nitrate hexahydrate or zinc acetate, with a concentration of 0.05-0.2 mol / L. The organic ligand is 2-methylimidazole or benzimidazole, with a concentration of 0.2-1.0 mol / L. The molar ratio of metal salt to organic ligand is 1:4-12. The dropping rate is 1-5 mL / min, the stirring speed is 200-500 rpm, and the standing reaction time is 1-4 h.

[0065] The steric hindrance effect of the amorphous titanium dioxide isolation layer passivates the in-plane region of the bismuth halide sheet, allowing the zeolite imidazole ester framework material to nucleate and grow only at edge sites with higher energy and more abundant surface defects, thus fundamentally avoiding the in-plane blocking of the visible light absorption window of bismuth halide by the framework material.

[0066] The trivalent titanium defect sites on the surface of the isolation layer exert a strong chemical anchoring effect on zinc ions, significantly enhancing the interfacial bonding strength between the framework material and the heterojunction substrate, and delaying the hydrolysis and dissolution of the framework material under weakly alkaline and humid alternating environments.

[0067] After the reaction is complete, the product is washed with methanol 2-3 times to remove unreacted raw materials.

[0068] Subsequently, vacuum activation treatment is performed to remove residual solvent molecules in the pores of the framework material, fully exposing the microporous structure of the framework material and endowing it with the ability to reversibly adsorb and release carbon dioxide, thus obtaining a visible light responsive titanium dioxide composite photocatalyst for formaldehyde removal and odor elimination; wherein, the vacuum activation temperature is 100-200℃ and the activation time is 1-6h.

[0069] In the gypsum board surface coating, the obtained composite photocatalyst, with its edge-loaded zeolite imidazole ester framework material, generates gas perturbations through the reversible adsorption and release of carbon dioxide. This perturbs the stagnant gas concentration boundary layer on the surface of the board surface layer, forcibly pumping the slowly released formaldehyde from deep within the board core to the catalytic site. Under the premise of ensuring efficient utilization of visible light and long-term structural stability, it solves the purification stagnation problem caused by the pseudo-deactivation of the surface catalytic layer in a quasi-static air environment.

[0070] To further simplify and make the present invention achieve its objectives and effects, the present invention will be further illustrated in conjunction with the following specific embodiments and comparative examples, but the present invention is not limited to the scope of the embodiments described herein.

[0071] It should be noted that the raw materials used in the examples and comparative examples are described below:

[0072] Titanium aluminum carbide: purity 98.5%, purchased from Shijiazhuang Dongming New Material Technology Co., Ltd.

[0073] Lithium fluoride: molecular weight 25.94, density 2.635, CAS number 7789-24-4, purchased from Jinan Zian Chemical Co., Ltd.

[0074] Bismuth nitrate pentahydrate: purity 99%, molecular weight 485.07, CAS number 10035-06-0, purchased from Jiangxi Haoshuo Chemical Co., Ltd.

[0075] Bismuth chloride: content 99%, density 4.75, CAS number 7787-60-2, purchased from Shandong Xindongneng Chemical Co., Ltd.

[0076] Potassium iodide: 98% purity, CAS number 7681-11-0, purchased from Wuhan Jiyesheng Chemical Co., Ltd.

[0077] Sodium iodide: 99% purity, CAS number 7681-82-5, purchased from Wuhan Jiyesheng Chemical Co., Ltd.

[0078] Tetrabutyl titanate: 99% purity, CAS number 5593-70-4, purchased from Shandong Shengrui Chemical Technology Co., Ltd.

[0079] Isopropyl titanate: 99% purity, molecular weight 284.215, CAS number 546-68-9, purchased from Shandong Xuguang Chemical Co., Ltd.

[0080] Zinc nitrate hexahydrate: purity 99%, product number 10196-18-6, purchased from Hubei Rishengchang New Material Technology Co., Ltd.

[0081] Zinc acetate: purity 99.5%, CAS number 557-34-6, purchased from Chongqing Maidekai Pharmaceutical Co., Ltd.

[0082] 2-Methylimidazole: purity 99%, CAS number 693-98-1, purchased from Shandong Daike Biotechnology Co., Ltd.

[0083] Benzimidazole: purity ≥98%, CAS number 51-17-2, purchased from Hubei Weideli Chemical Reagent Co., Ltd.

[0084] Hydrochloric acid: Product number 1270110101600, CAS number 7647-01-0, molecular weight 36.46, purchased from Xilong Scientific Co., Ltd.

[0085] Ethylene glycol: purity 99.5%, CAS number 107-21-1, purchased from Shandong Changxing Plastic Additives Co., Ltd.

[0086] Anhydrous ethanol: Shandong Yifei Science and Trade Co., Ltd.

[0087] Methanol: Nanjing Chemical Reagent Co., Ltd.

[0088] Argon gas: purity 99.999%, purchased from Hubei Newride Electronic Gas Co., Ltd.

[0089] Example 1:

[0090] S1. Weigh 1 part of titanium aluminum carbide powder and 2 parts of lithium fluoride. Dissolve the lithium fluoride in 9 mol / L hydrochloric acid to prepare an etching solution. Then add titanium aluminum carbide powder to the solution, controlling the solid-liquid ratio to 1:20 g / mL. Etch at 35℃ for 27 h. After etching, wash repeatedly with deionized water until the pH is 6.5. Then, perform ultrasonic peeling in an ice bath under an argon protective atmosphere. The ultrasonic power is 200 W and the ultrasonic time is 2 h to obtain titanium carbide nanosheets with a thickness of 2-10 nm.

[0091] S2. The obtained titanium carbide nanosheets were dispersed in ethylene glycol and ultrasonically dispersed under ice bath conditions. The ultrasonic power was 200W and the ultrasonic time was 45min to obtain a titanium carbide dispersion in which the dispersion concentration of titanium carbide nanosheets was 3mg / mL.

[0092] S3. Add an ethanol solution containing bismuth nitrate pentahydrate and potassium iodide to the above titanium carbide dispersion, controlling the molar ratio of titanium carbide to bismuth source to be 0.0275:1 and the molar ratio of bismuth element to halogen element to be 1:2; after stirring and mixing evenly, transfer to a reaction vessel and solvothermal reaction at 160℃ for 16h. After natural cooling, wash and dry to obtain bismuth halide-titanium carbide heterojunction.

[0093] S4. The obtained bismuth halide-titanium carbide heterojunction was dispersed in anhydrous ethanol, and tetrabutyl titanate was added, with 1 part heterojunction and 0.055 parts tetrabutyl titanate. Under ice bath stirring conditions, deionized water was added dropwise at a rate of 1.25 mL / min, with the amount added being twice the volume of tetrabutyl titanate. The stirring and hydrolysis reaction was continued for 4 h to form an amorphous titanium dioxide layer on the surface of the heterojunction. After filtration and washing, the mixture was calcined at 300 °C for 1.75 h in an argon atmosphere to obtain an isolation layer coating the heterojunction. This isolation layer contains trivalent titanium self-doped defect sites.

[0094] S5. The obtained isolation layer-coated heterojunction is dispersed in methanol and ultrasonically dispersed at an ultrasonic power of 200W for 45min to obtain a heterojunction-coated dispersion, wherein the dispersion concentration of the isolation layer-coated heterojunction is 3mg / mL.

[0095] S6. Under an argon protective atmosphere and with stirring at a speed of 350 rpm, a methanol solution of zinc nitrate hexahydrate with a concentration of 0.125 mol / L and a methanol solution of 2-methylimidazole with a concentration of 0.6 mol / L were simultaneously added dropwise to the above-mentioned heterojunction-coated dispersion. The molar ratio of metal salt to organic ligand was controlled at 1:8, and the dropping rate was 3 mL / min. After the addition was completed, the reaction was allowed to stand for 2.5 h to allow the zeolite imidazole ester framework material to grow in a directional manner at the edge sites of the heterojunction coated by the isolation layer. After the reaction was completed, the mixture was washed three times with methanol and then activated under vacuum at 150 °C for 3.5 h to obtain a visible light responsive titanium dioxide composite photocatalyst for formaldehyde removal and odor elimination.

[0096] Example 2:

[0097] This embodiment is basically the same as that of embodiment 1, except that the bismuth source in S3 is different. Specifically, in step S3, bismuth pentahydrate nitrate is replaced with bismuth chloride. The molar ratio of bismuth to halogen is still 1:2. The rest is the same as in embodiment 1.

[0098] Example 3:

[0099] This embodiment is basically the same as that of embodiment 1, except that the halogen source in S3 is different. Specifically, in step S3, potassium iodide is replaced with sodium iodide, and the molar ratio of bismuth to halogen is still 1:2. The rest is the same as in embodiment 1.

[0100] Example 4:

[0101] This embodiment is basically the same as that of embodiment 1, except that the titanium source in S4 is different. Specifically, in step S4, tetrabutyl titanate is replaced with isopropyl titanate, and the amount is still 0.055 parts. The rest is the same as that of embodiment 1.

[0102] Example 5:

[0103] This embodiment is basically the same as that of embodiment 1, except that the metal salt in S6 is different. Specifically, in step S6, zinc nitrate hexahydrate is replaced with zinc acetate, and the molar ratio of metal salt to organic ligand is still 1:8. The rest is the same as in embodiment 1.

[0104] Example 6:

[0105] This embodiment is basically the same as that of embodiment 1, except that the organic ligand in S6 is different. Specifically, in step S6, 2-methylimidazole is replaced with benzimidazole, and the molar ratio of metal salt to organic ligand is still 1:8. The rest is the same as that of embodiment 1.

[0106] Example 7:

[0107] This embodiment is basically the same as Embodiment 1, except that: in S1, the mass ratio of titanium aluminum carbide to lithium fluoride is taken as the minimum value of the range, specifically: the mass ratio of titanium aluminum carbide to lithium fluoride is changed to 1:1, and the remaining steps are the same as in Embodiment 1.

[0108] Example 8:

[0109] This embodiment is basically the same as Embodiment 1, except that: in S1, the mass ratio of titanium aluminum carbide to lithium fluoride is taken as the maximum value in the range, specifically: the mass ratio of titanium aluminum carbide to lithium fluoride is changed to 1:3, and the remaining steps are the same as in Embodiment 1.

[0110] Example 9:

[0111] This embodiment is basically the same as Embodiment 1, except that: in S3, the molar ratio of titanium carbide to bismuth source is taken as the minimum value of the range, specifically: the molar ratio of titanium carbide to bismuth source is changed to 0.005:1, and the remaining steps are the same as in Embodiment 1.

[0112] Example 10:

[0113] This embodiment is basically the same as Embodiment 1, except that: in S3, the molar ratio of titanium carbide to bismuth source is taken as the maximum value of the range, specifically: the molar ratio of titanium carbide to bismuth source is changed to 0.05:1, and the remaining steps are the same as in Embodiment 1.

[0114] Example 11:

[0115] This embodiment is basically the same as Embodiment 1, except that: in S6, the molar ratio of metal salt to organic ligand is taken as the minimum value of the range, specifically: the molar ratio of metal salt to organic ligand is changed to 1:4, and the remaining steps are the same as in Embodiment 1.

[0116] Example 12:

[0117] This embodiment is basically the same as Embodiment 1, except that: in S6, the molar ratio of metal salt to organic ligand is taken as the maximum value of the range, specifically: the molar ratio of metal salt to organic ligand is changed to 1:12, and the remaining steps are the same as in Embodiment 1.

[0118] Example 13:

[0119] This embodiment is basically the same as that of embodiment 1, except that the dispersion concentration of titanium carbide nanosheets in S2 is taken as the minimum value of the range, specifically: the dispersion concentration of titanium carbide nanosheets is changed to 1 mg / mL, and the remaining steps are the same as those in embodiment 1.

[0120] Example 14:

[0121] This embodiment is basically the same as that of Embodiment 1, except that the dispersion concentration of titanium carbide nanosheets in S2 is taken as the maximum value of the range, specifically: the dispersion concentration of titanium carbide nanosheets is changed to 5 mg / mL, and the remaining steps are the same as those in Embodiment 1.

[0122] Example 15:

[0123] This embodiment is basically the same as Embodiment 1, except that: in S4, the mass ratio of bismuth halide-titanium carbide heterojunction to titanium source is taken as the minimum value in the range, specifically: the mass ratio of bismuth halide-titanium carbide heterojunction to tetrabutyl titanate is changed to 1:0.01, and the remaining steps are the same as in Embodiment 1.

[0124] Example 16:

[0125] This embodiment is basically the same as Embodiment 1, except that: in S4, the mass ratio of bismuth halide-titanium carbide heterojunction to titanium source is taken as the maximum value in the range, specifically: the mass ratio of bismuth halide-titanium carbide heterojunction to tetrabutyl titanate is changed to 1:0.1, and the remaining steps are the same as in Embodiment 1.

[0126] Comparative Example 1:

[0127] The process method of this comparative example differs from that of Example 1. It adopts a conventional pure-phase bismuth halide photocatalyst preparation process, and the specific steps are as follows:

[0128] S1. Add bismuth nitrate pentahydrate and potassium iodide to ethylene glycol at a molar ratio of bismuth to iodine of 1:2. Stir at 300 rpm for 20 min at room temperature to fully dissolve the solid raw materials and obtain a clear and transparent precursor solution.

[0129] S2. Transfer the above precursor solution to a stainless steel reactor lined with polytetrafluoroethylene, seal it, and place it in a constant temperature oven for a solvothermal reaction at 160°C for 16 hours. After the reaction is completed, allow it to cool naturally to room temperature.

[0130] S3. Open the reaction vessel, separate the obtained precipitate from the reaction liquid, and wash the precipitate three times alternately with deionized water and anhydrous ethanol. After each washing, centrifuge at 4000 rpm for 5 min to collect the precipitate.

[0131] S4. Place the washed precipitate in a vacuum drying oven at 60℃ and dry for 12 hours to fully remove residual solvent.

[0132] S5. Grind the dried product into a uniform powder using an agate mortar, pass it through a 200-mesh sieve, collect the sieve residue, and obtain a pure phase bismuth iodide photocatalyst.

[0133] Comparative Example 2:

[0134] This comparative example is basically the same as Example 1, except that the ice bath ultrasonic peeling step in S1 is omitted. The specific steps of S1 are as follows: Weigh 1 part of titanium aluminum carbide powder and 2 parts of lithium fluoride, dissolve lithium fluoride in hydrochloric acid with a concentration of 9 mol / L to prepare an etching solution, then add titanium aluminum carbide powder to it, control the solid-liquid ratio to be 1:20 g / mL, and etch at 35°C for 27 h; after etching, wash repeatedly with deionized water until the pH is 6.5, and then filter and dry directly under an argon protective atmosphere without ice bath ultrasonic peeling to obtain multilayer stacked titanium carbide material. The remaining steps are the same as in Example 1.

[0135] Comparative Example 3:

[0136] This comparative example is basically the same as Example 1, except that: the titanium carbide nanosheets in S3 are omitted and the heterojunction is not constructed. The specific steps of S3 are as follows: the ethanol solution containing bismuth nitrate pentahydrate and potassium iodide is directly transferred into the reaction vessel without adding titanium carbide dispersion, and the reaction is carried out at 160°C for 16 hours in a solvothermal manner. After natural cooling, the mixture is washed and dried to obtain pure phase bismuth halide. The remaining steps are the same as in Example 1.

[0137] Comparative Example 4:

[0138] This comparative example is basically the same as Example 1, except that the amorphous titanium dioxide isolation layer construction in S4 is omitted. The specific steps of S4 are: the obtained bismuth halide-titanium carbide heterojunction is directly used as the isolation layer to coat the heterojunction without titanium source hydrolysis coating and calcination treatment, and directly proceeds to S5. The remaining steps are the same as in Example 1.

[0139] Comparative Example 5:

[0140] This comparative example is basically the same as Example 1, except that the inert atmosphere calcination step in S4 is omitted. The specific steps of S4 are as follows: the obtained bismuth halide-titanium carbide heterojunction is dispersed in anhydrous ethanol, and tetrabutyl titanate is added, with 1 part of heterojunction and 0.055 parts of tetrabutyl titanate; under ice bath stirring conditions, deionized water is added dropwise at a rate of 1.25 mL / min, with the amount added being twice the volume of tetrabutyl titanate, and the stirring and hydrolysis reaction is continued for 4 hours to form an amorphous titanium dioxide layer on the surface of the heterojunction; after filtration and washing, it is directly dried without inert atmosphere calcination to obtain an isolation layer coating the heterojunction, and the remaining steps are the same as in Example 1.

[0141] Comparative Example 6:

[0142] This comparative example is basically the same as Example 1, except that the isolation layer coating heterojunction in S6 is omitted, and ZIF-8 is synthesized directly under substrate-free conditions. The specific steps of S6 are as follows: under an argon protective atmosphere and with stirring at a speed of 350 rpm, a methanol solution of zinc nitrate hexahydrate with a concentration of 0.125 mol / L and a methanol solution of 2-methylimidazole with a concentration of 0.6 mol / L are added dropwise to methanol simultaneously, controlling the molar ratio of metal salt to organic ligand to be 1:8, and the dropping rate to be 3 mL / min; after the addition is completed, the reaction is allowed to stand for 2.5 h; after the reaction is completed, the mixture is washed three times with methanol, and then activated under vacuum at 150 °C for 3.5 h to obtain pure phase ZIF-8 material, which is then mixed with the isolation layer coating heterojunction by stirring for 2 h. The remaining steps are the same as in Example 1.

[0143] Comparative Example 7:

[0144] This comparative example is basically the same as Example 1, except that the mass ratio of titanium aluminum carbide to lithium fluoride in S1 is lower than the minimum value in the range. The specific steps of S1 are as follows: the mass ratio of titanium aluminum carbide to lithium fluoride is changed to 1:0.5, and the remaining steps are the same as in Example 1.

[0145] Comparative Example 8:

[0146] This comparative example is basically the same as Example 1, except that the mass ratio of titanium aluminum carbide to lithium fluoride in S1 is higher than the maximum value in the range. The specific steps of S1 are as follows: the mass ratio of titanium aluminum carbide to lithium fluoride is changed to 1:4. The remaining steps are the same as in Example 1.

[0147] Comparative Example 9:

[0148] This comparative example is basically the same as Example 1, except that the molar ratio of titanium carbide to bismuth source in S3 is lower than the minimum value in the range. The specific steps of S3 are as follows: the molar ratio of titanium carbide to bismuth source is changed to 0.001:1. The remaining steps are the same as in Example 1.

[0149] Comparative Example 10:

[0150] This comparative example is basically the same as Example 1, except that the molar ratio of titanium carbide to bismuth source in S3 is higher than the maximum value in the range. The specific steps of S3 are as follows: the molar ratio of titanium carbide to bismuth source is changed to 0.1:1. The remaining steps are the same as in Example 1.

[0151] Comparative Example 11:

[0152] This comparative example is basically the same as Example 1, except that the molar ratio of metal salt to organic ligand in S6 is lower than the minimum value in the range. The specific steps of S6 are as follows: the molar ratio of metal salt to organic ligand is changed to 1:2. The remaining steps are the same as in Example 1.

[0153] Comparative Example 12:

[0154] This comparative example is basically the same as Example 1, except that the molar ratio of metal salt to organic ligand in S6 is higher than the maximum value in the range. The specific steps of S6 are as follows: the molar ratio of metal salt to organic ligand is changed to 1:15. The remaining steps are the same as in Example 1.

[0155] Comparative Example 13:

[0156] This comparative example is basically the same as Example 1, except that the dispersion concentration of titanium carbide nanosheets in S2 is lower than the minimum value of the range. The specific steps of S2 are as follows: the dispersion concentration of titanium carbide nanosheets is changed to 0.5 mg / mL, and the rest is the same as S2 in Example 1.

[0157] Comparative Example 14:

[0158] This comparative example is basically the same as Example 1, except that the dispersion concentration of titanium carbide nanosheets in S2 is higher than the maximum value in the range. The specific steps of S2 are as follows: the dispersion concentration of titanium carbide nanosheets is changed to 6 mg / mL, and the rest is the same as S2 in Example 1.

[0159] Comparative Example 15:

[0160] This comparative example is basically the same as Example 1, except that the mass ratio of bismuth halide-titanium carbide heterojunction to titanium source in S4 is lower than the minimum value in the range. The specific steps of S4 are as follows: the mass ratio of bismuth halide-titanium carbide heterojunction to tetrabutyl titanate is changed to 1:0.005, and the rest is the same as S4 in Example 1.

[0161] Comparative Example 16:

[0162] This comparative example is basically the same as Example 1, except that the mass ratio of the bismuth halide-titanium carbide heterojunction to the titanium source in S4 is higher than the maximum value in the range. The specific steps of S4 are as follows: the mass ratio of the bismuth halide-titanium carbide heterojunction to tetrabutyl titanate is changed to 1:0.15, and the rest is the same as S4 in Example 1.

[0163] Performance testing: The visible light responsive titanium dioxide composite formaldehyde removal and odor elimination photocatalysts obtained in Examples 1-16 and Comparative Examples 1-16 were subjected to performance tests in sequence, including in-plane shading loss rate, core formaldehyde escape rate, boundary layer breaking coefficient, active site coverage index, and skeleton shedding rate. The results are shown in Table 1.

[0164] In-plane occlusion loss rate: 20 mg each of the composite photocatalyst of this invention and a control sample without titanium dioxide isolation layer were taken. The diffuse reflectance spectra were measured in the 400-800 nm wavelength range using a UV-Vis diffuse reflectance spectrometer, with barium sulfate as a reference. The diffuse reflectance spectra were converted to the absorption function F(R) using the Kubelka-Munk function, and the integrated absorption area of ​​each sample in the visible region was calculated. The integrated area of ​​the sample of this invention is denoted as... The integral area of ​​the control sample is denoted as In-plane occlusion loss rate Calculate using the following formula: The unit is a percentage. The lower the value, the more effective the isolation layer is in spatial regulation of ZIF-8 nucleation sites, and the smaller the loss of visible light utilization caused by in-plane shading.

[0165] Formaldehyde emission rate from the core of the board: Plasterboard coated with photocatalyst was placed in a 1m... 3In a sealed reaction chamber, the bottom and sides of the gypsum board were sealed with aluminum foil tape, exposing only the front coating. 50 μL of a formaldehyde standard solution (1000 ppm concentration) was injected into the core of the board, and the injection port was immediately sealed after injection. The LED visible light source inside the chamber was turned on at a light intensity of 5000 lux, and the formaldehyde concentration inside the chamber was continuously monitored for 72 hours. The formaldehyde concentration at 24 hours and 72 hours was recorded. and Formaldehyde release rate from the core of the board Calculate using the following formula: The unit is a percentage. This value reflects the ability of gas micro-perturbations generated by the ZIF-8 edge load to continuously break the stagnant boundary layer. The higher the value, the better the effect of continuously pumping formaldehyde deep in the core to the catalytic site.

[0166] Boundary layer breaking coefficient: A gypsum board coated with photocatalyst was placed in a horizontal laminar flow duct with an air velocity of 0.1 m / s. The local airflow velocity at distances of 0.5 mm, 1 mm, 2 mm, 3 mm, 5 mm, and 10 mm from the board surface was measured using a hot-wire anemometer and recorded as _____. A blank gypsum board without photocatalyst coating was used as a control. The airflow velocity at various distances on the control board surface was recorded as follows: Boundary layer failure coefficient Calculate using the following formula: A value greater than 1 indicates that the gas perturbation on the surface of the photocatalyst has a breaking effect on the stagnant boundary layer.

[0167] Active site coverage index: 20 mg each of the composite photocatalyst of this invention and the control sample without titanium dioxide isolation layer were placed in a quartz tube fixed bed reactor. An air stream containing 100 ppb formaldehyde was introduced under visible light irradiation at a space velocity of 10000 h⁻¹. -1 The CO2 concentration in the outlet gas was continuously monitored using an online mass spectrometer. The steady-state CO2 concentration was recorded after the CO2 generation rate stabilized. The CO2 concentration of the sample in this invention is denoted as [missing information]. The CO2 concentration of the sample without the isolation layer is denoted as Active site coverage index Calculate using the following formula: The unit is a percentage; a higher value indicates that the isolation layer avoids in-plane occlusion of active sites by the framework material.

[0168] Framework shedding rate: 50 mg of the composite photocatalyst of this invention was placed in 100 mL of sodium bicarbonate buffer solution (pH 8.5) and incubated at 40 °C with constant shaking for 24 h at a shaking frequency of 150 rpm. After shaking, the mixture was centrifuged, and the supernatant was collected. The zinc ion concentration in the supernatant was determined using inductively coupled plasma atomic emission spectrometry (ICP-AES). Separately, an equal volume of the original sample that was not soaked in buffer solution was digested with aqua regia and its total zinc content was determined. Skeletal detachment rate Calculate using the following formula: ,in The buffer volume is 100 mL, and m is the sample mass of 50 mg. The unit is percentage. The lower the value, the stronger the anchoring effect of trivalent titanium defects on zinc ions.

[0169] Table 1: Performance test results of visible light responsive titanium dioxide composite photocatalysts for formaldehyde removal and odor elimination in Examples 1-16 and Comparative Examples 1-16

[0170] Group In-plane occlusion loss rate (%) Formaldehyde evaporation rate from the core of the board (%) Boundary layer failure coefficient Active site coverage index (%) Skeletal detachment rate (%) Example 1 3.2 91.7 3.58 95.4 3.8 Example 2 3.5 90.2 3.42 94.8 4.1 Example 3 3.4 90.8 3.49 95.1 4.0 Example 4 3.3 91.2 3.52 95.3 3.9 Example 5 3.6 90.5 3.45 94.9 4.2 Example 6 3.7 90.1 3.41 94.6 4.3 Example 7 3.8 89.5 3.35 94.2 4.5 Example 8 3.1 92.3 3.65 95.8 3.6 Example 9 3.9 89.2 3.31 94.0 4.6 Example 10 3.0 92.8 3.71 96.0 3.5 Example 11 3.8 89.8 3.38 94.3 4.4 Example 12 3.1 92.0 3.62 95.6 3.7 Example 13 3.6 90.4 3.44 94.7 4.2 Example 14 3.3 91.3 3.53 95.2 3.9 Example 15 3.9 89.0 3.28 93.8 4.8 Example 16 2.8 93.5 3.78 96.5 3.2 Comparative Example 1 45.6 52.3 0.85 51.2 28.5 Comparative Example 2 18.7 68.4 1.52 72.6 15.3 Comparative Example 3 42.8 48.6 0.78 48.9 32.1 Comparative Example 4 35.2 55.8 0.92 55.4 24.6 Comparative Example 5 6.8 78.5 2.15 88.3 18.9 Comparative Example 6 28.4 62.1 1.18 63.7 22.4 Comparative Example 7 12.5 75.3 1.85 80.5 12.8 Comparative Example 8 8.2 82.1 2.42 85.6 9.5 Comparative Example 9 10.8 77.6 2.05 82.3 11.2 Comparative Example 10 6.5 83.4 2.58 87.1 8.8 Comparative Example 11 14.2 72.8 1.72 76.4 14.5 Comparative Example 12 7.8 84.2 2.68 86.5 8.2 Comparative Example 13 11.6 76.5 1.95 81.2 12.3 Comparative Example 14 6.2 84.8 2.75 87.8 7.9 Comparative Example 15 22.5 65.8 1.35 69.4 18.2 Comparative Example 16 5.5 86.5 2.92 90.2 7.2

[0171] A comparison between Example 1 and Comparative Example 1 reveals that: Comparative Example 1 is a pure-phase bismuth oxyiodide photocatalyst, lacking titanium carbide electron transport medium; in pure-phase bismuth oxyiodide, photogenerated electrons cannot be effectively extracted, and electrons and holes undergo radiative recombination in the bulk phase, resulting in a reduction in the number of holes migrating to the surface; simultaneously, the pure-phase bismuth oxyiodide surface lacks ZIF-8, thus failing to generate a gas disturbance effect, and the stagnant boundary layer remains intact, reducing the formaldehyde escape rate from the core to 52.3%; due to the lack of an isolation layer, the bismuth oxyiodide sheets undergo hydroxylation transformation on the surface in a weakly alkaline environment, gradually deactivating active sites, and increasing the skeleton shedding rate to 28.5%.

[0172] A comparison between Example 1 and Comparative Example 2 reveals that: Comparative Example 2 omitted the ice bath ultrasonic exfoliation step, resulting in a multilayered, densely stacked state of titanium carbide; suitable ice bath ultrasonic exfoliation utilizes the cavitation effect to dissociate the multilayered titanium carbide into nanosheets with a thickness of 2 nm to 10 nm along the interlayer van der Waals force direction, while the ice bath inhibits the oxidation of Ti atoms on the nanosheet surface to form a TiOx insulating layer; without exfoliation, the interlayer spacing of titanium carbide decreases, the specific surface area decreases, bismuth oxyhalide can only nucleate at limited sites on the outer surface of the aggregate, the contact area of ​​the heterojunction interface decreases, the electron interface transfer efficiency decreases, the in-plane shading loss rate increases to 18.7%, and the formaldehyde escape rate of the core plate decreases to 68.4%.

[0173] A comparison between Example 1 and Comparative Example 3 shows that: Comparative Example 3 completely omits titanium carbide nanosheets and synthesizes pure phase bismuth halide alone; the introduction of titanium carbide provides a highly conductive carrier, whose Fermi level is lower than the conduction band bottom of bismuth halide. After the two come into contact, a built-in electric field is established, which shortens the electron migration time to the picosecond level and greatly reduces the recombination probability; without titanium carbide, electrons have nowhere to migrate, the recombination rate increases, and the active site coverage index drops to 48.9%. At the same time, ZIF-8 is directly loaded in the bismuth halide plane, and the in-plane shading loss rate reaches 42.8%.

[0174] A comparison between Example 1 and Comparative Example 4 reveals that: Comparative Example 4 omitted the construction of the titanium dioxide isolation layer, and ZIF-8 was directly loaded onto the bismuth halide-titanium carbide heterostructure; without the isolation layer, the nucleation barrier difference between the in-plane region and the edge region was not significant, and ZIF-8 grew non-selectively both in-plane and at the edges; the in-plane ZIF-8 particle size ranged from 50 nm to 200 nm, covering the 001 crystal plane of bismuth halide, blocking the photon incident path and shielding the active sites, with the in-plane shielding loss rate increasing to 35.2% and the active site coverage index reaching 55.4%; in addition, without the isolation layer anchoring, ZIF-8 was attached only by van der Waals forces, and the framework detachment rate reached 24.6%.

[0175] A comparison between Example 1 and Comparative Example 5 shows that: Comparative Example 5 omitted the inert atmosphere calcination step, and no trivalent titanium defects were formed in the titanium dioxide layer; without calcination, all titanium elements were in the form of Ti. 4+ Existence, lack of Ti 3+ The 3d unpaired electron orbitals cannot interact with Zn 2+ To form ligand field-stabilized bonds, the ZIF-8 zinc cluster nodes are attached only by electrostatic force, resulting in insufficient interfacial bonding strength and a framework detachment rate of 18.9%. At the same time, the uncalcined titanium dioxide layer has a loose structure, weakening the spatial confinement effect. Some ZIF-8 can still nucleate in the plane, with an in-plane shading loss rate of 6.8%.

[0176] A comparison between Example 1 and Comparative Example 6 reveals that: Comparative Example 6 synthesized pure-phase ZIF-8 separately and then physically mixed it with a heterostructure coated with an isolation layer; during the physical mixing, ZIF-8 had no chemical bonding or epitaxial relationship with the substrate, and ZIF-8 was randomly distributed, possibly adhering to edges or within the surface, thus losing the selectivity of nucleation sites; the lattice micro-strain generated by CO2 adsorption-desorption in the ZIF-8 channels could not be effectively transferred to the substrate, making it difficult to generate gas disturbance, with a boundary layer breaking coefficient of only 1.18 and a formaldehyde escape rate of 62.1% from the core; the loosely contacted ZIF-8 was easily detached in the liquid phase, with a skeleton detachment rate of 22.4%.

[0177] A comparison of Examples 1 and Examples 2-6 reveals that: Examples 2-6 respectively replaced the bismuth source with bismuth chloride, the halogen source with sodium iodide, the titanium source with isopropyl titanate, the metal salt with zinc acetate, and the organic ligand with benzimidazole; the hydrolysis rate of bismuth chloride was faster than that of bismuth nitrate pentahydrate, resulting in excessively rapid formation of bismuth halide nuclei and a decrease in crystallinity; the different iodide ion release rates in sodium iodide affected the anisotropy of the bismuth halide morphology; the smaller steric hindrance of the alkyl chain in isopropyl titanate led to a faster hydrolysis and polycondensation rate, resulting in slightly poorer uniformity of the titanium dioxide layer; the different solubility of zinc acetate in methanol and the different zinc ion dissociation rates compared to zinc nitrate affected the nucleation density of ZIF-8; the larger molecular size of benzimidazole than that of 2-methylimidazole caused changes in the micropore size and CO2 adsorption capacity of ZIF-8; all the above substitutions resulted in slightly lower performance indicators than in Example 1, but all were superior to the comparative example.

[0178] A comparison of Examples 1 / 7-8 with Comparative Examples 7-8 reveals that the mass ratio of Ti3AlC2 to LiF affects the amount of HF generated during the etching reaction. Examples 7 (mass ratio 1:1) and 8 (mass ratio 1:3) yielded 2 to 5 layers of titanium carbide with lateral dimensions of 200 nm to 500 nm. In Comparative Example 7 (mass ratio 1:0.5), insufficient HF resulted in incomplete etching of the aluminum atomic layers, leading to a titanium carbide yield of only 30% and a reduction in the effective heterojunction area. In Comparative Example 8 (mass ratio 1:4), excessive HF over-etched the titanium carbide, introducing lattice vacancies and edge defects, disrupting the two-dimensional conductive network, decreasing electron mobility, and causing the nanosheets to break into fragments smaller than 50 nm, thus losing the large planar conditions required for epitaxial growth.

[0179] A comparison of Examples 1 / 9-10 and Comparative Examples 9-10 reveals that the molar ratio of titanium carbide to bismuth source determines the composition ratio of the heterojunction. In Example 9, a molar ratio of 0.005:1 and in Example 10, a molar ratio of 0.05:1 resulted in a continuous and uniform interface. In Comparative Example 9, with a molar ratio of 0.001:1, the titanium carbide volume fraction was too low, resulting in a large amount of bismuth halide without titanium carbide contact, lacking electron extraction channels, and causing an exponential increase in recombination probability when electrons migrate along grain boundaries. In Comparative Example 10, with a molar ratio of 0.1:1, excess titanium carbide spontaneously stacked and agglomerated, forming a phase-separated structure. Exposed titanium carbide became non-specific nucleation sites, leading to indiscriminate deposition of ZIF-8 and a decrease in the active site coverage index to 87.1%.

[0180] A comparison of Examples 1 / 11-12 and Comparative Examples 11-12 shows that: Zn 2+ The molar ratio of ZIF-8 to 2-methylimidazolium determines the nucleation density and crystal integrity of ZIF-8; in the comparative example, the molar ratio of 1:2 indicates insufficient ligand, resulting in only partial Zn formation. 2+ Participating in skeleton construction, free Zn 2+The edge ZIF-8 nuclei were washed away, resulting in a small number of nuclei and a weakened gas disturbance effect, with a boundary layer breaking coefficient of 1.72. In the comparative example, the molar ratio of 1:15 was 12, with an excess of ligands. The homogeneous nucleation rate in the liquid phase was accelerated, and a large number of ZIF-8 nuclei were formed independently in the liquid phase, consuming the precursor. This resulted in a decrease in the load on the substrate edges, and the formaldehyde escape rate of the core was 84.2%.

[0181] A comparison of Examples 1 / 13-14 and Comparative Examples 13-14 reveals that the concentration of titanium carbide dispersion affects the collision frequency with the bismuth source precursor. In Example 13, a concentration of 1 mg / mL and in Example 14, a concentration of 5 mg / mL maintained stable monodispersion. In Comparative Example 13, a concentration of 0.5 mg / mL resulted in insufficient titanium carbide per unit volume, leading to homogeneous aggregation of bismuth halide nuclei and reduced heterojunction recombination efficiency. In Comparative Example 14, a concentration of 6 mg / mL reduced the spacing between titanium carbides, resulting in face-to-face stacking and edge overlap, forming three-dimensional aggregates. The internal titanium carbides could not contact the bismuth source, reducing effective utilization, and the aggregates were prone to sedimentation.

[0182] A comparison of Examples 1 / 15-16 and Comparative Examples 15-16 reveals that the mass ratio of the heterojunction to the titanium source determines the thickness of the isolation layer. In Example 15, a mass ratio of 1:0.01 and in Example 16, a mass ratio of 1:0.1 corresponds to thicknesses of 1 nm to 2 nm and 4 nm to 5 nm, respectively, forming a continuous and dense layer. In Comparative Example 15, a mass ratio of 1:0.005 results in insufficient titanium source, leading to an isolated island-like distribution of the isolation layer, with exposed in-plane regions. This induces in-plane nucleation of ZIF-8, increasing the in-plane shading loss rate to 22.5% and reducing the active site coverage index to 69.4%. In Comparative Example 16, a mass ratio of 1:0.15 results in an isolation layer thickness exceeding 10 nm. This excessive thickness increases the electron tunneling distance, reduces interface transfer efficiency, and simultaneously buries edge defect sites, leading to a decrease in ZIF-8 loading and a formaldehyde escape rate of 86.5% from the core.

[0183] Based on the preferred embodiments of the present invention described above, those skilled in the art can make various changes and modifications without departing from the inventive concept. The technical scope of this invention is not limited to the contents of the specification, but must be determined according to the scope of the claims.

Claims

1. A method for preparing a visible light-responsive titanium dioxide composite photocatalyst for formaldehyde removal and odor elimination, characterized in that, Includes the following steps: S1. Titanium aluminum carbide powder is etched in hydrochloric acid etching solution containing lithium fluoride, washed until neutral, and then ultrasonically exfoliated in an ice bath under a protective atmosphere to obtain titanium carbide nanosheets; wherein, the mass ratio of titanium aluminum carbide to lithium fluoride is 1:1-3. S2. The titanium carbide nanosheets are dispersed in ethylene glycol and ultrasonically dispersed in an ice bath to obtain a titanium carbide dispersion; wherein the dispersion concentration of the titanium carbide nanosheets is 1-5 mg / mL. S3. Add an organic solution of bismuth source and halogen source to the titanium carbide dispersion, stir and mix, and then perform a solvothermal reaction to obtain a bismuth halide-titanium carbide heterojunction; wherein, the molar ratio of titanium carbide to bismuth source in the titanium carbide dispersion is 0.005-0.05:

1. S4. The bismuth halide-titanium carbide heterojunction is dispersed in anhydrous ethanol, a titanium source is added, and water is added dropwise under ice bath stirring to hydrolyze the titanium source, forming an amorphous titanium dioxide layer. The layer is then calcined in an inert atmosphere to obtain an isolation layer coating the heterojunction. S5. The isolation layer-coated heterojunction is dispersed in methanol and ultrasonically dispersed to obtain a heterojunction-coated dispersion; wherein the dispersion concentration of the isolation layer-coated heterojunction is 1-5 mg / mL. S6. Under a protective atmosphere and with stirring, a metal salt solution and an organic ligand solution are simultaneously added dropwise to the coated heterojunction dispersion. The mixture is allowed to stand for reaction, washed, and activated under vacuum to obtain the final complex. The molar ratio of the metal salt to the organic ligand is 1:4-12.

2. The preparation method of the visible light responsive titanium dioxide composite formaldehyde removal and odor-eliminating photocatalyst according to claim 1, characterized in that: In step S1, the solid-liquid ratio of titanium aluminum carbide to the hydrochloric acid etching solution is 1:10-30, the etching temperature is 20-50℃, and the etching time is 18-36h; the thickness of the titanium carbide nanosheets is 2-10nm.

3. The preparation method of the visible light responsive titanium dioxide composite formaldehyde removal and odor-eliminating photocatalyst according to claim 1, characterized in that: In step S1, the concentration of hydrochloric acid is 8-10M, and the washing is water washing until the pH is 6.0-7.

0.

4. The preparation method of the visible light responsive titanium dioxide composite formaldehyde removal and odor-eliminating photocatalyst according to claim 1, characterized in that: In step S3, the bismuth source is bismuth nitrate pentahydrate or bismuth chloride, the halogen source is potassium iodide or sodium iodide, and the molar ratio of bismuth source to halogen source is 1:1-3 based on bismuth element to halogen element; the temperature of the solvothermal reaction is 120-200℃, and the time is 8-24h.

5. The preparation method of the visible light responsive titanium dioxide composite photocatalyst for formaldehyde removal and odor elimination according to claim 1, characterized in that: In step S4, the titanium source is isopropyl titanate or tetrabutyl titanate; the mass ratio of the bismuth halide-titanium carbide heterojunction to the titanium source is 1:0.01-0.

1.

6. The preparation method of the visible light responsive titanium dioxide composite formaldehyde removal and odor-eliminating photocatalyst according to claim 1, characterized in that: In step S4, the thickness of the amorphous titanium dioxide layer is 1-5 nm, and the isolation layer covers the surface of the heterojunction containing trivalent titanium self-doped defect sites.

7. The preparation method of the visible light responsive titanium dioxide composite formaldehyde removal and odor-eliminating photocatalyst according to claim 1, characterized in that: In step S4, the calcination temperature is 200-400℃ and the time is 0.5-3h.

8. The preparation method of the visible light responsive titanium dioxide composite formaldehyde removal and odor-eliminating photocatalyst according to claim 1, characterized in that: In step S6, the metal salt is zinc nitrate hexahydrate or zinc acetate, and the organic ligand is 2-methylimidazole or benzimidazole.

9. The preparation method of the visible light responsive titanium dioxide composite photocatalyst for formaldehyde removal and odor elimination according to claim 1, characterized in that: In step S6, the static reaction time is 1-4 hours, and the vacuum activation temperature is 100-200℃ for 1-6 hours.