A method for preparing lithium sulfate from lithium carbonate mother liquor

By combining acidification treatment and selective electrodialysis with two-stage resin to deeply remove impurity ions, the pollution and efficiency problems in the process of preparing lithium sulfate from lithium carbonate mother liquor were solved, realizing the industrial production of high-purity lithium sulfate and improving the comprehensive utilization rate of lithium resources.

CN123105683APending Publication Date: 2026-11-17JINGMEN GEM NEW MATERIAL CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611502083.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for preparing lithium sulfate from lithium carbonate mother liquor suffer from problems such as colloidal and heavy metal contamination of the membrane and resin, short equipment lifespan, poor operational stability, difficulty in achieving both sodium removal depth and lithium recovery rate with a single sodium removal unit, long process route, high energy consumption, and insufficient economic efficiency.

Method used

Acidification was used to remove colloidal suspended matter and heavy metals. Lithium and sodium were coarsely separated by concentration and selective electrodialysis. Impurity ions were removed by two-stage tandem resin, and the mixture was purified in stages. Finally, high-purity lithium sulfate crystals were prepared by crystallization.

Benefits of technology

It achieves efficient removal of colloids and heavy metals, reduces resin load, has low lithium loss, and introduces no organic impurities, making it suitable for industrial-scale production. It can prepare high-purity lithium sulfate crystals with a purity of over 99.58% and a lithium recovery rate of over 96.5%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This application provides a method for preparing lithium sulfate from lithium carbonate mother liquor, comprising the following steps: acidifying the lithium carbonate mother liquor with concentrated sulfuric acid to remove colloidal suspended matter to obtain a sulfate solution; subjecting the sulfate solution to heavy metal removal treatment to obtain a pretreated solution; concentrating the pretreated solution to obtain a concentrated feed solution; subjecting the concentrated feed solution to selective electrodialysis treatment to obtain a low-sodium lithium sulfate solution; using a two-stage tandem resin to adsorb and remove impurities from the low-sodium lithium sulfate solution to obtain a lithium sulfate-rich solution; and crystallizing the lithium sulfate-rich solution to obtain lithium sulfate crystals. The method for preparing lithium sulfate from lithium carbonate mother liquor provided in this application can directly prepare high-purity lithium sulfate crystals from lithium carbonate mother liquor, making it suitable for industrial-scale applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of lithium carbonate mother liquor treatment technology, and relates to a method for preparing lithium sulfate from lithium carbonate mother liquor. Background Technology

[0002] Lithium carbonate is a core lithium salt used in lithium-ion battery cathode materials and electrolyte salts. The lithium carbonate precipitation process generates a large amount of lithium carbonate mother liquor. This mother liquor still contains a certain concentration of lithium ions (typically 1–10 g / L), along with various impurity ions such as sodium, potassium, calcium, magnesium, and heavy metals, as well as suspended solids such as silicate colloids and aluminum hydroxide colloids. Direct discharge of this mother liquor not only results in a serious waste of lithium resources but also causes environmental pollution. Therefore, the efficient recovery of lithium from lithium carbonate mother liquor and the production of high-value-added lithium sulfate products has significant economic and environmental value. Lithium sulfate, especially battery-grade lithium sulfate, is an important raw material for the preparation of lithium-ion battery cathode materials and electrolyte lithium salts, and market demand continues to grow. The production of lithium sulfate from lithium carbonate mother liquor can achieve the cascade utilization of lithium resources, extend the industrial chain, and improve the comprehensive utilization rate of lithium resources.

[0003] The existing technologies for preparing lithium sulfate from lithium carbonate mother liquor generally have the following technical bottlenecks: (1) impurities such as colloids and heavy metals in the mother liquor can easily cause subsequent membrane module fouling and resin poisoning, resulting in short equipment life and poor operational stability; (2) a single sodium removal unit cannot take into account both sodium removal depth and lithium recovery rate, either resulting in large lithium loss or incomplete sodium removal, making it impossible to stably produce battery-grade lithium sulfate; (3) the solvent extraction route introduces organic impurities, posing a risk of product contamination; (4) the process route is long, energy consumption is high, and reagent consumption is large, resulting in insufficient economic efficiency and making it difficult to achieve industrial-scale application.

[0004] Therefore, developing a method for preparing lithium sulfate from lithium carbonate mother liquor that can efficiently remove colloids and heavy metals, remove sodium impurities in a stepwise and deep manner, has low lithium loss, does not introduce organic impurities, is stable in operation, and is suitable for industrial scale-up is a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the purpose of this application is to provide a method for preparing lithium sulfate from lithium carbonate mother liquor. This application first pre-treats the lithium carbonate mother liquor by acidification to remove colloidal suspended solids and heavy metals, preventing contamination of the membrane and resin by colloids and heavy metals. After concentration and selective electrodialysis, lithium and sodium are coarsely separated, reducing the subsequent resin load. Then, a two-stage series resin is used to deeply remove impurity ions, resulting in graded purification with low lithium loss and no introduction of organic impurities. The resulting lithium sulfate solution can be directly crystallized to produce battery-grade lithium sulfate crystals. This method realizes the recovery of lithium carbonate mother liquor to prepare high-purity lithium sulfate crystals, suitable for industrial-scale production.

[0006] To achieve the purpose of this application, the following technical solution is adopted: This application provides a method for preparing lithium sulfate from lithium carbonate mother liquor, the method comprising the following steps: After acidifying the lithium carbonate mother liquor with concentrated sulfuric acid to remove colloidal suspended matter, a sulfate solution is obtained. The sulfate solution is then subjected to heavy metal removal treatment to obtain a pretreated solution. The pretreatment solution is concentrated to obtain a concentrated feed solution, which is then subjected to selective electrodialysis to obtain a low-sodium lithium sulfate solution. A low-sodium lithium sulfate solution was subjected to adsorption and impurity removal treatment using a two-stage tandem resin to obtain a lithium sulfate-rich solution. The lithium sulfate-rich solution was then subjected to crystallization treatment to obtain lithium sulfate crystals.

[0007] In some possible implementations, the endpoint pH of the acidification treatment is 4 to 6.

[0008] In some possible implementations, the stirring speed of the acidification treatment is 150 rpm to 300 rpm.

[0009] In some possible implementations, the method of removing colloidal suspensions includes precision ultrafiltration.

[0010] In some possible implementations, the heavy metal removal agent used in the heavy metal removal treatment includes oxalic acid.

[0011] In some possible implementations, the pH of the heavy metal removal treatment is 3 to 5.

[0012] In some possible implementations, the pretreatment solution contains Ca 2+ Mass concentration <1 mg / L, Mg 2+ The mass concentration is <1.5 mg / L.

[0013] In some possible implementations, the concentrated feed liquid contains Li + The mass concentration is 3g / L~7g / L.

[0014] In some possible implementations, the concentrated feed liquid contains Na + mass concentration <Na + saturation concentration.

[0015] In some possible implementations, the selective electrodialysis treatment of the concentrated feed solution includes: assembling an electrodialysis membrane stack using a lithium sodium ion selective permeation membrane between the electrode chambers, setting up alternating dilute and concentrated chambers, passing the concentrated feed solution into the dilute chamber, passing dilute sulfuric acid into the concentrated chamber, using sodium sulfate electrolyte in the electrode chambers, performing electrodialysis treatment by applying electricity, collecting a low-sodium lithium sulfate solution in the concentrated chamber, and obtaining a high-sodium sulfate solution in the dilute chamber.

[0016] In some possible implementations, the lithium sodium ion selective permeation membrane comprises an LCM composite membrane.

[0017] In some possible implementations, the molar concentration of the sodium sulfate electrolyte in the electrode chamber is 0.05 mol / L to 0.2 mol / L.

[0018] In some possible implementations, the current density of the electrodialysis treatment is 10 mA / cm². 2 ~15mA / cm 2 .

[0019] In some possible implementations, during the electrodialysis treatment, the flow rate of the concentrated feed solution is 5 L / (h·m). 2 ~15L / (h·m) 2 ).

[0020] In some possible implementations, the low-sodium lithium sulfate solution contains Na + and Li + The molar ratio is ≤5:1, preferably ≤1:1.

[0021] In some possible implementations, the first stage of the two-stage tandem resin comprises an aminophosphonic acid chelating resin.

[0022] In some possible implementations, the second stage of the two-stage tandem resin comprises a crown ether type monovalent cationic selective resin.

[0023] In some possible implementations, during the adsorption and impurity removal process, the flow rate of the low-sodium lithium sulfate solution is 1 BV / h to 4 BV / h.

[0024] In some possible implementations, the lithium sulfate-rich solution contains Na + Content <10ppm.

[0025] In some possible implementations, the cooling rate of the crystallization process is 0.3℃ / h to 1.5℃ / h.

[0026] In some possible implementations, the crystallization treatment temperature is 58°C to 62°C.

[0027] In some possible implementations, the crystallization process is followed by centrifugation and drying to obtain lithium sulfate crystals and a mother liquor, the mother liquor being recycled as a pretreatment solution.

[0028] The numerical range described in this application includes not only the point values ​​listed above, but also any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific point values ​​included in the range.

[0029] Compared with the prior art, this application has the following advantages: (1) The method for preparing lithium sulfate from lithium carbonate mother liquor provided in this application first acidifies the lithium carbonate mother liquor to remove colloidal suspended matter and performs heavy metal pretreatment to avoid contamination of subsequent membranes and resins by colloidal and heavy metals; then, it achieves coarse separation of lithium and sodium by concentration and selective electrodialysis to reduce the resin treatment load; then, it uses two-stage series resin to deeply remove sodium impurities, and performs graded purification. It has strong anti-interference ability, low lithium loss, and does not introduce organic impurities. High-purity lithium sulfate crystals can be directly prepared from lithium carbonate mother liquor, which is suitable for industrial-scale application.

[0030] (2) The method for preparing lithium sulfate from lithium carbonate mother liquor provided in this application can achieve a purity of over 99.58% and a lithium recovery rate of over 96.5% for lithium sulfate prepared from lithium carbonate mother liquor. Detailed Implementation

[0031] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.

[0032] The scope of this application can be defined by lower and upper limits. The selected lower and upper limits define the boundaries of a specific range. The range defined in this way can be defined by the inclusion or exclusion of endpoints. Any endpoint can be independently selected for inclusion or exclusion, and all lower and upper limits can be arbitrarily combined to form new ranges. That is, any lower limit can be combined with any upper limit to form a valid range. For example, if the ranges of 60~120 and 80~110 are listed for specific parameters, it should be understood that the ranges of 60~110 and 80~120 also fall within the scope of this application. In addition, if the minimum range values ​​1 and 2 are listed, and the maximum range values ​​3, 4 and 5 are also listed, then all ranges of 1~3, 1~4, 1~5, 2~3, 2~4 and 2~5 fall within the scope of this application. In this application, the numerical range "a~b" represents a shortened representation of any combination of real numbers between a and b, where a and b are both real numbers. For example, the numerical range "0~5" means that all real numbers between 0 and 5 have been fully listed in this document, and "0~5" is only a shortened representation of this set of numerical combinations. When a parameter is expressed as an integer ≥2, it is equivalent to listing positive integers that meet the requirements, such as 2, 3, 4, 5, 6, 7, 8, 9, 10, etc. When a parameter is expressed as an integer selected from "2~10", it is equivalent to listing any integer among 2, 3, 4, 5, 6, 7, 8, 9, and 10.

[0033] In this application, "at least two combinations" refers to a quantity greater than or equal to 2 unless otherwise specified. For example, "any one or at least two combinations" means any one of the listed items, or a combination of at least two of the listed items formed in a manner that does not conflict and enables the implementation of this application. In this application, unless otherwise specified, the features or solutions corresponding to "and / or" cover any one of two or more related listed items, as well as any and all combinations of the related listed items. The arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. For example, "A and / or B" represents a set consisting of A, B, and combinations of A and B, where "containing A and / or B" can be understood, depending on the context of the statement, as containing A, containing B, or simultaneously containing both A and B. In this application, "optional" means that the corresponding feature, component, step or solution is not necessary, that is, it is selected from either "with" or "without". If there are multiple "optional" limitations in a technical solution, unless otherwise specified and there is no technical conflict or mutual constraint, each "optional" limitation is independent and does not affect the others.

[0034] In this application, technical features or solutions described using open-ended terms such as "comprising" or "including" do not exclude additional non-conflicting elements beyond those listed unless otherwise specified. They are considered to disclose both closed-ended features or solutions consisting solely of the listed elements and open-ended features or solutions that may include additional non-conflicting elements beyond the listed elements. For example, if A includes a1, a2, and a3, unless otherwise specified, this means that A can consist only of a1, a2, and a3, or it can include other non-conflicting elements based on a1, a2, and a3. This corresponds to the disclosure of technical solutions such as "A consists of a1, a2, and a3," "A is selected from a1, a2, and a3," and "A not only includes a1, a2, and a3, but may also include other non-conflicting elements." All embodiments and optional embodiments of this application, unless otherwise specified and without technical conflict, can be combined to form new technical solutions, and such combinations fall within the scope of this application. The term "embodiment" as used in this application means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of this application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. Those skilled in the art can understand, explicitly and implicitly, that the embodiments described in this application can be combined with other embodiments that do not conflict with the technology.

[0035] In this application, the order in which the steps are written in the methods described in the various embodiments does not imply a strict order of execution. The actual order of execution of each step should be determined according to its function and possible internal logic. Unless otherwise specified, all steps in this application can be executed in the order in which they are written or in any order without technical conflict.

[0036] This application provides a method for preparing lithium sulfate from lithium carbonate mother liquor, the method comprising the following steps: After acidifying the lithium carbonate mother liquor with concentrated sulfuric acid to remove colloidal suspended matter, a sulfate solution is obtained. The sulfate solution is then subjected to heavy metal removal treatment to obtain a pretreated solution. The pretreatment solution is concentrated to obtain a concentrated feed solution, which is then subjected to selective electrodialysis to obtain a low-sodium lithium sulfate solution. A low-sodium lithium sulfate solution was subjected to adsorption and impurity removal treatment using a two-stage tandem resin to obtain a lithium sulfate-rich solution. The lithium sulfate-rich solution was then subjected to crystallization treatment to obtain lithium sulfate crystals.

[0037] This application first uses concentrated sulfuric acid to remove CO3 from the lithium carbonate mother liquor. 2- and HCO3 - The substance is converted and removed as CO2, simultaneously transforming into a sulfate system and removing the colloidal suspensions generated therein, in order to remove Ca. 2+ Mg 2+ Other heavy metal impurities were removed to obtain a pretreated solution. This pretreated solution was then concentrated to obtain a feed solution with suitable lithium and sodium concentrations. Electrodialysis was then performed using a suitable ion exchange membrane to achieve preliminary separation of lithium and sodium. By selecting appropriate ion exchange membranes for Li... + and Na + Ion exchange membranes with differentially selective permeation properties enable Li + Prioritize migration to the product side, while transferring most of the Na + The sodium content in the resulting lithium sulfate solution is significantly reduced by retaining or enriching it on the other side, thus lowering the processing load of subsequent deep sodium removal processes. A two-stage tandem resin is then used to adsorb and remove impurities from the low-sodium lithium sulfate solution, deeply removing residual trace amounts of calcium, magnesium, other transition metal impurities, and residual trace sodium ions, resulting in a high-purity lithium sulfate-rich solution that meets the pre-treatment requirements for battery-grade raw materials. After concentration and crystallization, high-purity lithium sulfate crystals are obtained, enabling lithium recovery.

[0038] In some embodiments, the endpoint pH of the acidification treatment is 4 to 6, for example: 4, 4.5, 5, 5.5 or 6, etc., not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0039] The lithium carbonate mother liquor contains silica-alumina colloids, heavy metals, and calcium and magnesium hydroxides, which can easily cause membrane module fouling and resin pore poisoning. This application addresses this by first acidifying the lithium carbonate mother liquor with concentrated sulfuric acid to remove CO3 from it. 2- and HCO3 - The process completely decomposes and destroys silica and aluminum hydroxide colloids, removes colloidal suspensions through flocculation and filtration, and completely converts the salts in them into sulfates, thus achieving preliminary impurity removal.

[0040] In some embodiments, the stirring speed of the acidification treatment is 150 rpm to 300 rpm, for example: 150 rpm, 180 rpm, 200 rpm, 250 rpm or 300 rpm, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0041] In some embodiments, the method for removing colloidal suspensions includes precision ultrafiltration.

[0042] In some embodiments, the heavy metal removal agent used in the heavy metal removal treatment includes oxalic acid.

[0043] This application uses oxalic acid to remove heavy metals, which removes most of the heavy metals in the system without introducing other impurities, reduces membrane fouling in subsequent electrodialysis and prevents resin adsorption sites from being competitively occupied, thus extending the service life of the membrane stack and resin and reducing the cost of impurity removal.

[0044] In some embodiments, the pH of the heavy metal removal treatment is 3 to 5, for example: 3, 3.5, 4, 4.5 or 5, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0045] In some embodiments, the pretreatment solution contains Ca 2+ Mass concentration <1 mg / L, Mg 2+ The mass concentration is <1.5 mg / L.

[0046] In some embodiments, the concentrated feed liquid contains Li + The mass concentration is 3g / L to 7g / L, for example: 3g / L, 4g / L, 5g / L, 6g / L or 7g / L, etc., not limited to the listed values, and other unlisted values ​​within this range also apply.

[0047] In some embodiments, the concentrated feed liquid contains Na + mass concentration <Na + saturation concentration.

[0048] This application involves concentrating the pretreatment solution to increase the lithium ion concentration within the system, thereby improving the lithium-sodium separation efficiency. The concentrated feed solution contains Na... + mass concentration <Na+ The saturation concentration, i.e., the concentration of sodium sulfate, is less than the saturation solubility of sodium sulfate at that concentration.

[0049] In some embodiments, the selective electrodialysis treatment of the concentrated feed solution includes: assembling an electrodialysis membrane stack using a lithium sodium ion selective permeation membrane between the electrode chambers, setting up alternating dilute and concentrated chambers, passing the concentrated feed solution into the dilute chamber, passing dilute sulfuric acid into the concentrated chamber, using sodium sulfate electrolyte in the electrode chambers, performing electrodialysis treatment by applying electricity, collecting a low-sodium lithium sulfate solution in the concentrated chamber, and obtaining a high-sodium sulfate solution in the dilute chamber.

[0050] In some embodiments, the lithium-sodium ion selective permeation membrane comprises an LCM composite membrane.

[0051] This application uses a specific LCM composite membrane for electrodialysis treatment. The specific LCM composite membrane allows lithium ions to pass through preferentially, while only a small amount of sodium ions can pass through. The separation selectivity of lithium and sodium can reach more than 10, and at a low current density, the separation selectivity of lithium and sodium can reach more than 40, but the separation efficiency is too low. This application uses electrodialysis treatment to achieve the preliminary separation of lithium and sodium, reducing the pressure of subsequent resin impurity removal.

[0052] In some embodiments, the molar concentration of the sodium sulfate electrolyte in the electrode chamber is 0.05 mol / L to 0.2 mol / L, for example: 0.05 mol / L, 0.08 mol / L, 0.1 mol / L, 0.15 mol / L or 0.2 mol / L, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0053] In some embodiments, the current density of the electrodialysis treatment is 10 mA / cm². 2 ~15mA / cm 2 For example: 10mA / cm 2 11mA / cm 2 12mA / cm 2 13mA / cm 2 14mA / cm 2 Or 15mA / cm 2 The term "etc." is not limited to the listed values; it also applies to other unlisted values ​​within the range.

[0054] In some embodiments, during the electrodialysis process, the flow rate of the concentrated feed solution is 5 L / (h·m). 2 ~15L / (h·m) 2 For example: 5L / (h·m) 2 ), 8L / (h·m 2 ), 10L / (h·m 2 ), 12L / (h·m2 ) or 15L / (h·m 2 )wait.

[0055] In some embodiments, in the low-sodium lithium sulfate solution, Na + and Li + The molar ratio is ≤5:1, preferably ≤1:1.

[0056] In some embodiments, the first stage of the two-stage tandem resin comprises an aminophosphonic acid chelating resin.

[0057] In some embodiments, the second stage of the two-stage tandem resin comprises a crown ether type monovalent cationic selective resin.

[0058] This application uses a two-stage series resin for impurity removal. The first stage uses aminophosphonic acid chelating resin to deeply remove residual trace amounts of calcium, magnesium and transition metal impurities. The second stage is filled with crown ether type monovalent cation selective resin to selectively adsorb residual trace amounts of sodium ions. Lithium ions permeate out, and the sodium ion content of the feed solution is reduced to below 10 ppm after treatment, which meets the pre-selective indicators for battery-grade raw materials.

[0059] In some embodiments, during the adsorption and impurity removal process, the flow rate of the low-sodium lithium sulfate solution is 1 BV / h to 4 BV / h.

[0060] In some embodiments, the lithium sulfate-rich solution contains Na + Content <10ppm.

[0061] In some embodiments, the cooling rate of the crystallization process is 0.3℃ / h to 1.5℃ / h, for example: 0.3℃ / h, 0.5℃ / h, 1℃ / h, 1.2℃ / h or 1.5℃ / h, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0062] In some embodiments, the temperature of the crystallization process is 58°C to 62°C, for example: 58°C, 59°C, 60°C, 61°C or 62°C, etc., and is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0063] In some embodiments, after the crystallization treatment, centrifugation and drying are performed to obtain lithium sulfate crystals and crystallization mother liquor, wherein the crystallization mother liquor is recycled as a pretreatment solution.

[0064] This application describes a process where a refined high-purity lithium sulfate solution is concentrated to a slightly supersaturated state via MVR evaporation, during which no solid crystals precipitate. The supersaturated solution is then transferred to a cooling crystallizer and cooled at a gradient rate of 0.3℃ / h to 1.5℃ / h to suppress sodium salt crystal inclusions. Cooling is stopped at 58℃ to 62℃, and crystal growth is performed within this isothermal range to directionally precipitate lithium sulfate monohydrate crystals. After centrifugal solid-liquid separation and hot air drying at 60℃ to 90℃, battery-grade lithium sulfate crystals are obtained, and the mother liquor is recycled as a pretreatment solution.

[0065] The mass concentrations of each element in the lithium carbonate mother liquor used in the embodiments and comparative examples of this application are shown in Table 1 below: Table 1 The mass composition of the LCM composite membrane used in the embodiments of this application is as follows: 50.5% LICGC, 25.5% PECH-DABCO, 18% PES-NH2 and 6% BRIJ76.

[0066] Example 1 This embodiment provides a method for preparing lithium sulfate from lithium carbonate mother liquor, the method comprising the following steps: Concentrated sulfuric acid was mixed with lithium carbonate mother liquor and acidified at a stirring speed of 200 rpm until the final pH of the acidification was 5. Colloidal suspensions were removed by precision ultrafiltration to obtain a sulfate solution. Oxalic acid was then mixed with the sulfate solution, and heavy metal removal was performed while maintaining the pH at 4 to obtain Ca. 2+ The mass concentration is 0.2 mg / L, Mg 2+ The pretreatment solution had a mass concentration of 0.5 mg / L; The pretreatment solution was concentrated to obtain Li. + A concentrated feed solution with a mass concentration of 5 g / L (the concentrated feed solution contains Na) + The mass concentration of Na at this temperature is < + (At the saturated concentration, no sodium sulfate precipitated), an electrodialysis membrane stack is assembled using an LCM composite membrane between the electrode chambers, with alternating dilute and concentrated chambers. The concentrated feed solution is passed into the dilute chamber at a flow rate of 10 L / (h·m). 2 0.1 mol / L dilute sulfuric acid is passed into the concentration chamber, and 0.1 mol / L sodium sulfate electrolyte is used in the electrode chamber. An electric current is applied at 12 mA / cm². 2 Electrodialysis was performed, and a low-sodium lithium sulfate solution (Na) was collected in the concentration chamber. + and Li + The molar ratio was 0.5:1), and a high sodium sulfate solution was obtained in the dilute chamber. Using a two-stage tandem resin (the first stage being an aminophosphonic acid chelating resin and the second stage being a crown ether type monovalent cation selective resin), the flow rate of the low-sodium lithium sulfate solution was controlled at 2 BV / h to adsorb and remove impurities, resulting in a lithium sulfate-rich solution. The lithium sulfate-rich solution was then concentrated to a slightly supersaturated state by MVR evaporation, without the precipitation of solid crystals during the MVR concentration process. The supersaturated solution was transferred to a cooling crystallizer and cooled in a gradient at a rate of 1℃ / h until it reached 60℃. Cooling was then stopped, and crystal growth was carried out in this isothermal range to directionally precipitate lithium sulfate monohydrate crystals. After centrifugal solid-liquid separation and hot air drying at 70℃, lithium sulfate crystals were obtained, and the mother liquor was recycled as a pretreatment solution.

[0067] Example 2 This embodiment provides a method for preparing lithium sulfate from lithium carbonate mother liquor, the method comprising the following steps: Concentrated sulfuric acid was mixed with lithium carbonate mother liquor and acidified at a stirring speed of 150 rpm until the final pH of the acidification was 4. Colloidal suspensions were removed by precision ultrafiltration to obtain a sulfate solution. Oxalic acid was then mixed with the sulfate solution, and heavy metal removal was performed while maintaining the pH at 3 to obtain Ca. 2+ The mass concentration is 0.15 mg / L, Mg 2+ The pretreatment solution had a mass concentration of 0.4 mg / L; The pretreatment solution was concentrated to obtain Li. + A concentrated feed solution with a mass concentration of 3 g / L (the concentrated feed solution contains Na) + The mass concentration of Na at this temperature is < + (At the saturated concentration, no sodium sulfate precipitated), an electrodialysis membrane stack is assembled using an LCM composite membrane between the electrode chambers, with alternating dilute and concentrated chambers. The concentrated feed solution is passed into the dilute chamber at a flow rate of 15 L / (h·m). 2 0.1 mol / L dilute sulfuric acid is passed into the concentration chamber, and 0.05 mol / L sodium sulfate electrolyte is used in the electrode chamber. An electric current is applied at 10 mA / cm². 2 Electrodialysis was performed, and a low-sodium lithium sulfate solution (Na) was collected in the concentration chamber. + and Li + The molar ratio was 0.3:1), and a high sodium sulfate solution was obtained in the dilute chamber. A two-stage tandem resin (the first stage being an aminophosphonic acid chelating resin, and the second stage being a crown ether type monovalent cation selective resin) was used to adsorb and remove impurities from the low-sodium lithium sulfate solution at a flow rate of 4 BV / h, resulting in a lithium sulfate-rich solution. This solution was then concentrated to a slightly supersaturated state using MVR evaporation, without the precipitation of solid crystals during the MVR concentration process. The supersaturated solution was transferred to a cooling crystallizer and cooled at a gradient rate of 0.3℃ / h until it reached 62℃. Cooling was then stopped, and crystal growth was performed within this isothermal range to directionally precipitate lithium sulfate monohydrate crystals. After centrifugal solid-liquid separation and hot air drying at 80℃, lithium sulfate crystals were obtained. The mother liquor from the crystallization was recycled as a pretreatment solution.

[0068] Example 3 This embodiment provides a method for preparing lithium sulfate from lithium carbonate mother liquor, the method comprising the following steps: Concentrated sulfuric acid was mixed with lithium carbonate mother liquor and acidified at a stirring speed of 300 rpm until the final pH of the acidification was 6. Colloidal suspensions were removed by precision ultrafiltration to obtain a sulfate solution. Oxalic acid was then mixed with the sulfate solution, and heavy metal removal was performed while maintaining the pH at 5 to obtain Ca. 2+ The mass concentration is 0.3 mg / L, Mg 2+ The pretreatment solution had a mass concentration of 0.7 mg / L; The pretreatment solution was concentrated to obtain Li. + A concentrated feed solution with a mass concentration of 7 g / L (the concentrated feed solution contains Na) + The mass concentration of Na at this temperature is < + (At the saturation concentration, no sodium sulfate precipitated), an electrodialysis membrane stack is assembled using an LCM composite membrane between the electrode chambers, with alternating dilute and concentrated chambers. The concentrated feed solution is passed into the dilute chamber at a flow rate of 5 L / (h·m). 2 0.1 mol / L dilute sulfuric acid is passed into the concentration chamber, and 0.2 mol / L sodium sulfate electrolyte is used in the electrode chamber. An electric current is applied at 15 mA / cm². 2 Electrodialysis was performed, and a low-sodium lithium sulfate solution (Na) was collected in the concentration chamber. + and Li + The molar ratio was 0.8:1), and a high sodium sulfate solution was obtained in the dilute chamber. A two-stage tandem resin (the first stage being an aminophosphonic acid chelating resin, and the second stage being a crown ether type monovalent cation selective resin) was used to adsorb and remove impurities from the low-sodium lithium sulfate solution at a flow rate of 1 BV / h, resulting in a lithium sulfate-rich solution. This solution was then concentrated to a slightly supersaturated state using MVR evaporation, without the precipitation of solid crystals during the MVR concentration process. The supersaturated solution was transferred to a cooling crystallizer and cooled at a gradient rate of 1.5℃ / h until it reached 58℃. Cooling was then stopped, and crystal growth was performed within this isothermal range to directionally precipitate lithium sulfate monohydrate crystals. After centrifugal solid-liquid separation and hot air drying at 80℃, lithium sulfate crystals were obtained. The mother liquor was recycled as a pretreatment solution.

[0069] Example 4 The only difference between this embodiment and Embodiment 1 is that the current density for electrodialysis is 20 mA / cm². 2 Other conditions and parameters are exactly the same as in Example 1.

[0070] Example 5 The only difference between this embodiment and Embodiment 1 is that, during the electrodialysis process, the flow rate of the concentrated feed solution is 20 L / (h·m). 2 The other conditions and parameters are exactly the same as in Example 1.

[0071] Example 6 The only difference between this embodiment and Embodiment 1 is that the flow rate of the low-sodium lithium sulfate solution is 0.5 BV / h during the adsorption and impurity removal process. All other conditions and parameters are exactly the same as in Embodiment 1.

[0072] Example 7 The only difference between this embodiment and Embodiment 1 is that the flow rate of the low-sodium lithium sulfate solution is 5 BV / h during the adsorption and impurity removal process; all other conditions and parameters are exactly the same as in Embodiment 1.

[0073] Comparative Example 1 The only difference between this comparative example and Example 1 is that electrodialysis is not performed; all other conditions and parameters are exactly the same as in Example 1.

[0074] Comparative Example 2 The only difference between this comparative example and Example 1 is that only a crown ether type monovalent cation selective resin is used for adsorption and impurity removal; all other conditions and parameters are exactly the same as in Example 1.

[0075] Performance testing: The purity of lithium sulfate was tested and the lithium recovery rate was calculated. The test results are shown in Table 2. Table 2 As can be seen from Table 2, as shown in Examples 1 to 7, the method for preparing lithium sulfate from lithium carbonate mother liquor provided in this application can achieve a purity of over 98.93% and a lithium recovery rate of over 93.5% for lithium sulfate obtained using lithium carbonate mother liquor. By adjusting the preparation conditions, the purity of the obtained lithium sulfate can reach over 99.58% and the lithium recovery rate can reach over 96.5%.

[0076] A comparison of Examples 1 and 4-5 shows that, in the method for preparing lithium sulfate from lithium carbonate mother liquor provided in this application, the flow rate of the concentrated feed solution and the current density of the electrodialysis process both affect the recovery effect. Controlling the flow rate of the concentrated feed solution at 5 L / (h·m) is recommended. 2 ~15L / (h·m) 2 The current density for electrodialysis treatment was controlled at 10 mA / cm². 2 ~15mA / cm 2 The recovery effect is relatively good. If the flow rate of the concentrated feed liquid is too fast or the current density of the electrodialysis treatment is too high, the lithium-sodium selectivity will decrease significantly, and the purity of the lithium sulfate and the lithium recovery rate will both decrease (if the flow rate of the concentrated feed liquid is too slow or the current density of the electrodialysis treatment is too low, although the separation effect of lithium and sodium can be slightly improved, the efficiency will be significantly reduced).

[0077] Comparing Examples 1 and 6-7, it can be seen that in the method for preparing lithium sulfate from lithium carbonate mother liquor provided in this application, the flow rate of the low-sodium lithium sulfate solution affects the impurity removal effect during the adsorption and impurity removal process. Controlling the flow rate of the low-sodium lithium sulfate solution to 1 BV / h~4 BV / h during the adsorption and impurity removal process yields better impurity removal results. If the flow rate of the low-sodium lithium sulfate solution is too fast, impurity ions do not have enough time to fully diffuse into the internal pores of the resin particles, only surface adsorption occurs, and the ion exchange reaction flows out of the resin column before reaching equilibrium, resulting in a decreased impurity removal effect. If the flow rate of the low-sodium lithium sulfate solution is too slow, the solution stays in the resin bed for too long, and some Li... + Lithium is adsorbed and retained by the resin, resulting in a decrease in lithium recovery rate.

[0078] As can be seen from the comparison between Example 1 and Comparative Example 1, this application uses a specific LCM composite membrane for electrodialysis treatment. The specific LCM composite membrane allows lithium ions to pass through preferentially, achieving the initial separation of lithium and sodium and reducing the pressure of subsequent resin impurity removal.

[0079] As can be seen from the comparison between Example 1 and Comparative Example 2, this application uses two-stage series resins for impurity removal. The first stage uses aminophosphonic acid chelating resin to deeply remove residual trace amounts of calcium, magnesium and transition metal impurities. The second stage is filled with crown ether type monovalent cation selective resin to selectively adsorb residual trace amounts of sodium ions. Multiple impurity removal ensures that the lithium sulfate solution meets the pre-selective indicators for battery-grade raw materials.

[0080] The applicant declares that the above description is only a specific implementation of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. A method for preparing lithium sulfate from lithium carbonate mother liquor, characterized in that, The method includes the following steps: After acidifying the lithium carbonate mother liquor with concentrated sulfuric acid to remove colloidal suspended matter, a sulfate solution is obtained. The sulfate solution is then subjected to heavy metal removal treatment to obtain a pretreated solution. The pretreatment solution is concentrated to obtain a concentrated feed solution, which is then subjected to selective electrodialysis to obtain a low-sodium lithium sulfate solution. A low-sodium lithium sulfate solution was subjected to adsorption and impurity removal treatment using a two-stage tandem resin to obtain a lithium sulfate-rich solution. The lithium sulfate-rich solution was then subjected to crystallization treatment to obtain lithium sulfate crystals.

2. The method as described in claim 1, characterized in that, The endpoint pH of the acidification treatment is 4-6; And / or, the stirring speed for the acidification treatment is 150 rpm to 300 rpm; And / or, the method of removing colloidal suspensions includes precision ultrafiltration.

3. The method as described in claim 1 or 2, characterized in that, The heavy metal removal agent used in the heavy metal removal treatment includes oxalic acid; And / or, the pH of the heavy metal removal treatment is 3-5; And / or, the Ca in the pretreatment solution 2+ Mass concentration <1 mg / L, Mg 2+ The mass concentration is <1.5 mg / L.

4. The method according to any one of claims 1-3, characterized in that, Li in concentrated feed liquid + The mass concentration is 3 g / L~7 g / L; And / or, the concentrated feed liquid contains Na + mass concentration <Na + saturation concentration.

5. The method according to any one of claims 1-4, characterized in that, The selective electrodialysis treatment of the concentrated feed solution includes: A lithium-sodium ion-selective permeation membrane is used to assemble an electrodialysis membrane stack between the electrode chambers. Alternating dilute and concentrated chambers are set up. The concentrated feed solution is passed into the dilute chamber, and dilute sulfuric acid is passed into the concentrated chamber. The electrode chamber uses sodium sulfate electrolyte. Electrodialysis is performed by passing electricity. A low-sodium lithium sulfate solution is collected in the concentrated chamber, and a high-sodium sulfate solution is obtained in the dilute chamber.

6. The method as described in claim 5, characterized in that, The lithium-sodium ion selective permeation membrane includes an LCM composite membrane; And / or, the molar concentration of the sodium sulfate electrolyte in the electrode chamber is 0.05 mol / L to 0.2 mol / L; And / or, the current density of the electrodialysis treatment is 10 mA / cm². 2 ~15mA / cm 2 ; And / or, during the electrodialysis treatment, the flow rate of the concentrated feed solution is 5 L / (h·m). 2 ~15L / (h·m) 2 ).

7. The method according to any one of claims 1-6, characterized in that, In the low-sodium lithium sulfate solution, Na + and Li + The molar ratio is ≤5:1, preferably ≤1:

1.

8. The method according to any one of claims 1-7, characterized in that, The first stage of the two-stage tandem resin includes an aminophosphonic acid chelating resin. And / or, the second stage of the two-stage tandem resin comprises a crown ether type monovalent cationic selective resin.

9. The method according to any one of claims 1-8, characterized in that, During the adsorption and impurity removal process, the flow rate of the low-sodium lithium sulfate solution is 1 BV / h to 4 BV / h. And / or, the Na in the lithium sulfate-rich solution + Content <10ppm.

10. The method according to any one of claims 1-9, characterized in that, The cooling rate of the crystallization process is 0.3℃ / h to 1.5℃ / h; And / or, the temperature of the crystallization treatment is 58°C to 62°C; And / or, after the crystallization treatment, centrifugation and drying are performed to obtain lithium sulfate crystals and crystallization mother liquor, wherein the crystallization mother liquor is recycled as a pretreatment solution.