Method for efficiently leaching lithium from waste lithium iron phosphate battery powder

Through the multiple leaching method of combining acid liquid and oxidant, the problems of organic solvent contamination and low lithium ion extraction efficiency in lithium iron phosphate battery recycling are solved, and the preparation of high-purity lithium carbonate is realized, showing an efficient and stable recycling process.

CN119040659APending Publication Date: 2024-11-29ANHUI LVWO RECYCLING ENERGY TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411495791.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-25
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art uses organic solvents in the recycling of lithium iron phosphate batteries to cause environmental pollution, and it is difficult to effectively extract lithium ions, and the leaching rate of other metal elements cannot be comprehensively considered.

Method used

After the waste lithium iron phosphate battery powder is crushed, pyrolyzed and sieved, the pH value is adjusted by combining acid and oxidizing agent, and the leaching rate of lithium ions is gradually increased, and other removals are removed through sodium hydroxide solution Metal ions are used to prepare high-purity and high conversion rate lithium carbonate.

Benefits of technology

It realizes efficient leaching of lithium ions and high purity of lithium carbonate products, avoids the use of organic solvents, improves the selectivity and leaching efficiency of lithium ions, and has a simple process and high stability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for efficiently leaching lithium by using waste lithium iron phosphate battery powder, and relates to the technical field of lithium battery recovery, and the method comprises the following steps: firstly, carrying out charged crushing, pyrolysis and screening on waste lithium iron phosphate batteries to obtain waste lithium iron phosphate battery powder; the lithium element in the waste lithium iron phosphate battery powder is selectively and efficiently leached by utilizing the synergistic effect of the acid liquor and the oxidizing agent through a multi-time leaching process, and a leaching solution is obtained; removing a small amount of impurity metal ions in the leachate by using a sodium hydroxide solution; and finally, precipitating with a sodium carbonate solution to obtain a high-purity lithium carbonate product. The method is simple in technological process and high in stability, efficient leaching of lithium ions can be achieved, and the purity of the lithium carbonate product is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of lithium battery recycling, and in particular to a method for efficiently leaching lithium using waste lithium iron phosphate battery powder. Background Art

[0002] Lithium-ion batteries have the advantages of high specific energy, long cycle stability, high operating voltage and low environmental pollution. They are widely used in new energy vehicles, energy storage power stations and portable devices. At present, the power batteries of new energy vehicles mainly include lithium cobalt oxide (LCO), lithium iron phosphate (LFP), ternary lithium (nickel cobalt manganese (NCM)) and nickel cobalt aluminum (NCA) batteries. Among them, lithium iron phosphate batteries stand out due to their low cost, good cycleability and high stability. However, the service life of lithium iron phosphate batteries is generally 5-8 years. With the increase in the scale of application of lithium iron phosphate batteries, their scrap volume is also increasing year by year. If the waste lithium iron phosphate batteries are not properly disposed of, it will not only cause a waste of resources such as lithium and iron, but may also cause serious environmental pollution problems.

[0003] The repair and regeneration process can repair the components and crystal defects of waste lithium iron phosphate active materials without destroying the original crystal structure of the material, and restore its electrochemical performance. For example, the publication number CN 115259130 A discloses a regeneration method for lithium iron phosphate recycled materials and a carbon-coated lithium iron phosphate material. First, the lithium iron phosphate recycled material, a lithium source and an organic solvent are mixed to obtain a mixed solution, and then iron citrate and / or ammonium iron citrate are added for iron supplementation. Then, a primary calcination and a secondary calcination are performed in sequence to obtain a carbon-coated lithium iron phosphate recycled material, which effectively repairs the crystal structure of the lithium iron phosphate recycled material, but the use of organic solvents such as benzene and toluene still brings many environmental problems. In addition, the repaired lithium iron phosphate positive electrode material is generally difficult to meet the standards of new power electrode materials. Summary of the invention

[0004] The purpose of the present invention is to provide a method for efficiently leaching lithium using waste lithium iron phosphate battery powder. One of the technical problems to be solved is to avoid the use of organic solvents in the process of recycling waste lithium iron phosphate batteries, and to only focus on the extraction of lithium without comprehensively considering the leaching rates of other metal elements such as iron.

[0005] To achieve the above object, the present invention provides the following technical solutions: A method for efficiently leaching lithium using waste lithium iron phosphate battery powder comprises the following steps: (1) The waste lithium iron phosphate battery is subjected to charged crushing, pyrolysis and screening to obtain waste lithium iron phosphate battery powder, and the pyrolysis temperature is 400-600°C; (2) Weigh the waste lithium iron phosphate battery powder obtained in step (1), add it to deionized water, heat it to 40-90° C., and stir it for 30-90 minutes to obtain a slurry; (3) adding acid and oxidant to the slurry obtained in step (2), adjusting the pH value, and then heating to 40-90° C. and stirring to react for 1-5 hours. After the reaction is completed, vacuum filtration is performed to obtain a leachate and leach residue; (4) Repeating the following steps more than once with the leached residue obtained in step (3): adding the leaching solution to the leached residue, stirring evenly, adding the acid solution and the oxidant, adjusting the pH value, heating to 40-90° C., stirring and reacting for 1-5 hours, and after the reaction is completed, vacuum filtering to obtain multiple leaching solutions; (5) Adding sodium hydroxide solution dropwise to the multiple leaching solutions obtained in step (4) to adjust the pH to 4-5, allowing the solution to stand for 0.5-2 hours, and obtaining a primary filtrate after impurity removal by vacuum filtration; (6) Add sodium hydroxide solution dropwise to the primary filtrate obtained in step (5) to adjust the pH to 8-9, let stand for 0.5-2 hours, and obtain a secondary filtrate after impurity removal by vacuum filtration; (7) The secondary filtrate obtained in step (6) after impurity removal is placed in a water bath at 80-95°C to concentrate it to 20-30 g / L, and then sodium carbonate solution is added dropwise, stirred for reaction for 15-60 min, and filtered while hot to obtain a primary filter cake; (8) The primary filter cake obtained in step (7) is transferred to deionized water at 80-95°C, stirred and washed for 15-30 minutes, and filtered while hot to obtain a secondary filter cake, which is placed in an oven at 50-80°C and dried for 3-6 hours. The obtained white powder is lithium carbonate.

[0006] Preferably, the mass ratio of the waste lithium iron phosphate battery powder and deionized water in step (2) is 1:2-1:6.

[0007] Preferably, the acid solution in step (3) and step (4) is one or more combinations of sulfuric acid, hydrochloric acid, nitric acid and phosphoric acid.

[0008] Preferably, the oxidant in step (3) and step (4) is one or more combinations of hydrogen peroxide, oxygen, sodium persulfate and sodium hypochlorite.

[0009] Preferably, the pH value adjusted in step (3) and step (4) is 1.5-3.5.

[0010] Preferably, the mass ratio of the leached residue to the leached liquid in step (4) is 1:2 to 1:4.

[0011] Preferably, the concentration of the sodium hydroxide solution in steps (5) and (6) is 15-35 wt%.

[0012] Compared with the prior art, the present invention has the following beneficial effects: The present invention utilizes waste lithium iron phosphate batteries, and by adding acid solution and oxidant combined with multiple leaching methods, the leaching rate of lithium ions is highly selectively increased, and the leaching of iron and phosphorus elements is reduced. A small amount of sodium hydroxide solution is further added to the leaching solution to remove metal ions other than lithium in the solution, thereby achieving the purpose of recovering and preparing high-purity and high-conversion lithium carbonate. The present invention has a simple process flow and high stability, and can achieve efficient leaching of lithium ions and improve the purity of lithium carbonate products. DETAILED DESCRIPTION

[0013] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0014] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.

[0015] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0016] The technical solution of the present invention is described in detail below in conjunction with embodiments, but the protection scope is not limited thereto. Example 1

[0017] The preparation method of waste lithium iron phosphate battery powder 1 specifically comprises the following steps: The first batch of waste lithium iron phosphate batteries were subjected to charged crushing, pyrolysis and screening in turn to obtain waste lithium iron phosphate battery powder 1. The pyrolysis temperature was 400-600°C. The contents of metallic lithium, iron, copper and aluminum in the waste lithium iron phosphate battery powder 1 were determined by ICP plasma emission spectrometry, as shown in Table 1. Example 2

[0018] The preparation method of waste lithium iron phosphate battery powder 2 specifically comprises the following steps: The second batch of waste lithium iron phosphate batteries were subjected to charged crushing, pyrolysis and screening in turn to obtain waste lithium iron phosphate battery powder 2. The pyrolysis temperature was 400-600°C. The contents of metallic lithium, iron, copper and aluminum in the waste lithium iron phosphate battery powder 2 were determined by ICP plasma emission spectrometry, as shown in Table 1. Example 3

[0019] A method for efficiently leaching lithium from waste lithium iron phosphate battery powder, specifically comprising the following steps: (1) Weigh 100 parts by mass of the waste lithium iron phosphate battery powder 1 of Example 1, add them into 300 parts of deionized water in batches, heat to 60° C., stir and slurry for 60 min to obtain a slurry; (2) Add sulfuric acid and hydrogen peroxide to the slurry obtained in step (1), adjust the pH value to 3, raise the temperature to 60°C and stir to react for 2 hours. After the reaction is completed, the product is vacuum filtered to obtain a leachate and leach residue; (3) Repeat the following steps once for the leached residue obtained in step (2): add the leaching solution obtained in step (2) to the leached residue at a mass ratio of 1:3, stir evenly, add sulfuric acid and hydrogen peroxide, adjust the pH value to 2, heat to 60°C, stir and react for 2 h, and after the reaction is completed, vacuum filter to obtain a secondary leaching solution; determine the concentrations of lithium ions and iron ions in the secondary leaching solution by ICP plasma emission spectrometry, and calculate the leaching rates of lithium ions and iron ions, as shown in Table 2; (4) adding sodium hydroxide solution dropwise to the secondary leachate obtained in step (3), adjusting the pH to 5, standing for 1 hour, and vacuum filtering to obtain a primary filtrate after impurity removal; (5) Add 20 wt% sodium hydroxide solution to the first filtrate obtained in step (4), adjust the pH to 9, let stand for 1 h, and obtain a second filtrate by vacuum filtration; (6) The secondary filtrate obtained in step (5) after impurity removal was placed in a 90°C water bath to be concentrated to 20 g / L, and then 300 g / L sodium carbonate solution was added dropwise, stirred for reaction for 30 min, and filtered while hot to obtain a primary filter cake; (7) The primary filter cake obtained in step (6) was transferred to deionized water at 90°C, stirred and washed for 15 min, and filtered while hot to obtain a secondary filter cake, which was placed in an oven at 60°C and dried for 4 h to obtain a white powder, namely lithium carbonate. The purity of the obtained lithium carbonate was measured by ICP plasma emission spectrometry, as shown in Table 2. Example 4

[0020] A method for efficiently leaching lithium from waste lithium iron phosphate battery powder, comprising the following steps: (1) Weigh 50 parts by mass of the waste lithium iron phosphate battery powder 1 of Example 1, add them into 100 parts of deionized water in batches, then heat to 80° C., stir and slurry for 30 min to obtain a slurry; (2) Add hydrochloric acid and hydrogen peroxide to the slurry obtained in step (1), adjust the pH value to 2.5, raise the temperature to 50°C and stir to react for 3 hours. After the reaction is completed, the product is vacuum filtered to obtain a leachate and leach residue; (3) Repeat the following steps twice on the leached residue obtained in step (2): add the leaching solution to the leached residue at a mass ratio of 1:2, stir evenly, add hydrochloric acid and hydrogen peroxide, adjust the pH value to 2, heat to 60°C and stir for 3 h, after the reaction is completed, obtain three leaching solutions by vacuum filtration; wherein the leaching solution used in the next repetition of this step is the leaching solution obtained in the previous leaching; determine the concentrations of lithium ions and iron ions in the total leaching solution by ICP plasma emission spectrometry, and calculate the leaching rates of lithium ions and iron ions, as shown in Table 2; (4) Add 20 wt % sodium hydroxide solution dropwise to the tertiary leachate obtained in step (3), adjust the pH to 5, let stand for 1 hour, and obtain a primary filtrate after impurity removal by vacuum filtration; (5) Add 25 wt% sodium hydroxide solution to the primary filtrate obtained in step (4), adjust the pH to 9, let stand for 1 hour, and obtain a secondary filtrate after impurity removal by vacuum filtration; (6) The secondary filtrate obtained in step (5) after impurity removal was placed in a 90°C water bath to be concentrated to 25 g / L, and then 300 g / L sodium carbonate solution was added dropwise, stirred for reaction for 30 min, and filtered while hot to obtain a primary filter cake; (7) The primary filter cake obtained in step (6) was transferred to deionized water at 90° C., stirred and washed for 15 min, and filtered while hot to obtain a secondary filter cake, which was placed in an oven at 60° C. and dried for 4 h to obtain a white powder, namely lithium carbonate. The purity of the obtained lithium carbonate was measured by ICP plasma emission spectrometry, as shown in Table 2. Example 5

[0021] A method for efficiently leaching lithium from waste lithium iron phosphate battery powder, comprising the following steps: (1) Weigh 100 parts of the waste lithium iron phosphate battery powder 1 of Example 1 by weight, add them into 400 parts of deionized water in batches, then heat to 50° C., stir and slurry for 90 minutes to obtain a slurry; (2) Add hydrochloric acid and sodium hypochlorite to the slurry obtained in step (1), adjust the pH value to 2.5, raise the temperature to 70°C and stir to react for 2 h. After the reaction is completed, the product is vacuum filtered to obtain a leachate and leach residue; (3) Repeat the following steps three times on the leached residue obtained in step (2): add the leaching solution to the leached residue at a mass ratio of 1:2, stir evenly, add hydrochloric acid and hydrogen peroxide, adjust the pH value to 2, heat to 60°C and stir for 3 h, and after the reaction is completed, obtain four leaching solutions by vacuum filtration; wherein the leaching solution used in the next repetition of this step is the leaching solution obtained by the previous leaching; determine the concentrations of lithium ions and iron ions in the four leaching solutions by ICP plasma emission spectrometry, and calculate the leaching rates of lithium ions and iron ions, as shown in Table 2; (4) Add 30 wt % sodium hydroxide solution dropwise to the four leaching solutions obtained in step (3), adjust the pH to 5, let stand for 1 hour, and obtain a primary filtrate after impurity removal by vacuum filtration; (5) Add 30 wt % sodium hydroxide solution to the first filtrate obtained in step (4), adjust the pH to 9, let stand for 1.5 h, and obtain a second filtrate after impurity removal by vacuum filtration; (6) The secondary filtrate obtained in step (5) after impurity removal was placed in a 95°C water bath to be concentrated to 25 g / L, and then 250 g / L sodium carbonate solution was added dropwise, stirred for reaction for 30 min, and filtered while hot to obtain a primary filter cake; (7) The primary filter cake obtained in step (6) was transferred to deionized water at 90° C., stirred and washed for 30 min, and filtered while hot to obtain a secondary filter cake, which was placed in an oven at 80° C. and dried for 3 h to obtain a white powder, namely lithium carbonate. The purity of the obtained lithium carbonate was measured by ICP plasma emission spectrometry, as shown in Table 2. Example 6

[0022] A method for efficiently leaching lithium from waste lithium iron phosphate battery powder, comprising the following steps: Weigh 100 parts of the waste lithium iron phosphate battery powder 2 of Example 2 in parts by mass, add them to 300 parts of deionized water in batches, heat to 60° C., stir and slurry for 60 min to obtain a slurry; (2) adding hydrochloric acid and hydrogen peroxide to the slurry obtained in step (1), adjusting the pH value to 2.5, raising the temperature to 60° C. and stirring for reaction for 2 h. After the reaction is completed, the product is vacuum filtered to obtain a primary leachate and leach residue; (3) Repeat the following steps twice with the leached residue obtained in step (2): add the leaching solution to the leached residue at a mass ratio of 1:3, stir evenly, add sulfuric acid and hydrogen peroxide, adjust the pH value to 2, heat to 60°C and stir for 2 h, and after the reaction is completed, obtain three leaching solutions by vacuum filtration; wherein the leaching solution used in the next repetition of this step is the leaching solution obtained in the previous leaching; determine the concentrations of lithium ions and iron ions in the three leaching solutions by ICP plasma emission spectrometry, and calculate the leaching rates of lithium ions and iron ions, as shown in Table 2; (4) Add 30 wt % sodium hydroxide solution dropwise to the tertiary leachate obtained in step (3), adjust the pH to 5, let stand for 1 hour, and obtain a primary filtrate after impurity removal by vacuum filtration; (5) Add 25 wt% sodium hydroxide solution to the primary filtrate obtained in step (4), adjust the pH to 9, let stand for 1 hour, and obtain a secondary filtrate after impurity removal by vacuum filtration; (6) The secondary filtrate obtained in step (5) after impurity removal was placed in a 90°C water bath to be concentrated to 25 g / L, and then 250 g / L sodium carbonate solution was added dropwise, stirred for reaction for 30 min, and filtered while hot to obtain a primary filter cake; (7) The primary filter cake obtained in step (6) was transferred to deionized water at 90° C., stirred and washed for 30 min, and filtered while hot to obtain a secondary filter cake, which was placed in an oven at 80° C. and dried for 3 h to obtain a white powder, namely lithium carbonate. The purity of the obtained lithium carbonate was measured by ICP plasma emission spectrometry, as shown in Table 2. Example 7

[0023] A method for efficiently leaching lithium from waste lithium iron phosphate battery powder, comprising the following steps: (1) Weigh 1500 parts of the waste lithium iron phosphate battery powder 2 of Example 2 in parts by mass, add them into 4500 parts of deionized water in batches, then heat to 60° C., stir and slurry for 60 min to obtain a slurry; (2) Add sulfuric acid and hydrogen peroxide to the slurry obtained in step (1), adjust the pH value to 3, and then heat to 60°C and stir to react for 2 hours. After the reaction is completed, the product is vacuum filtered to obtain a leachate and leach residue; (3) Repeat the following steps once for the leached residue obtained in step (2): add the leaching solution obtained in step (2) to the leached residue at a mass ratio of 1:3, stir evenly, add sulfuric acid and hydrogen peroxide, adjust the pH value to 2, heat to 60°C and stir for 2 h, and after the reaction is completed, obtain a secondary leaching solution by vacuum filtration. The concentrations of lithium ions and iron ions in the secondary leaching solution are determined by ICP plasma emission spectrometry, and the leaching rates of lithium ions and iron ions are calculated, as shown in Table 2; (4) Add 25 wt% sodium hydroxide solution dropwise to the secondary leachate obtained in step (3), adjust the pH to 4, let stand for 1.5 h, and obtain a primary filtrate after impurity removal by vacuum filtration; (5) Add 30 wt% sodium hydroxide solution to the first filtrate obtained in step (4), adjust the pH to 8, let stand for 2 h, and obtain a second filtrate by vacuum filtration; (6) The secondary filtrate obtained in step (5) after impurity removal was placed in a 95°C water bath to be concentrated to 25 g / L, and then 200 g / L sodium carbonate solution was added dropwise, stirred for reaction for 30 min, and filtered while hot to obtain a primary filter cake; (7) The primary filter cake obtained in step (6) was transferred to deionized water at 85°C, stirred and washed for 20 min, and filtered while hot to obtain a secondary filter cake, which was placed in an oven at 50°C and dried for 5 h to obtain a white powder, namely lithium carbonate. The purity of the obtained lithium carbonate was measured by ICP plasma emission spectrometry, as shown in Table 2.

[0024] Comparative Example 1 The method of the present invention is not used to leach lithium from waste lithium iron phosphate batteries. The specific steps are derived from Example 1 in Patent Publication No.: CN116732343A, as follows: (1) placing the waste lithium iron phosphate battery in a saturated sodium chloride solution, disassembling it after it is completely discharged, and obtaining the positive electrode sheet of the battery; placing the positive electrode sheet of the battery in a vacuum atmosphere tubular electric furnace, heating it to 600° C. under a nitrogen atmosphere, and separating the lithium iron phosphate powder from the aluminum foil to obtain the lithium iron phosphate powder; (2) Mixing citric acid and glycine in deionized water, wherein the molar ratio of citric acid, glycine and deionized water is 1:1:1, and stirring in a constant temperature heated magnetic stirrer at 80°C and 1000 r / min for 1 h until a clear solution is obtained, wherein the clear solution is the new deep eutectic solvent; (3) placing 1 g of lithium iron phosphate powder from step (1) in a beaker containing the novel low eutectic solvent from step (2) at a mass ratio of 1:20, placing the beaker in a constant temperature heated magnetic stirrer for stirring and leaching, the leaching temperature being 60° C., the leaching time being 2 h, and the rotation speed being 800 r / min, to leach lithium from the positive electrode material; (4) After the leaching is completed, the beaker is removed from the agitator, and a filter membrane is used to separate the liquid and solid of the reaction product to obtain a lithium ion solution, thereby completing the recovery of lithium from the waste lithium iron phosphate battery.

[0025] Comparative Example 2 The method of the present invention is not used to leach lithium from waste lithium iron phosphate batteries. The specific steps are derived from Example 1 in Patent Publication No.: CN114927788A, as follows: (1) Weigh 1 g of waste lithium iron phosphate positive electrode material and 1 g of sodium persulfate as a co-grinding agent, put them into a 100 mL ball mill, and add 1 mL of 30% hydrogen peroxide as a grinding aid into the ball mill; (2) Place the ball mill in step (1) in a planetary ball mill for ball milling at room temperature for 5 min, control the speed of the planetary ball mill to be 500 rpm, and the ball-to-powder ratio to be 20 g / g; (3) The ball-milled mixture was placed in a 250 mL conical flask, and deionized water was added to the conical flask at a solid-liquid ratio of 30 g / L. The mixture was then leached at 40 °C for 20 min. The leaching process was stirred at a stirring speed of 300 rpm. (4) After the leaching in step (3) is completed, the leaching solution is filtered to obtain a filtrate rich in lithium and iron elements, and the filtrate is subsequently subjected to an atomic absorption test.

[0026] Experimental data and analysis: 1. The contents of metallic lithium, iron, copper and aluminum in the waste lithium iron phosphate battery powder of Example 1-2 are shown in Table 1.

[0027] Table 1 Contents of metallic lithium, iron, copper and aluminum in the waste lithium iron phosphate battery powder of Examples 1-2 Li Cu Fe Al Example 1 3.73% 0.67% 25.93% 0.17% Example 2 2.81% 0.20% 20.76% 0.44% 2. The lithium ion and iron ion leaching rates and lithium carbonate purity of Examples 3-7 and Comparative Examples 1-2 are shown in Table 2.

[0028] Table 2 shows the lithium ion leaching rate and lithium carbonate purity of Examples 3-7 and Comparative Examples 1-2 Example 3 Example 4 Example 5 Example 6 Example 7 Comparative Example 1 Comparative Example 2 Lithium ion leaching rate (%) 98.92 99.54 99.92 99.43 99.02 91.02 98.3 Iron ion leaching rate (%) 0.093 0.186 0.348 0.082 0.089 -- 2.5 Lithium carbonate purity (%) 99.24 99.61 99.63 99.57 99.35 -- -- From the data in Table 2, it can be found that the waste lithium iron phosphate battery powder obtained by the charged crushing, high-temperature pyrolysis and screening of the waste lithium iron phosphate battery, by adding acid and oxidant, combined with the process of multiple leaching, in Example 5, the leaching rate of lithium ions can reach 99.9%, and the leaching rate of iron ions is only 0.348%, indicating that the method of the present invention can achieve selective and efficient leaching of lithium ions in the waste lithium iron phosphate battery powder; in addition, under the same reaction conditions, even if the waste lithium iron phosphate battery powder with different lithium contents is used as raw materials in Example 3 and Example 7, the leaching rate of lithium ions can reach about 99%, which shows that the method of the present invention has high stability for the leaching of lithium ions.

[0029] Comparing the lithium ion leaching rates of Example 3 and Comparative Example 1, under the conditions of a leaching temperature of 60° C. and a leaching time of 2 h, Example 3 can effectively increase the lithium ion leaching rate from 91.02% to 98.92%; although the lithium ion leaching rate in Comparative Example 2 is comparable to that in Example 3, its iron ion leaching rate reaches 2.3%, which is almost 27 times that of Example 3, further illustrating that the method of the present invention has high selectivity for leaching lithium ions in waste lithium iron phosphate battery powder.

[0030] It can be further seen from the data in Table 2 that the lithium carbonate prepared by the method of the present invention has a high purity; among them, the purity of the lithium carbonate prepared in Example 5 is as high as 99.63%.

[0031] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.

Claims

1. A method for efficiently leaching lithium using waste lithium iron phosphate battery powder, characterized in that: The following steps are involved: (1) The waste lithium iron phosphate battery is subjected to charged crushing, pyrolysis and screening to obtain waste lithium iron phosphate battery powder, and the pyrolysis temperature is 400-600°C; (2) Weigh the waste lithium iron phosphate battery powder obtained in step (1), add it to deionized water, heat it to 40-90° C., and stir it for 30-90 minutes to obtain a slurry; (3) adding acid and oxidant to the slurry obtained in step (2), adjusting the pH value, and then heating to 40-90° C. and stirring to react for 1-5 hours. After the reaction is completed, vacuum filtration is performed to obtain a leachate and leach residue; (4) Repeating the following steps more than once with the leached residue obtained in step (3): adding the leaching solution to the leached residue, stirring evenly, adding the acid solution and the oxidant, adjusting the pH value, heating to 40-90° C., stirring and reacting for 1-5 hours, and after the reaction is completed, vacuum filtering to obtain multiple leaching solutions; (5) adding sodium hydroxide solution dropwise to the multiple leaching solutions obtained in step (4), adjusting the pH to 4-5, standing for 0.5-2 hours, and vacuum filtering to obtain a primary filtrate after impurity removal; (6) Add sodium hydroxide solution dropwise to the primary filtrate obtained in step (5) to adjust the pH to 8-9, let stand for 0.5-2 hours, and obtain a secondary filtrate after impurity removal by vacuum filtration; (7) The secondary filtrate obtained in step (6) after impurity removal is placed in a water bath at 80-95°C to concentrate it to 20-30 g / L, and then sodium carbonate solution is added dropwise, stirred for reaction for 15-60 min, and filtered while hot to obtain a primary filter cake; (8) The primary filter cake obtained in step (7) is transferred to deionized water at 80-95°C, stirred and washed for 15-30 minutes, and filtered while hot to obtain a secondary filter cake, which is placed in an oven at 50-80°C and dried for 3-6 hours. The obtained white powder is lithium carbonate.

2. The method for efficiently leaching lithium using waste lithium iron phosphate battery powder according to claim 1, characterized in that: The mass ratio of the waste lithium iron phosphate battery powder and deionized water in step (2) is 1:2 to 1:

6.

3. The method for efficiently leaching lithium using waste lithium iron phosphate battery powder according to claim 1, characterized in that: The acid solution in step (3) and step (4) is one or more combinations of sulfuric acid, hydrochloric acid, nitric acid and phosphoric acid.

4. The method for efficiently leaching lithium using waste lithium iron phosphate battery powder according to claim 1, characterized in that: The oxidant in step (3) and step (4) is one or more combinations of hydrogen peroxide, oxygen, sodium persulfate and sodium hypochlorite.

5. The method for efficiently leaching lithium using waste lithium iron phosphate battery powder according to claim 1, characterized in that: The pH value adjusted in step (3) and step (4) is 1.5-3.

5.

6. The method for efficiently leaching lithium using waste lithium iron phosphate battery powder according to claim 1, characterized in that: The mass ratio of the leached residue to the leached liquid in step (4) is 1:2 to 1:

4.

7. The method for efficiently leaching lithium using waste lithium iron phosphate battery powder according to claim 1, characterized in that: The concentration of the sodium hydroxide solution in steps (5) and (6) is 15-35wt%.

Citation Information

Patent Citations

  • Method of recovering lithium and copper from waste lithium iron phosphate battery selectively

    CN111187913A

  • Recovery method of lithium iron phosphate waste powder

    CN112410556A

Cited By

  • Electrochemical-assisted green leaching method of retired lithium ion battery

    CN120082737A

  • A method of electrochemically assisted green leaching of retired lithium-ion batteries

    CN120082737B

  • Method for selectively recycling lithium element in waste lithium iron phosphate battery by using eutectic solvent

    CN120527505A