Ultrasonic coating equipment, coating methods and photovoltaic welding ribbon
By setting up multiple spaced ultrasonic vibration units and guide fixtures in the tin furnace, and optimizing the ultrasonic frequency and energy distribution in combination with heating components, the problems of uneven coating thickness and unstable quality in ultrasonic plating technology are solved, coating adhesion and production efficiency are improved, and the risk of strip breakage is reduced.
Patent Information
- Application Number
- CN202611536699.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-17
AI Technical Summary
Existing ultrasonic coating technology suffers from problems such as uneven coating thickness, unstable coating quality, and easy breakage of the solder strip. In particular, the oxide layer on the surface of ultra-thin substrates is difficult to completely remove, resulting in insufficient coating adhesion and defects such as micro-pinholes and localized incomplete coating, leading to low production efficiency.
Multiple ultrasonic vibration units are arranged at intervals along the length of the tin furnace. The auxiliary vibration head is at least partially immersed in the molten metal. Each unit is controlled to work at a preset frequency. Combined with the guide fixture, the solder strip substrate is constrained to travel along a preset path. The heating component ensures that the tin furnace is heated evenly in the circumference. The ultrasonic frequency and energy distribution are optimized to improve the uniformity and adhesion of the plating layer.
It improves the uniformity and adhesion of the coating thickness, reduces the probability of incomplete plating and micro-pinhole defects, reduces the risk of solder ribbon breakage, and improves production efficiency and coating smoothness.
Smart Images

Figure CN123108459A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of photovoltaic ribbon preparation technology, specifically to an ultrasonic coating equipment, a coating method, and a photovoltaic ribbon. Background Technology
[0002] Photovoltaic solder ribbons are key conductive components in solar photovoltaic modules that enable electrical connections between cells. They typically consist of a copper substrate and a plating layer covering the surface of the copper substrate. The uniformity, density, and adhesion of the plating layer to the substrate directly affect the welding reliability and long-term service life of the photovoltaic module.
[0003] Currently, hot-dip plating is commonly used for substrate plating. This involves continuously passing a copper substrate through a tin furnace containing molten metal, allowing the molten metal to wet and adhere to the substrate surface, followed by cooling and solidification to form a plating layer. However, an oxide film inevitably exists on the surface of the copper substrate. This oxide film hinders direct contact between the molten metal and the substrate, resulting in poor wettability of the molten metal and insufficient adhesion of the plating layer.
[0004] To overcome the above problems, an ultrasonic-assisted plating scheme has been proposed in related technologies. This involves installing an ultrasonic vibration unit inside the solder bath, utilizing the cavitation effect generated when ultrasound propagates in the molten metal to remove the oxide film on the surface of the solder strip substrate, allowing the molten metal to directly wet and adhere to the surface of the solder strip substrate to form a plating layer. This scheme improves the microscopic wettability of the molten metal to some extent and reduces pinhole defects in the plating layer. However, this ultrasonic-assisted plating technology still has at least one of the following drawbacks in practical applications: The coating thickness is not uniform. There is a thickness gradient along the length and width of the same weld strip. It is difficult to guarantee the coating in the edge area and narrow side of the weld strip, resulting in local omissions and uneven coating thickness.
[0005] The coating quality is unstable, the micro-oxide layer on the surface of the ultra-thin substrate is difficult to completely remove, the micro-wetting of the molten metal is poor, and the coating is prone to defects such as micro-pinholes, local incomplete plating, peeling and flaking, making it difficult to guarantee batch consistency and yield.
[0006] During the plating process, the welding strip is prone to warping, stretching deformation, and even breakage. Thin strips are easily unstable under liquid turbulence and fluid impact, resulting in high scrap rate and low production efficiency.
[0007] After plating, the surface of the solder strip has obvious ripples and poor flatness, which affects the welding quality of subsequent processes.
[0008] The above problems also occur in other photovoltaic welding ribbon coating scenarios where non-molten metal liquid is used.
[0009] Therefore, there is an urgent need for a new coating solution to address at least one of the defects in the aforementioned ultrasonic coating solutions. Summary of the Invention
[0010] This application aims to provide an ultrasonic coating equipment, a coating method, and a photovoltaic welding ribbon to solve the technical problems existing in the prior art of ultrasonic coating, such as uneven coating thickness, incomplete coating, unstable coating quality, and easy breakage of the welding ribbon.
[0011] In a first aspect, according to at least some embodiments of this application, this application provides an ultrasonic plating apparatus, including a tin furnace and N ultrasonic vibration units. The tin furnace is configured to hold molten metal. The N ultrasonic vibration units are disposed inside the tin furnace, and each ultrasonic vibration unit includes a transducer and an auxiliary vibration head. The transducer applies ultrasonic waves to the molten metal through the auxiliary vibration head; wherein the auxiliary vibration heads of M ultrasonic vibration units are arranged at intervals along the length direction of the tin furnace, M≤N and M≥2.
[0012] Furthermore, the M vibration-aiding heads are arranged linearly at equal intervals along the length of the tin furnace.
[0013] Furthermore, along the width direction of the tin furnace, the effective size of the working surface of the vibration aid head is not less than 120mm.
[0014] Furthermore, along the width direction of the tin furnace, the size of the furnace cavity is not less than 15mm.
[0015] Furthermore, a heating element is provided circumferentially on the outer side of the tin furnace cavity.
[0016] Furthermore, the ultrasonic plating equipment also includes: a guide fixture, which is rotatably configured relative to the tin furnace and is configured to enter the furnace cavity of the tin furnace or rotate out of the furnace cavity of the tin furnace during rotation. The guide fixture is provided with an inlet for the solder strip substrate to pass through and an outlet for the solder strip substrate to pass through, for constraining the solder strip substrate on a preset passage path.
[0017] Furthermore, the guide fixture includes a fixed part and a rotating part. The fixed part is disposed in the solder pot, and the rotating part is rotatably connected to the fixed part, configured to enter the furnace cavity of the solder pot or rotate out of the furnace cavity of the solder pot during rotation. The rotating part and the bottom wall of the solder pot together define an inlet for the solder strip substrate to enter and an outlet for the solder strip substrate to exit.
[0018] Secondly, according to at least some embodiments of this application, this application also provides a method for plating using the above-mentioned ultrasonic plating equipment, the method comprising: controlling the solder strip substrate to enter the molten metal along a preset travel path and exit from the molten metal; during the travel of the solder strip substrate, controlling the ultrasonic vibration unit to operate so as to apply ultrasonic waves to the molten metal to plating the solder strip substrate.
[0019] Furthermore, controlling the operation of the ultrasonic vibration unit includes controlling each ultrasonic vibration unit to operate at its corresponding preset frequency, wherein at the preset frequency, the sound intensity difference between the edge region and the center region of the working surface of the vibration aid head in the width direction is lower than a preset threshold.
[0020] Furthermore, the preset frequency is f and 50kHz ≥ f ≥ 7kHz.
[0021] Furthermore, the thickness of the welding strip substrate is 0.1 mm to 0.15 mm, and the width is 10 mm to 15 mm.
[0022] Furthermore, the vibration-assisted head is at least partially immersed in the molten metal liquid.
[0023] Furthermore, the vibration-assisted head is completely immersed in the molten metal liquid.
[0024] Furthermore, the vertical distance between the working surface of the vibration-assisted head and the height position of the preset travel path of the welding strip substrate is 10 mm to 22 mm.
[0025] Thirdly, according to at least some embodiments of this application, this application also provides a photovoltaic welding ribbon, which is prepared using the ultrasonic coating equipment or the coating method described above.
[0026] By adopting the above technical solution, this application has at least one of the following technical effects: By setting multiple vibration heads arranged at intervals along the length direction inside the tin furnace, the total processing time and path of the solder strip in the ultrasonic action zone are extended. Each vibration head acts continuously during the movement of the solder strip substrate, which is conducive to the sequential removal of residual oxide layer and continuous wetting of molten metal. This reduces the probability of oxide layer residue and plating defects caused by insufficient ultrasonic action time in a single session, and also helps to improve the adhesion of the plating layer.
[0027] By immersing at least part of the vibrating head in the molten metal, the ultrasonic energy can be directly propagated in the molten metal, which helps to reduce energy loss caused by gas-liquid interface reflection, and the cavitation effect is more sufficient. This helps to improve the removal effect of oxide layer on substrate surface and reduce the probability of micro-pinholes, local incomplete plating, peeling and flaking of coating.
[0028] By setting the effective size of the working surface of the vibration head in the width direction to not less than 120mm, a wide ultrasonic action zone is formed, covering the entire width of the solder strip substrate. This is beneficial for uniform coating on both sides and narrow sides of the solder strip substrate, reducing the probability of missed coating. Moreover, this wide area can accommodate multiple solder strip substrates to be coated in parallel in the width direction, which helps to improve production efficiency.
[0029] By controlling each ultrasonic vibration unit at its corresponding preset frequency, the sound intensity difference between the edge and center regions of the working surface in the width direction is lower than a preset threshold when each unit operates at the preset frequency. This helps to reduce the sound intensity difference between the center and edge of the working surface, thereby improving the uniformity of the coating in the width direction of the solder strip substrate. At the same time, each unit operates near its own preset frequency, and the ultrasonic field is uniformly connected along the length of the solder pot, which helps to reduce the possibility of mutual interference.
[0030] By controlling the operating frequency of the ultrasonic vibration unit to 50kHz≥f≥7kHz, the transverse sound field distribution of ultrasonic waves is more uniform when propagating in molten metal within this frequency range. This helps to reduce the sound intensity difference between the central and edge areas of the working surface of the vibration head, thereby improving the coating uniformity in the width direction of the solder strip substrate. At the same time, the cavitation bubble collapse impact force is relatively mild within this frequency range, which helps to reduce the probability of impact damage to the ultra-thin solder strip substrate. It also reduces the violent disturbance of the molten metal, which helps to improve the surface smoothness of the coating.
[0031] By setting heating components along the circumference of the solder pot, the solder pot is heated evenly in the circumference direction, which helps to reduce the temperature gradient in the width direction of the solder pot, thereby reducing the probability of thermal stress deformation of the solder strip substrate, especially the ultra-thin solder strip substrate, due to local temperature differences.
[0032] By setting a rotatable guide fixture, the strip can be rotated out of the solder bath during the threading process, completed outside the bath, and then rotated back in, which simplifies the threading operation. The inlet and outlet constrain the solder strip substrate to the preset path, which helps to reduce the possibility of deviation.
[0033] Of course, implementing any embodiment of this application does not necessarily require achieving all of the effects described above at the same time. Attached Figure Description
[0034] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the embodiments will be briefly described below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. In addition, similar numbers in the figures are used to represent similar components, wherein: Figure 1 This is a three-dimensional structural schematic diagram of the tin plating equipment 10 in this embodiment; Figures 2A to 2C yes Figure 1 Partial three-dimensional cross-sectional views of the tin plating equipment 10 shown from different perspectives; Figure 3 for Figure 1 A three-dimensional structural schematic diagram of the ultrasonic vibration unit 110 of the tin plating equipment 10 shown. Figure 4 for Figure 1 A three-dimensional structural schematic diagram of the guide fixture 130 of the tin plating equipment 10 shown. Figure 5 This is a schematic diagram of the plating method in Example 2. Detailed Implementation
[0035] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0036] The technical solution of this application will be further described in detail below with reference to the accompanying drawings. The specific embodiments described are only used to explain the technical concept of this application and are not intended to limit the scope of protection of this application. Based on reading this application specification, those skilled in the art can combine, modify, and make equivalent substitutions for the various embodiments, all of which fall within the scope of protection claimed by this application.
[0037] The term "molten metal liquid" as used in this application refers to a molten metal or alloy used for hot-dip plating. The molten metal liquid can be tin liquid, including tin-based alloys such as pure tin, tin-lead alloys, tin-silver-copper alloys, tin-bismuth alloys, or tin-copper alloys; it can also be a molten liquid of other low-melting-point metals or alloys, such as zinc, aluminum, or zinc-aluminum alloys. The following specific embodiments of this application will use tin liquid as an example for illustration.
[0038] In this application, "plating" refers to the process of immersing a substrate in molten metal and forming a metal or alloy plating layer on the surface of the substrate through hot-dip plating. For example, a copper substrate is continuously passed through a tin furnace containing molten metal, where the molten metal wets and adheres to the surface of the substrate, and after cooling and solidification, a plating layer is formed.
[0039] In this application, "photovoltaic ribbon" refers to a strip-shaped conductive component used in photovoltaic modules to achieve electrical connections between cells or between cell strings. The photovoltaic ribbon includes a metal substrate (such as a copper substrate) and a plating layer covering the surface of the substrate. The photovoltaic ribbon can be a busbar or an interconnecting strip (also known as an interconnecting bar). Busbars are typically used for electrical connections between cell strings in photovoltaic modules, and are relatively wide and thin; interconnecting strips are typically used for direct string welding connections between cells, and are relatively narrow. The ultrasonic plating equipment and method provided in this application are applicable to both types of ribbons, and are particularly suitable for the precision plating of ultra-thin, narrow-width ribbons with a thickness of 0.1mm to 0.15mm and a width of 10mm to 15mm.
[0040] Example 1 This embodiment provides an ultrasonic tin plating device 10. Figure 1 This is a three-dimensional structural diagram of the tin plating equipment 10 in this embodiment. Figures 2A to 2C yes Figure 1 Partial three-dimensional cross-sectional views of the tin plating equipment 10 from different perspectives.
[0041] See Figure 1 , Figures 2A to 2C The tin plating equipment 10 includes a tin furnace 100. The tin furnace 100 is configured to hold molten tin for hot-dip plating of the solder strip substrate 400. For ease of description, the X direction is defined as the length direction of the tin furnace 100, which is also the direction of travel of the solder strip substrate 400 (dashed line in the figure) during tin plating; the Y direction is the width direction of the tin furnace 100, which is also the width direction of the solder strip substrate 400 during tin plating (i.e., the width direction of the solder strip); and the Z direction is the depth direction of the tin furnace 100, i.e., the vertical direction.
[0042] The material of the solder pot 100 can be selected as needed. For example, the solder pot 100 can be made of stainless steel. For example, the solder pot 100 can also be made of a composite furnace body lined with titanium alloy, ceramic or enamel to slow down the wetting and corrosion of the furnace body by the molten solder.
[0043] The specific shape of the tin furnace 100 can be set according to actual needs. For example, Figure 1 The tin furnace 100 shown is rectangular. It should be understood that the tin furnace 100 can also be other shapes, such as a rounded rectangular prism or an elliptical tank.
[0044] Taking a rectangular solder bath 100 as an example, its specific length can be set as needed. In one example, the length of the solder bath 100 can be set based on the required plating path length of the solder ribbon substrate 400 to meet the plating path length of the solder ribbon substrate 400 within the solder bath 100. For example, the length of the solder bath 100 can be set slightly larger than the plating path length of the solder ribbon substrate 400 within the solder bath 100. The plating path length of the solder ribbon substrate 400 within the solder bath 100 is determined based on the traveling speed of the solder ribbon substrate 400 and the plating time. The faster the traveling speed and the longer the plating time, the longer the required plating path length, and correspondingly, the longer the length of the solder bath 100.
[0045] In another example, the length of the tin furnace 100 can be set according to the number of ultrasonic vibration units 110 to be set later, the length of the ultrasonic vibration units 110 and the adjacent spacing, and the length of the tin furnace 100 must be sufficient to accommodate these ultrasonic vibration units 110.
[0046] As a specific example, the length of the tin furnace 100 is set to 500mm to 1000mm, such as 500mm, 800mm, 1000mm, etc.
[0047] The width (Y direction) dimension of the solder pot 100 can also be set as needed. In one example, the width (Y direction) dimension of the solder pot 100 is set based on factors such as the width of the solder strip substrate 400, the number of solder strip substrates 400 to be tinned in parallel, and the spacing between adjacent solder strip substrates 400. For example, when only a single solder strip substrate 400 needs to be tinned at a time and the width of the solder strip substrate 400 is 12mm, the dimension of the furnace cavity 104 of the solder pot 100 in the width direction (Y direction) should be at least greater than 12mm. In at least some embodiments, it is set to not less than 15mm to avoid or reduce the solder strip substrate 400 scraping against the furnace wall and to leave a gap between the solder strip substrate 400 and the furnace wall for the convection of molten solder. As another example, when six solder strip substrates 400 need to be tinned in parallel in a batch, the dimension of the furnace cavity 104 in the width direction (Y direction) needs to be greater than 6×12mm, and further considering the spacing between adjacent solder strips (e.g., 5mm to 10mm), it can be set to 120mm.
[0048] The depth (Z-direction) of the solder pot 100 can also be set as needed. In one example, the depth of the solder pot 100 can be set by considering factors such as the height of the ultrasonic vibration unit 110 and the required depth of molten solder, to avoid the solder being too shallow, resulting in incomplete immersion of the solder strip or insufficient ultrasonic action, while also avoiding the solder being too deep, which would lead to unnecessary increases in solder consumption and heating power consumption. As a specific example, the depth of the solder pot 100 is 40mm-200mm, such as 40mm, 70mm, 100mm, 150mm, 200mm, etc.
[0049] It should be understood that the furnace wall of the tin furnace 100 can be a single-layer structure, or it can be a two-layer or more-layer structure. For example... Figures 2A to 2C As shown, at least a portion of the furnace wall region of the tin furnace 100 has an inner wall 101 and an outer wall 102, with a hollow cavity 103 formed between the inner wall 101 and the outer wall 102. The hollow cavity 103 can be used to accommodate at least a portion of the heating components and / or the ultrasonic vibration unit 110 mentioned later (which will be further described in the relevant sections below).
[0050] See further Figure 1 and Figures 2A to 2C The tin plating equipment 10 also includes N ultrasonic vibration units 110 disposed inside the tin furnace 100, where N is an integer greater than or equal to 2. For example, Figure 1 and Figures 2A to 2C In the formula N=6, it should be understood that N can also be 2, 3, 4, 5, 7, or other quantities, depending on the actual tin plating process requirements. Generally, the higher the adhesion requirement of the tin plating layer, the larger the number of ultrasonic vibration units 110.
[0051] Figure 3 A three-dimensional structural schematic diagram of the ultrasonic vibration unit 110 is shown below. Figure 3 Each ultrasonic vibration unit 110 includes a transducer 111 and a vibration head 112.
[0052] Transducer 111 is a component that converts electrical energy into mechanical vibration. It is electrically connected to an ultrasonic generator (not shown in the figure), converting electrical signals into mechanical vibration and transmitting them to the vibration head 112. As an example, transducer 111 is a piezoelectric ceramic transducer, which is composed of several piezoelectric ceramic sheets stacked and clamped together. As another example, transducer 111 is a magnetostrictive transducer.
[0053] The vibration head 112 is an acoustic component that radiates the mechanical vibration output from the transducer 111 into the molten solder. One end of the head is connected to the output end of the transducer 111, transmitting the vibration to the working surface 1121 at the other end, causing the working surface 1121 to vibrate and radiate ultrasonic waves into the molten solder. When the ultrasonic waves propagate in the molten solder, they generate a cavitation effect. When the cavitation bubbles collapse, local high temperature and pressure and micro-jets are formed near the surface of the solder substrate 400, which peel off the oxide film on the surface of the substrate and allow the molten solder to directly wet the substrate, thereby completing the tin plating under flux-free conditions.
[0054] The applicant's research found that when a single ultrasonic vibration unit 110 is set inside the tin furnace 100, the photovoltaic solder ribbon only passes through a single ultrasonic action zone once to complete the processing. The effective ultrasonic action time is extremely short (usually 0.1 to 0.2 seconds), the oxide layer is not sufficiently removed, and the microscopic oxide layer remaining on the surface of the solder ribbon substrate hinders the wetting of the molten tin, resulting in insufficient coating adhesion and easy occurrence of plating defects.
[0055] Therefore, in this embodiment, the auxiliary vibration heads 112 of the M ultrasonic vibration units 110 are arranged at intervals along the length direction (X direction) of the tin furnace 100, where M ≤ N and M ≥ 2. The M auxiliary vibration heads 112 are arranged at intervals, meaning they are sequentially arranged along the length direction (X direction) of the tin furnace 100, with a certain distance between adjacent heads. For example, Figure 1 and Figures 2A to 2C In the formula M=6, it should be understood that M can also be 2, 3, 4, 5, 7 or other quantities, which can be set according to the actual tin plating process requirements.
[0056] By arranging the auxiliary vibration heads 112 of multiple ultrasonic vibration units 110 at intervals along the length direction (X direction) of the solder bath 100, the ultrasonic fields of adjacent auxiliary vibration heads 112 are interconnected and complementary, extending the total processing time and path of the solder strip substrate 400 within the ultrasonic action zone. Specifically, the multiple auxiliary vibration heads 112 arranged along the length direction can achieve functional division and cooperation. The ultrasonic action area corresponding to the preceding auxiliary vibration head 112 is used to fully remove the oxide layer on the surface of the solder strip substrate 400, and the ultrasonic action area corresponding to the subsequent auxiliary vibration head 112 is used to maintain the ultrasonic action on the activated substrate surface to promote sufficient wetting and spreading of the molten solder, thereby reducing the probability of oxide layer residue and incomplete plating defects caused by insufficient ultrasonic action time in a single session.
[0057] In at least some embodiments, such as Figure 1 As shown in Figure 2, N=M, meaning that the auxiliary vibration heads 112 of all ultrasonic vibration units 110 are arranged in a linear array with equal spacing along the length direction.
[0058] In an alternative embodiment, M < N, meaning that at least some of the vibration aids 112 are not spaced apart along the length direction (X direction) of the solder pot 100. In one example where M < N, some of the vibration aids 112 may be spaced apart along the width direction (Y direction) of the solder pot 100. When multiple vibration aids 112 are arranged along the width direction, the effective size of the working surface 1121 of each vibration aid 112 can be relatively reduced, and the multiple vibration aids 112 arranged along the width direction can collaboratively cover the ultrasonic action area of the solder strip substrate throughout the entire width direction.
[0059] As an example, the auxiliary vibration heads 112 of the M ultrasonic vibration units 110 are arranged at equal intervals along the length direction (X direction) of the solder pot 100. This arrangement is beneficial for uniform plating along the length direction. When it is necessary to apply ultrasonic treatment differently to different sections of the solder strip substrate, at least some of the auxiliary vibration heads 112 of the M ultrasonic vibration units 110 can be arranged at non-equal intervals along the length direction (X direction) of the solder pot 100.
[0060] It should be understood that the spacing between adjacent auxiliary vibration heads 112 can be set according to the power and frequency of the ultrasonic vibration unit 110 and the attenuation characteristics of the solder on the ultrasonic waves. If the spacing is too large, a blind zone may appear between the ultrasonic fields of adjacent auxiliary vibration heads 112, and the solder substrate 400 cannot obtain effective ultrasonic action in this area; if the spacing is too small, the ultrasonic fields of adjacent auxiliary vibration heads 112 will overlap excessively, resulting in energy waste and potentially uneven local sound intensity distribution due to standing waves formed by ultrasonic interference. In specific applications, a suitable spacing range can be determined through experiments or simulations based on actual process requirements. For example, the spacing between adjacent auxiliary vibration heads 112 can be 50mm to 500mm, such as 50mm, 100mm, 200mm, 350mm, or 500mm.
[0061] In at least some embodiments, the working surface 1121 of the vibration-assisted head 112 is a rectangular plane, but it can also be set to other shapes or non-planar surfaces as needed. For example, the working surface 1121 can also be an arc surface, a sawtooth surface, or a surface with grooves.
[0062] The effective dimension of the working surface 1121 of the vibration head 112 in the width direction (Y direction) can be set as needed. In one example, the effective dimension of the working surface 1121 is set according to the width of a single solder strip substrate 400. For example, if the width of a single solder strip substrate 400 is 12mm, then the effective dimension of the working surface 1121 in the width direction (Y direction) is at least 12mm, or it can be greater than 12mm, such as 14mm, to ensure that the entire width of the solder strip substrate 400 is within the ultrasonic action range. When multiple solder strip substrates 400 need to be tinned in parallel, the effective dimension of the working surface 1121 in the width direction (Y direction) is set by comprehensively considering the total width of all solder strip substrates 400 and the spacing between adjacent solder strip substrates 400. For example, if a batch of six solder strips of substrate 400 are to be tin-plated in parallel, each strip is 12mm wide and the spacing between adjacent solder strips is 5mm, then the effective size of the working surface 1121 is at least 6×12mm+5×5mm=97mm. Considering the possible sway allowance during the movement of the solder strip substrate, the effective size of the working surface 1121 in the width direction (Y direction) can be set to be greater than 97mm, such as 120mm, 130mm, etc.
[0063] In one specific example, the effective dimension of the working surface 1121 in the width direction (Y direction) is not less than 120mm, in order to accommodate the requirement of simultaneous tin plating of multiple solder strip substrates 400.
[0064] The applicant's research revealed that in relevant ultrasonic tin plating technologies, the ultrasonic booster head is typically positioned above the surface of the molten tin, not extending into the molten tin. This forces the ultrasonic waves to pass through an air layer before reaching the molten tin. Due to the significant difference in acoustic impedance between air and molten tin, the ultrasonic waves undergo strong reflection at the air-liquid interface, with most of the energy reflected back into the air, and only a small portion penetrating into the molten tin. Furthermore, even the portion that penetrates the molten tin attenuates rapidly along the depth direction, resulting in significantly insufficient sound field intensity in deeper regions below the surface. Consequently, the ultrasonic energy received by the solder ribbon as it travels below the molten tin surface is greatly attenuated, the cavitation effect is weak, the oxide layer is not thoroughly removed, and defects in the plating layer are prone to occur.
[0065] In view of this, in at least some embodiments of this application, the vibration-assisted head 112 extends from the transducer 111 toward the interior of the furnace cavity 104 of the solder furnace 100 and is at least partially inserted into the molten solder. Exemplarily, the vibration-assisted head 112 may be fully inserted into the molten solder, so that the working surface 1121 is completely submerged in the molten solder; it may also be mostly inserted into the molten solder; or only one end of the working surface 1121 may be inserted into the molten solder, while the remaining portion of the vibration-assisted head 112 is outside the molten solder. Thus, by extending at least partially into the molten solder, the working surface 1121 is in direct contact with the molten solder, and the ultrasonic waves do not need to pass through the gas-liquid interface, but propagate directly in the molten solder, thereby significantly reducing the interface reflection loss of ultrasonic energy and enabling the solder ribbon substrate to obtain sufficient ultrasonic intensity within the molten solder.
[0066] It should be understood that the vibration head 112 can be inserted into the molten solder from bottom to top (i.e., from the bottom of the solder pot 100 towards the liquid surface) or from top to bottom (i.e., from the top or side wall of the solder pot 100 towards the bottom wall of the solder pot). In comparison, when the vibration head 112 is inserted into the molten solder from bottom to top, it is located outside the travel path below the solder strip substrate 400, and has less impact on the travel process of the solder strip substrate 400.
[0067] It should be understood that the transducer 111 of the ultrasonic vibration unit 110 may be located outside the solder furnace 100. As a different example, see [link to relevant documentation]. Figures 2A to 2C As shown, the transducer 111 of the ultrasonic vibration unit 110 is located inside the hollow cavity 103 of the tin furnace 100, rather than outside the tin furnace 100. Specifically, the transducer 111 is located inside the hollow cavity 103 between the inner and outer bottom walls of the tin furnace 100, and the auxiliary vibration head 112 extends into the furnace cavity 104 from bottom to top through the inner wall 101.
[0068] In at least some embodiments, see Figures 2A to 2C The plating equipment 10 also includes a heating component 120 arranged circumferentially along the tin furnace 100 for heating the molten tin in the tin furnace 100, so that the tin material is kept in a molten state and the set temperature is maintained.
[0069] The heating component 120 can be disposed inside the furnace cavity 104 of the solder furnace 100 or outside the solder furnace 100. However, when the heating component 120 is disposed inside the furnace cavity 104, it is immersed in the molten solder, which occupies internal space and may interfere with the movement of the solder strip substrate 400. When the heating component 120 is disposed outside the solder furnace 100, it is exposed to the environment, making it susceptible to damage from external forces and resulting in rapid heat dissipation and lower heating efficiency. In view of this, in at least some embodiments, see Figures 2A to 2C The heating component 120 is disposed in the hollow cavity 103 between the inner layer 101 and the outer layer 102 of the solder pot 100. In this way, the heating component 120 will not occupy the internal space of the furnace cavity 104, will not interfere with the movement of the solder strip substrate 400, and is protected by the outer layer 102 so that it is not easily damaged. At the same time, the space of the hollow cavity 103 itself has a certain heat preservation effect, which helps to reduce heat loss and improve heating efficiency.
[0070] The arrangement of the heating components 120 can be configured as needed. In at least some embodiments, the heating components 120 are arranged along the entire circumference of the solder pot 100, surrounding the peripheral wall of the solder pot 100, so that the solder pot 100 is heated evenly in the circumference, which helps to eliminate the temperature gradient in the circumference of the solder pot 100. In at least some embodiments, the heating components 120 can also be disposed on the bottom wall of the solder pot 100, or simultaneously disposed on the peripheral wall and the bottom wall, to further optimize the overall temperature distribution uniformity of the solder pot 100.
[0071] The heating component 120 can employ any one or more combinations of resistance heating, liquid heating, electromagnetic induction heating, or quartz heating tubes. For example, in this embodiment, the heating component 120 is a resistance heating strip, which is simple in structure, low in cost, and easy to maintain.
[0072] In at least some embodiments, the heating assembly 120 may include multiple heating units, such as two or more heating tubes arranged around the perimeter of the tin furnace 100 along the height direction. By arranging multiple heating tubes along the height direction, the temperature uniformity of the tin furnace 100 in the height direction can be increased, avoiding the impact on plating quality due to temperature gradients in the depth direction of the molten tin.
[0073] The heating component 120 can be controlled by a single integrated temperature control or by a multi-segment, independently controlled temperature control structure. In at least some embodiments, the heating component 120 uses a single integrated temperature control method, where a single temperature controller keeps the molten solder temperature near a set value. In at least some embodiments, the heating component 120 uses a multi-segment, independently controlled temperature control structure, with multiple independent temperature control zones set along the length of the solder furnace 100. Each temperature control zone independently detects its temperature and adjusts its heating power to further optimize the temperature uniformity of the molten solder along the entire length of the furnace and reduce plating quality deviations caused by temperature fluctuations.
[0074] For example, in this embodiment, the temperature of the molten tin is controlled at 300℃±5℃ by a temperature controller. It should be understood that when the molten tin is other tin-based alloys (such as tin-lead alloy, tin-silver-copper alloy, tin-bismuth alloy, etc.), the set temperature can be adaptively adjusted according to the melting point and fluidity of the specific alloy. For example, the temperature of tin-lead alloy can be controlled at 250℃~280℃. The specific temperature can be determined by those skilled in the art according to the actual process conditions, and this application does not make any special limitation in this regard.
[0075] In at least some embodiments, the solder furnace 100 is further provided with a temperature sensing unit (not shown in the figure). The temperature sensing unit is used to detect the temperature of the molten solder and adjust the heating power of the heating component 120 according to the temperature detection result, thereby maintaining the temperature of the molten solder at a set temperature. The temperature sensing unit may be any one or more combinations of thermocouples, thermistors, or infrared temperature sensors.
[0076] In at least some embodiments, see Figure 1 The tin plating equipment 10 also includes a guide fixture 130. The guide fixture 130 is rotatably disposed in the tin furnace 100 and configured to enter or exit the tin furnace 100 during rotation. The guide fixture 130 is provided with an inlet 133 for the solder strip substrate 400 to enter and an outlet 134 for the solder strip substrate 400 to exit, used to constrain the solder strip substrate 400 on a preset travel path A, allowing the solder strip substrate 400 to travel along the preset travel path A in the molten tin. When the guide fixture 130 enters the tin furnace 100 during rotation, it is positioned above the vibration head 112.
[0077] Figure 4 A three-dimensional structural diagram of a guide fixture 130 is shown. (See attached diagram) Figure 4 The guide fixture 130 includes a fixed part 131 and a rotating part. The fixed part 131 is connected to the wall of the tin furnace 100, and the rotating part is rotatably connected to the fixed part 131.
[0078] Specifically, the rotating part includes a rectangular frame, with a connecting rod 1321 and 1322 on each side of the rectangular frame. One end of the connecting rod 1321 has two connecting portions 1323, which are respectively connected to the fixing portions 131 located at both ends. A rotating shaft 1324 is provided between the connecting portions 1323 and the fixing portions 131. One end of the connecting rod 1322 on the other side is connected to a support portion 1325, used to support the connecting rod 1322 against the top wall of the tin furnace 100.
[0079] An inlet 133 for the solder strip substrate 400 to pass through is formed between the connecting rod 1321 and the bottom wall of the solder pot 100, and an outlet 134 for the solder strip substrate 400 to exit is formed between the connecting rod 1322 and the bottom wall of the solder pot 100. A constraint space is formed between the rectangular frame and the bottom wall of the solder pot 100 to constrain the solder strip substrate 400 on the preset passage path A.
[0080] During the initial threading process, the guide fixture 130 is rotated to a position where it exits the solder pot 100 (e.g., above the solder pot 100). In the open environment outside the pot, the end of the solder strip substrate 400 is inserted into the guide fixture 130 through the inlet 133, allowing the solder strip substrate 400 to travel along the guide channel inside the guide fixture 130 and then exit through the outlet 134. The guide fixture 130 is then rotated back into the solder pot 100, thus completing the threading process. At this point, the solder strip substrate 400 travels within the solder pot 100 along a preset path A, constrained by the inlet 133 and outlet 134.
[0081] During the operation of the plating equipment, the solder strip substrate 400 enters the area above the tin furnace 100 from outside the tin furnace 100 in a roughly horizontal direction. It then bends downwards into the molten tin, and then bends again to a roughly horizontal direction, entering the constraint space of the guide fixture 130 through the inlet 133. It travels horizontally along a preset path A in the molten tin to the outlet 134, then bends upwards to leave the molten tin, and finally bends again to a roughly horizontal direction to exit the tin furnace 100. The inlet 133 and outlet 134 form two-point constraints on the solder strip substrate 400, ensuring that the solder strip substrate 400 maintains the preset path A throughout the entire immersion plating process inside the molten tin, preventing deviation and scraping of the furnace wall during travel.
[0082] In this embodiment, the ultrasonic tin plating equipment 10 first heats the tin material in the tin furnace 100 to melt and holds it at a set temperature through the heating component 120. The guide fixture 130 is then moved out of the tin furnace 100, and after the strip is threaded outside the furnace, it is moved into the tin furnace 100. Each ultrasonic vibration unit 110 is activated, causing each auxiliary vibration head 112 to vibrate at a set frequency and radiate ultrasonic waves to the molten tin. The solder strip substrate 400 enters the tin furnace 100 from the photovoltaic solder strip input position and travels along the preset path A below the liquid surface. Under the action of ultrasonic cavitation, the oxide film on the surface of the substrate is removed, and the tin liquid is uniformly wetted and adheres to the surface of the solder strip substrate 400. After the solder strip substrate 400 is threaded out, it is cooled and wound up to obtain the tin-plated photovoltaic solder strip.
[0083] In at least some embodiments, the control of the ultrasonic vibration unit 110 and / or the heating component 120 can be manual or automatic. In the automatic control mode, the tin plating equipment 10 also includes a controller (not shown in the figure), which is communicatively connected to the ultrasonic vibration unit 110 and the heating component 120, and is used to automatically control the ultrasonic vibration unit 110 to turn on and off, adjust its frequency and power, and the heating component 120 to turn on and off, set its temperature and adjust its power. Each ultrasonic vibration unit 110 may have a separate controller, or multiple ultrasonic vibration units 110 may be independently controlled by the same controller to achieve independent adjustment of each ultrasonic vibration unit 110. The controller may be a programmable logic controller, a microcontroller, or an industrial computer.
[0084] In at least some embodiments, the tin plating apparatus 10 further includes a tin plating quality inspection unit (not shown in the figure). The tin plating quality inspection unit is positioned along the path of the solder strip substrate 400 after it exits the tin furnace 100, and is used to inspect the plating quality of the solder strip substrate 400 after tin plating. The tin plating quality inspection unit includes an image sensor and an image analyzer. The image sensor is used to acquire images of the surface of the solder strip substrate 400, and the image analyzer is used to analyze the images acquired by the image sensor to identify defects on the plating surface such as incomplete plating, pinholes, peeling, and uneven thickness. The tin plating quality inspection unit is communicatively connected to a controller. The analysis results from the image analyzer can be fed back to the controller. Based on the analysis results, the controller automatically adjusts at least one of the following: the frequency and / or power of the ultrasonic vibration unit 110, the temperature of the heating component 120, and the traveling speed of the solder strip substrate 400, to perform closed-loop control of the tin plating quality.
[0085] Example 2 This second embodiment provides a method for tin plating using the ultrasonic tin plating equipment 10 of the first embodiment. Figure 5 This is a flowchart illustrating the tin plating method of Embodiment 2. (See attached diagram.) Figure 5 The method includes the following steps: Step S1: Control the solder strip substrate to enter the molten solder in the solder furnace along the preset travel path, and exit from the molten solder.
[0086] The preset travel path A refers to the predetermined travel route of the solder strip substrate 400 in the tin furnace 100 from entering the molten tin to exiting the molten tin, which is located below the surface of the molten tin. It is constrained by the inlet 133 and outlet 134 of the guide fixture 130, so that the solder strip substrate 400 maintains a set depth in the molten tin and has sufficient immersion stroke.
[0087] Step S2: Control the ultrasonic vibration unit to apply ultrasonic waves to the molten tin and tin-plate the photovoltaic solder ribbon.
[0088] In step S2, the ultrasonic vibration unit 110 is controlled to work, that is, the transducer 111 is controlled to output mechanical vibration with preset working parameters, and ultrasonic waves are radiated to the molten tin through the auxiliary vibration head 112.
[0089] In one example, the preset operating parameters of each ultrasonic vibration unit 110 include a preset frequency. The preset frequency can be determined based on the following benchmark: ensuring that the difference in sound intensity between the edge region and the center region of the working surface 1121 of the auxiliary vibration head 112 in the width direction is lower than a preset threshold. The preset threshold can be preset according to the coating uniformity requirements; for example, when the ratio of the sound intensity in the edge region to the sound intensity in the center region is not less than 80%, the sound intensity difference is considered to be within an acceptable range.
[0090] The working surface 1121 of the vibratory head 112 has a certain width. Ultrasonic waves are not uniformly distributed on the working surface of the vibratory head. Due to the influence of factors such as the elastic wave propagation characteristics of the vibratory head material, boundary reflection, and vibration modes, the sound intensity in the central region of the working surface is usually higher, while the sound intensity in the edge region is lower, forming a "strong center, weak edge" sound field distribution characteristic. At different excitation frequencies, the vibration modes excited inside the vibratory head 112 are different, and the vibration displacement distribution on the working surface 1121 also changes accordingly. At certain frequencies, the vibration amplitude in each region of the working surface 1121 tends to be uniform, and the difference in sound intensity between the center and the edge is small; while at other frequencies, non-uniform modes may be excited, leading to a significant increase in the difference in sound intensity between the center and the edge. Therefore, by selecting an appropriate preset frequency, the vibration modes of the vibratory head 112 can be adjusted, making the sound intensity distribution in the width direction of the working surface 1121 tend to be uniform.
[0091] Due to differences in manufacturing tolerances, assembly conditions, and positions within the tin furnace 100, the vibration characteristics of the auxiliary vibration head 112 of each ultrasonic vibration unit 110 vary. Each ultrasonic vibration unit 110 can independently determine its own preset frequency, which can be the same or different.
[0092] By selecting the aforementioned preset frequency, the sound intensity distribution along the width of the working surface 1121 can be made more uniform, and the ultrasonic cavitation intensity received at each position along the width of the solder strip substrate 400 can be made more consistent. This improves the uniformity of the plating layer along the width of the solder strip substrate 400 and reduces the probability of edge plating defects. At the same time, each ultrasonic vibration unit 110 operates at its own optimal preset frequency, reducing the interference of ultrasonic fields or standing wave dead zones caused by forcing all ultrasonic vibration units 110 to operate at the same frequency. The ultrasonic field is uniformly connected along the length of the solder pot, which helps to improve the batch consistency of tin plating quality.
[0093] As a specific example, the preset frequency range is 50kHz ≥ f ≥ 7kHz, such as 7kHz, 10kHz, 15kHz, 20kHz, 30kHz, 50kHz, etc.
[0094] It should be understood that when the operating frequency is below 7kHz, the sound waves enter the audible range, and the surface of the molten solder is violently disturbed, easily causing splashing, making it difficult to achieve uniform and controllable strip removal. When the operating frequency is above 50kHz, the ultrasonic wavelength is too short, and the propagation attenuation in the molten solder increases sharply, significantly shortening the effective working distance and potentially resulting in insufficient strip removal capability. Therefore, setting the preset frequency within the range of 7kHz to 50kHz can ensure sufficient cavitation strip removal while also considering the uniformity of the sound field distribution, controllable propagation attenuation, and adaptability to ultra-thin solder strips.
[0095] It should be understood that the selection of the preset frequency is also related to the traveling speed of the solder ribbon substrate 400. When the traveling speed of the solder ribbon is high, the travel distance of the solder ribbon substrate 400 through each ultrasonic action zone per unit time increases, and the ultrasonic treatment time of a single auxiliary vibration head 112 on a specific section of the solder ribbon is shortened. In order to achieve sufficient oxide layer removal and plating activation within a shorter action time, the preset frequency can be appropriately adjusted to enhance the instantaneous action intensity of cavitation bubble collapse, thereby completing the cavitation treatment of the surface of the solder ribbon substrate 400 in a shorter time. Conversely, when the traveling speed of the solder ribbon substrate 400 is low, the residence time of the solder ribbon substrate 400 in the ultrasonic action zone is longer. The preset frequency can be adjusted to achieve sufficient oxide layer removal effect at a lower cavitation intensity, while also helping to further reduce molten solder disturbance and improve the surface smoothness of the plating layer.
[0096] The specific optimal frequency value can be determined through experiments or simulations based on the actual solder strip substrate specification 400, the molten solder temperature, and the plating quality requirements.
[0097] In one example, the preset operating parameters of each ultrasonic vibration unit 110 include a preset power. For example, the output power of all ultrasonic vibration units 110 is 15kW to 30kW. Within this power range, the ultrasonic waves can generate a sufficient cavitation effect in the molten solder, enough to remove the micro-oxide layer on the surface of the solder strip substrate 400, while also exhibiting good industrial mass production adaptability. It should be understood that the specific value of the ultrasonic power can be adjusted according to actual process requirements. When the solder strip travel speed is high or the oxide layer on the solder strip surface is thick, the ultrasonic power can be appropriately adjusted to enhance the cavitation film removal effect; when the solder strip substrate 400 is thin (e.g., 0.1mm) or sensitive to fluid impact, the ultrasonic power can be appropriately adjusted to reduce the impact on the solder strip.
[0098] The frequency and power selection settings described above in this application embodiment constitute a flexible ultrasonic action mode. In this mode, it is beneficial to maintain a low-disturbance state of the molten solder while ensuring efficient oxide layer removal, which helps improve the plating smoothness of the solder strip surface and reduces the probability of incomplete plating and pinhole defects.
[0099] In at least some embodiments, the vibration aid head 112 is at least partially immersed in the molten solder, i.e., located below the surface of the molten solder. Further, the vibration aid head 112 is completely immersed in the molten solder.
[0100] In at least some embodiments, the vertical distance between the working surface 1121 of the vibration aid head 112 and the height position of the preset travel path A of the solder ribbon substrate 400 is 10mm to 22mm, such as 10mm, 15mm, 20mm, 22mm, etc. It should be understood that when this vertical distance is too close (e.g., less than 10mm), the impact force generated by the collapse of cavitation bubbles acts directly on the surface of the solder ribbon substrate 400, which may cause excessive erosion of the plating or coarsening of the surface structure. Simultaneously, the molten solder layer between the solder ribbon substrate 400 and the vibration aid head 112 is too thin, resulting in insufficient cavitation development. When this vertical distance is too far (e.g., greater than 22mm), the propagation distance of the ultrasonic waves in the molten solder increases, energy attenuation intensifies, and the sound intensity reaching the surface of the solder ribbon substrate 400 is insufficient to produce an effective cavitation film removal effect. During the equipment debugging phase, the uniformity and adhesion of the plating layer on the surface of the solder ribbon substrate 400 at different distances can be measured to select the distance that optimizes the plating quality as the set value.
[0101] The dimensions of the solder ribbon substrate 400, such as its width and thickness, can be selected as needed. In at least some embodiments, the thickness of the solder ribbon substrate 400 is 0.1 mm to 0.15 mm, and its width is 10 mm to 15 mm. For example, the thickness of the solder ribbon substrate 400 is 0.12 mm, and its width is 14 mm. Ultra-thin, narrow-width solder ribbons within this thickness and width range are sensitive to the cleaning effect of ultrasonic cavitation and have low resistance to the impact of molten tin. The ultrasonic tin plating method of this embodiment can achieve good coating uniformity and adhesion within this specification range. It should be understood that the method of this embodiment can also be applied to solder ribbon substrates 400 of other specifications, but the effect is more significant for ultra-thin, narrow-width solder ribbon substrates 400.
[0102] It should be understood that the operating parameters of the ultrasonic vibration unit 110 (such as frequency and power), the specifications of the solder strip substrate 400 (such as thickness and width) and its traveling speed, the depth of the molten solder in the solder pot 100, the vertical distance between the working surface 1121 of the auxiliary vibration head 112 and the solder strip substrate 400, and the immersion depth of the solder strip substrate 400 in the molten solder are all interconnected and jointly affect the final plating quality. The synergistic relationship between the parameters can be briefly described as follows: the higher the power, the higher the cavitation intensity, which can be matched with a higher traveling speed or a thicker solder strip; the higher the frequency, the more severe the propagation attenuation, which requires a corresponding reduction in the vertical distance or an increase in power; when the vertical distance increases, the propagation attenuation intensifies, which can be compensated by increasing the power or decreasing the frequency; when the immersion depth of the solder strip substrate 400 in the molten solder increases, the power needs to be increased accordingly to compensate for the energy attenuation.
[0103] In one specific embodiment, the parameters can be adjusted within the following ranges according to actual process requirements: the power of each ultrasonic vibration unit 110 is 15 kW to 30 kW, the frequency is 7 kHz to 50 kHz, the thickness of the solder strip substrate 400 is 0.1 mm to 0.15 mm, the width is 10 mm to 15 mm, the traveling speed is 30 m / min to 150 m / min, the depth of the molten solder is 50 mm to 80 mm, the depth of the solder strip substrate 400 in the molten solder is 30 mm to 55 mm, and the vertical distance between the working surface 1121 of the auxiliary vibration head 112 and the solder strip substrate 400 is 10 mm to 22 mm. When one or more of the parameters change, the other parameters can be adjusted accordingly. The specific combination of parameters can be determined by those skilled in the art through a limited number of experiments based on actual process conditions, and this application does not impose any particular limitation on this.
[0104] It should be understood that steps S1 and S2 are performed synchronously during equipment operation. The solder strip substrate 400 moves continuously, and the ultrasonic vibration unit 110 continuously radiates ultrasonic waves to the molten solder, so that the solder strip substrate 400 is in the effective ultrasonic action zone throughout the entire immersion process below the liquid surface, and continuously completes the demolding, wetting and plating.
[0105] Example 3 This embodiment three provides a photovoltaic welding strip, which is prepared using the ultrasonic coating equipment 10 of embodiment one or the coating method of embodiment two.
[0106] The photovoltaic ribbon specifically includes a ribbon substrate 400 and a coating covering the surface of the ribbon substrate 400.
[0107] It should be noted that related parts in different embodiments of this application can be referred to each other, and repeated parts will not be described again in this application. For example, the content not described in detail in this embodiment two can be referred to in embodiment one, and the content not described in detail in this embodiment three can be referred to in embodiment one and embodiment two respectively.
[0108] The technical solutions provided in this application have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of this application. The descriptions of the embodiments above are only for the purpose of helping to understand the method and core ideas of this application. Furthermore, those skilled in the art will recognize that, based on the ideas of this application, there will be changes in the specific implementation methods and application scope. Therefore, the content of this specification should not be construed as a limitation of this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. An ultrasonic coating device, characterized in that, The ultrasonic coating equipment includes: A tin furnace, equipped with a furnace cavity for holding molten metal; N ultrasonic vibration units are arranged inside the tin furnace. Each ultrasonic vibration unit includes a transducer and a vibration head. The transducer applies ultrasonic waves to the molten metal through the vibration head. Among them, the M ultrasonic vibration units are arranged at intervals along the length of the tin furnace, M≤N and M≥2.
2. The ultrasonic coating equipment according to claim 1, characterized in that, The M vibration-aiding heads are arranged linearly at equal intervals along the length of the tin furnace.
3. The ultrasonic coating equipment according to claim 1, characterized in that, Along the width direction of the tin furnace, the effective size of the working surface of the vibration head is not less than 120mm.
4. The ultrasonic coating equipment according to claim 1, characterized in that, Along the width direction of the tin furnace, the size of the furnace cavity is not less than 15mm.
5. The ultrasonic coating equipment according to claim 1, characterized in that, Heating components are arranged circumferentially on the outer side of the tin furnace cavity.
6. The ultrasonic coating equipment according to claim 1, characterized in that, The ultrasonic coating equipment also includes: A guide fixture is rotatably configured relative to the tin furnace and is configured to enter or exit the furnace cavity of the tin furnace during rotation. The guide fixture is provided with an inlet for the solder strip substrate to pass through and an outlet for the solder strip substrate to pass through, and is used to constrain the solder strip substrate on a preset travel path.
7. A coating method using the ultrasonic coating equipment according to any one of claims 1 to 6, characterized in that, The method includes: The welding strip substrate is controlled to enter the molten metal along a preset path and exit from the molten metal; During the passage of the welding strip substrate, the ultrasonic vibration unit is controlled to apply ultrasonic waves to the molten metal liquid to coat the welding strip substrate and form a coating layer.
8. The method according to claim 7, characterized in that, The control of the ultrasonic vibration unit includes: Each ultrasonic vibration unit is controlled to operate at its corresponding preset frequency. At the preset frequency, the sound intensity difference between the edge region and the center region of the working surface of the vibration head in the width direction is lower than a preset threshold.
9. The method according to claim 8, characterized in that, The preset frequency is f, and 50kHz ≥ f ≥ 7kHz.
10. The method according to claim 7, characterized in that, The thickness of the welding strip substrate is 0.1 mm to 0.15 mm, and the width is 10 mm to 15 mm.
11. The method according to claim 7, characterized in that, The vibration-assisted head is at least partially immersed in the molten metal liquid.
12. The method according to claim 11, characterized in that, The vibration-assisted head meets at least one of the following criteria: Completely immersed in the molten metal liquid; The vertical distance between the working surface of the vibration-assisted head and the height of the preset travel path is 10mm to 22mm.
13. A photovoltaic welding strip, characterized in that, It is prepared using the ultrasonic coating equipment according to any one of claims 1 to 6 or the coating method according to any one of claims 7 to 12.