A method for the preparation of transition metal silicon nitride thin films from single layer transition metal chalcogenide precursors
The method of converting monolayer transition metal chalcogenides into transition metal silicon nitrides solves the problem of preparing high-quality MSi2N4 thin films in the prior art, and achieves efficient and stable material conversion, which is suitable for electronic devices and optoelectronic devices.
Patent Information
- Application Number
- CN202611238054.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to efficiently prepare high-quality transition metal silicon nitride films, especially MSi2N4, due to its complex and unstable chemical reaction pathways, which limits its application in electronic and optoelectronic devices.
Using a single-layer transition metal chalcogenide as a substrate, a combination of nitriding and silicon nitride passivation processes, including preliminary nitriding and high-temperature silicon nitride passivation steps, is used to transform the material into a transition metal silicon nitride on a metal substrate. The reaction temperature and time are controlled by using van der Waals forces or physical bonding to ensure the integrity of the material structure and the uniformity of the phases.
We have achieved the preparation of high-quality, structurally intact MSi2N4 thin films, maintaining atomic-level thickness and two-dimensional morphology, and possessing excellent electrical properties and thermal conductivity, making them suitable for next-generation electronic and optoelectronic devices.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of two-dimensional materials and semiconductor materials preparation technology, specifically relating to a method for preparing transition metal silicon nitrides MSi2N4 using monolayer transition metal chalcogenides as precursors, providing a new technical solution for the large-scale preparation of two-dimensional materials. Background Technology
[0002] Monolayer transition metal chalcogenides (such as MoS2 and WS2) hold significant promise for applications in next-generation electronic devices, optoelectronic devices, and catalysis due to their unique atomic-level thickness and excellent electrical and optical properties. However, some transition metal chalcogenides exhibit insufficient stability under environmental conditions, failing to meet the requirements of specific applications. Transforming two-dimensional materials into other two-dimensional materials holds promise for inheriting their atomic-level thickness structure while possessing superior stability and physicochemical properties.
[0003] Transition metal silicon nitrides (MSi₂N₄, where M = Mo, W, etc.) are novel two-dimensional van der Waals layered materials, attracting considerable attention due to their excellent physicochemical properties. Among them, representative materials MoSi₂N₄ and WSi₂N₄ are high-performance two-dimensional semiconductors with moderate band gaps (1.94 eV, 2.25 eV), high carrier mobility, excellent optical transmittance, high thermal conductivity (MoSi₂N₄: 173 W / m·K), and outstanding mechanical strength and stability. These characteristics make them highly promising for applications in electronic devices, optoelectronic devices, spintronic devices, and energy conversion materials, especially as channel materials for next-generation CMOS devices.
[0004] Controllable preparation of high-quality MSi₂N₄ thin films is a core prerequisite for their device applications and industrialization. However, MSi₂N₄ is composed of three elements: transition metal M, silicon, and nitrogen. Its chemical reaction pathway is more complex than that of unary or binary two-dimensional materials, and it can only be prepared by chemical vapor deposition. Therefore, there is an urgent need to develop a stable, simple, and efficient method for the synthesis of MSi₂N₄ and its multi-element alloys, thereby laying the material foundation for the practical application of this novel two-dimensional material. Summary of the Invention
[0005] This invention provides a method for preparing transition metal silicon nitrides using a single-layer transition metal chalcogenide as a substrate through a combination of nitriding and silicon nitride passivation processes, aiming to obtain two-dimensional transition metal silicon nitride materials with complete structure and uniform phase.
[0006] A method for preparing transition metal silicon nitrides by conversion of monolayer transition metal chalcogenides includes the following steps: (a) Substrate assembly: High-quality monolayer transition metal chalcogenides (e.g., monolayer MoS2, WS2, Mo) are obtained by one or more of the following methods: chemical vapor deposition, mechanical exfoliation, or liquid phase exfoliation. x W 1-x Using S2 alloy, etc., as the starting substrate, the above-mentioned monolayer substrate is grown in situ, transferred, or spin-coated onto the surface of a clean metal substrate, wherein the metal substrate is selected from copper foil, gold foil, or gold / copper plated substrate, and is brought into close contact by van der Waals forces or physical adhesion; (b) Preliminary nitriding: The assembled substrate is placed in a tube furnace or chemical vapor deposition system, and a mixture of hydrogen and ammonia is introduced. The temperature is increased to 600–800°C at a rate of 5–25°C / min and held for 30–120 minutes to induce a preliminary nitriding reaction on the surface of the monolayer material, forming a transition metal nitride intermediate; (c) High-temperature silicon nitride passivation: Maintain the same hydrogen / ammonia atmosphere and continue to raise the temperature to above 1000℃. At the same time, introduce a silicon source and perform high-temperature treatment at this temperature for 60 to 180 minutes. Silicon atoms diffuse together with nitrogen atoms and replace chalcogen elements, ultimately completely converting the original transition metal chalcogen compounds into transition metal silicon nitrides (such as MoSi2N4, WSi2N4, etc.).
[0007] The shape, thickness, and size of the MSi2N4 obtained by conversion depend on the shape, thickness, and size of MX2, meaning that the shape and size are the same before and after conversion.
[0008] Furthermore, the above method also includes a post-processing step, namely, using a wet transfer method or a dry transfer method to separate the transition metal silicon nitride (MSi2N4) film grown on the surface of the non-metallic substrate from the surface of the growth substrate; or directly retaining the MSi2N4 film grown on the substrate for use together.
[0009] The design principle of this invention is based on a single-layer transition metal chalcogenide MX2 as a template, placed on a copper or gold substrate, and transformed in two steps in an H2 / NH3 atmosphere: firstly, a low-temperature preliminary nitriding is performed at 600–800 °C, NH3 decomposes to produce active nitrogen species, and H2 reduces and removes chalcogen elements, generating vacancies to form a metastable MN. x An intermediate is then heated to over 1000℃ and a silicon source is introduced. Silicon and nitrogen atoms diffuse into the crystal lattice together, completely replacing the residual chalcogen elements and driving the structural rearrangement into a seven-atom-layer MSi2N4. The metal substrate catalyzes the decomposition of NH3, promotes silicon atom migration, and suppresses side reactions; the confinement effect of the monolayer template ensures that the product maintains atomic-level thickness and a continuous two-dimensional morphology.
[0010] The advantages and beneficial effects of this invention are: Compared with the prior art, the present invention has the following advantages: 1. This invention uses a single-layer transition metal chalcogenide as a template, which can precisely control the thickness, morphology and elemental composition of the final product, and obtain transition metal silicon nitrides and their alloys that maintain a two-dimensional morphology, and have the ability to be patterned.
[0011] 2. This invention is compatible with various methods of obtaining single-layer materials, including but not limited to chemical vapor deposition, mechanical exfoliation, and electrochemical exfoliation, and has a wide range of precursor sources and strong applicability.
[0012] This method uses a single-layer two-dimensional chalcogenide as a structural template and achieves a phase transformation of the material through a two-step atmosphere conversion process, while maintaining atomic-level thickness. This yields large-area, uniform, and high-quality transition metal silicon nitride films. The process is stable and controllable, and the resulting product exhibits excellent electrical properties, thermal conductivity, and air stability. It can be used as a transistor channel material and has broad application prospects in next-generation electronic devices, optoelectronic devices, and channel materials. Attached Figure Description
[0013] Figure 1 Schematic diagram of the process for preparing transition metal silicon nitride MSi2N4 by conversion of monolayer transition metal chalcogenides MX2 (where X represents sulfur, selenium, and tellurium). Figure 2 Optical photograph of MoS2 / Au before conversion.
[0014] Figure 3 Optical photograph of the converted MoSi2N4 / Au.
[0015] Figure 4 Raman spectra of the samples before and after conversion.
[0016] Figure 5 Secondary ion mass spectrometry (SIMS) image of the converted MoSi2N4 / Au.
[0017] Figure 6 Optical photograph of WSe2 / Au before conversion.
[0018] Figure 7 Optical photograph of WSi2N4 / Au after conversion.
[0019] Figure 8 Raman spectra of samples before and after WSe2 / Au conversion. Detailed Implementation
[0020] The present invention will now be described in further detail with reference to embodiments and accompanying drawings.
[0021] Example 1 A monolayer MoS2 / Au substrate (10 μm thick) was prepared as a precursor / substrate composite structure using chemical vapor deposition and placed in the center of a quartz tube within a tube furnace. The system was evacuated to below 5 Pa, and a hydrogen / ammonia mixture (H2:NH3 volume ratio of 1:20, total flow rate of 210 sccm) was introduced before restoring to atmospheric pressure. The system was heated from room temperature to the nitriding reaction temperature of 800℃ at a heating rate of 25℃ / min and held at that temperature for 30 min for preliminary nitriding treatment.
[0022] Maintaining the same hydrogen / ammonia mixed atmosphere, the preliminary nitriding product was heated again to 1050℃ at a rate of 25℃ / min. The reaction was carried out at this temperature for 120 minutes, allowing the silicon atoms provided by the quartz tube and the nitrogen atoms from the ammonia decomposition to fully diffuse and replace sulfur atoms, thus completing silicon-nitrogen passivation. After the reaction, the product was naturally cooled to room temperature under a H2 / NH3 protective atmosphere, resulting in a MoSi2N4 monolayer film on the gold substrate.
[0023] Finally, the film can be completely transferred to any target substrate using a polydimethylsiloxane (PDMS)-assisted dry transfer technique, a polymethyl methacrylate (PMMA)-assisted wet transfer technique, or an electrochemical bubble transfer technique, facilitating subsequent detailed characterization, device fabrication, and performance testing.
[0024] The morphology and color of MoS2 and MoSi2N4 thin films or crystals were observed using an optical microscope, the vibrational characteristic peak positions and crystal structure were characterized using a Raman spectrometer, and the elemental composition was characterized by collecting the nucleus-mass ratio and its surface distribution using a secondary ion mass spectrometer, indicating that MoSi2N4 crystals were successfully obtained. Figure 2 Optical microscopy characterization of 3 shows the morphology of the crystal domains before and after the nitriding-passivation reaction. Figure 4 Raman spectroscopy revealed characteristic peaks in the samples before and after the nitriding-passivation reaction, confirming the successful preparation of high-quality MoSi2N4 crystals. Figure 5 Secondary particle mass spectrometry surface scan analysis confirmed that MoSi2N4 crystals were successfully obtained after the nitriding-passivation reaction.
[0025] Example 2 A monolayer WSe2 / Au substrate (10 μm thick) was prepared as a precursor / substrate composite structure using chemical vapor deposition and placed in the center of a quartz tube within a tube furnace. The system was evacuated to below 5 Pa, and a hydrogen / ammonia mixture (H2:NH3 volume ratio of 1:20, total flow rate of 210 sccm) was introduced before restoring to atmospheric pressure. The system was heated to 800 °C at a heating rate of 25 °C / min and held at that temperature for 30 min for preliminary nitriding treatment.
[0026] Maintaining the same hydrogen / ammonia mixed atmosphere, the preliminary nitriding product was heated again to 1050℃ at a rate of 25℃ / min. The reaction was then carried out at this temperature for 120 min to allow sufficient diffusion of silicon atoms provided by the quartz tube and nitrogen atoms from the decomposition of ammonia to replace sulfur atoms, thus completing silicon-nitrogen passivation. After the reaction, the product was naturally cooled to room temperature under a protective atmosphere of H2 / NH3, resulting in a WSi2N4 thin film on the gold substrate.
[0027] Finally, the film can be completely transferred to any target substrate using a polydimethylsiloxane (PDMS)-assisted dry transfer technique, a polymethyl methacrylate (PMMA)-assisted wet transfer technique, or an electrochemical bubble transfer technique, facilitating subsequent detailed characterization, device fabrication, and performance testing.
[0028] The morphology and color of WSe2 and WSi2N4 thin films or crystals were observed using an optical microscope; the vibrational characteristic peak positions and crystal structure were characterized using Raman spectroscopy; and the elemental composition was characterized using secondary ion mass spectrometry, indicating that WSi2N4 crystals were successfully obtained. (Figure 6 and...) Figure 7 Domain morphology before and after nitriding-passivation reaction Figure 8 Raman spectroscopy revealed characteristic peaks in the samples before and after the nitriding-passivation reaction, confirming the successful preparation of high-quality WSi2N4 thin films.
[0029] Example 3 This embodiment is basically the same as Embodiment 1, except that a mechanical exfoliation method is used to transfer the monolayer MoS2 onto the upper surface of a copper substrate (25 μm thick). Polydimethylsiloxane (PDMS) is used to assist in the exfoliation of the bulk MoS2. ACS Nano (2024, 18, 250009) A monolayer MoS2 crystal was obtained and transferred to a Cu substrate (25 μm thick) using a two-dimensional transfer platform.
[0030] The above MoS2 / Cu composite structure was placed in the center of a tube furnace. The system was evacuated to below 5 Pa, and a hydrogen / ammonia mixture (H2:NH3 volume ratio of 1:20, total flow rate of 210 sccm) was introduced to restore the pressure to atmospheric pressure. The system was heated to 800℃ at a heating rate of 25℃ / min and held at that temperature for 30 min for preliminary nitriding treatment.
[0031] Maintaining the same hydrogen / ammonia mixed atmosphere, the preliminary nitriding product was heated again to 1050℃ at a rate of 25℃ / min. The reaction was carried out at this temperature for 120 min to allow the silicon atoms provided by the quartz tube and the nitrogen atoms from the ammonia decomposition to fully diffuse and replace the sulfur atoms, thus completing silicon-nitrogen passivation. After the reaction, the mixture was naturally cooled to room temperature under a H2 / NH3 protective atmosphere, resulting in a MoSi2N4 thin film on the copper substrate.
[0032] Finally, the film can be completely transferred to any target substrate using a polydimethylsiloxane (PDMS)-assisted dry transfer technique, a polymethyl methacrylate (PMMA)-assisted wet transfer technique, or an electrochemical bubble transfer technique, facilitating subsequent detailed characterization, device fabrication, and performance testing.
[0033] The morphology and color of MoS2 and MoSi2N4 thin films or crystals were observed using an optical microscope, the vibrational characteristic peak positions and crystal structure were characterized using Raman spectroscopy, and the elemental composition was characterized using secondary ion mass spectrometry, indicating that MoSi2N4 crystals were successfully obtained.
[0034] Example 4 This embodiment follows the same process and conditions as Example 1, except that a 1 mg / ml monolayer MoS2 suspension, obtained through a commercial electrochemical exfoliation method, is spin-coated onto a copper substrate to form a monolayer MoS2 film. The MoS2 / Au film is placed in the center of a tube furnace. The system is evacuated to below 5 Pa, and a hydrogen / ammonia mixture (H2:NH3 volume ratio 1:20, total flow rate 210 sccm) is introduced to restore atmospheric pressure. The temperature is then increased to 800°C at a rate of 25°C / min and held at that temperature for 30 min for preliminary nitriding treatment.
[0035] Maintaining the same hydrogen / ammonia mixed atmosphere, the preliminary nitriding product was heated again to 1050℃ at a rate of 25℃ / min. The reaction was then carried out at this temperature for 120 min to allow sufficient diffusion of silicon atoms provided by the quartz tube and nitrogen atoms from ammonia decomposition, replacing sulfur atoms and completing silicon-nitrogen passivation. After the reaction, the product was naturally cooled to room temperature under a H2 / NH3 protective atmosphere, resulting in a transition metal silicon nitride (MoSi2N4) film on the gold substrate surface.
[0036] Finally, the film can be completely transferred to any target substrate using a polydimethylsiloxane (PDMS)-assisted dry transfer technique, a polymethyl methacrylate (PMMA)-assisted wet transfer technique, or an electrochemical bubble transfer technique, facilitating subsequent detailed characterization, device fabrication, and performance testing.
[0037] The morphology and color of MoS2 and MoSi2N4 thin films or crystals were observed using an optical microscope, the vibrational characteristic peak positions and crystal structure were characterized using Raman spectroscopy, and the elemental composition was characterized using secondary ion mass spectrometry, indicating that MoSi2N4 crystals were successfully obtained.
[0038] Example 5 A monolayer MoS2 / Au substrate (10 μm thick) was prepared as a precursor / substrate composite structure using chemical vapor deposition (CVD) and placed in the center of a quartz tube within a tube furnace. The system was evacuated to below 5 Pa, and a hydrogen / ammonia mixture (H2:NH3 volume ratio 1:10, total flow rate 210 sccm) was introduced before restoring to atmospheric pressure. The temperature was then increased to 1050 °C at a rate of 25 °C / min. The reaction was carried out at this temperature for 120 min to allow sufficient diffusion of silicon atoms provided by the quartz tube and nitrogen atoms from ammonia decomposition, replacing sulfur atoms and completing silicon-nitrogen passivation. After the reaction, the substrate was naturally cooled to room temperature under a H2 / NH3 protective atmosphere, resulting in a MoSi2N4 thin film on the gold substrate surface.
[0039] Finally, the film can be completely transferred to any target substrate using a polydimethylsiloxane (PDMS)-assisted dry transfer technique, a polymethyl methacrylate (PMMA)-assisted wet transfer technique, or an electrochemical bubble transfer technique, facilitating subsequent detailed characterization, device fabrication, and performance testing.
[0040] The morphology and color of MoS2 and MoSi2N4 thin films or crystals were observed using an optical microscope, the vibrational characteristic peak positions and crystal structure were characterized using Raman spectroscopy, and the elemental composition was characterized using secondary ion mass spectrometry, indicating that MoSi2N4 crystals were successfully obtained.
[0041] Comparative Example 1 A monolayer WSe2 / Au substrate (10 μm thick) was prepared as a precursor / substrate composite structure using chemical vapor deposition and placed in the center of a quartz tube within a tube furnace. The system was evacuated to below 5 Pa, hydrogen gas was introduced (flow rate 210 sccm), and then restored to atmospheric pressure. The temperature was raised to 800 °C at a rate of 25 °C / min and held at that temperature for 30 min for preliminary nitriding. Maintaining the same hydrogen flow rate, the temperature was again raised to 1000 °C at 25 °C / min. The reaction was carried out at this temperature for 120 min, without ammonia to provide nitrogen. After the reaction, the substrate was naturally cooled to room temperature under a protective atmosphere of H2 / NH3, yielding W particles on the gold substrate surface.
[0042] Comparative Example 2 A monolayer WSe2 / Au substrate (10 μm thick) was prepared as a precursor / substrate composite structure using chemical vapor deposition (CVD) and placed in the center of a quartz tube within a tube furnace. The system was evacuated to below 5 Pa, and a hydrogen / ammonia mixture (H2:NH3 volume ratio 1:1, total flow rate 210 sccm) was introduced before restoring to atmospheric pressure. The temperature was then increased to 1050 °C at a rate of 25 °C / min. The reaction was carried out at this temperature for 120 min, allowing nitrogen atoms from the decomposition of excess ammonia to fully diffuse and replace sulfur atoms, thus completing silicon-nitrogen passivation. After the reaction, the substrate was naturally cooled to room temperature under a H2 / NH3 protective atmosphere, resulting in WN crystals on the gold substrate surface.
[0043] Comparative Example 3 A monolayer WSe2 / SiO2 / Si substrate (oxide layer thickness 280 nm) was prepared as a precursor / substrate composite structure using chemical vapor deposition (CVD) and placed in the center of a quartz tube within a tube furnace. The system was evacuated to below 5 Pa, and a hydrogen / ammonia mixture (H2:NH3 volume ratio 1:1, total flow rate 210 sccm) was introduced to restore atmospheric pressure. The temperature was then increased to 1050 °C at 25 °C / min. The reaction was carried out at this temperature for 120 min, utilizing silicon atoms provided by the quartz tube and nitrogen atoms from the decomposition of ammonia, but without metal catalysis. After the reaction, the substrate was naturally cooled to room temperature under a H2 / NH3 protective atmosphere, yielding WN crystals on the gold substrate surface.
[0044] Comparative Example 4 A monolayer WSe2 / Au substrate (10 μm thick) was prepared as a precursor / substrate composite structure using chemical vapor deposition (CVD) and placed in the center of a quartz tube within a tube furnace. The system was evacuated to below 5 Pa, and a hydrogen / ammonia mixture (H2:NH3 volume ratio 1:20, total flow rate 210 sccm) was introduced to restore atmospheric pressure. The temperature was then increased to 900 °C at a rate of 25 °C / min. The reaction was carried out at this temperature for 120 min, which was considered too low. After the reaction, the substrate was allowed to cool naturally to room temperature under a H2 / NH3 protective atmosphere, resulting in WN crystals on the gold substrate surface.
[0045] Comparative Example 5 A monolayer WSe2 / Au substrate (10 μm thick) was prepared as a precursor / substrate composite structure using chemical vapor deposition (CVD) and placed in the center of a quartz tube within a tube furnace. The system was evacuated to below 5 Pa, and a hydrogen / ammonia mixture (H2:NH3 volume ratio 1:20, total flow rate 210 sccm) was introduced before restoring to atmospheric pressure. The temperature was then increased to 1050 °C at a rate of 25 °C / min. The reaction was carried out at this temperature for 30 min to allow sufficient diffusion of silicon atoms provided by the quartz tube and nitrogen atoms from ammonia decomposition to replace sulfur atoms. Due to insufficient reaction time, the passivation reaction was not completed. After the reaction, the substrate was naturally cooled to room temperature under a H2 / NH3 protective atmosphere, resulting in WN crystals on the gold substrate surface.
[0046] Comparative Example 6 A multilayer WSe2 / Au substrate (10 μm thick) was prepared as a precursor / substrate composite structure using chemical vapor deposition (CVD) and placed in the center of a quartz tube within a tube furnace. The system was evacuated to below 5 Pa, and a hydrogen / ammonia mixture (H2:NH3 volume ratio 1:20, total flow rate 210 sccm) was introduced before restoring to atmospheric pressure. The temperature was then increased to 1050 °C at a rate of 25 °C / min. The reaction was carried out at this temperature for 120 min, with the substrate thickness limiting the passivation process. After the reaction, the substrate was naturally cooled to room temperature under a H2 / NH3 protective atmosphere, resulting in WN crystals on the gold substrate surface.
[0047] like Figure 2 As shown, the reaction product obtained after the nitriding-passivation reaction is MoSi2N4.
[0048] like Figure 3 As shown in Figure 4, the Raman spectra of MoS2 (reaction substrate) and MoSi2N4 (reaction product) before and after the nitriding-passivation reaction confirm that MoS2 was successfully converted into MoSi2N4.
[0049] like Figure 5 As shown, the reaction product MoSi2N4 obtained after the nitriding-passivation reaction is characterized by secondary particle mass spectrometry (SIMS).
[0050] like Figure 6 As shown, WSe2 grown on the Au surface by chemical vapor deposition is used as the reaction substrate.
[0051] like Figure 7 As shown, the reaction product obtained after the nitriding-passivation reaction is WSi2N4.
[0052] like Figure 8 As shown, the Raman spectra of WSe2 (reaction substrate) and WSi2N4 (reaction product) before and after the nitriding-passivation reaction confirm that WSe2 was successfully converted into WSi2N4.
[0053] The above results demonstrate that the present invention proposes a controllable method for preparing transition metal silicon nitrides and their multi-element alloys by conversion of monolayer transition metal chalcogenides.
[0054] The embodiments provided above are merely illustrative and should not be considered as limiting the scope of the present invention. Any method that makes equivalent substitutions or changes to the technical solutions and inventive concepts of the present invention should be covered within the protection scope of the present invention.
Claims
1. A method for the preparation of transition metal silicon nitride thin films from single layer transition metal chalcogenide precursors, characterized in that, Includes the following steps: (a) Substrate assembly: High-quality monolayer transition metal chalcogenides are obtained as starting substrates by one or more of the following methods: in-situ growth by chemical vapor deposition, mechanical exfoliation and transfer, or liquid phase exfoliation and spin coating of nanosheets, and the assembly of monolayer transition metal chalcogenides MX2 on the surface of metal substrates is realized. (b) Preliminary nitriding: The assembled substrate with the substrate is placed in a mixed atmosphere of hydrogen and ammonia, and the temperature is raised from room temperature to 600℃~800℃ and held for 0~240 minutes to allow the monolayer transition metal chalcogenide to undergo a preliminary nitriding reaction, forming a transition metal nitride intermediate; (c) High-temperature silicon nitride passivation: Maintain the same hydrogen / ammonia mixed atmosphere as in step (b), continue to raise the temperature to above 1000°C, and introduce a silicon source at the same time. React for 60 to 180 minutes to convert the transition metal nitride intermediate into transition metal silicon nitride MSi2N4.
2. The method of claim 1, wherein, The transition metal M mentioned in step (a) is selected from at least one or more of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, and W, and X is at least one or more of sulfur, selenium, or tellurium. M and X form a transition metal chalcogenide and its alloy chalcogenide MX2.
3. The method of claim 1, wherein, The metal substrate mentioned in step (a) is one or more of copper foil, gold foil, copper-plated substrate or gold-plated substrate, and the single-layer transition metal chalcogenide is in contact with the surface of the metal substrate by van der Waals force or physical bonding.
4. The method of claim 1, wherein, The volume ratio of hydrogen to ammonia in step (b) is 1:10 to 1:20, preferably 1:15 to 1:20, and the heating rate is 5 to 25 °C / min, from room temperature to the nitriding reaction temperature.
5. The method according to claim 1 or 4, characterized in that, The reaction time for the low-temperature nitriding in step (b) is 30 to 180 minutes, preferably 30 to 120 minutes.
6. The method according to claim 1 or 4, characterized in that, The temperature for low-temperature nitriding in step (b) is 600℃~800℃, preferably 700-800℃.
7. The method of claim 1, wherein, The silicon source mentioned in step (c) is provided at high temperature by one or more of the following: the quartz tube wall, quartz powder, etc., in the reactor of the reaction apparatus.
8. The method of claim 1, wherein, The high-temperature silicon nitride passivation temperature in step (c) is above 1000°C, preferably 1020-1080°C, and more preferably 1040-1060°C.
9. The method of claim 1, wherein, It also includes a post-processing step: transferring the transition metal silicon nitride (MSi2N4) thin film grown on the surface of the metal substrate to the target substrate by dry transfer, wet transfer or electrochemical bubbling transfer method; Alternatively, it can be used directly on a metal substrate.
10. A transition metal silicon nitride (MSi2N4) thin film prepared by the method according to any one of claims 1 to 9.