Coated steel
By using a one-stage plating method to configure a lower alloy layer, an intermediate alloy layer, and an upper plating layer with specific compositions on the surface of steel, the problems of easy plating disappearance and uneven alloy layer are solved, achieving high corrosion resistance and stability while reducing costs.
Patent Information
- Application Number
- CN202480091071.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2026-11-17
AI Technical Summary
The existing coated steel coating is prone to disappearing during welding, resulting in insufficient corrosion resistance. Furthermore, the two-stage coating method is costly, the uneven alloy layer structure affects corrosion resistance, and the concentration of Cr is difficult to control.
A single-stage plating method is adopted, in which a lower alloy layer, an intermediate alloy layer and an upper plating layer are sequentially applied to the surface of the steel. The thickness of the lower alloy layer is more than 5 μm, the thickness of the intermediate alloy layer is more than 1.0 μm, and the total thickness is more than 6 μm. The alloy layer composition is specific, and the composition of the upper plating layer meets a specific ratio. The reactivity of the plating layer is improved by controlling the Ni content in the plating bath.
It improves the corrosion resistance of coated steel, especially its stability in harsh corrosive environments, reduces costs, avoids uneven alloy layer problems, and ensures the corrosion protection effect of the coating.
Smart Images

Figure CN123125360A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to coated steel. Background Technology
[0002] In the civil engineering / infrastructure field, steel structures are used. Especially in harsh corrosive environments such as coastal areas and areas where de-icing salt is applied, stainless steel is used as the raw material for steel structures to maintain long-term corrosion resistance.
[0003] On the other hand, stainless steel contains expensive alloying elements such as Cr and Ni, making the construction of steel structures using stainless steel a costly issue. Therefore, recently, cheaper coated steel sheets (e.g., Zn-Al-Mg coated steel) have been used as raw materials for steel structures.
[0004] However, when manufacturing large or tubular steel structures using galvanized steel sheets as raw materials, the galvanized steel sheets need to be cut into specified shapes and joined together by welding or other methods to manufacture the steel structure. However, the galvanization at the welded portion sometimes disappears during welding, resulting in insufficient corrosion resistance in the finished steel structure. Furthermore, sometimes the cut ends of the galvanized steel sheets remain within the steel structure, and corrosion may occur originating from these cut ends. Therefore, to ensure the corrosion resistance of the steel structure, a post-plating treatment (dipping coating) is performed after manufacturing the steel structure using steel sheets, pipes, or structural steel as raw materials.
[0005] As such a post-plating treatment, molten Zn plating has been widely used, but in order to improve corrosion resistance, Zn-Al-Mg plating is also used.
[0006] On the other hand, in post-plating treatments other than molten Zn plating (such as Zn-Al-Mg plating), plating components such as Al and Mg sometimes hinder the reactivity of the plating bath and the flux, resulting in poor adhesion of the coating. Therefore, as shown in Patent Document 1 (Japanese Patent Application Publication No. 2010-70810) or Patent Document 2 (Japanese Patent Application Publication No. 2002-47548), a two-stage plating method is adopted, in which the steel is plated by immersing it in a Zn-Al-Mg plating bath as the second stage of plating treatment, based on the molten Zn plating treatment of the steel.
[0007] However, a drawback of the two-stage plating method is that the coating formed in the first stage participates in the coating formation reaction during the second stage. Consequently, the microstructure of the alloy layer adjacent to the steel in the coating is not a homogeneous structure composed of Al-Fe alloys, but rather a mixed-phase structure consisting of island-like or mesh-like Al-Fe alloys and Zn-Al-Mg alloys. Therefore, the barrier effect provided by the homogeneous Al-Fe alloy microstructure is reduced, and sometimes the overall corrosion resistance of the coating is decreased.
[0008] In addition, the two-stage plating method is sometimes more expensive than the one-stage plating method because it requires immersing the steel in two different plating baths twice.
[0009] Several methods for performing Zn-Al-Mg plating in a single step have also been disclosed. For example, in Patent Document 3 (Japanese Patent Application Publication No. 2017-66524), it is specified that the growth of the alloy layer is controlled by adding Cr. However, Cr is difficult to add to the plating bath, and sometimes it is difficult to manage the concentration.
[0010] Existing technical documents Patent documents Patent Document 1: Japanese Patent Application Publication No. 2010-70810 Patent Document 2: Japanese Patent Application Publication No. 2002-47548 Patent Document 3: Japanese Patent Application Publication No. 2017-66524 Summary of the Invention
[0011] The problem that the invention aims to solve
[0012] The present invention was made in view of the above circumstances, and its objective is to provide coated steel with superior corrosion resistance compared to the past.
[0013] means for solving problems
[0014] To address the aforementioned issues, the present invention employs the following configuration.
[0015] [1] A plated steel material comprising steel and a metal coating disposed on the surface of said steel, The metal coating is provided sequentially from the steel side as follows: a lower alloy layer containing more than 22.5% Fe, an intermediate alloy layer containing more than 20.0% Fe and 0.5 to 10.0% Ni, and an upper coating formed of a Zn-based alloy containing 0 to 5.0% Fe. The thickness of the lower alloy layer is 5 μm or more, the thickness of the intermediate alloy layer is 1.0 μm or more, and the combined thickness of the lower alloy layer and the intermediate alloy layer is 6 μm or more. The chemical composition of the lower alloy layer, expressed in % by mass, includes Zn: 5.0~30.0%, Al: 30.0~55.0% Fe: 22.5~50.0%, Si: 0~10.0% Ni: 0~less than 0.5% Mg: 0~1.0%, Balance: Impurities The chemical composition of the intermediate alloy layer, expressed as a percentage by mass, includes Zn: 5.0~35.0%, Al: 25.0~60.0% Fe: 20.0~45.0%, Si: 0~10.0% Ni: 0.5~10.0% Mg: 0~1.0%, The total of one or more elements selected from Ca, Sn, Bi, In, Y, La, Ce, Sr, B, P, Cr, Ti, Co, V, Nb, Cu, Mn, Mo, W, Zr, Ag, Li, Na, K, and Ba: 0~2.0%. Balance: impurities.
[0016] [2] According to the plated steel described in [1], wherein, The chemical composition of the upper coating, expressed as a percentage by mass, includes: Al: 6.0%~25.0% Mg: ≥3.0%~12.5%, Ni: 0.001% to less than 0.5% Si: 0%~1.5% Ca: 0%~3.0% Sn: 0%~3.0% Bi: 0%~1.0% In: 0%~1.0%, Y: 0%~0.5% La: 0%~0.5% Ce: 0%~0.5% Sr: 0%~0.5% B: 0%~1.0% P: 0%~0.5% Cr: 0%~0.25% Ti: 0%~0.25% Co: 0%~0.25%, V: 0%~0.25% Nb: 0%~0.25%, Cu: 0%~1.0% Mn: 0%~0.25%, Mo: 0%~0.25%, W: 0%~0.25% Zr: 0%~0.25% Ag: 0%~1.0% Li: 0%~0.5% Na: 0%~0.05% K: 0%~0.05% Ba: 0%~0.25% Fe: 0%~5.0%, Balance: More than 50% Zn and impurities.
[0017] [3] According to [2], the plated steel, wherein the upper coating satisfies the following formula (1) and the following formula (2). Mg / Al≤0.5…(1) 2×Ca+Sr+Y+La+Ce≥0.05…(2) In equations (1) and (2), Mg, Al, Ca, Sr, Y, La, and Ce represent the contents (mass%) of the upper coating, respectively. If the element is not present, substitute 0.
[0018] Invention Effects
[0019] According to the present invention, Zn-Al-Mg based coated steel with superior corrosion resistance compared to previous methods can be provided. Thus, even in harsh corrosive environments, inexpensive steel structures exhibiting stable corrosion resistance can be achieved. Attached Figure Description
[0020] Figure 1A It is a diagram illustrating the method for measuring the total thickness of the intermediate alloy layer and the lower alloy layer, and it is an SEM photograph showing the cross-section of the metal coating.
[0021] Figure 1B It is a diagram illustrating the method for measuring the total thickness of the intermediate alloy layer and the lower alloy layer, and a schematic diagram showing the cross-section of the metal coating.
[0022] Figure 1C It is a diagram illustrating the method for measuring the total thickness of the intermediate alloy layer and the lower alloy layer, and a schematic diagram showing the cross-section of the metal coating.
[0023] Figure 1DIt is a diagram illustrating the method for measuring the total thickness of the intermediate alloy layer and the lower alloy layer, and a schematic diagram showing the cross-section of the metal coating.
[0024] Figure 1E It is a diagram illustrating the method for measuring the total thickness of the intermediate alloy layer and the lower alloy layer, and a schematic diagram showing the cross-section of the metal coating.
[0025] Figure 1F It is a diagram illustrating the method for measuring the total thickness of the intermediate alloy layer and the lower alloy layer, and a schematic diagram showing the cross-section of the metal coating.
[0026] Figure 1G It is a diagram illustrating the method for measuring the total thickness of the intermediate alloy layer and the lower alloy layer, and a schematic diagram showing the cross-section of the metal coating.
[0027] Figure 1H It is a diagram illustrating the method for measuring the total thickness of the intermediate alloy layer and the lower alloy layer, and a schematic diagram showing the cross-section of the metal coating.
[0028] Figure 2 This is a cross-sectional SEM image of the metal coating in Example No. 12.
[0029] Figure 3 This is the elemental mapping analysis result of Fe contained in the metal coating of Example No. 12.
[0030] Figure 4 This is the elemental mapping analysis result of Ni contained in the metal coating of Example No. 12.
[0031] Figure 5 This is the elemental mapping analysis result of Zn contained in the metal coating of Example No. 12.
[0032] Figure 6 This is the elemental mapping analysis result of Al contained in the metal coating of Example No. 12.
[0033] Figure 7 This is the elemental mapping analysis result of Mg contained in the metal coating of Example No. 12. Detailed Implementation
[0034] Typically, when forming Zn-based coatings using melt plating, a flux is used to treat the steel surface to improve the reactivity of the steel with the plating bath. A typical flux treatment involves applying an aqueous solution containing zinc chloride and ammonium chloride to the steel surface, allowing the flux film to adhere. Then, the flux-treated steel is immersed in a melt plating bath to obtain a melt coating. However, when using a flux containing ammonium chloride (NH4Cl) to form Zn-Al-Mg-based coatings, the Mg in the plating bath reacts with the Cl (chlorine) in the flux to form halides such as magnesium chloride and aluminum chloride. These halides adhere firmly to the steel surface as flux residues, sometimes resulting in incomplete coating. Furthermore, the corrosion resistance of the coating can sometimes be reduced due to the presence of halogen compounds and other flux residues. Therefore, in the past, in order to avoid non-coating and stably manufacture Zn-Al-Mg coatings with excellent corrosion resistance, a molten zinc coating was first formed on the surface of the steel, and then a Zn-Al-Mg coating was formed by a molten plating method, thus manufacturing coated steel through the so-called two-stage plating method.
[0035] In order to reduce the burden of manufacturing coated steel, the inventors studied the manufacture of Zn-Al-Mg coated steel with excellent corrosion resistance by a one-stage coating method. The results showed that by including a small amount of Ni in the molten plating bath, the occurrence of non-coating could be suppressed, and the corrosion resistance of the coating was significantly improved compared with the past.
[0036] The coated steel material according to embodiments of the present invention will be described below.
[0037] The plated steel of this embodiment is characterized by comprising steel and a metal coating disposed on the surface of the steel. The metal coating, arranged sequentially from the steel side, includes a lower alloy layer containing 22.5% or more Fe, an intermediate alloy layer containing 20.0% or more Fe and 0.5 to 10.0% Ni, and an upper coating layer formed of a Zn-based alloy containing 0 to 5.0% Fe. The thickness of the lower alloy layer is 5 μm or more, the thickness of the intermediate alloy layer is 1.0 μm or more, and the total thickness of the lower alloy layer and the intermediate alloy layer is 6 μm or more. The chemical composition of the lower alloy layer, by mass%, includes Zn: 5.0 to 30.0%, Al: 30.0 to 55.0%, and Fe: 22.5 to 5%. 0.0%, Si: 0~10.0%, Ni: 0~less than 0.5%, Mg: 0~1.0%, balance: less than 1% of impurities. The chemical composition of the intermediate alloy layer, by mass%, includes Zn: 5.0~35.0%, Al: 25.0~60.0%, Fe: 20.0~45.0%, Si: 0~10.0%, Ni: 0.5~10.0%, Mg: 0~1.0%, and the total of one or more elements from Ca, Sn, Bi, In, Y, La, Ce, Sr, B, P, Cr, Ti, Co, V, Nb, Cu, Mn, Mo, W, Zr, Ag, Li, Na, K and Ba: 0~2.0%, balance: impurities.
[0038] Furthermore, in this embodiment, the preferred chemical composition of the upper coating of the plated steel is, by mass%, Al: 6.0%~25.0%, Mg: more than 3.0%~12.5%, Ni: 0.001%~less than 0.5%, Si: 0%~1.5%, Ca: 0%~3.0%, Sn: 0%~3.0%, Bi: 0%~1.0%, In: 0%~1.0%, Y: 0%~0.5%, La: 0%~0.5%, Ce: 0%~0.5%, Sr: 0%~0.5%, B: 0%~1.0%, P: 0%~0.5%, C r: 0%~0.25%, Ti: 0%~0.25%, Co: 0%~0.25%, V: 0%~0.25%, Nb: 0%~0.25%, Cu: 0%~1.0%, Mn: 0%~0.25%, Mo: 0%~0.25%, W: 0%~0.25%, Zr: 0%~0.25%, Ag: 0%~1.0%, Li: 0%~0.5%, Na: 0%~0.05%, K: 0%~0.05%, Ba: 0%~0.25%, Fe: 0%~5.0%, Balance: more than 50% Zn and impurities.
[0039] In addition, in the plated steel of this embodiment, the upper coating preferably satisfies the following formula (1) and the following formula (2). Mg / Al≤0.5…(1) 2×Ca+Sr+Y+La+Ce≥0.05…(2) In equations (1) and (2), Mg, Al, Ca, Sr, Y, La, and Ce represent the contents (mass%) of the upper coating layer, respectively. If the element is not present, substitute 0.
[0040] The plated steel of this embodiment includes steel and a metal coating formed on the surface of the steel. In the metal coating, a lower alloy layer, an intermediate alloy layer, and an upper plating layer are sequentially arranged from the steel side toward the surface side of the plated steel. Alternatively, a chemical conversion treatment layer may be formed on the upper plating layer of the metal coating.
[0041] In this embodiment, the surface of the plated steel is coated with a lower alloy layer mainly composed of an Al-Fe alloy. An intermediate alloy layer containing Al, Fe, and Ni is formed on the lower alloy layer. Furthermore, an upper coating with excellent sacrificial corrosion resistance is formed on the intermediate alloy layer. This improves the corrosion resistance of the plated steel. More specifically, the intermediate alloy layer containing Al, Fe, and Ni suppresses the formation of red rust. Additionally, the presence of the intermediate alloy layer prevents corrosion reactions from locally propagating towards the depth of the metal coating, thus inhibiting early corrosion of the steel. Furthermore, an upper coating mainly composed of Zn is formed on the intermediate alloy layer, which exhibits excellent sacrificial corrosion resistance. Moreover, the upper coating has excellent chemical conversion treatment properties, thus allowing for further improvement of the steel's durability through chemical conversion treatment.
[0042] The shape of the steel used to form the coated steel in this embodiment is not particularly limited, and various shapes of steel can be used, such as wire, plate, mesh, tube, rod, and other three-dimensional shapes. For example, small substrates such as bolts, nuts, and power transmission metal fittings can be used, as well as large substrates such as high railings, pillars, bridge guardrails, road signs, road fencing, river railings, rockfall prevention nets, and steel pipes.
[0043] There are no particular restrictions on the type of steel used. For example, various types of steel can be used, including general steel, Ni-plated steel, Al-killed steel, very low carbon steel, high carbon steel, various high-tensile steels, and some high-alloy steels (steels containing strengthening elements such as Ni and Cr). Furthermore, there are no particular restrictions on the manufacturing methods of the steel and the manufacturing methods of the steel plates (hot rolling, pickling, cold rolling, etc.). Moreover, steel with a metallic or alloy film of less than 1 μm formed on Zn, Ni, Sn, Bi, or their alloys can also be used.
[0044] Next, the lower alloy layer, the intermediate alloy layer and the upper plating layer that constitute the metal coating will be described in detail.
[0045] In the following explanation, the percentage (%) for the content of each element in the chemical composition refers to "mass %". Additionally, the numerical range indicated by "~" refers to the range including the values before and after "~" as lower and upper limits. It should be noted that when values before and after "~" are marked "more than" or "less than", the numerical range excludes these values as lower or upper limits.
[0046] "Corrosion resistance" refers to the property of a metal coating itself being difficult to corrode. Zn-based coatings have a sacrificial corrosion protection effect on steel. Therefore, the corrosion process of coated steel is as follows: before the steel corrodes, the upper coating corrodes and turns into white rust. After the white rust on the upper coating disappears, corrosion proceeds in the order of the middle alloy layer and the lower alloy layer, eventually causing the steel to corrode and produce red rust.
[0047] The top coating is a Zn-based alloy layer formed on the surface of the coated steel. The top coating is formed by solidifying the plating bath composition on the surface of the steel, and except for a few elements, it represents a composition concentration approximately the same as that of the plating bath.
[0048] The lower alloy layer is formed on the surface of the steel and contains an Al-Fe alloy that is connected to the surface of the steel as the main body.
[0049] In addition, an intermediate alloy layer is formed between the lower alloy layer and the upper plating layer. The intermediate alloy layer contains an Al-Fe-Ni alloy as the main component.
[0050] In the following description, the lower alloy layer and the intermediate alloy layer are sometimes referred to together as the alloy layer.
[0051] The Zn-based alloy constituting the upper coating can also be a Zn-Al-Mg alloy, consisting of Zn with alloying elements such as Al and Mg. Coatings formed from Zn-Al-Mg alloys exhibit improved corrosion resistance compared to ordinary Zn coatings. For example, even a coating formed from a Zn-Al-Mg alloy, with a thickness approximately half that of a Zn coating, possesses the same corrosion resistance. Therefore, the upper coating is preferably formed from a Zn-Al-Mg alloy. Zn-Al-Mg alloys mainly consist of a ternary eutectic structure of Zn phase, Al phase, Mg2Zn phase, and [Zn / Al / MgZn2].
[0052] When the upper coating is composed of a Zn-Al-Mg alloy, the preferred composition concentration range is as follows.
[0053] It should be noted that when describing the concentration range of the upper coating, the plating bath used to manufacture the metal coating is described. The composition of the upper coating is almost identical to that of the plating bath, except for a few elements. The elements that differ in the composition of the upper coating from those in the plating bath include Al and Ni. The upper coating contains less Al and Ni than the plating bath. This is because, during the period from when the steel is lifted from the plating bath until the plating bath adheres to the steel and solidifies, Al and Ni transfer from the plating bath to the alloy layers (intermediate alloy layer and lower alloy layer). Besides the main elements such as Al, Mg, and Zn, elements such as Si, Cr, Mn, and Mo also tend to transfer to the alloy layer; similarly, these elements, like Al and Ni, are present in lower amounts in the upper coating compared to the plating bath composition.
[0054] Al: 6.0%~25.0% When the coating is a Zn-Al-Mg alloy, Al exists as an Al phase or a ternary eutectic structure such as [Zn / Al / MgZn2]. Al has a small sacrificial corrosion protection effect, but its presence in the coating improves corrosion resistance. Furthermore, without Al in the plating bath, Mg cannot be stably maintained; therefore, Al is added to the plating bath. A preferred Al content of 6.0% or more in the upper coating is necessary to ensure a certain level of corrosion resistance; below this content, it is difficult to ensure the corrosion resistance of the upper coating. Additionally, by maintaining an Al concentration of 6.0% or more in the upper coating, alloy layer growth becomes more active, and the thickness of the alloy layer can be stably ensured. On the other hand, if the Al content is excessive, the lower alloy layer overgrows during manufacturing, making growth control difficult and easily leading to defects such as coating burn-out at the coating surface. Therefore, the Al content in the upper coating is 25.0% or less.
[0055] Mg: ≥3.0%~12.5% Mg has a sacrificial corrosion protection effect and is an element that improves the corrosion resistance of the upper coating. By containing a certain level or more of Mg, a MgZn2 phase is formed in the upper coating. The higher the Mg content in the upper coating, the more MgZn2 phase is formed. A Mg content exceeding 3.0% is the concentration required to achieve corrosion resistance; when the Mg content is below 3.0%, sufficient corrosion resistance is not obtained. On the other hand, excessive Mg content makes the manufacture of the upper coating difficult, therefore its upper limit is 12.5% or less. A more preferred Mg content is more than 5.0% and less than 12.5%, which can be more than 5.0% and less than 10.0%, or more than 5.0% and less than 8.0%.
[0056] Ni: 0.001% to less than 0.5% Ni is included in the metal coating to form an Al-Fe-Ni alloy, but Ni tends to accumulate in the intermediate alloy layer during plating solidification. Therefore, the Ni concentration in the upper coating is 0.001% to less than 0.5%. Thus, the Ni concentration in the upper coating is low, and therefore, an Al-Fe-Ni alloy is not present in the upper coating, or if it is, it is present in trace amounts.
[0057] Si: 0%~1.5% Si is a semi-metallic element. In the upper coating, Si causes the precipitation of single-phase Si or Mg₂Si. Furthermore, when Ca is present in the coating along with Si, Al-Ca-Si compounds precipitate. This improves the corrosion resistance of the upper coating. There is an upper limit to the Si content; exceeding this limit leads to increased adhesion of scum and other contaminants, and a general deterioration in corrosion resistance. Additionally, excessive Si in the plating bath significantly inhibits the formation of the alloy layer described later; therefore, the Si concentration in the upper coating is within an appropriate range. Thus, Si is preferably 0% or more and 1.5% or less, and more than 0% but less than 1.0%.
[0058] Sn: 0%~3.0% Bi: 0%~1.0% In: 0%~1.0% Sn, Bi, and In enhance the sacrificial corrosion resistance of the upper coating. That is, they inhibit the formation of red rust on the steel during localized corrosion. However, there are upper limits to the content of these elements. Exceeding these limits leads to increased adhesion of slag and other contaminants, making the cost disproportionate to the performance improvement. Therefore, Sn is set to 0-3.0%, more preferably more than 0% to less than 3.0%. Bi is set to 0%-1.0%, more preferably more than 0% to less than 1.0%. In is set to 0%-1.0%, more preferably more than 0% and less than 1.0%.
[0059] Ca: 0%~3.0% Y: 0%~0.5% La: 0%~0.5% Ce: 0%~0.5% Sr: 0%~0.5% Ca, Y, La, Ce, and Sr are easily oxidized in the atmosphere. When these elements are present in the plating bath, they form a dense oxide film on the bath surface, which prevents the oxidation of Mg. This effect stabilizes the Mg concentration, making it easier to manufacture the upper coating with the target composition. To achieve this effect appropriately, the content of these elements is set to more than 0%, more preferably more than 0.01%. However, there is an upper limit to the content of each element; exceeding this limit tends to make bath preparation difficult. Furthermore, there is a tendency for increased adhesion of scum and other contaminants, and a deterioration in weldability. Therefore, Ca is set to 0% to 3.0%. Y, La, Ce, and Sr are each set to 0% to 0.5%, preferably more than 0 and less than 0.5%, more preferably more than 0.01% and less than 0.5%.
[0060] B: 0%~1.0% P: 0%~0.5% Boron (B) and phosphorus (P) are semi-metallic elements that improve the corrosion resistance of the upper coating. These elements generally also affect corrosion resistance, but there are upper limits to their content. Exceeding these limits tends to increase the adhesion of scum and other contaminants, and worsen corrosion resistance. Therefore, the concentrations of B and P are 0%~1.0% and 0%~0.5%, respectively.
[0061] Cr: 0%~0.25% Ti: 0%~0.25% Co: 0%~0.25% V: 0%~0.25% Nb: 0%~0.25% Cu: 0%~1.0% Mn: 0%~0.25% Mo: 0%~0.25% W: 0%~0.25% Zr: 0%~0.25% Ag: 0%~1.0% Li: 0%~0.5% Na: 0%~0.05% K: 0%~0.05% Cr, Ti, Co, V, Nb, Cu, Mn, Mo, W, Zr, Ag, Li, Na, and K are metallic elements introduced into the upper coating to create a substitution solid solution and a new high-melting-point intermetallic compound. This improves corrosion resistance. There are upper limits to the content of each element; exceeding these limits tends to increase the adhesion of scum and other contaminants. Therefore, Na and K are each set to 0%~0.05%, preferably more than 0% and less than 0.05%. Cr, Ti, Co, V, Nb, Mn, Mo, W, and Zr are each set to 0%~0.25%, preferably more than 0% and less than 0.25%. Li is set to 0%~0.5% or less, preferably more than 0% and less than 0.5%. Cu and Ag are each set to 0%~1.0%, preferably more than 0% and less than 1.0%.
[0062] Ba: 0%~0.25% Ba is an element with properties similar to Zn. Therefore, the presence of Ba does not produce any particularly significant effect, but it can easily create zinc flower patterns and other effects on the appearance of the plating. However, if it is present in excess, the corrosion resistance of the upper plating layer may decrease. Therefore, Ba is set at 0% to 0.25%, preferably more than 0% and less than 0.25%.
[0063] Fe: 0%~5.0% Fe is inevitably present in the upper coating. This is because it sometimes diffuses from the iron base into the upper coating during the plating process. It has been confirmed that if the Fe content is below 5.0%, it will not affect the corrosion resistance of the upper coating. Therefore, the Fe content can be between 0% and 5.0%, exceeding 0% but less than 5.0%.
[0064] Balance: Zn and impurities When Zn is a low-melting-point metal and the upper coating is a Zn-Al-Mg alloy, it forms a ternary eutectic structure of Zn phase, Mg2Zn phase, or [Zn / Al / MgZn2], and further becomes Mg2Zn. 11 The Zn content is equal to that of the steel. Zn is an element necessary to ensure the corrosion resistance of the upper coating and to provide sacrificial corrosion protection to the steel. Preferably, Zn contains 50.00% or more, more preferably over 50.00%. When Zn content is less than 50.00% or below, the sacrificial corrosion protection of the coating decreases. That is, it becomes difficult to suppress the formation of red rust from the steel during localized corrosion. The Zn content is more preferably set at 65.00% or more or 70.00% or more. It should be noted that the upper limit of the Zn content is the amount remaining after considering elements and impurities other than Zn.
[0065] Impurities in the upper coating refer to components contained in the raw materials or components mixed in during the manufacturing process. For example, in the coating, due to the mutual atomic diffusion between the steel (iron-based) and the plating bath, components other than Fe are sometimes mixed in in trace amounts as impurities.
[0066] In addition, in the plated steel of this embodiment, the upper coating preferably satisfies the following formula (1) and the following formula (2). Mg / Al≤0.5…(1) 2×Ca+Sr+Y+La+Ce≥0.05…(2) In equations (1) and (2), Mg, Al, Ca, Sr, Y, La, and Ce represent the contents (mass%) of the upper coating layer. If the upper coating layer does not contain these elements, substitute 0.
[0067] Mg has the effect of inhibiting the alloying reaction of Al-Fe, but by satisfying equation (1), the thickness of the upper coating can be ensured.
[0068] In addition, Ca, Sr, Y, La, and Ce are easily oxidized in the atmosphere. When present in the plating bath, they form a dense oxide film on the bath surface, which has the effect of preventing the oxidation of Mg. By ensuring that the content of these elements satisfies Equation (2), the Mg concentration in the upper coating is stabilized, and the upper coating with the target composition can be formed.
[0069] The average chemical composition of the upper coating can be determined by ICP-MS or ICP-luminescence spectrophotometry. Specifically, a solution is obtained by peeling and dissolving the upper coating with an acid containing an inhibitor that suppresses corrosion of the alloy layers (intermediate alloy layer, lower alloy layer) or an alkaline solution. More specifically, in the case of acid peeling and dissolution, an acid solution of Ibit No. 700AS containing 0.01% by mass of a commercially available inhibitor in a 10% by mass hydrochloric acid aqueous solution can be used. For alkaline peeling, a 5% by mass NaOH aqueous solution can be used. Then, if the resulting solution is acidic, it is determined by emission spectrophotometry or ICP-MS; if it is alkaline, it is determined by emission spectrophotometry or ICP-MS after acid treatment.
[0070] The thickness of the upper coating can be determined by subtracting the thickness of the alloy layer (described later) from the thickness of the metal coating. The thickness of the metal coating is derived by observing the cross-sectional microstructure. Specifically, a section perpendicular to the surface of the plated steel is exposed. The exposed section is mirror-finished. In the SEM reflectance electron image of the cross-section of the metal coating appearing in the section, the distance in the thickness direction between the outermost surface of the metal coating (the surface of the plated steel) and the surface of the steel is measured at 10 locations, and the average value is calculated as the thickness of the metal coating. The distance between the measurement locations is preferably about 100 μm. Furthermore, the thickness of the upper coating can be derived by subtracting the thickness of the alloy layer (described later) from the thickness of the metal coating.
[0071] Ideally, the upper coating should contain as few quasi-crystalline phases as possible. When steel is immersed in a Mg-containing bath (containing 8% or more Mg) and cooled immediately after being pulled up, a high cooling rate can sometimes lead to the appearance of Mg in the coating microstructure. 32 (Zn, Al) 49 The quasicrystalline phase is composed of a brittle structure. Therefore, when the upper coating of this embodiment contains a quasicrystalline phase, cracking occurs in the upper coating, which can sometimes negatively impact corrosion resistance. Therefore, from the viewpoint of further improving corrosion resistance, the area ratio of the quasicrystalline phase in the upper coating is preferably 0.5% or less. The area ratio of the quasicrystalline phase can be 0%.
[0072] The area ratio of the quasicrystalline phase can be determined by observing the cross-sectional microstructure. First, a section perpendicular to the surface of the coated steel is exposed. The exposed section is mirror-finished. Within the exposed section, a specific measurement area of the upper coating is defined. When the thickness of the upper coating is 20 μm, the longitudinal extent of the measurement area extends from the surface of the coated steel to a depth of 16 μm. Furthermore, the transverse extent of the measurement area of the upper coating is set to 40 μm, parallel to the surface of the coated steel. Five measurement areas are defined.
[0073] Next, elemental mapping of Mg was performed on the measurement areas of the upper coating using an electron probe microanalysis (EPMA). As a result, areas with a Mg concentration of 19% by mass or higher were identified as pure crystalline phases, and the area ratio of quasicrystalline phases was calculated for the five measurement areas. Then, the average area ratio of the quasicrystalline phases in the five measurement areas was taken as the quasicrystalline area ratio.
[0074] Regarding the measurement conditions of EPMA, the output power of the electron beam was set to 15kV and 50nA using an electron probe microanalyzer JXA-8230 manufactured by NEC Corporation, and the irradiation time was measured at 50 milliseconds.
[0075] It should be noted that a quasicrystalline phase is a phase containing quasicrystalline elements. Quasicrystalline elements, first discovered in 1982, are crystal structures with an icosahedron atomic arrangement. This crystal structure exhibits a unique rotational symmetry, for example, a non-periodic crystal structure with five-fold symmetry, unobtainable in ordinary metals and alloys. It is known to be equivalent to non-periodic structures represented by three-dimensional Penrose patterns. To identify this metallic substance, confirmation is made, for example, by electron beam diffraction observation based on TEM, obtaining an electron beam diffraction pattern of radially arranged regular decagons originating from the icosahedron structure.
[0076] The quasicrystalline phase that may form based on the composition of the plating bath in this embodiment is simply represented by X-ray diffraction as Mg. 32 (Zn, Al) 49 The diffraction peaks can be identified as those on JCPDS card: PDF#00-019-0029 or #00-039-0951. Most diffraction peaks are observed around 36.3 to 8°. However, in this embodiment, the region with a Mg concentration of 19% by mass or higher can also be designated as a pure crystalline phase.
[0077] Next, the alloy layers (lower alloy layer and intermediate alloy layer) will be explained.
[0078] The thickness and morphology of the alloy layer vary depending on the steel grade and the manufacturing conditions of the metal coating, but it is generally formed as a layer mainly composed of Al-Fe alloys or Al-Fe alloys containing substitutional elements or solid solution elements such as Ni and Si. The morphology of the alloy layer can be broadly classified into two types. Specifically, they are as follows: when observing the cross-sectional microstructure, the Al-Fe alloy forms a homogeneous structure as a homogeneous layer; and the Al-Fe alloy forms an island-like or mesh-like structure, forming a mixed-phase microstructure similar to that of a Zn-based alloy where the plating bath essentially solidifies directly between the alloy layers.
[0079] The microstructure of the alloy layer formed by the one-stage plating method described in this embodiment differs from that formed by the two-stage plating method, sometimes allowing identification of the manufacturing method. This is due to the formation behavior of the alloy layer. In the one-stage plating method, the alloy layer formed by the reaction of steel with the plating bath containing Al is a homogeneous layer containing an Al-Fe alloy. On the other hand, in the two-stage plating method, when the material to be plated, on which an Fe-Zn alloy layer has already been formed, is immersed in a plating bath containing Al, the Fe-Zn alloy layer changes into an Al-Fe alloy layer. The change from Fe-Zn alloy to Al-Fe alloy is accompanied by volume shrinkage, thus forming an island-like or mesh-like Al-Fe alloy.
[0080] The morphological differences in Al-Fe alloys manifest as differences in the average composition of the alloy layers. Specifically, when determining the composition of the alloy layers through EPMA-based elemental mapping analysis of cross-sectional microstructures, in the case of a homogeneous microstructure, the composition closely approximates the analytical values of the Al-Fe alloy composition analyzed by point analysis. On the other hand, when performing surface analysis on a miscible microstructure, due to the presence of Zn-based alloys, a higher Zn concentration and a lower Fe concentration are observed compared to a homogeneous microstructure.
[0081] The lower alloy layer will be described below.
[0082] The lower alloy layer is formed on the surface of the steel. Therefore, the region containing Al-Fe alloy on the surface of the steel can be used as the lower alloy layer.
[0083] The thickness and morphology of the lower alloy layer containing Al-Fe alloys vary depending on the steel grade and the manufacturing conditions of the metal coating. However, when manufactured by a one-stage plating method as in this embodiment, the lower alloy layer is formed as a homogeneous layer containing Al-Fe alloys.
[0084] The lower alloy layer is formed on the surface of the steel, and its microstructure contains the Al5Fe2 phase as the main phase. The lower alloy layer can also be composed primarily of an Al-Fe alloy, occupying the largest area or volume proportion. This Al-Fe alloy is formed through atomic diffusion between the iron matrix (steel) and the plating bath. However, when using a melt plating method, immersing the steel in an Al-containing plating bath easily forms an Al-Fe alloy, but when the plating bath contains a certain concentration of Al or higher, the Al5Fe2 phase forms the most. However, atomic diffusion takes time, and there are also regions with higher Fe concentrations near the iron matrix. Therefore, the Al-Fe alloy contained in the lower alloy layer sometimes also partially contains AlFe, Al3Fe, and Al5Fe phases. Furthermore, since the plating bath contains a certain concentration of Zn, some of the Zn in the Al-Fe alloy constituting the lower alloy layer is dissolved or partially replaced by Zn. Therefore, the lower alloy layer also contains Zn.
[0085] Furthermore, when the metal coating contains Si, Si readily enters the Al-Fe alloy forming the underlying alloy layer, sometimes forming an Al-Fe-Si intermetallic compound phase within the lower alloy layer. Specific intermetallic compound phases include the AlFeSi phase, and as isomers, α, β, q1, and q2-AlFeSi phases exist. Therefore, these AlFeSi phases are sometimes detected in Al-Fe alloys.
[0086] The lower alloy layer has a chemical composition comprising Zn: 5.0~30.0%, Al: 30.0~55.0%, Fe: 22.5~50.0%, Si: 0~10.0%, Ni: 0~less than 0.5%, Mg: 0~1.0%, and the balance being impurities.
[0087] Zn is contained in the lower alloy layer of Al-Fe alloys. Zn-free Al-Fe alloys form red rust upon corrosion, but Zn-containing Al-Fe alloys do not form red rust, instead forming yellow or black rust. To prevent red rust formation, the lower alloy layer needs to contain at least 5.0% Zn. However, the upper limit for Zn concentration in Al-Fe alloys is around 30.0%, and it is difficult to increase it further when the Al-Fe alloy has a homogeneous structure. Therefore, the Zn content in the lower alloy layer can be below 30.0%. Thus, the Zn content in the lower alloy layer ranges from 5.0% to 30.0%.
[0088] Al in the lower alloy layer is the main element constituting the Al-Fe alloy. The lower and upper limits of the Al concentration are determined by the phase composition of the formed Al-Fe alloy, but in this embodiment, the lower alloy layer may contain Al in a proportion of 30.0% to 55.0%.
[0089] Fe in the lower alloy layer is the main element constituting the Al-Fe alloy. The lower and upper limits of the Fe concentration are determined by the phase composition of the formed Al-Fe alloy, but in this embodiment, Fe is included in the lower alloy layer in a proportion of 22.5% to 50.0%.
[0090] Si, when included in the plating bath, has the effect of inhibiting the alloying reaction between Al and Fe. Therefore, it can also be added to the plating bath to control the alloying of Al and Fe. However, when the Si concentration in the plating bath exceeds approximately 1.5%, the lower alloy layer hardly grows at bath temperatures below 540°C, failing to ensure the barrier properties based on the Al-Fe alloy, thus reducing corrosion resistance. Furthermore, Si tends to accumulate in Al-Fe or Al-Fe-Ni alloys, and the Si concentration in the lower alloy layer is sometimes higher than that in the upper plating layer. Nevertheless, if the Si concentration in the plating bath is below 1.5%, the Si in the lower alloy layer will not exceed 10.0%. Therefore, the upper limit for Si in the lower alloy layer is set to below 10.0%. It should be noted that if the plating bath does not contain Si, the Si in the lower alloy layer is 0%. Therefore, the Si content in the lower alloy layer is set to 0~10.0%.
[0091] It should be noted that when using a two-stage plating method with a Si-containing plating bath to produce coated steel, a mixed-phase structure is sometimes obtained, consisting of Al-Fe alloy and Zn alloy that has almost directly solidified in the plating bath. However, in such a mixed-phase structure, corrosion occurs along the Zn alloy that has almost directly solidified in the plating bath, so the corrosion resistance of the Al-Fe alloy cannot be produced, and the corrosion resistance of the metal coating itself becomes lower.
[0092] Ni is included in the metal coating to form an Al-Fe-Ni alloy, but Ni tends to accumulate in the intermediate alloy layer during plating solidification. Therefore, the Ni concentration in the lower alloy layer is 0% to less than 0.5%. As a result, the Ni concentration in the lower alloy layer is low, and therefore, an Al-Fe-Ni alloy does not exist in the lower alloy layer, or if it does, it is present in trace amounts.
[0093] In addition, Mg is sometimes present in the lower alloy layer, but Mg has low solid solubility in Al-Fe alloys. Therefore, its content is less than 1.0% if the Al-Fe alloy does not form a miscible structure with the solidified structure from the plating bath. Thus, the Mg content is set to a range of 0 to 1.0%.
[0094] The remaining amount in the lower alloy layer is impurities. Like the upper plating layer, impurities in the lower alloy layer refer to components contained in the raw materials or those introduced during the manufacturing process. For example, in the lower alloy layer, due to the mutual atomic diffusion between the steel (iron-based) and the plating bath, trace amounts of components other than Fe may sometimes be introduced as impurities.
[0095] Additionally, the lower alloy layer may contain one or more of the elements included in Ca, Sn, Bi, In, Y, La, Ce, Sr, B, P, Cr, Ti, Co, V, Nb, Cu, Mn, Mo, W, Zr, Ag, Li, Na, K, and Ba, in a total range of 0 to 2.0%. These elements constitute the upper coating, but sometimes small amounts of them are mixed into the lower alloy layer.
[0096] The average chemical composition of the lower alloy layer can be determined by analyzing the cross-section of the lower alloy layer using an electron probe microanalysis (EPMA) system, and by quantitatively analyzing the elements contained in the region of the lower alloy layer. Details will be described later.
[0097] From a corrosion resistance perspective, the thickness of the lower alloy layer needs to be certain. To ensure sufficient corrosion resistance, a thickness of 5 μm or more is preferred, and 30 μm or more is also acceptable, with 50 μm or more being even more preferable. The method for measuring the thickness will be described later.
[0098] Next, the intermediate alloy layer will be described. The intermediate alloy layer is disposed between the lower alloy layer and the upper plating layer. That is, the intermediate alloy layer is formed on the side closer to the upper plating layer than the lower alloy layer. The intermediate alloy layer contains an Al-Fe-Ni alloy. The Al-Fe-Ni alloy is an Al-Fe alloy containing Ni. The Al-Fe-Ni alloy is formed by creating a metal coating layer using a plating bath with added Ni.
[0099] It should be noted that when producing coated steel using a two-stage plating method with a Ni-containing plating bath, a mixed-phase structure is sometimes obtained, consisting of an Al-Fe-Ni alloy and a Zn alloy that solidifies almost directly from the plating bath. However, in such a mixed-phase structure, corrosion proceeds along the Zn alloy, and thus the corrosion resistance of the Al-Fe-Ni alloy is sometimes not achieved. The corrosion resistance of the metal coating itself becomes lower, which is therefore not preferred.
[0100] The intermediate alloy layer may also consist entirely of an Al-Fe-Ni alloy. Alternatively, the intermediate alloy layer may contain structures other than Al-Fe-Ni alloys, but in this case, it is preferable that the structure composed of Al-Fe-Ni alloys constitutes the largest area or volume proportion.
[0101] The intermediate alloy layer shares the same composition of Al and Fe as the lower alloy layer, but the lower alloy layer can be distinguished by whether it contains more than 0.5% Ni. Specifically, this can be achieved by mapping the regions where Fe, Al, and Ni are present in the EPMA. Al-Fe-Ni alloys, due to their Ni content, exhibit higher corrosion resistance compared to Al-Fe alloys constituting the lower alloy layer. The intermediate alloy layer containing such an Al-Fe-Ni alloy is distributed approximately parallel to the steel surface and exists as a coating over the lower alloy layer, thus providing a high barrier effect. Furthermore, Al-Fe-Ni alloys have poor wettability with flux residues; therefore, during the formation of the Al-Fe-Ni alloy, flux residues rapidly detach from the steel surface and float to the plating bath. In other words, flux detachment is improved. This suppresses adverse conditions such as reduced corrosion resistance caused by uncoated areas or residual flux residues.
[0102] Al-Fe-Ni alloys consist of an Al3Fe phase or an Al5Fe2 phase containing Ni, but sometimes they also partially contain AlFe, Al3Fe, or Al5Fe phases. Furthermore, since the plating bath contains a certain concentration of Zn, Al-Fe-Ni alloys also contain Zn. Zn can exist in the form of substitution with Al, solid solution, or both. Moreover, when the metal coating contains Si, Al-Fe-Ni-Si intermetallic compound phases sometimes form. Among the intermetallic compound phases identified here is the AlFeSi phase, which exists as isomers such as α, β, q1, and q2-AlFeSi phases. Therefore, these AlFeSi phases are sometimes detected in Al-Fe-Ni alloys.
[0103] The Al-Fe-Ni alloy contained in the intermediate alloy layer is preferably composed of Zn: 5.0~30.0%, Al: 30~60%, Fe: 30~50%, Si: 0~10%, Ni: 0.5~10%, Mg: 0~1.0%, with the balance being impurities.
[0104] The intermediate alloy layer has a chemical composition comprising Zn: 5.0~35.0%, Al: 25.0~60.0%, Fe: 20.0~45.0%, Si: 0~10.0%, Ni: 0.5~10.0%, Mg: 0~1.0%, and balance: impurities.
[0105] Zn in the intermediate alloy layer is mainly found in Al-Fe-Ni alloys. Al-Fe-Ni alloys without Zn form red rust during corrosion, but those containing Zn do not, instead forming yellow or black rust. To suppress red rust formation, the intermediate alloy layer needs to contain at least 5.0% Zn.
[0106] On the other hand, the upper limit of the Zn concentration in Al-Fe-Ni alloys is about 30.0%. Therefore, when Al-Fe-Ni alloys have a homogeneous structure, the amount of solidified phase in the intermediate alloy layer is not that large, thus making the Zn content in the intermediate alloy layer below 35.0%.
[0107] Al in the intermediate alloy layer is the main element constituting the Al-Fe-Ni alloy, and the lower and upper limits of its Al concentration are determined by the phase composition of the formed Al-Fe alloy. In this embodiment, it is preferable that the intermediate alloy layer contains Al in a proportion of 25.0% to 60.0%.
[0108] Fe in the intermediate alloy layer is the main element constituting the Al-Fe-Ni alloy, and the lower and upper limits of its Fe concentration are determined by the phase composition of the formed Al-Fe-Ni alloy. In this embodiment, Fe can be contained in the intermediate alloy layer at a ratio of 20.0% to 45.0%.
[0109] Similar to Si in the lower Al-Fe alloy layer, Si in the intermediate alloy layer tends to be enriched in Al-Fe-Ni alloys. Therefore, the Si concentration in the intermediate alloy layer is sometimes higher than that in the upper coating. Nevertheless, when the upper limit of Si concentration in the plating bath is 1.5%, since the Si concentration in the intermediate alloy layer does not exceed 10.0%, the upper limit of Si is 10.0%. It should be noted that if the plating bath contains no Si, the Si content in the intermediate alloy layer is 0%. Therefore, the Si content in the intermediate alloy layer is set to 0~10.0%.
[0110] When the metal coating solidifies, Ni is concentrated in the intermediate alloy layer. Therefore, the Ni concentration in the intermediate alloy layer is higher than that in the lower alloy layer and the upper coating. When the upper coating contains more than 0.5% Ni, its corrosion resistance deteriorates; therefore, the Ni added to the plating bath needs to be less than 3.0%. In this case, it is difficult to make the Ni concentration in the intermediate alloy layer exceed 10%; therefore, the Ni concentration in the intermediate alloy layer is set to 10.0% or less. Furthermore, by containing more than 0.5% Ni in the intermediate alloy layer, an Al-Fe-Ni alloy is sufficiently formed; therefore, the Ni content is set to 0.5% or more.
[0111] In addition, Mg is sometimes present in the intermediate alloy layer, but Mg has low solid solubility in Al-Fe-Ni alloys, so its content is set to below 1.0%. Therefore, the Mg content is set in the range of 0 to 1.0%.
[0112] Additionally, the intermediate alloy layer may contain one or more of the elements included in Ca, Sn, Bi, In, Y, La, Ce, Sr, B, P, Cr, Ti, Co, V, Nb, Cu, Mn, Mo, W, Zr, Ag, Li, Na, K, and Ba, in a total range of 0 to 2.0%. These elements constitute the upper coating, but sometimes small amounts of them are mixed into the intermediate alloy layer.
[0113] The remainder in the intermediate alloy layer is impurities. Like the upper and lower alloy layers, impurities in the intermediate alloy layer refer to components contained in the raw materials or those introduced during the manufacturing process. For example, in the intermediate alloy layer, due to the mutual atomic diffusion between the steel (iron-based) and the plating bath, trace amounts of components other than Fe may sometimes be introduced as impurities.
[0114] The thickness of the intermediate alloy layer is preferably 1.0 μm or more. On the other hand, since it is difficult to make the thickness of the intermediate alloy layer exceed 40 μm, the thickness of the intermediate alloy layer is 1.0 μm or more and 40 μm or less.
[0115] The overall thickness of the metallic coating is preferably set to 25-200 μm. Generally, the thickness of metallic coatings, such as plating films, is related to corrosion resistance; thicker coatings exhibit superior corrosion resistance and stronger resistance to damage. On the other hand, the thickness of plating films has a limit due to the increase in plating bath capacity. Furthermore, increasing the thickness of the plating film requires a large amount of plating metal, leading to increased costs. Therefore, in this embodiment, the thickness of the metallic coating is preferably set to 200 μm or less. Additionally, when the thickness of the metallic coating is less than 25 μm, corrosion resistance decreases; therefore, the thickness of the metallic coating can be 25 μm or more.
[0116] The various measurement methods are explained below.
[0117] The thickness of the alloy layer (the total thickness of the lower alloy layer and the intermediate alloy layer) is determined by identifying the boundary between the upper plating layer and the alloy layer based on the SEM reflected electron image of the cross-section of the metal coating. When determining the boundary between the upper plating layer and the alloy layer, consideration is given to the Al-Fe-Ni alloys and Al-Fe alloys contained within the alloy layer.
[0118] First, expose a section perpendicular to the surface of the plated steel. The exposed section is mirror-finished. Figure 1A The image shown is an SEM image of a cross-section perpendicular to the surface of the plated steel. The SEM image magnification is set to 1000x. It should be noted that... Figure 1A It is a reflection electron image from SEM. Additionally, Figure 1B The middle shows Figure 1A A schematic diagram. In Figure 1B In the diagram, symbol 1 represents steel, symbol 2 represents the metal coating, symbol 2a represents the surface of the coated steel (the surface of the metal coating), symbol 2b represents the upper coating, symbol 2c represents the alloy layers (the middle alloy layer and the lower alloy layer), and symbol 3 represents the cross-sectional outline of the interface between steel 1 and metal coating 2. Additionally, the curve in symbol 4 represents the boundary between the dark gray area and the white or light gray area in the SEM image, and is presumed to be the boundary line between the upper coating 2b and the alloy layer 2c.
[0119] Next, in Figure 1B In this embodiment, the interface between the steel 1 and the metal coating 2 is a cross-sectional profile 3. The interface between the steel 1 and the metal coating 2 is a surface with uneven surfaces, therefore its cross-sectional profile 3 is a continuous, irregular curve.
[0120] Next, as Figure 1CAs shown, the centerline CL of the cross-sectional profile 3 of a specific interface is defined. Specifically, the cross-sectional profile 3 of the interface is set as a line roughness curve, i.e., a roughness curve, with a cutoff value λc = 0.8 mm. Then, a straight line CL with a length of 40 μm, approximately parallel to the roughness curve (cross-sectional profile 3), is superimposed on the roughness curve (cross-sectional profile 3). By superimposing the roughness curve (cross-sectional profile 3) on the straight line CL, the cross-sectional profile 3 and the straight line CL have multiple intersection points, forming multiple regions enclosed by the cross-sectional profile 3 and the straight line CL. These multiple regions are located on the upper side (opposite to the steel side) and the lower side (steel side) of the straight line CL. Furthermore, the straight line CL is positioned such that the total area of the region located on the upper side of the straight line CL is equal to the total area of the region located on the lower side of the straight line CL. The positioned straight line CL is used as the centerline of the roughness curve of the interface.
[0121] Next, as Figure 1D As shown, multiple imaginary lines K1 with a length of 40 μm are set parallel to the center line CL of the surface roughness curve. Multiple imaginary lines K1 are set at 10 μm intervals in the thickness direction of the metal coating.
[0122] Next, for each first imaginary line K1, the length of overlap between the Al-Fe-Ni alloy or Al-Fe alloy (hereinafter collectively referred to as the test alloy) and the first imaginary line K1 is measured. Furthermore, the percentage (%) of the length of overlap with the test alloy relative to the total length (40 μm) of the first imaginary line K1 is calculated for each first imaginary line K1.
[0123] The percentage (%) of the length overlapping with the alloy being measured relative to the total length of the first imaginary line K1 is derived from the brightness distribution on the first imaginary line K1 obtained from the SEM reflected electron image. Al-Fe-Ni alloys or Al-Fe alloys are darker than Zn phases and steel, but brighter than Al and Mg phases, thus easily distinguishable from these phases. The percentage of brightness corresponding to the alloy being measured on the first imaginary line K1 is calculated using image processing software and set as the percentage of the length overlapping with the first imaginary line K1. Image processing software such as ImageJ, which is a common domain image processing software, can be used. Images observed using SEM at magnification of 1000x or higher are set as image data, and the percentage (%) of the length overlapping with the alloy being measured relative to the total length of the first imaginary line K1 is measured using the measurement function of ImageJ. Image processing software is not limited to ImageJ; any software with equivalent functionality to ImageJ can be used.
[0124] It should be noted that the alloys being measured refer to Al-Fe-Ni alloys contained in the intermediate alloy layer and Al-Fe alloys contained in the lower alloy layer. As described in the description of the intermediate and lower alloy layers, these alloys may contain Zn, Si, Ni, etc.
[0125] Next, as Figure 1E As shown, there are several imaginary lines K50L and K50U, among the specific first imaginary lines K1, where the overlap ratio with the alloy being measured is less than 50%. In the case of multiple imaginary lines K50L with an overlap ratio less than 50%, the imaginary line located closest to the steel is specifically selected. These imaginary lines K50L and K50U are used as reference lines.
[0126] Next, as Figure 1F As shown, between the baselines K50L and K50U, multiple second imaginary lines K2, parallel to the baselines K50L and K50U and with a length of 40μm, are set at 1μm intervals. Thereafter, the baselines K50L and K50U are contained within the second imaginary lines K2.
[0127] Next, the length of overlap between the test alloy and the second imaginary line K2 is measured for each second imaginary line K2. Then, the percentage (%) of the overlap length with the test alloy relative to the total length (40 μm) of the second imaginary line K2 is calculated for each second imaginary line K2. The method for determining the percentage (%) of the overlap length with the test alloy relative to the total length of the second imaginary line K2 is the same as that for the first imaginary line K1.
[0128] Next, as Figure 1G As shown, among a plurality of second imaginary lines K2, the second imaginary line K50 with an overlap ratio of less than 50% with the alloy being measured is selected, and then the imaginary line K50A located on the steel side of the selected second imaginary line K50 is selected. Furthermore, the imaginary line K50B located on the steel side of imaginary line K50A and most adjacent to imaginary line K50A is selected.
[0129] And, as Figure 1H As shown, the distance t between the imaginary line 50B and the straight line CL is set as the thickness of the alloy layer.
[0130] The above operation is performed on 5 SEM images, and the average thickness of the alloy layer obtained in each SEM image is taken as the total thickness of the alloy layer, i.e., the middle alloy layer and the lower alloy layer.
[0131] The thickness of the upper coating is the value obtained by subtracting the thickness of the alloy layer from the thickness of the metal coating.
[0132] The thickness of the intermediate alloy layer was determined using an EPMA image of the metallic coating in a cross-section perpendicular to the surface of the coated steel. Specifically, using the SEM image used in determining the alloy layer thickness, elemental mapping of Ni was performed by electron probe microanalysis (EPMA), and regions with Ni concentrations of 0.5% or higher were extracted during image processing. The EPMA measurement conditions were the same as those used to determine the area ratio of the quasicrystalline phase.
[0133] Next, similar to the determination of the alloy layer thickness, an imaginary line of 40 μm length parallel to the center line CL of the roughness curve of the steel surface was drawn. Specifically, an imaginary line with a length ratio of 50% or more overlapping with the region where Ni is 0.5% or more (Al-Fe-Ni alloy) was selected. The imaginary line closest to the center line CL of the roughness curve was taken as the boundary line of the intermediate alloy layer. Regarding the thickness of the intermediate alloy layer, the boundary line of the intermediate alloy layer in the SEM images of five fields of view was measured. Figures 1B-1G The distance of a specific imaginary line 50B is taken as its average.
[0134] Regarding the composition of the intermediate alloy layer, in five fields of view, perpendicular lines were drawn from both ends of the boundary line of the intermediate alloy layer along the surface thickness direction. Elemental surface analysis was performed on the region enclosed by the imaginary line 50B using EPMA, and the average value was derived as the composition of the intermediate alloy layer. The EPMA measurement conditions were the same as those used to determine the area ratio of the quasicrystalline phase.
[0135] The thickness of the lower alloy layer is derived by subtracting the thickness of the intermediate alloy layer from the thickness of the alloy layer. Furthermore, regarding the composition of the lower alloy layer, the region along a perpendicular line drawn from the center line CL of the steel surface roughness curve to the boundary line of the intermediate alloy layer is defined as the region of the lower alloy layer. Elemental surface analysis of this region is performed using EPMA, and the average values are derived as the composition of the lower alloy layer. The EPMA measurement conditions are the same as those used to determine the area ratio of the quasicrystalline phase.
[0136] The method for confirming the morphology of the intermediate alloy layer is explained. Whether the metallic microstructure in the intermediate alloy layer is miscible or homogeneous can be determined by compositional analysis based on surface data. Specifically, in the case of a miscible microstructure, the Fe concentration is less than 20%, which is lower than in a homogeneous microstructure, thus allowing for determination based on Fe concentration.
[0137] Next, it is preferable that the metal coating of the plated steel in this embodiment contains as few halides as possible. Specifically, the fluorescence X-ray intensity of the halogen elements in the metal coating, as determined by fluorescence X-ray analysis, is preferably in the range of 0 to 0.6 kcps.
[0138] As described below, the plated steel of this embodiment forms a metallic coating by immersing the steel in a plating bath after treating the steel surface with a flux. However, when the plating bath contains a total of 5% or more of Al and Mg, significant flux residue adhesion sometimes occurs. Excessive flux residue remaining in the metallic coating can sometimes result in incomplete plating and reduce the corrosion resistance of the metallic coating. Magnesium chloride, aluminum chloride, etc., can be considered as flux residues.
[0139] Therefore, in this embodiment, as a countermeasure to reduce flux residue, which is a cause of non-coating, a flux free of NH4Cl is selected. This reduces the likelihood of flux residue remaining in the metal coating, suppressing non-coating and preventing a decrease in the corrosion resistance of the metal coating. The amount of flux residue in the metal coating can be evaluated by the fluorescence X-ray intensity of halogen elements in the metal coating. If the fluorescence X-ray intensity of halogen elements in the metal coating, as obtained by fluorescence X-ray analysis, is in the range of 0 to 0.6 kcps, then the flux residue is minimal, thereby reducing the possibility of adverse effects on corrosion resistance.
[0140] The fluorescence X-ray intensity of halogen elements in the metal coating was determined as follows.
[0141] As the analytical apparatus for fluorescence X-ray analysis of the surface (metal-coated surface) of coated steel, a RIGAKU ZSXPrismIII+ was used. The analysis range was the interior of a circle with a diameter of 30 mm. Measurements were performed by irradiating the upper surface with the EZ-scan program set (target: Rh, 30 kV-80 mA, spectrophotometer: Ge, detector: proportional counter, measurement peak: 92.8°, detector speed: 10 deg / min).
[0142] Next, the manufacturing method of the plated steel according to an embodiment of the present invention will be described. The plated steel of this embodiment is cleaned by degreasing and pickling the surface of the steel, and then manufactured by immersion-type melt plating method (batch melt plating method) after flux treatment.
[0143] There are no particular restrictions on the size, shape, or surface morphology of the steel to be plated. Any type of steel, such as ordinary steel, high-tensile steel, or stainless steel, can be used. More specifically, various types of steel can be used, including general steel, Ni-pre-plated steel, Al-killed steel, very low carbon steel, high carbon steel, various high-tensile steels, and some high-alloy steels (steels containing strengthening elements such as Ni and Cr). Steel strips of general structural steel are preferred.
[0144] For steel, surface finishing processes such as shot peening and grinding can be performed beforehand, and Ni, Zn, and Sn plating can be applied to the surface at a density of 3g / m. 2 There is no problem with the following metal or alloy films, which can then be plated.
[0145] Then, as a pre-treatment of the steel, it is thoroughly cleaned through degreasing and pickling. There are no particular restrictions on the conditions for degreasing and pickling.
[0146] Next, the cleaned steel surface is treated with a flux. Flux treatment involves immersing the steel in a flux aqueous solution at approximately 60°C for at least 20 seconds, followed by lifting and drying. The flux is based on ZnCl2 and contains various salts such as NaCl, NaF, KCl, SnCl2, SnCl4, and BiCl3, as well as surfactants. An acidic solution such as hydrochloric acid is used as needed. By applying the flux to the steel before plating, a metallic coating layer in which Ni segregates in the intermediate alloy layer is obtained.
[0147] For plating fluxes that do not produce flux residues, it is preferable to use fluxes that do not contain NH4Cl. Examples of fluxes include those consisting of 5-14% by mass of NaCl, 1.2-5% by mass of BiCl3, 7-18% by mass of KCl, and the balance ZnCl2, dissolved in water at a concentration of 150-300 g / L, with the pH adjusted to 1.5 or lower. Other examples include fluxes containing, by mol%, (a) 65-85% ZnCl2, (b) 0.5-3% of any one or more of NaF, KF, MgF2, and Na2SiF6, (c) 5-25% of any one or more chlorides of alkali metals or alkaline earth metals, and (d) more than 5% and less than 20% of any one or more chlorides of Sn, In, Tl, Sb, and Bi.
[0148] Based on the aforementioned flux, when manufacturing coated steel using a one-stage plating method, the likelihood of flux residue remaining on the steel or the coated surface is low. Therefore, coated steel with sufficient corrosion resistance can be obtained.
[0149] Next, the steel treated with the flux is immersed in a plating bath prepared with a specified composition. The composition of the plating bath only needs to be roughly the same as the target composition of the upper plating layer. However, since elements such as Al and Ni are enriched in the lower and intermediate alloy layers, the composition of the plating bath is based on the target composition of the upper plating layer, with the Al and Ni amounts increasing from the target composition of the upper plating layer. For example, the standard is that the Al concentration in the plating bath is about 1.5 to 5% higher than the Al concentration (mass%) in the upper plating layer, and the Ni concentration in the plating bath is 5 to 20 times higher than the Ni concentration (mass%) in the upper plating layer.
[0150] Specifically, to obtain the alloy layer of the present invention, the Al concentration of the plating bath composition needs to be in the range of 2.0 to 84.98% by mass, the Zn concentration in the range of 15.0% to 97.98% by mass, and the Ni concentration in the range of less than 0.02% to 3.0% by mass. Furthermore, in order to form the upper plating layer within the preferred range, the plating bath composition preferably has an Al concentration in the range of 7.5% to 30.0% by mass, a Zn concentration in the range of more than 50% and less than 89.48% by mass, a Ni concentration in the range of less than 0.02% to 3.0% by mass, and a Mg concentration in the range of more than 3.0% to 12.5% by mass.
[0151] The bath temperature for plating is 440℃~600℃, preferably 460℃~520℃. At higher bath temperatures, the growth of the lower alloy layer is faster, resulting in excellent productivity, but the Al-Fe reaction may be uncontrollable. At lower bath temperatures, plating defects such as incomplete plating are more likely to occur, especially with high Mg concentrations. Furthermore, the Al-Fe reaction is inhibited, preventing the formation of an alloy layer of appropriate thickness. Therefore, the bath temperature is 440℃~600℃. It should be noted that while higher bath temperatures may sometimes result in a higher Fe concentration in the upper plating layer, below 600℃, the Fe concentration in the upper plating layer typically converges to below 5.00%.
[0152] The immersion time of steel in the plating bath should be between 50 and 1000 seconds, preferably between 100 and 600 seconds. Immersion time directly affects productivity, but it is not strictly determined by the nature of flux-based immersion plating. The bath temperature and immersion time are not the only determining factors, but rather a balance between productivity and quality, considering the heat capacity of the material being plated.
[0153] In the case of steel materials of a specified shape, such as bolts and screws, after being lifted from the plating bath, centrifugal separation is performed to adjust the amount of molten metal adhering to the plate and adjust the metal coating to the specified thickness.
[0154] Cooling is performed immediately after the thickness of the metal coating is adjusted. Cooling to solidify the molten metal is achieved through venting or air cooling. The average cooling rate from the start to the end of cooling is adjusted according to the temperature of the plating bath as follows.
[0155] When the temperature of the plating bath exceeds 500℃, the average cooling rate is 4~6℃ / s when the bath temperature is between 500℃ and 300℃, and the average cooling rate is 2~5℃ / s when the bath temperature is between 500℃ and 300℃.
[0156] When the temperature of the plating bath is below 500℃, the average cooling rate between the bath temperature and 300℃ is 2~5℃ / s.
[0157] When the temperature of the plating bath exceeds 500°C, and the average cooling rate of the bath temperature ~500°C exceeds 6°C / s, the area ratio of the quasicrystalline phase sometimes increases. In addition, sometimes an alloy layer with the desired composition concentration cannot be obtained.
[0158] In addition, when the average cooling rate at a bath temperature of ~500℃ is less than 4℃ / s, the Al-Fe reaction cannot be suppressed, and an alloy layer with the desired composition concentration cannot be obtained.
[0159] Furthermore, when the average cooling rate between 500 and 300°C exceeds 5°C / s, it is sometimes impossible to obtain an alloy layer with the desired composition concentration.
[0160] When the average cooling rate between 500 and 300°C is less than 2°C / s, the Al-Fe reaction cannot be suppressed, and an alloy layer with the desired composition concentration cannot be obtained.
[0161] When the bath temperature is below 500°C, and the average cooling rate between the bath temperature and 300°C exceeds 5°C / s, it is sometimes impossible to obtain an alloy layer with the desired composition concentration.
[0162] In addition, when the average cooling rate between the bath temperature and 300°C is less than 2°C / s, the Al-Fe reaction cannot be suppressed, and an alloy layer with the desired composition concentration cannot be obtained.
[0163] Alternatively, the coated steel can be cooled to a temperature below 300°C by air cooling or venting before water cooling. When water cooling is used, from the viewpoint of preventing unevenness on the surface of the metal coating, it is preferable to immerse the steel in water after the upper coating has solidified.
[0164] The above steps are used to manufacture the plated steel of this embodiment.
[0165] After the coating cools, various chemical conversion treatments and coating processes can be performed. In addition, to further improve corrosion resistance, repair touch coatings and spray plating can be applied to welded and machined parts.
[0166] In the plated steel of this embodiment, a film can be formed on the coating. One or more films can be formed. Examples of films directly above the coating include chromate films, phosphate films, and chromate-free films. Chromate treatments, phosphate treatments, and chromate-free treatments used to form these films can be performed using known methods. However, chromate treatments often deteriorate weldability on the coating surface; therefore, to fully utilize the weldability improvement effect of the coating, its thickness is preferably less than 1 μm.
[0167] Chromate treatments include: electrolytic chromate treatment, which forms a chromate film through electrolysis; reactive chromate treatment, which forms a film by reacting with the raw material and then rinsing off excess treatment solution; and coating-type chromate treatment, which involves applying the treatment solution to the substrate and drying it without washing to form a film. Any treatment can be used.
[0168] Examples of electrolytic chromate treatments include those using chromic acid, silica sol, resins (phosphoric acid, acrylic resin, vinyl ester resin, vinyl acetate acrylic emulsion, carboxylated styrene-butadiene latex, diisopropanolamine modified epoxy resin, etc.) and hard silica.
[0169] Examples of phosphate treatments include zinc phosphate treatment, calcium zinc phosphate treatment, and manganese phosphate treatment.
[0170] Chromate-free treatment is preferred as it does not impose a significant environmental burden. Types of chromate-free treatments include: electrolytic chromate-free treatment, which forms a chromate-free film through electrolysis; reactive chromate-free treatment, which forms a film by reacting with the raw materials and then rinsing off excess treatment solution; and coating-type chromate-free treatment, which involves applying the treatment solution to the substrate and drying it without washing to form a film. Any treatment method can be used.
[0171] Furthermore, one or more layers of organic resin film may be present on the film directly above the coating. The organic resin is not limited to a specific type; examples include polyester resin, polyurethane resin, epoxy resin, acrylic resin, polyolefin resin, or modified forms of these resins. Here, a modified form refers to a resin obtained by reacting reactive functional groups contained in the structure of these resins with other compounds (monomers, crosslinking agents, etc.) containing functional groups capable of reacting with those functional groups.
[0172] As such an organic resin, one or more organic resins (unmodified organic resins) can be used in combination, or at least one organic resin modified from another organic resin can be used in combination in the presence of at least one organic resin. Furthermore, the organic resin film can contain any coloring pigments or anti-rust pigments. Aqueous substances that are dissolved or dispersed in water can also be used.
[0173] Example
[0174] The embodiments of the present invention will be described below.
[0175] The base steel for the galvanized steel was cut from 1.6mm thick hot-rolled steel sheets in 200mm x 100mm dimensions. All were SS400 (general steel with black scale). After surface cleaning with a commercially available alkaline degreaser, the surface oxide scale was removed by pickling with 10% hydrochloric acid. The pickled steel sheet was then rinsed with 60℃ hot water and immersed in a 60℃ flux (ZnCl2 / NaCl / KCl / SnCl2 = 200(g / l) / 20(g / l) / 40(g / l) / 6(g / l), pH=1.0) for approximately 1 minute, followed by heating and drying in a 200℃ furnace under atmospheric conditions for 5 minutes. The steel sheet was then immersed in the plating bath for 60-900 seconds to complete the plating process, lifted out, and allowed to cool naturally. After complete solidification, it was then water-cooled. When the bath temperature exceeds 500℃, the average cooling rate is set to 4~8℃ / s between the bath temperature and 500℃, and 2~5℃ / s between 500℃ and 300℃. When the bath temperature is below 500℃, the average cooling rate is 2~5℃ between the bath temperature and 300℃. In this way, coated steel products No. 1~31 and 37 are manufactured using a single-stage coating method.
[0176] Furthermore, for the coated steels No. 32 to 36, the original plates are cleaned and pickled in the same manner as described above, then treated with a flux in the same way, and subsequently immersed in a zinc plating bath to form a 50 μm thick zinc coating on the surface of the steel. Next, as described above, the steel plates with the zinc coating are immersed in the plating bath for 60 to 120 seconds to complete the plating process, then lifted out and allowed to cool naturally. After the coating has completely solidified, they are water-cooled. In this way, various coated steels are manufactured using a two-stage plating method. The conditions for natural cooling are shown in the table.
[0177] The composition of the plating bath is roughly the same as that of the upper plating layer described in Tables 1A and 1B, but the Al concentration of the plating bath is increased by about 0-5% by mass relative to the Al concentration (mass%) of the plating layer, and the Ni concentration of the plating bath is 5-20 times higher than the Ni concentration (mass%) of the upper plating layer. Among them, plating baths No. 25-28, 31 and 37 are removed from the preferred concentrations.
[0178] (Determination of the chemical composition and thickness of the upper coating)
[0179] The composition of the upper coating was determined by ICP-based luminescence spectrophotometry. Specifically, the test material was immersed in a 5% NaOH aqueous solution containing an inhibitor and dissolved, yielding a solution with the upper coating dissolved and peeled off. The endpoint of alkaline dissolution was defined as the point at which foaming on the surface of the immersed test material ceased, and more than 90% of the surface changed to a black appearance due to the exposure of the alloy layer. The resulting solution was then acid-treated with HCl, and its composition was analyzed by luminescence spectrophotometry.
[0180] The thickness of the upper coating is derived by subtracting the thickness of the alloy layer (described later) from the thickness of the metallic coating. The thickness of the metallic coating is derived through cross-sectional microstructure observation. Specifically, in the SEM reflectance electron image of the cross-section of the metallic coating, the distance between the outermost surface of the metallic coating and the steel is measured at 10 locations, and the average value is calculated as the thickness of the metallic coating. The distance between the measurement locations is set to approximately 100 μm. Then, the thickness of the metallic coating is subtracted from the thickness of the alloy layer (described later) to derive the thickness of the upper coating.
[0181] (Determination of the chemical composition and thickness of the alloy layer)
[0182] The thickness of the alloy layer (the total thickness of the lower alloy layer and the intermediate alloy layer) was measured as described above. However, in No. 26, since there are regions without Al, regions containing 5% or more Fe were measured as alloy layers.
[0183] The thickness of the intermediate alloy layer was measured as described above. However, No. 26 does not contain Al, and the alloy layer is formed by an Fe-Zn alloy. Therefore, the ζ phase was measured as the intermediate alloy layer and the γ phase as the lower alloy layer. Furthermore, the composition of the intermediate alloy layer was measured as described above.
[0184] The thickness of the lower alloy layer is derived by subtracting the thickness of the intermediate alloy layer from the thickness of the alloy layer. Furthermore, the composition of the lower alloy layer is determined as described above.
[0185] The method for confirming the morphology of the intermediate alloy layer is explained. The composition of the metal structure in the intermediate alloy layer is determined by elemental mapping analysis based on EPMA, to determine whether it is a miscible or homogeneous structure. Specifically, in the case of a miscible structure, the Fe concentration is less than 20%, which is lower than that of a homogeneous structure; therefore, the determination is based on the Fe concentration.
[0186] The determination of the area fraction of the quasicrystalline phase in the upper coating and the determination of the chlorine (Cl) content in the metal coating are as described above.
[0187] (Corrosion resistance evaluation)
[0188] Cut the test material into 120×50mm pieces and conduct tests according to JASOM 609 to confirm the formation of red rust. Red rust should occur at a rate of more than 5% of the sample area.
[0189] The evaluation of corrosion resistance is as follows. "B" is set as unacceptable, and "A" through "S" are set as acceptable.
[0190] Red rust was observed in cycles with a count less than 450: "B" Red rust formation after 450-600 cycles: "A" Red rust formation after 600-750 cycles: "AA" Red rust appears after 750-900 cycles: "AAA" No red rust appeared during the 900-cycle test: "S" As shown in Tables 1A to 4B, in Nos. 1 to 24, 29, and 30 (all examples), the chemical composition and thickness of the intermediate and lower alloy layers are within the scope of this invention, exhibiting good corrosion resistance. It should be noted that the cross-sectional SEM image and elemental surface analysis results of the metal coating layer in No. 12 are shown in... Figures 2-7 Especially as Figure 4 As shown, Ni was confirmed to be enriched in the presence region of the intermediate alloy layer.
[0191] Nos. 25-28 and 31 have poor corrosion resistance because the composition of the plating bath is inappropriate, resulting in the chemical composition of the intermediate alloy layer and the lower alloy layer or the thickness of each layer being outside the scope of this invention.
[0192] That is, No. 25 sets the Si composition of the plating bath to 2.5%, but because it is a relatively high composition, it inhibits the growth of the intermediate and lower alloy layers, resulting in thinner alloy layers and reduced corrosion resistance.
[0193] No. 26 sets the Al composition of the plating bath to 0.1%, but because it is a relatively low composition, it is not possible to fully form an Fe-Al alloy. The amount of Al in the intermediate and lower alloy layers is insufficient, resulting in reduced corrosion resistance.
[0194] The Ni composition of the No. 27 plating bath is 3.0%, so the Ni concentration in the plating bath becomes excessive. As a result, the amount of Ni in the intermediate alloy layer becomes excessive, and the corrosion resistance is reduced.
[0195] The Ni composition of the No. 28 plating bath is 0%, therefore no intermediate alloy layer is formed, resulting in reduced corrosion resistance.
[0196] The Zn content in the No. 31 plating bath is insufficient, resulting in insufficient Zn content in the intermediate and lower alloy layers, thus reducing corrosion resistance.
[0197] No. 37 Due to inappropriate manufacturing conditions, 10% of the quasicrystalline phase in the upper coating was precipitated by volume, the chemical composition of the alloy layer was outside the range of this invention, and the corrosion resistance was reduced.
[0198] Steels No. 32 and 34-36 are manufactured using a two-stage plating method, but the composition of the intermediate and lower alloy layers does not meet the scope of this invention, resulting in reduced corrosion resistance. Furthermore, the metallic microstructure of the intermediate alloy layer in Nos. 32 and 34-36 is a mesh-like mixed phase.
[0199] No. 33 was manufactured using a two-stage plating method, but the composition of the plating bath was inappropriate, and therefore no intermediate alloy layer was formed.
[0200]
[0201]
[0202]
[0203]
[0204]
[0205]
[0206]
[0207]
[0208] Industrial availability This invention provides Zn-Al-Mg based coated steel with excellent corrosion resistance. Therefore, it enables the production of inexpensive steel structures that exhibit stable corrosion resistance even in harsh corrosive environments, making it industrially viable.
[0209] Explanation of reference numerals in the attached figures 1…steel, 2…metal coating, 2a…surface of steel (surface of metal coating), 2b…top coating, 2c…alloy layer.
Claims
1. A plated steel material comprising a steel material and a metal coating disposed on the surface of the steel material, The metal coating is provided sequentially from the steel side as follows: a lower alloy layer containing more than 22.5% Fe, an intermediate alloy layer containing more than 20.0% Fe and 0.5 to 10.0% Ni, and an upper coating formed of a Zn-based alloy containing 0 to 5.0% Fe. The thickness of the lower alloy layer is 5 μm or more, the thickness of the intermediate alloy layer is 1.0 μm or more, and the combined thickness of the lower alloy layer and the intermediate alloy layer is 6 μm or more. The chemical composition of the lower alloy layer, expressed in % by mass, includes Zn: 5.0~30.0%, Al:30.0~55.0%、 Fe: 22.5~50.0%, Si: 0~10.0% Ni: 0~less than 0.5% Mg: 0~1.0%, Balance: Impurities The chemical composition of the intermediate alloy layer, expressed as a percentage by mass, includes Zn: 5.0~35.0%, Al:25.0~60.0%、 Fe: 20.0~45.0%, Si: 0~10.0% Ni: 0.5~10.0% Mg: 0~1.0%, The total of one or more elements selected from Ca, Sn, Bi, In, Y, La, Ce, Sr, B, P, Cr, Ti, Co, V, Nb, Cu, Mn, Mo, W, Zr, Ag, Li, Na, K, and Ba: 0~2.0%. Balance: impurities.
2. The plated steel according to claim 1, wherein, The chemical composition of the upper coating, expressed as a percentage by mass, includes: Al:6.0%~25.0%、 Mg: ≥3.0%~12.5%, Ni: 0.001% to less than 0.5% Si: 0%~1.5% Ca: 0%~3.0% Sn: 0%~3.0% Bi: 0%~1.0% In: 0%~1.0%, Y:0%~0.5%、 La: 0%~0.5% Ce: 0%~0.5% Sr:0%~0.5%、 B:0%~1.0%、 P:0%~0.5%、 Cr:0%~0.25%、 Ti: 0%~0.25% Co: 0%~0.25%, V:0%~0.25%、 Nb: 0%~0.25%, Cu: 0%~1.0% Mn: 0%~0.25%, Mo: 0%~0.25%, W:0%~0.25%、 Zr:0%~0.25%、 Ag: 0%~1.0% Li: 0%~0.5% Na: 0%~0.05% K:0%~0.05%、 Ba: 0%~0.25% Fe: 0%~5.0%, Balance: More than 50% Zn and impurities.
3. The plated steel material according to claim 2, wherein The upper coating satisfies the following equations (1) and (2): Mg / Al≤0.5…(1) 2×Ca+Sr+Y+La+Ce≥0.05…(2) In equations (1) and (2), Mg, Al, Ca, Sr, Y, La, and Ce represent the contents (mass%) of the upper coating, respectively. If the element is not present, substitute 0.
Citation Information
Patent Citations
High corrosion resistant plated steel material and its producing method
JP2002047548A
Plated steel having high corrosion resistance and excellent workability and method for producing the same
JP2010070810A
Plating steel having excellent corrosion resistance
JP2017066524A