Device for synthesizing lithium carbonate from lithium iron phosphate positive electrode powder by hydrochloric acid method
The device that synthesizes lithium carbonate through the hydrochloric acid method of lithium iron phosphate cathode powder solves the problem of recycling and processing of used lithium iron phosphate batteries, achieves efficient recovery of valuable metal lithium and lithium carbonate, reduces environmental pollution and resource waste, and is in line with green and low-carbon Sustainable development requirements.
Patent Information
- Application Number
- CN202420373439.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2034-02-28
AI Technical Summary
The lack of specialized recycling of used lithium iron phosphate batteries leads to environmental pollution and resource waste.
The device for synthesizing lithium carbonate using the hydrochloric acid method of lithium iron phosphate cathode powder, including aluminum removal kettle, filter press, acid leaching kettle, alkaline impurity removal kettle, lithium precipitation kettle and other equipment, through alkali solution aluminum removal, acid leaching, lithium, Processes such as alkali adjustment to remove impurities and mother liquor lithium extraction realize the recovery of valuable metal lithium and the synthesis of lithium carbonate. The entire process is processed by a wet process.
It achieves efficient recovery of valuable metal lithium, reduces environmental pollution and resource waste, and the process is controllable, saving energy and reducing consumption, which meets the needs of green, low-carbon and sustainable development.
Smart Images

Figure CN221832309U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of lithium resource extraction and recovery, in particular to a device for synthesizing lithium carbonate by using lithium iron phosphate positive electrode powder through a hydrochloric acid method. Background Art
[0002] As one of the electrode materials for lithium-ion batteries, lithium iron phosphate has greater advantages in safety, cost, and cycle life than other types, and has the potential for fast charging. Therefore, since its commercialization, it has been widely used in many fields including new energy vehicles, ships, and energy storage.
[0003] The present invention provides a process for synthesizing lithium carbonate from lithium iron phosphate positive electrode powder by hydrochloric acid method. The crushed lithium iron phosphate positive electrode powder is subjected to the steps of removing aluminum with alkali solution, dissolving lithium with acid, removing impurities with alkali, extracting lithium from mother liquor, etc., to recover valuable metal lithium and synthesize battery-grade lithium carbonate. The whole process is processed by wet process. Utility Model Content
[0004] The utility model aims to overcome the shortcomings of existing waste lithium iron phosphate batteries, which lead to environmental pollution and waste of resources due to the lack of special recycling treatment, and proposes a device for synthesizing lithium carbonate from lithium iron phosphate positive electrode powder by hydrochloric acid method.
[0005] In order to achieve the above purpose, the utility model adopts the following technical solutions:
[0006] A device for synthesizing lithium carbonate from lithium iron phosphate positive electrode powder by hydrochloric acid method comprises an aluminum removal kettle, wherein the top of the aluminum removal kettle is connected to a positive electrode powder bin and an alkali solution high-level tank box, one side of the aluminum removal kettle is connected to a filter press through a delivery pump, a filter cake is processed in the filter press, an acid leaching kettle is connected to the filter press, the acid leaching kettle is also connected to a hydrogen peroxide high-level tank box and a hydrochloric acid high-level tank box, the acid leaching kettle is connected to a neutral impurity removal kettle through a delivery pump, the neutral impurity removal kettle is connected to an alkaline impurity removal kettle, the alkaline impurity removal kettle is connected to a filter, the filter is connected to a lithium precipitation kettle, the lithium precipitation kettle is connected to a centrifuge, the centrifuge is connected to a leaching water pipe, and lithium carbonate crystals are discharged from the centrifuge.
[0007] Preferably, a filter press is provided between the acid leaching kettle and the neutral impurity removal kettle, a liquid alkali high-level tank is connected to the neutral impurity removal kettle, and the filter press and the neutral impurity removal kettle are provided with filtrate A, and the filtrate A is a solution containing lithium chloride.
[0008] Preferably, a filter press is provided between the neutral impurity removal kettle and the alkaline impurity removal kettle, and the filter press processes filtrate B, which is an impurity removal solution containing sodium hydroxide.
[0009] Preferably, the filter is processed with filtrate C, the filtrate C is a solution containing ethylenediaminetetraacetic acid, and the lithium precipitation kettle is connected to a sodium carbonate solution high-level tank.
[0010] Compared with the prior art, the beneficial effects of the utility model are:
[0011] 1. Acid leaching and dissolving lithium process, using hydrogen peroxide, or oxidants such as sodium chlorate, in the hydrochloric acid system, without introducing extra anions and cations;
[0012] 2. Remove impurities and filter residue, collect takeaway, and recover valuable metals such as copper, iron, and magnesium;
[0013] 3. In alkaline impurity removal, if the Ca2+ is too high, add an appropriate amount of Na2CO3 to remove Ca2+, because Ca(OH)2 is slightly soluble, while CaCO3 is insoluble, so the high Ca2+ can be removed;
[0014] 4. In addition to aluminum mother liquor, aluminum powder can be added to consume excess NaOH to prepare Al(OH)3 and increase the value of by-products;
[0015] 5. Lithium carbonate has a certain solubility in water. The filtrate after lithium extraction is returned to the acid leaching lithium dissolution process and used as water to prevent the lithium element from escaping.
[0016] In summary, the utility model can recover valuable metal lithium and synthesize battery-grade lithium carbonate from the crushed lithium iron phosphate positive electrode powder through processes such as removing aluminum with alkali solution, dissolving lithium with acid, removing impurities with alkali, and extracting lithium from mother liquor. The entire process is processed by wet process, the key nodes are precisely controllable, the overall recovery rate is high, and it is relatively environmentally friendly, energy-saving and consumption-reducing, which meets the needs of green, low-carbon and sustainable development of the industry, and avoids the problem of environmental pollution and waste of resources caused by the lack of special recycling and treatment of existing waste lithium iron phosphate batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is an overall structural diagram of a device for synthesizing lithium carbonate using a lithium iron phosphate positive electrode powder by a hydrochloric acid method proposed in the utility model.
[0018] In the figure: 1. positive electrode powder bin; 2. aluminum removal kettle; 3. alkali solution high-level tank box; 4. delivery pump; 5. filter press; 6. hydrogen peroxide high-level tank box; 7. acid leaching kettle; 8. hydrochloric acid high-level tank box; 9. filter cake; 10. filtrate A; 11. liquid alkali high-level tank box; 12. neutral impurity removal kettle; 13. alkaline impurity removal kettle; 14. filtrate B; 15. filter; 16. filtrate C; 17. lithium precipitation kettle; 18. sodium carbonate solution high-level tank box; 19. leaching water pipe; 20. centrifuge; 21. lithium carbonate crystallization. DETAILED DESCRIPTION
[0019] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0020] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0021] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0022] Unless otherwise specified, the raw materials used in the examples were purchased commercially.
[0023] Reference Figure 1 A device for synthesizing lithium carbonate from lithium iron phosphate positive electrode powder by hydrochloric acid method, comprising an aluminum removal kettle 2, a positive electrode powder bin 1 and an alkali liquid high-level tank box 3 are connected to the top of the aluminum removal kettle 2, a filter press 5 is connected to one side of the aluminum removal kettle 2 through a delivery pump 4, a filter cake 9 is processed in the filter press 5, an acid leaching kettle 7 is connected to the filter press 5, a hydrogen peroxide high-level tank box 6 and a hydrochloric acid high-level tank box 8 are also connected to the acid leaching kettle 7, the acid leaching kettle 7 is connected to a neutral impurity removal kettle 12 through a delivery pump 4, a filter press 5 is arranged between the acid leaching kettle 7 and the neutral impurity removal kettle 12, a liquid alkali high-level tank box 11 is connected to the neutral impurity removal kettle 12, a filtrate A10 is arranged between the filter press 5 and the neutral impurity removal kettle 12, and the filtrate A10 contains The solution of lithium chloride, the neutral impurity removal kettle 12 is connected to the alkaline impurity removal kettle 13, a filter press 5 is arranged between the neutral impurity removal kettle 12 and the alkaline impurity removal kettle 13, the filter press 5 processes the filtrate B14, the filtrate B14 is the impurity removal solution containing sodium hydroxide, the alkaline impurity removal kettle 13 is connected to the filter 15, the filter 15 processes the filtrate C16, the filtrate C16 is the solution containing ethylenediaminetetraacetic acid, the lithium precipitation kettle 17 is connected to the sodium carbonate solution high-level tank 18, the filter 15 is connected to the lithium precipitation kettle 17, the lithium precipitation kettle 17 is connected to the centrifuge 20, the centrifuge 20 is connected to the leaching water pipe 19, and the centrifuge 20 discharges lithium carbonate crystals 21. Process:
[0024] 1. Alkali solution aluminum removal: Based on the amphoteric characteristics of aluminum metal powder, react in sodium hydroxide solution to generate sodium aluminate, and remove aluminum by solid-liquid separation. Quantitatively add 5-20% sodium hydroxide solution at a solid-liquid ratio of 1:1-1:3, stir at room temperature-80℃ for 0.5-3h, filter, first wash and filter with sodium hydroxide solution of pH=11, then wash and filter with water, and the filter cake is acid-leached to dissolve lithium in the next step;
[0025] 2. Acid leaching and dissolving lithium: Add appropriate amount of deionized water to the filter cake, stir, slowly drip the measured hydrogen peroxide and hydrochloric acid solution at room temperature -80℃, slowly drip for 1-3h, and then continue to react for 1h. The lithium element in the material is dissolved in the solution with lithium chloride, filtered, and the filter residue is washed 1-2 times with dilute hydrochloric acid solution with PH=1∽2. The washing solution is mixed with the filtered solution. The washed filter residue can be used as a raw material for preparing crude iron phosphate. The mixed filtrate is used to remove impurities and lithium in the next step;
[0026] 3. Alkali adjustment to remove impurities: Impurity removal is generally divided into neutral impurity removal and alkaline impurity removal.
[0027] 4. Neutral impurity removal: gradually heat the filtrate to 60-90°C, slowly adjust the pH to 7 with 5-20% sodium hydroxide solution, keep warm and stir for 0.5h, filter, wash the residue with water, and mix the filtrate;
[0028] 5. Alkaline impurity removal: add a small amount of activated carbon to the filtrate, gradually raise the temperature to 50-90℃, slowly adjust the pH to 11-12 with 5-20% sodium hydroxide solution, keep warm and stir for 0.5h, filter, wash the residue with water, and mix the filtrate;
[0029] 6. Lithium extraction from mother liquor: Add a small amount of EDTA to the filtrate (lithium precipitation purification solution), slowly heat to 80-95°C, dissolve a measured amount of sodium carbonate powder in an appropriate amount of deionized water, and add it to the filtrate to crystallize lithium carbonate crystals. Keep warm and stir for 0.5-2h, hot filter, rinse the filter cake with hot water, and dry it to obtain battery-grade lithium carbonate products.
[0030] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
Claims
1. A device for synthesizing lithium carbonate from lithium iron phosphate positive electrode powder by hydrochloric acid method, comprising an aluminum removal kettle (2), characterized in that: The top of the aluminum removal kettle (2) is connected to a positive electrode powder bin (1) and an alkali solution high-level tank box (3); one side of the aluminum removal kettle (2) is connected to a filter press (5) through a delivery pump (4); a filter cake (9) is processed in the filter press (5); the filter press (5) is connected to an acid leaching kettle (7); the acid leaching kettle (7) is also connected to a hydrogen peroxide high-level tank box (6) and a hydrochloric acid high-level tank box (8); the acid leaching kettle (7) is connected to a delivery pump (4) A neutral impurity removal kettle (12) is connected, the neutral impurity removal kettle (12) is connected to an alkaline impurity removal kettle (13), the alkaline impurity removal kettle (13) is connected to a filter (15), the filter (15) is connected to a lithium precipitation kettle (17), the lithium precipitation kettle (17) is connected to a centrifuge (20), the centrifuge (20) is connected to a rinsing water pipe (19), and the centrifuge (20) discharges lithium carbonate crystals (21).
2. The device for synthesizing lithium carbonate from lithium iron phosphate positive electrode powder by hydrochloric acid method according to claim 1, characterized in that: A filter press (5) is provided between the acid leaching kettle (7) and the neutral impurity removal kettle (12), a liquid alkali high-level tank (11) is connected to the neutral impurity removal kettle (12), and a filtrate A (10) is provided between the filter press (5) and the neutral impurity removal kettle (12), and the filtrate A (10) is a solution containing lithium chloride.
3. The device for synthesizing lithium carbonate from lithium iron phosphate positive electrode powder by hydrochloric acid method according to claim 2, characterized in that: A filter press (5) is provided between the neutral impurity removal kettle (12) and the alkaline impurity removal kettle (13). The filter press (5) processes a filtrate B (14), and the filtrate B (14) is an impurity removal solution containing sodium hydroxide.
4. The device for synthesizing lithium carbonate from lithium iron phosphate positive electrode powder by hydrochloric acid method according to claim 3, characterized in that: The filter (15) is processed with a filtrate C (16), and the filtrate C (16) is a solution containing ethylenediaminetetraacetic acid. The lithium precipitation kettle (17) is connected to a sodium carbonate solution high-level tank (18).
Citation Information
Cited By
Device and method for preparing iron phosphate by using waste batteries
CN120229696A
An apparatus and method for preparing iron phosphate from waste batteries
CN120229696B