Composite asphalt pavement structural surface layer
By using a combination of modified asphalt composite layer and ultra-high performance concrete layer in asphalt pavement and combining gravel aggregate particle layer, the problem of poor mechanical strength of the asphalt pavement structural layer is solved, and the resistance to rut, water loss and Mechanical properties extend service life.
Patent Information
- Application Number
- CN202420257916.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-01
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2034-02-01
AI Technical Summary
The poor mechanical strength of the existing asphalt pavement structural layer leads to problems such as ruts, shear deformation and water damage, which affects service life and maintenance costs.
The composite asphalt pavement structure surface layer is adopted, including modified asphalt composite layer and ultra-high performance concrete layer. The modified asphalt composite layer has pores, and ultra-high performance concrete particles are poured into it, and a gravel aggregate particle layer is set between the two layers. , improve binding strength.
It improves the load-bearing capacity and fatigue service life of composite asphalt pavement, reduces the thickness of the surface layer, enhances the resistance to rut, water loss and mechanical properties, and extends the service life.
Smart Images

Figure CN221956454U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of composite pavement, and more specifically to a composite asphalt pavement structure surface layer. Background Art
[0002] Asphalt is a common pavement material for modern highways, and it has the characteristics of good driving comfort. At present, asphalt roads have a large traffic volume, heavy vehicles, frequent braking and starting, and are prone to rutting, shear deformation, water damage, etc. After the surface layer cracks, the erosion of asphalt pavement by rainwater will also cause serious early damage to the pavement, increase the maintenance cost, and affect the performance and service life of the pavement. Therefore, it is urgent to develop a new pavement structure with good anti-rutting performance, good water stability, good durability, and high bearing capacity.
[0003] Ultra-high performance concrete is a new type of cement-based composite material that was successfully developed by the French Bouygues Company at the end of the 20th century after high-strength and high-performance concrete. It is composed of well-graded fine aggregate (excluding coarse aggregate), cement, quartz powder, silica powder, high-efficiency water reducer, fiber, etc., and has ultra-high strength, low brittleness, high toughness, high impact resistance, excellent durability and broad application prospects.
[0004] Based on the performance advantages of ultra-high performance concrete itself, when addressing the above-mentioned shortcomings of traditional asphalt pavement, if the ultra-high mechanical properties, ultra-high density and high durability of ultra-high performance concrete can be used to improve the mechanical strength of asphalt pavement, it is expected to have broad market application prospects. However, the combination of ultra-high performance concrete and asphalt layer still needs further exploration. Utility Model Content
[0005] The utility model aims to overcome at least one defect of the above-mentioned prior art and provide a composite asphalt pavement structure surface layer for solving the problem of poor mechanical strength of the existing asphalt pavement structure layer.
[0006] The solution of the utility model is to provide a composite asphalt pavement structure surface layer, including a modified asphalt composite layer and an ultra-high performance concrete layer, wherein the modified asphalt composite layer and the ultra-high performance concrete layer are stacked up and down, wherein the modified asphalt composite layer has a plurality of pores, and the pores are all filled with ultra-high performance concrete particles.
[0007] The utility model also obtains a modified asphalt composite layer with high mechanical strength by pouring ultra-high performance concrete particles into the pores of the modified asphalt surface layer. Furthermore, by stacking the modified asphalt composite layer and the ultra-high performance concrete layer up and down, the bearing capacity and fatigue service life of the surface layer of the composite asphalt pavement structure are improved, and the overall thickness of the surface layer is reduced, so that the material consumption is reduced while also improving the anti-rutting performance and anti-water damage performance.
[0008] Furthermore, the thickness of the ultra-high performance concrete layer is 30 to 100 mm.
[0009] Furthermore, the thickness of the modified asphalt composite layer is 20 to 50 mm.
[0010] By adopting the thickness dimension set as above, the surface layer of the composite asphalt pavement structure can be made thinner and lighter, while also ensuring good mechanical properties.
[0011] Furthermore, the porosity of the modified asphalt composite layer is ≥30%.
[0012] This solution allows the modified asphalt composite layer to be combined with a sufficient amount of ultra-high performance concrete particles, thereby improving the rutting resistance and water damage resistance of the asphalt layer.
[0013] Furthermore, a crushed stone aggregate particle layer is provided, and the crushed stone aggregate particle layer is located between the modified asphalt composite layer and the ultra-high performance concrete layer.
[0014] Furthermore, the crushed stone aggregate particle layer is composed of a layer of crushed stone aggregate particles, each of which includes an upper particle part and a lower particle part, the upper particle part is embedded in the lower surface of the modified asphalt composite layer, and the lower particle part is embedded in the upper surface of the ultra-high performance concrete layer.
[0015] In this solution, the crushed stone aggregate plays the role of connecting the upper modified asphalt composite layer and the lower ultra-high performance concrete layer, which can improve the bonding strength between the modified asphalt composite layer and the ultra-high performance concrete layer, and improve the overall mechanical properties of the composite asphalt pavement structure surface layer.
[0016] Furthermore, the particle size of the crushed stone aggregate particles is 5 to 16 mm.
[0017] By setting the particle size range in this scheme, the upper part of the crushed stone aggregate particles exposed on the upper surface of the ultra-high performance concrete layer can be of moderate size, thereby ensuring good bonding strength between the ultra-high performance concrete layer and the modified asphalt composite layer.
[0018] Furthermore, the size of the upper portion of the particle is 1 / 3 to 1 / 2 of the particle size of the corresponding crushed stone aggregate particle.
[0019] Within the size range set in this scheme, the ultra-high performance concrete layer and the modified asphalt composite layer are firmly bonded, and the resulting composite asphalt pavement structure surface layer has optimal mechanical properties.
[0020] Furthermore, the particle size of the ultra-high performance concrete particles is ≤0.63 mm.
[0021] The ultra-high performance concrete particles of this scheme have better pore bonding with the modified asphalt composite layer, which can significantly improve the bonding strength between the asphalt material and the ultra-high performance concrete particles in the modified asphalt composite layer, thereby improving the rutting resistance, shear deformation resistance, water damage resistance of the modified asphalt composite layer and obtaining a higher bearing capacity, and can also appropriately reduce the thickness of the asphalt layer based on the improvement of mechanical strength.
[0022] Furthermore, the ultra-high performance concrete layer has the following parameters: compressive strength ≥ 120 MPa, and / or flexural strength ≥ 13 MPa, and / or shrinkage value ≤ 400 ppm, and / or thermal expansion coefficient ≤ 1.1*10 -5 / ℃.
[0023] The ultra-high performance concrete layer based on this solution can make the surface layer of the composite asphalt pavement structure have good mechanical strength.
[0024] Furthermore, the bonding interface between the ultra-high performance concrete and the modified asphalt composite layer has the following parameters: flexural strength ≥ 10 MPa, and / or thermal expansion coefficient ≤ 1.3*10 -5 / ℃, and / or, shear strength ≥3MPa, and / or, tensile strength ≥0.6MPa.
[0025] Based on the parameter setting of this scheme, it is possible to ensure a close bond between the ultra-high performance concrete and the modified asphalt composite layer, thereby improving the mechanical strength of the overall structure of the composite asphalt pavement structure surface layer.
[0026] Compared with the prior art, the beneficial effects of the utility model are as follows: the utility model utilizes the high mechanical properties, high density, high fatigue resistance and high durability of ultra-high performance concrete to improve the bearing capacity and fatigue service life of the composite asphalt pavement, reduce the overall thickness of the surface layer, reduce the material consumption, and at the same time improve the rutting resistance and water damage resistance, so that the composite asphalt pavement structure surface layer of the utility model has the characteristics of small overall thickness of the composite surface layer, good rutting resistance, good shear deformation resistance, good water damage resistance, good durability, high bearing capacity, long service life, etc., and can be suitable for new highways, temporary roads, road repair and other projects, and has a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a structural schematic diagram of the surface layer of the composite asphalt pavement structure of the utility model.
[0028] Figure 2 It is a schematic structural diagram of the ultra-high performance concrete layer of the utility model.
[0029] Figure 3 for Figure 1 A magnified schematic diagram of part A in the figure.
[0030] Reference numerals: ultra-high performance concrete layer 1 , modified asphalt composite layer 2 , ultra-high performance concrete particles 21 , crushed stone aggregate particle layer 3 , crushed stone aggregate particles 31 , particle upper portion 311 , particle lower portion 312 . DETAILED DESCRIPTION
[0031] like Figure 1-3 As shown, this embodiment first provides a composite asphalt pavement structure surface layer, including a modified asphalt composite layer 2 and an ultra-high performance concrete layer 1, wherein the modified asphalt composite layer 2 and the ultra-high performance concrete layer 1 are stacked up and down, wherein the modified asphalt composite layer 2 has a plurality of pores, and the pores are all filled with ultra-high performance concrete particles 21. In specific implementation, ultra-high performance concrete slurry can be poured into the surface of the modified asphalt surface layer, and the ultra-high performance concrete slurry can penetrate into the pores of the modified asphalt surface layer and solidify, so that the pores of the modified asphalt composite layer 2 can be filled with ultra-high performance concrete particles 21.
[0032] During specific implementation, the thickness of the ultra-high performance concrete layer 1 is 30 to 100 mm, and / or the thickness of the modified asphalt composite layer 2 is 20 to 50 mm. Based on this size setting, the surface layer of the composite asphalt pavement structure obtained can be relatively light and thin, and can also ensure good mechanical properties. In addition, in order to improve the performance of the modified asphalt layer 2, the modified asphalt layer 2 is an SBS modified asphalt layer, which can be specifically prepared using SBS modified asphalt. During specific construction, the modified asphalt surface layer is in a high temperature state during pouring, has adhesiveness, and can be adhesively bonded with the ultra-high performance concrete layer, thereby achieving a tight bond between the two hierarchical structures.
[0033] Preferably, the porosity of the modified asphalt composite layer 2 is ≥30%, so that the modified asphalt composite layer can be combined with a sufficient amount of ultra-high performance concrete particles to improve the anti-rutting performance and water damage resistance of the asphalt layer.
[0034] like Figure 1 As shown, a crushed stone aggregate particle layer 3 is also provided, and the crushed stone aggregate particle layer 3 is located between the modified asphalt composite layer 2 and the ultra-high performance concrete layer 1. In specific implementation, the crushed stone aggregate particle layer 3 is composed of a layer of crushed stone aggregate particles 31. Figure 2The crushed stone aggregate particles 31 each include an upper particle portion 311 and a lower particle portion 312, wherein the upper particle portion 311 is embedded in the lower surface of the modified asphalt composite layer 2, and the lower particle portion 312 is embedded in the upper surface of the ultra-high performance concrete layer 1. It can be understood that the crushed stone aggregate plays a role in connecting the upper modified asphalt composite layer 2 and the lower ultra-high performance concrete layer 1, which can improve the bonding strength between the modified asphalt composite layer 2 and the ultra-high performance concrete layer 1, and improve the overall mechanical properties of the composite asphalt pavement structure surface layer.
[0035] During implementation, the crushed stone aggregate particle layer 3 can be directly formed based on the upper surface of the ultra-high performance concrete layer 1. Specifically, a layer of etching retarder can be sprayed on the upper surface of the cast ultra-high performance concrete mixture to delay the solidification of the ultra-high performance concrete on the upper surface, and then the crushed stone aggregate particle layer 3 can be prepared by flushing the upper surface of the ultra-high performance concrete layer 1.
[0036] In a preferred embodiment, the particle size of the crushed stone aggregate particles 31 is 5 to 16 mm. Through testing, it is found that when the particle size range is within the range, the upper part 311 of the crushed stone aggregate particles 31 exposed on the upper surface of the ultra-high performance concrete layer 1 can be of moderate size, thereby ensuring good bonding strength between the ultra-high performance concrete layer 1 and the modified asphalt composite layer 2.
[0037] In addition, especially when the size of the upper part 311 of the particle is set to 1 / 3 to 1 / 2 of the particle size of the corresponding crushed stone aggregate particle 31, the bonding strength between the ultra-high performance concrete layer 1 and the modified asphalt composite layer 2 is high, which can make the mechanical properties of the surface layer of the composite asphalt pavement structure obtained optimal.
[0038] In specific implementation, the particle size of the ultra-high performance concrete particles 21 is ≤0.63mm, which can improve the bonding strength between the asphalt material and the ultra-high performance concrete particles 21 in the modified asphalt composite layer 2, thereby improving the rutting resistance, shear deformation resistance, water damage resistance of the modified asphalt composite layer 2 and obtaining a higher bearing capacity. It can also appropriately reduce the thickness of the asphalt layer based on the improvement of mechanical strength, and reduce the amount of raw materials used to a certain extent.
[0039] Specifically, the ultra-high performance concrete layer 1 is set to the following parameters: compressive strength ≥ 120 MPa, and / or flexural strength ≥ 13 MPa, and / or shrinkage value ≤ 400 ppm, and / or thermal expansion coefficient ≤ 1.1*10 -5 / ℃, so that the prepared composite asphalt pavement structure surface layer can have good mechanical strength.
[0040] In addition, the bonding interface between the ultra-high performance concrete and the modified asphalt composite layer 2 is set to the following parameters: flexural strength ≥ 10 MPa, and / or thermal expansion coefficient ≤ 1.3*10 -5 / ℃, and / or, shear strength ≥3MPa, and / or, tensile strength ≥0.6MPa, which can ensure the close bonding between the ultra-high performance concrete and the modified asphalt composite layer 2 and improve the mechanical strength of the overall structure of the composite asphalt pavement structure surface layer.
[0041] The following will further clearly and completely describe the technical solutions in the embodiments of the utility model in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the utility model, not all of the embodiments. Based on the embodiments of the utility model, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the utility model.
[0042] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.
[0043] Example 1
[0044] This embodiment provides a composite asphalt pavement structure surface layer, which includes an ultra-high performance concrete layer at the bottom and a modified asphalt composite layer at the top. The thickness of the ultra-high performance concrete layer is set to 30 mm, and the ultra-high performance concrete layer has a compressive strength of not less than 120 MPa, a flexural strength of not less than 13 MPa, a shrinkage value of not more than 400 ppm, and a thermal expansion coefficient of not more than 1.1*10 -5 / ℃. The modified asphalt composite layer is a surface layer of SBS modified asphalt mixture combined with ultra-high performance concrete particles. The maximum particle size of ultra-high performance concrete particles is 0.63mm. The grouting slurry used to form the ultra-high performance concrete particles has the following parameters: fluidity not less than 300mm, compressive strength not less than 100MPa, and expansion stress of 0.01-0.1MPa. The combined surface layer of the ultra-high performance concrete layer and the modified asphalt composite layer has a flexural strength of not less than 10MPa and a thermal expansion coefficient of not more than 1.3*10 -5 / ℃, the shear strength of the bonding interface between the ultra-high performance concrete layer and the modified asphalt composite layer shall not be less than 3MPa, and the tensile strength shall not be less than 0.6MPa.
[0045] There is also a crushed stone aggregate particle layer between the ultra-high performance concrete layer and the modified asphalt composite layer, and the crushed stone particle size is 5 to 16 mm. The pores of the upper SBS modified asphalt composite layer are filled with ultra-high performance concrete particles to improve the wear resistance, deformation resistance and high temperature shear deformation resistance of the SBS modified asphalt surface layer; the thickness of the SBS modified asphalt composite layer is 50 mm, which reduces the thickness of the surface asphalt layer.
[0046] Example 2
[0047] In this embodiment, the thickness of the ultra-high performance concrete layer is 100 mm, and the thickness of the modified asphalt composite layer is 50 mm. Other conditions are the same as those in Embodiment 1.
[0048] Example 3
[0049] In this embodiment, the thickness of the ultra-high performance concrete layer is 65 mm, and the thickness of the modified asphalt composite layer is 35 mm. In addition, other conditions are the same as those in Example 1.
[0050] Example 4
[0051] In this embodiment, the thickness of the ultra-high performance concrete layer is 30 mm, and the thickness of the modified asphalt composite layer is 20 mm. Other conditions are the same as those in Embodiment 1.
[0052] Comparative Example 1
[0053] refer to Figure 1-2 Compared with Example 1, this comparative example does not have a crushed stone aggregate particle layer 3, and other structures are consistent with Example 1.
[0054] Comparative Example 2
[0055] refer to Figure 1 , Figure 3 Compared with Example 1, the comparative example does not pour the ultra-high performance concrete particles 21 into the modified asphalt composite layer 2, and the other structures are consistent with those of Example 1.
[0056] Comparative Example 3
[0057] refer to Figure 1-2 Compared with Example 1, the size of the upper portion 311 of the crushed stone aggregate particle 31 in this comparative example is smaller than 1 / 3 of the particle size of the crushed stone aggregate particle 31, and the other structures are consistent with those in Example 1.
[0058] Comparative Example 4
[0059] refer to Figure 1-2 Compared with Example 1, the size of the upper portion 311 of the crushed stone aggregate particle 31 in this comparative example is larger than 1 / 2 of the particle size of the crushed stone aggregate particle 31, and the other structures are consistent with those in Example 1.
[0060] Test Case
[0061] The composite asphalt pavement structure surface layers prepared in implementation cases 1 to 4 and comparison cases 1 to 4 were cut and tested for bending, tensile and shear strengths. The experimental data are shown in Table 1.
[0062] Table 1
[0063]
[0064]
[0065] Result analysis: The asphalt pavement structure surface layer of comparative example 1 does not have a crushed stone aggregate particle layer 3, resulting in poor bonding between the modified asphalt composite layer 2 of the upper layer and the ultra-high performance concrete layer 1 of the lower layer. Therefore, the test results in Table 1 show that compared with Example 1, the bending strength, tensile strength and shear strength of comparative example 1 are greatly reduced;
[0066] Combination Figure 1 and Figure 3 It is understood that since the pores of the modified asphalt composite 2 of the comparative example 2 are not filled with the ultra-high performance concrete particles 21, the performance of the modified asphalt composite 2 is significantly reduced. Therefore, the test results in Table 1 show that compared with Example 1, the flexural strength, tensile strength, and shear strength are all reduced significantly;
[0067] Combination Figure 1 and Figure 2 It is understood that for the asphalt pavement structure surface layer of comparative example 3, since the size of the upper part 311 of the crushed stone aggregate particles 31 cannot reach 1 / 3 of the particle size of the crushed stone aggregate particles 31, the depth of the crushed stone aggregate particles 31 embedded in the lower surface of the modified asphalt composite 2 is insufficient, resulting in a decrease in the bonding force between the modified asphalt composite 2 and the ultra-high performance concrete layer 1. Therefore, the test results in Table 1 show that compared with Example 1, the flexural strength, tensile strength, and shear strength are all reduced significantly;
[0068] Combination Figure 1 and Figure 2 It is understood that since the size of the upper part 311 of the crushed aggregate particle 31 exceeds 1 / 2 of the particle size of the crushed aggregate particle 31, the depth of the crushed aggregate particle 31 embedded in the upper surface of the ultra-high performance concrete layer 1 is insufficient, resulting in a decrease in the strength of the crushed aggregate particle 31 bonded to the ultra-high performance concrete layer 1, which will also affect the bonding force between the modified asphalt composite 2 and the ultra-high performance concrete layer 1. Therefore, the test results in Table 1 show that compared with Example 1, the flexural strength, tensile strength, and shear strength are all significantly reduced.
[0069] refer to Figure 1-3A large number of tests have shown that the thickness of the ultra-high performance concrete layer 1, the thickness of the modified asphalt composite layer 2, the particle size of the crushed stone aggregate particles 31, and the size of the upper part 311 of the particles set in the utility model are all optimal parameters, so that the bonding performance of the ultra-high performance concrete layer 1 and the modified asphalt composite layer 2 is optimal, and the interface bonding strength between the ultra-high performance concrete layer 1 and the modified asphalt composite layer 2 is significantly improved. In particular, by pouring ultra-high performance concrete particles 21 into the pores of the modified asphalt composite layer 2 and setting the particle size of the ultra-high performance concrete particles 21 to ≤0.63mm, the mechanical properties of the modified asphalt composite layer can be significantly improved, thereby obtaining a composite asphalt pavement structure surface layer with better mechanical properties, especially improving the rutting resistance and water damage resistance of the composite asphalt pavement structure surface layer.
[0070] Obviously, the above embodiments are only examples for clearly explaining the technical solution of the utility model, and are not intended to limit the specific implementation methods of the utility model. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the claims of the utility model shall be included in the protection scope of the claims of the utility model.
Claims
1. A composite asphalt pavement structure surface layer, characterized in that: It comprises a modified asphalt composite layer and an ultra-high performance concrete layer, wherein the modified asphalt composite layer and the ultra-high performance concrete layer are stacked up and down, wherein the modified asphalt composite layer has a plurality of pores, and the pores are all filled with ultra-high performance concrete particles.
2. The composite asphalt pavement structure surface layer according to claim 1, characterized in that: The thickness of the ultra-high performance concrete layer is 30 to 100 mm.
3. The composite asphalt pavement structure surface layer according to claim 1, characterized in that: The thickness of the modified asphalt composite layer is 20-50 mm; and / or the porosity of the modified asphalt composite layer is ≥30%.
4. The composite asphalt pavement structure surface layer according to any one of claims 1 to 3, characterized in that: A crushed stone aggregate particle layer is also provided, and the crushed stone aggregate particle layer is located between the modified asphalt composite layer and the ultra-high performance concrete layer.
5. The composite asphalt pavement structure surface layer according to claim 4, characterized in that: The crushed stone aggregate particle layer is composed of a layer of crushed stone aggregate particles, each of which includes an upper particle part and a lower particle part. The upper particle part is embedded in the lower surface of the modified asphalt composite layer, and the lower particle part is embedded in the upper surface of the ultra-high performance concrete layer.
6. The composite asphalt pavement structure surface layer according to claim 5, characterized in that: The particle size of the crushed stone aggregate particles is 5 to 16 mm.
7. The composite asphalt pavement structure surface layer according to claim 5 or 6, characterized in that: The size of the upper part of the particle is 1 / 3 to 1 / 2 of the particle size of the corresponding crushed stone aggregate particle.
8. The composite asphalt pavement structure surface layer according to any one of claims 1 to 3, 5 to 6, characterized in that: The particle size of the ultra-high performance concrete particles is ≤0.63 mm.
9. The composite asphalt pavement structure surface layer according to any one of claims 1 to 3, 5 to 6, characterized in that: The ultra-high performance concrete layer has the following parameters: compressive strength ≥ 120 MPa, and / or flexural strength ≥ 13 MPa, and / or shrinkage value ≤ 400 ppm, and / or thermal expansion coefficient ≤ 1.1*10 -5 / ℃.
10. The composite asphalt pavement structure surface layer according to any one of claims 1 to 3, 5 to 6, characterized in that: The bonding interface between the ultra-high performance concrete and the modified asphalt composite layer has the following parameters: flexural strength ≥ 10 MPa, and / or thermal expansion coefficient ≤ 1.3*10 -5 / ℃, and / or, shear strength ≥3MPa, and / or, tensile strength ≥0.6MPa.