Composite magnetic field solidification structure treatment device
By using a composite magnetic field solidification tissue treatment device during the casting of magnesium alloy, and combining pulse and rotating magnetic fields to process the magnesium alloy, the problems of uneven composition and coarse structure of magnesium alloy are solved, and grain refinement and composition uniformization are achieved. Improves the strong plasticity and quality of the product.
Patent Information
- Application Number
- CN202420240697.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-01
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2034-02-01
AI Technical Summary
During the casting process, magnesium alloys are limited in their large-area applications due to uneven composition, thick structure, and poor fatigue resistance strength, and are especially prominent in rare earth magnesium alloys.
A composite magnetic field solidification tissue treatment device is used to apply a composite electromagnetic field to the metal melt to be processed in combination with a pulsed magnetic field and a rotating magnetic field. The grains are refined through stirring and Joule heat, and the components and temperature are uniformized to reduce segregation.
The grain refinement, structure uniformization and composition uniformization of magnesium alloy are achieved, which improves the strong plasticity and quality of the product, reduces overheating, and reduces segregation. It is greener and more efficient than traditional methods.
Smart Images

Figure CN222001829U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of metallurgy and metal material preparation, in particular to a composite magnetic field solidification tissue processing device. Background Art
[0002] Magnesium alloy is known as the "21st century green engineering material". It has low density and is one-third lighter than aluminum. It has higher strength than aluminum alloy. It is lightweight, anti-electromagnetic interference, good shielding performance, high strength, sound absorption, good thermal conductivity, corrosion resistance and other characteristics. It is widely used in automobiles, 3C electronic products, aerospace, national defense and other fields. However, due to its low stability of the original casting structure, coarse structure, poor fatigue strength and other factors, the large-scale application of magnesium alloy is limited. The casting process is the basis for obtaining ingots with stable chemical composition and uniform structure. Whether the casting method and process are appropriate is directly related to the quality of the ingot. In the die-casting production process, due to the large differences in the composition of the casting alloy and the solidification conditions of the casting, it is easy to cause defects such as uneven composition of the complex casting structure, coarse structure, cold shut and insufficient pouring. This is particularly prominent in alloys with a large proportion of solute elements such as rare earth magnesium alloys.
[0003] The inventors found that the unique penetration depth of the pulsed magnetic field is greater. Due to the instantaneous energy impact characteristics of the pulsed magnetic field, the effect on the solidification phase transformation behavior is particularly significant, and the inoculation treatment near the solidification point can refine the organization. The rotating magnetic field can improve the component segregation of alloy solidification, affect the fluid flow during the solidification process, change the heat conduction and material transfer, and help form a more uniform organizational structure. The use of a pulse-rotating composite electromagnetic field can achieve solute composition, temperature and flow control, thereby improving product quality in terms of organizational refinement, component homogenization, and defect control. Utility Model Content
[0004] The utility model aims to provide a composite magnetic field solidification structure processing device to solve the problems existing in the above-mentioned prior art and make the casting composition uniform and the grains refined.
[0005] To achieve the above purpose, the utility model provides the following solutions:
[0006] The utility model provides a composite magnetic field solidification tissue processing device, comprising: a processing chamber for containing or circulating a metal melt material to be processed, a pulse magnetic field generator and a rotating magnetic field generator;
[0007] A pulsed magnetic field generator, used for applying a pulsed magnetic field to the material to be processed in the processing chamber;
[0008] The rotating magnetic field generator is used to apply a rotating magnetic field to the material to be processed in the processing chamber.
[0009] Preferably, the effects of different duty cycles, different currents and different frequencies on the material to be processed under the action of a pulsed-rotating magnetic field are explored through orthogonal experiments, thereby obtaining the optimal process.
[0010] Preferably, the pulse magnetic field generator comprises a first copper coil and a pulse device power supply, the first copper coil is wound outside the processing chamber, and the pulse device power supply is electrically connected to the first copper coil.
[0011] Preferably, the rotating magnetic field generator includes a plurality of salient pole silicon steel yokes and a plurality of second copper coils, the plurality of salient pole silicon steel yokes are arranged outside the crucible and can rotate relative to the crucible, and on each of the salient pole silicon steel yokes, six coil windings of the same specification are wound by the second copper coil.
[0012] Preferably, the second copper coil on each of the salient pole silicon steel yokes is wound in 7 layers, with 8 turns in each layer, for a total of 56 turns.
[0013] Preferably, when working, the frequency of the pulse magnetic field generator is 20 Hz, the current is 100 A, and the duty cycle is 30%, and the frequency of the rotating magnetic field generator is 20 Hz, and the current is 100 A.
[0014] Compared with the prior art, the utility model has achieved the following technical effects:
[0015] The pulse-rotating composite magnetic field in the utility model affects the crystal nucleation and growth process by causing the melt to vibrate and stir and generating Joule heat to act on the alloy solidification process, thereby achieving the effect of grain refinement, reducing the superheat of the metal melt, promoting the uniformity of the liquid phase temperature field, and cooling as much as possible during the solidification process to reduce segregation. The Joule heat effect generated by the induced current caused by the pulse-rotating composite magnetic field in the melt can cause the primary phase dendrites to degenerate and even spheroidize the dendrites.
[0016] Compared with the traditional magnesium alloy casting grain refinement methods, such as adding refining agent, adding rare earth, accelerating cooling, etc., the utility model plays the role of grain refinement through electromagnetic regulation.
[0017] The utility model stirs the melt by pulse-rotating electromagnetic, stirs the slurry in a contactless manner, makes the slurry pollution-free, is more environmentally friendly than traditional stirring, reduces the superheat of the melt, promotes the uniformity of the liquid phase temperature field, cools as much as possible at the same time during the solidification process, and reduces component segregation.
[0018] The pulse-rotating magnetic field device in the utility model is simpler than other magnetic fields, and has an obvious refining effect on metal materials, so that the solidified primary phase grains are refined, the organizational components are homogenized, the secondary needle-shaped dendrites are spheroidized and refined, and the strength and plasticity thereof are increased.
[0019] The utility model explores the influence of different duty ratios, currents, frequencies, etc. on magnesium alloy under the action of a pulse-rotating magnetic field through orthogonal experiments, so as to obtain the optimal process. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the utility model or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the utility model. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 A schematic diagram of the structure of a composite magnetic field coagulation tissue treatment device provided by an embodiment of the utility model;
[0022] Figure 2 A schematic diagram of the structure of a rotating magnetic field generator in a composite magnetic field coagulation tissue treatment device provided by an embodiment of the utility model;
[0023] Figure 3 A schematic diagram of the structure of a pulsed magnetic field generator in a composite magnetic field coagulation tissue treatment device provided by an embodiment of the utility model;
[0024] Figure 4 A schematic diagram of numerical simulation and mesh division of a composite magnetic field coagulation tissue treatment device provided in an embodiment of the utility model;
[0025] Figure 5 The simulation results of the composite rotating magnetic field of the utility model are shown in FIG. (a) flow field of the longitudinal section of the melt, (b) flow field of the cross section of the melt;
[0026] Figure 6 The rare earth phase morphology of the alloy under different pulse duty ratios: (a) 0%; (b) 20%; (c) 40%; (d) 60%;
[0027] Figure 7 is the average length of the rare earth phase under different pulse duty ratios;
[0028] Figure 1 In the middle: 1-rotating device power supply; 2-pulsing device power supply; 3-second copper coil; 4-first copper coil; 5-melt; 6-processing chamber; 7-salient pole silicon steel yoke. Among them, 1, 3 and 7 form a rotating magnetic field generator; 2 and 4 form a pulsed magnetic field generator; DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the utility model to clearly and completely describe the technical solutions in the embodiments of the utility model. Obviously, the described embodiments are only part of the embodiments of the utility model, not all of the embodiments. Based on the embodiments in the utility model, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the utility model.
[0030] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.
[0031] The utility model provides a composite magnetic field coagulation tissue processing device, such as Figure 1 to Figure 4 As shown, it includes: a melt 5, a processing chamber 6, a pulsed magnetic field generator and a rotating magnetic field generator, wherein the processing chamber 6 is used to accommodate or circulate the material to be processed, that is, the melt 5; the pulsed magnetic field generator is used to apply a pulsed magnetic field to the material to be processed in the processing chamber 6; and the rotating magnetic field generator is used to apply a rotating magnetic field to the material to be processed in the processing chamber 6.
[0032] The utility model refines the grains through a composite magnetic field, stirs and pulses the melt through pulse-rotating electromagnetics, and performs contactless stirring of the slurry, making the slurry pollution-free. Compared with traditional stirring, it is greener, reduces the superheat of the melt, promotes the homogenization of the liquid phase temperature field, and tries to cool simultaneously during the solidification process to reduce component segregation.
[0033] In a preferred embodiment, orthogonal experiments are also performed to explore the effects of different duty cycles, different currents and different frequencies on the material to be processed under the action of a pulsed-rotating magnetic field, so as to obtain the optimal process.
[0034] In some embodiments, the pulse magnetic field generator includes a first copper coil 4 and a pulse device power supply 2 , the first copper coil 4 is wound outside the processing chamber 6 , and the pulse device power supply 2 is electrically connected to the first copper coil 4 .
[0035] In the preferred embodiment, the first copper coil 4 is a hollow structure, in which the cooling medium is passed. It can be understood that one end of the first copper coil 4 is an inlet and the other end is an outlet. Therefore, the utility model also needs to be equipped with a circulating cooling system. The circulating cooling system is connected to the first copper coil 4 and allows the cooling medium to circulate therein. When the cooling medium is conductive, the cavity in the first copper coil 4 needs to be insulated. It can be understood that the cooling medium can be a fluid that is not conductive or has weak conductivity.
[0036] In some embodiments, the rotating magnetic field generator includes a rotating device power supply 1, a plurality of salient pole silicon steel yokes 7 and a plurality of second copper coils 3. The plurality of salient pole silicon steel yokes 7 are arranged outside the crucible and can rotate relative to the crucible. On each salient pole silicon steel yoke 7, six coil windings of the same specification are wound by the second copper coil 3. The rotating device power supply 1 and each second copper coil 3 are electrically connected. The second copper coil 3 and the salient pole silicon steel yoke 7 are separated by an insulating material.
[0037] Specifically, the second copper coil 3 on each salient pole silicon steel yoke 7 is wound in 7 layers, each layer has 8 turns, and the total number of turns is 56.
[0038] In some embodiments, the processing chamber 6 can be a die-casting magnesium liquid quantitative transmission tube or a crucible in actual production. When the processing chamber 6 is a die-casting magnesium liquid quantitative transmission tube, a magnesium liquid smelting furnace and a die-casting machine are respectively provided at both ends of the die-casting magnesium liquid quantitative transmission tube.
[0039] In some embodiments, the absolute distance between the first copper coil 4 and the crucible should be maintained between 10 and 100 mm. If the distance is too far, it is easy to cause large magnetic loss, and if the distance is too close, the outer wall temperature is too high, causing the coil to burn.
[0040] In some embodiments, the first copper coil 4 is wound in 10 layers, each layer has 10 turns, and a total of 100 turns.
[0041] Figure 5 The simulation results of the composite rotating magnetic field of the utility model are shown in FIG. 1 ; (a) flow field of the longitudinal section of the melt, (b) flow field of the cross section of the melt.
[0042] The pulse magnetic field generator process is: frequency 20Hz, current 100A, duty cycle 30%, and the rotating magnetic field generator process is: frequency 20Hz, current 100A. The internal flow field diagram of the melt. Since the rotation speed is closely related to the crucible diameter, a crucible of 60mm can achieve uniform rotation stirring, and the maximum stirring speed can be 0.77m.
[0043] During operation, first turn on the rotating magnetic field generator to generate a rotating eddy current in the melt 5 in the processing chamber 6, so that the metal melt is evenly treated. After the temperature drops to the target temperature, turn off the rotating magnetic field generator, turn on the pulse magnetic field generator, adjust the appropriate parameters of the pulse device power supply 5, and subject the metal melt to electromagnetic pulse treatment for 1-5 minutes. The vibration stirring effect generated by the pulse magnetic field makes the temperature of the melt relatively uniform, thereby reducing the temperature of the melt.
[0044] The rotating electromagnetic field stirs the melt, and a stirring effect is generated in the melt by acting on the magnetic particles in the melt or the current in the liquid metal. This stirring can improve the uniformity of the melt temperature and composition, promote the mixing and heat transfer of the melt, and facilitate the solidification process.
[0045] The present invention uses specific examples to illustrate the principle and implementation of the present invention. The above examples are only used to help understand the method and core idea of the present invention. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
[0046] Specific Example 1: Effect of composite electromagnetic field on the second phase of rare earth magnesium alloy
[0047] In order to prevent the needle-like rare earth phase from agglomerating and causing segregation inside the crystal, which in turn causes grain boundary splitting and crystal defects, AZ91D-0.75La was selected as the pulsed magnetic field experimental material, and the influence of pulse duty ratio and pulse frequency in the pulsed magnetic field on its solidification structure and mechanical properties was studied.
[0048] Figure 6 and Figure 7 It is a statistical diagram of the alloy rare earth phase morphology and the average length of the needle-like rare earth phase under different pulse duty ratios. It can be seen from the figure that after applying the pulse magnetic field, the length of the needle-like rare earth phase Al2La is decreasing, and even tends to be spheroidized. As the pulse duty ratio gradually increases, the length of the needle-like rare earth phase Al2La also increases. When the pulse duty ratio is 20%, the average length of the needle-like rare earth phase Al2La decreases from 30.48μm when no electromagnetic field is applied to 14.42μm, and the effect of spheroidization of the needle-like compound is the best. However, the duty ratio will also affect the refinement of the primary phase structure. Combining the two, it is judged that a 30% duty ratio can achieve an ideal effect.
[0049] Specific Example 2: Effect of composite electromagnetic field on primary phase refinement and uniformity of tissue composition
[0050] The solidification experiment uses AZ91D alloy as the research object. After heating AZ91D magnesium alloy to 700℃, it is melted and kept warm for 10 minutes. Then the crucible is taken out and the surface oxide film is removed with a slag spoon, and then cast into the crucible for electromagnetic treatment until the sample is completely solidified. During this period, SF6 gas is used to protect the upper part of the crucible to prevent the magnesium alloy from oxidizing. The rotating electromagnetic field frequency parameter in the composite electromagnetic field is 20hz, the pulse electromagnetic field frequency parameter is 10hz, the duty cycle is 30%, and the current amplitude is set to 100A.
[0051] In order to compare the element segregation under different solidification conditions, ICP was used to determine the alloy element content. The relative deviations of the Al, Zn, and Mn element concentrations at the -1 / 2 radius of the ingot edge and between the edge and the center were calculated, and the results are shown in Table 1. It can be found that compared with the ingot solidified without a magnetic field, the homogenization degree of Al and Zn elements was improved after R-PEMP treatment.
[0052] Table 1 ICP element analysis results of ingot cross section
[0053]
Claims
1. A composite magnetic field coagulation tissue treatment device, characterized in that: include: a processing chamber for containing or circulating the material to be processed; A pulsed magnetic field generator, used for applying a pulsed magnetic field to the material to be processed in the processing chamber; The rotating magnetic field generator is used to apply a rotating magnetic field to the material to be processed in the processing chamber.
2. The composite magnetic field coagulation tissue treatment device according to claim 1, characterized in that: Through orthogonal experiments, the effects of different duty cycles, different currents and different frequencies on the material to be processed under the action of a pulsed-rotating magnetic field are explored to obtain the optimal process.
3. The composite magnetic field coagulation tissue treatment device according to claim 1, characterized in that: The pulse magnetic field generator comprises a first copper coil and a pulse device power supply, wherein the first copper coil is wound outside the processing chamber, and the pulse device power supply is electrically connected to the first copper coil.
4. The composite magnetic field coagulation tissue treatment device according to claim 1, characterized in that: The processing chamber is formed in the crucible, and the rotating magnetic field generator includes a plurality of salient pole silicon steel yokes and a plurality of second copper coils. The plurality of salient pole silicon steel yokes are arranged outside the crucible and can rotate relative to the crucible. On each of the salient pole silicon steel yokes, six coil windings of the same specification are wound by the second copper coil.
5. The composite magnetic field coagulation tissue treatment device according to claim 4, characterized in that: The second copper coil on each of the salient pole silicon steel yokes is wound in 7 layers, with 8 turns in each layer, for a total of 56 turns.
6. The composite magnetic field coagulation tissue treatment device according to claim 3, characterized in that: When working, the frequency of the pulse magnetic field generator is 20 Hz, the current is 100 A, and the duty cycle is 30%. The frequency of the rotating magnetic field generator is 20 Hz, and the current is 100 A.
Citation Information
Cited By
Composite magnetic field solidification structure treatment device and process thereof
CN118002765A