High-end metal blank preparation device combining suspension smelting and spray forming
By combining suspension smelting technology with jet forming technology, the problems of coarse grains and composition segregation when casting high-end metal materials are solved, and dense, high-purity high-end metal blanks are achieved, which is suitable for direct molding of high-temperature brittle materials, simplifying the Process flow and reduce manufacturing costs.
Patent Information
- Application Number
- CN202323290348.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-04
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2033-12-04
AI Technical Summary
When casting high-end metal materials, the ingot grains are coarse and the components are segregated, and there are defects such as shrinkage, pores, looseness and cracks. High-temperature brittle metals are prone to break during hot processing and cannot be formed directly.
Combining suspension smelting technology with jet forming technology, providing a metal liquid flow through suspension smelting equipment, spraying with high-pressure inert gas to form a solid/liquid atomization beam, solidify on the surface of the cooling substrate, forming a dense high-end metal blank, and The denseness of the material is further improved through thermal processing.
The preparation of high-end metal blanks with high purity, denseness and fine grains is achieved, which avoids defects in the traditional casting process and is suitable for direct molding of high-temperature brittle materials, simplifies the process flow and reduces manufacturing costs.
Smart Images

Figure CN222001858U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of metal smelting and forming, and in particular to a high-end metal blank preparation device combining suspension smelting and injection forming. Background Art
[0002] The development of modern technology depends on the development of various high-end metal materials. The suspension smelting technology can be used to smelt low-oxygen and high-purity materials. However, the ingots obtained by traditional casting technology often have coarse grains, segregated components, and almost all have defects such as shrinkage cavities, pores, looseness and cracks. In order to obtain shapes and sizes with specific requirements, most ingots need to undergo subsequent hot working and forming, and the material is densified by hot working, the cast structure is destroyed, and the grains are refined. However, the hot working procedure greatly increases the process links of the manufacturing process and increases the manufacturing cost. In addition, metals that are brittle at high temperatures will crack or break during the hot working process and cannot be formed by hot working. In view of these problems, a new technology needs to be developed, which can be directly formed after the smelting process, and the product has a dense material, fine grains, and a small degree of segregation, and can be made into a product after simple machining. The purpose of the utility model is to achieve such requirements by combining injection molding technology with suspension smelting technology. Utility Model Content
[0003] In view of the shortcomings of the prior art, the utility model proposes a solution to the technical difficulties of using suspension smelting equipment to provide a metal liquid flow for injection molding. The utility model combines suspension smelting technology with injection molding technology, so that the injection molding technology can be used to prepare billets of high-end materials. The suspension smelting-injection molding equipment is mainly composed of a cold crucible smelting device, an atomizing device and a solidifying device. The process of preparing the billet includes: using suspension smelting technology to form a liquid flow, using high-pressure inert gas to spray the liquid flow to form a solid / liquid two-phase atomized beam, and spraying the atomized beam onto the cooled substrate surface for solidification to form billets of rods, plates and pipes. Thermal processing methods can be used to further improve the density of the material. The billet obtained by this method has fine grains, low segregation, and dense material.
[0004] The utility model provides a high-end metal blank preparation device combining suspension smelting and injection molding, comprising a vacuum furnace body, a smelting device, an atomizing device and a curing device;
[0005] The vacuum furnace body includes a vacuum chamber, and the vacuum chamber is sequentially configured from top to bottom as a melting zone, an atomization zone, and a solidification forming zone;
[0006] The smelting device is installed in the smelting area, and includes a water-cooled copper crucible and an induction coil. The water-cooled copper crucible has a petal structure, and a cooling water path is arranged in each petal. The petals are filled with high-temperature resistant insulating materials. The induction coil is arranged to surround the water-cooled copper crucible, wherein a liquid flow hole is opened at the center of the bottom of the water-cooled copper crucible;
[0007] The atomizing device is installed in the atomizing area and below the water-cooled copper crucible, and includes a flow guide tube, a flow guide tube heater, a gas nozzle and a blowing gas source;
[0008] The guide tube is installed below the bottom of the water-cooled copper crucible, and the upper end is inserted into the liquid flow hole of the water-cooled copper crucible, and the lower end extends downward; an annular guide tube heater is arranged outside the guide tube; the nozzle is arranged around the guide tube, the blowing gas source is located outside the vacuum chamber, and the gas is sent into the vacuum chamber through the conduit and connected to the gas nozzle;
[0009] The curing device is installed below the nozzles in the curing and forming area and the atomizing area, and includes a base member, a base lifting mechanism and a forming driving mechanism;
[0010] Among them, the base member is located below the nozzle and faces the atomizing beam; the base lifting mechanism is installed below the vacuum chamber, and its lifting rod passes through the bottom of the vacuum chamber through the vacuum seal and extends into the vacuum chamber to support the base member; the forming drive mechanism drives the base member to move or rotate so that the blank can obtain different required shapes and sizes.
[0011] Furthermore, the smelting device also includes a crucible stand and a crucible moving mechanism to enable the water-cooled copper crucible to reciprocate in the horizontal direction, and to enable the liquid flow from the liquid flow hole to reciprocate, thereby generating a reciprocating scan of the atomized beam formed by the liquid flow;
[0012] The crucible stand is configured as a bracket for installing a water-cooled copper crucible, the induction coil is also installed on the crucible stand, and the induction coil and the crucible stand are insulated;
[0013] The crucible moving mechanism is installed outside the vacuum chamber, and its crucible driving rod is fixed to the crucible frame.
[0014] Furthermore, an induction coil is arranged around the guide tube to heat the molten metal in the guide tube by using a high-frequency electromagnetic field, and the induction coil applies an electromagnetic force to the molten metal to prevent the liquid flow from contacting the tube wall of the guide tube;
[0015] And / or, the flow guide tube and the induction coil surrounding it form an electromagnetic valve, and when the high-frequency power supply is cut off, the molten metal in the flow guide tube will immediately solidify to interrupt the liquid flow;
[0016] The guide pipe is made of copper tube and is divided into several petals of equal width along the length direction. A small hole is opened in each petal as a cooling water path. The water paths of adjacent petals are connected end to end to form an overall water path of the guide pipe.
[0017] Alternatively, the flow guide tube is made of a thin copper tube, and the thin copper tube is repeatedly bent into a plurality of mutually parallel arcuate segments, and the plurality of arcuate segments are then formed into a cylindrical flow guide tube around a center.
[0018] Further, the base member is plate-shaped, the base lifting mechanism and the molding drive mechanism are combined into one mechanism, and installed under the vacuum chamber, and configured to have the functions of lifting and rotating the plate-shaped base member;
[0019] Further, the base member includes a base plate and a track plate;
[0020] Wherein, the base plate is a plate-shaped device whose width and length meet the requirements of the slab size;
[0021] The track plate is arranged on the bottom surface of the base plate, and a track is arranged at the bottom of the track plate to limit the moving track of the base plate;
[0022] The lifting rod extends from the bottom of the chamber into the vacuum chamber, and its top end is engaged with the track at the bottom of the track plate;
[0023] The molding drive mechanism is installed on the side of the substrate plate along the length direction outside the vacuum chamber, and its first drive rod passes through the chamber wall through the vacuum dynamic seal and extends into the vacuum chamber in the horizontal direction, and is combined with the edge of the track plate;
[0024] Further, the base member is configured as a cylindrical mandrel, and the lifting rod is located below the mandrel to support the mandrel;
[0025] The molding drive mechanism is installed outside the side wall of the vacuum chamber along the length direction of the core rod, and its first drive rod extends into the vacuum chamber through the vacuum seal and combines with the end of the core rod. The molding drive mechanism is configured to have the function of driving the core rod to rotate and move in the direction away from the nozzle.
[0026] Furthermore, the track under the track plate should be configured in a zigzag or bow shape;
[0027] Wherein, a transverse driving mechanism is arranged on the side of the vacuum chamber along the width direction of the substrate plate, and drives the track plate to move through a second driving rod that moves transversely.
[0028] Furthermore, a crucible cover is provided at the upper end of the water-cooled copper crucible, and the crucible cover is provided with an inflation tube connected to an outdoor inert gas source, so that a closed space is formed inside the water-cooled copper crucible, so as to apply gas pressure to the molten metal pool in the water-cooled copper crucible, pressurize the liquid flow, and control the flow rate of the liquid flow.
[0029] Furthermore, the angle α formed by the gas ejected from the nozzle orifice is called the injection angle, wherein the injection angle is configured to be 10 to 100°;
[0030] And / or, the injection pressure is configured to be 0.1 to 30 MPa.
[0031] Furthermore, the smelting device also includes water-cooled electrodes, cables and an induction power supply;
[0032] The water-cooled electrode is installed in the electrode interface tube of the vacuum chamber wall and is insulated from the chamber wall;
[0033] The part of the water-cooled electrode in the vacuum chamber is connected to the induction coil, and the part outside the vacuum chamber is connected to the induction power supply through a cable.
[0034] The advantages of the utility model compared with the prior art are:
[0035] 1. During the injection molding process, the atomized beam of solid / liquid phases rapidly cools and solidifies on the surface of the cooled substrate. The resulting billet has fine grains, almost no segregation of components, dense material, and no metallurgical defects such as shrinkage cavities, pores, and looseness inside;
[0036] 2. For materials that are severely brittle at high temperatures and cannot be subjected to thermal processing, the suspension melting-injection molding technology can be used to directly produce high-quality products;
[0037] 3. The utility model uses suspension smelting technology to provide metal liquid flow for the injection molding process. The smelted metal is smelted in a water-cooled copper crucible, eliminating the pollution of the crucible material to the molten pool, so it can maintain a high purity. This design enables the injection molding technology to be applied in the field of high-end materials;
[0038] 4. The utility model is designed with a crucible cover and other devices for suspension smelting, which form a sealed structure for the crucible and provide conditions for regulating the speed of the sprayed liquid flow by gas pressure;
[0039] 5. The utility model designs a crucible moving device, which can be used to make the liquid flow scan back and forth horizontally, thereby increasing the width and uniformity of the atomized deposition layer;
[0040] 6. The design of the flow guide tube in the injection molding device using the suspension smelting technology is a technical problem. Under the condition of using a hot crucible, the liquid flow can be directly drawn out from the bottom or side openings of the crucible. Under the condition of suspension smelting, the molten metal will be cooled and solidified by the crucible wall at the opening of the crucible, and the liquid flow cannot be drawn out. Although the heated flow guide tube can draw out the liquid flow, various flow guide tubes will have a certain pollution effect on the liquid flow, which will cause some loss in the effect of suspension smelting to eliminate pollution. The electromagnetic flow guide tube designed by the utility model is completely pollution-free, which solves this technical problem. In addition, this flow guide tube also has the function of a freezing valve, because it can interrupt or resume the injection molding process at any time. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1This is a diagram of the structure inside the vacuum chamber;
[0042] Figure 2 This is a structural diagram of the smelting device;
[0043] Figure 3 The figure is a structural diagram of the atomization device;
[0044] Figure 4 This is a structural diagram of the electromagnetic flow guide tube made by cutting copper tube;
[0045] Figure 5 for Figure 4 Sectional view at AA;
[0046] Figure 6 This is a structural diagram of an electromagnetic flow guide tube made by bending a thin copper tube with a square cross section;
[0047] Figure 7 The schematic diagram is that the metal liquid in the electromagnetic flow guide tube is restrained by electromagnetic force to form a very thin liquid flow;
[0048] Figure 8 A structural diagram of a solidification device for preparing a rod blank;
[0049] Fig. 9 A structural diagram of a curing device for preparing a slab;
[0050] Fig.10 The schematic diagram of the "zigzag" track on the bottom of the track disk;
[0051] Fig.11 The schematic diagram of the "bow-shaped" track on the bottom of the track disk;
[0052] Fig.12 A top view of a curing device of a molding drive mechanism;
[0053] Fig.13 This is a structural diagram of the solidification device for preparing tube blanks.
[0054] Figure numerals: 1-vacuum furnace body, 2-melting device, 3-atomizing device, 4-curing device, 5-vacuum chamber, 6-melting area, 7-atomizing area, 8-curing molding area, 9-molten pool, 10-water-cooled copper crucible, 11-induction coil, 12-water-cooled electrode, 13-cable, 14-induction power supply, 15-crucible rack, 16-crucible moving mechanism, 17-liquid flow hole, 18-crucible cover, 19-inflating tube, 20-electrode interface cylinder, 21-crucible driving rod, 22-track, 23-atomizing beam, 24-guide tube, 25-guide tube heater, 26-nozzle, 2 7-blowing gas source, 28-nozzle, 29-injection angle, 30-conduit, 31-deposition layer, 32-blank, 33-substrate, 34-substrate lifting mechanism, 35-forming drive mechanism, 36-lifting rod, 37-substrate plate, 38-track disk, 39-track, 40-first drive rod, 41-slab, 42-transverse drive mechanism, 43-second drive rod, 44-core rod, 45-tube, 46-petal, 47-small hole, 48-integral water channel, 49-thin copper tube, 50-bow section, 51-induction coil, 52-electromagnetic force, 53-liquid flow. DETAILED DESCRIPTION
[0055] Combined with Figure 1-13 As shown, this embodiment provides a high-end metal billet preparation device combining suspension melting and injection molding, including a vacuum furnace body 1, a melting device 2, an atomizing device 3, a solidification device 4 and an auxiliary device.
[0056] Among them, combined Figure 1 As shown, the vacuum furnace body 1 includes a vacuum chamber 5, a vacuum unit and a gas filling system. Specifically, the vacuum chamber 5 is divided into three areas from top to bottom: a melting area 6, an atomizing area 7 and a solidification molding area 8, so as to provide installation and operation conditions for the melting device 2, the atomizing device 3 and the solidification device 4 respectively; the vacuum unit and the gas filling system are configured to establish a vacuum condition or a protective atmosphere condition in the vacuum chamber 5, and the gas filling system can use an inert gas, and the preferred inert gas is argon.
[0057] Combination Figure 2 As shown, the smelting device 2 is installed in the smelting area 6 of the vacuum chamber 5, and is configured to melt the solid material to form a molten pool 9. Specifically, the smelting device 2 includes a water-cooled copper crucible 10, an induction coil 11, a water-cooled electrode 12, a cable 13, an induction power supply 14, a crucible stand 15 and a crucible moving mechanism 16.
[0058] Specifically, the water-cooled copper crucible 10 is installed in the smelting area 6 of the vacuum chamber 5, and has a petal structure, in which a cooling water path is provided in each petal, and high-temperature resistant insulating materials are filled between the petals, so that the side wall of the water-cooled copper crucible 10 has sealing properties, thereby using the suspension smelting technology to provide pollution-free molten metal to the injection process. In order to achieve liquid injection, a liquid flow hole 17 is opened at the center of the bottom of the water-cooled copper crucible 10; in order to prepare a billet with a larger width, more than two liquid flow holes 17 can be provided at the bottom of the water-cooled copper crucible 10.
[0059] The upper end of the water-cooled copper crucible 10 is provided with a crucible cover 18, and the crucible cover 18 is provided with a gas charging pipe 19 connected to an outdoor inert gas source, so that after the metal in the water-cooled copper crucible 10 is melted, the inert gas is charged into the water-cooled copper crucible 10, and the flow rate of the molten metal flowing out of the water-cooled copper crucible 10 can be changed by adjusting the gas pressure in the water-cooled copper crucible 10. Preferably, the gas pressure is controlled in the range of 0.03MPa to 0.5MPa.
[0060] The crucible cover 18 can be made of high temperature resistant ceramic materials, such as alumina, magnesium oxide, zirconium oxide and other ceramic materials, or graphite or refractory metals. In this case, the crucible cover 18 needs to be slit to ensure that the magnetic lines of force pass through. The crucible cover 18 can also be made of a plate-like copper material with a petal structure, and a water channel structure for cooling water is made in each petal. A sealing structure is set between the crucible cover 18 and the upper port of the water-cooled copper crucible 10. The crucible cover 18 can be used to form a sealing structure for the water-cooled copper crucible 10, so that the design of regulating the liquid flow velocity by gas pressure becomes possible.
[0061] The induction coil 11 is configured as a copper water-cooled solenoid disposed around the water-cooled copper crucible 10, and the water-cooled electrode 12 is installed in the electrode interface tube 20 of the wall of the vacuum chamber 5 and is insulated from the wall. The part of the water-cooled electrode 12 in the vacuum chamber 5 is connected to the induction coil 11, and the part outside the vacuum chamber 5 is connected to the induction power supply 14 through the cable 13.
[0062] The crucible stand 15 is configured as a bracket for installing the water-cooled copper crucible 10, and the induction coil 11 is also installed on the crucible stand 15, and the induction coil 11 is insulated from the crucible stand 15. When the width of the blank is large, it is necessary to set a crucible moving mechanism 16 so that the water-cooled copper crucible 10 can be driven to move back and forth, so that the liquid flow flowing out of the liquid flow hole 17 moves back and forth, and then the atomization beam 23 formed by the liquid flow produces a reciprocating scanning effect. The crucible moving mechanism 16 is installed outside the vacuum chamber 5, and its crucible driving rod 21 is fixed to the crucible stand 15. In order to ensure the stability of the movement of the water-cooled copper crucible 10, the crucible stand 15 can also be installed on the track 22 in the vacuum chamber 5. When the crucible moving mechanism 16 is started, the crucible stand 15 drives the water-cooled copper crucible 10 and the induction coil 11 to move back and forth. In order to enable the induction coil 11 to have the ability to move, a dynamic seal is used at the position where the water-cooled electrode 12 is installed in the electrode interface tube 20.
[0063] Please continue reading Figure 3 The atomizing device 3 is a device for breaking up the liquid flow flowing out of the water-cooled copper crucible 10 to form an atomized beam 23. It is installed in the atomizing area 7 of the vacuum chamber 5 and below the water-cooled copper crucible 10, and includes a guide tube 24, a guide tube heater 25, a gas nozzle 26 and a blowing gas source 27.
[0064] Specifically, the guide tube 24 is a pipe for guiding the molten metal in the water-cooled copper crucible 10 to flow downward into the atomization zone 7. The guide tube 24 is installed below the bottom of the water-cooled copper crucible 10, and the upper end is inserted into the liquid flow hole 17 of the water-cooled copper crucible 10, and the lower end extends downward. Preferably, the inner diameter of the guide tube 24 is configured to be 1 to 30 mm, and the preferred inner diameter is configured to be 3 to 10 mm; along the height direction of the guide tube 24, its inner diameter can be the same or different, for example, the inner diameter of the upper end is small, and the inner diameter of the lower end is large.
[0065] In order to prevent the molten metal from solidifying in the guide tube 24, an annular guide tube heater 25 is provided outside the guide tube 24. It should be noted that, according to the melting point of the smelted metal, the guide tube heater 25 can be a resistance heater or an induction heater; the guide tube 24 is made of a material with high stability to the molten metal, for example: graphite can be used for metals such as copper, aluminum, and magnesium; quartz can be used for silicon; corundum, magnesium oxide, boron nitride ceramics or refractory metals can be used for iron-based, nickel-based and cobalt-based alloys; zirconium oxide-yttrium oxide membrane shells or refractory metals can be used for titanium alloys. Among them, when an induction heater is used as the guide tube heater 25, if a non-metallic guide tube 24 is used, a metal induction tube needs to be put on the outside of the guide tube 24 to heat the guide tube 24.
[0066] It is understandable that the above-mentioned graphite, ceramic or metal flow guide tube 24 will always cause slight pollution to the liquid flow. In order to completely eliminate the pollution caused by the flow guide tube 24, this embodiment designs a completely pollution-free electromagnetic flow guide tube 24.
[0067] like Figure 4-5 As shown, as an embodiment of the present invention, the electromagnetic flow guide tube 24 is made of a copper tube, which is divided into a number of petals 46 of equal width along the length direction. A small hole 47 is opened in each petal 46 as a cooling water path, and the water paths of adjacent petals 46 are connected end to end to form an overall water path 48 of the flow guide tube 24.
[0068] like Figure 6 As shown, as another embodiment, the electromagnetic flow guide tube 24 is made of a thin copper tube 49. Specifically, the thin copper tube is repeatedly bent into a plurality of arcuate segments 50 parallel to each other, and the plurality of arcuate segments 50 are then formed into a cylindrical flow guide tube 24 around a center, and each arcuate segment 50 is equivalent to a petal.
[0069] Combined with Figure 4-7 The inner diameter of the electromagnetic flow guide tube 24 is configured to be 2 to 30 mm, and the number of petals is configured to be 2 to 20 mm, and the number of petals increases with the increase of the tube diameter. In addition, an induction coil 51 is arranged around the electromagnetic flow guide tube 24. On the one hand, the induction coil 51 uses a high-frequency electromagnetic field to heat the molten metal in the tube, and on the other hand, the induction coil 51 applies an electromagnetic force 52 to constrain the molten metal into a very thin liquid flow 53. Therefore, the liquid flow 53 can maintain a high temperature because it does not contact the tube wall, and also eliminates the pollution caused by the tube wall.
[0070] Preferably, the frequency of the high-frequency power supply generating the electromagnetic field is configured to be 100 to 1000 kHz, and the smaller the pipe diameter, the higher the required frequency. When the high-frequency power supply is cut off, the molten metal in the pipe will be immediately frozen and solidified by the cooling water in the flow guide tube, interrupting the liquid flow and producing the effect of a freezing valve; if the injection molding process is required to continue, the high-frequency power supply can be restored to melt the solidified metal in the flow guide tube, so that the electromagnetic flow guide tube 24 can be used to prepare multiple injection-molded blanks using the molten pool of a water-cooled copper crucible 10.
[0071] Please continue reading Figure 3The nozzle 26 is arranged around the guide tube 24, and its structure includes annular gap type, annular hole type, V-type and Laval type. The angle α formed by the gas ejected from the nozzle 28 of the nozzle 26 is called the injection angle 29. Increasing the injection angle 29 can reduce the particle size of the atomized particles, but it is easy for the atomized particles to flow back to the nozzle 28 and cause blockage. Reducing the injection angle 29 can reduce the tendency of particle backflow and prevent the nozzle 28 from being blocked. The injection angle of this embodiment is configured to be 10 to 100°, and the preferred range is 20 to 50°. The relative position of the nozzle of the guide tube 24 to the nozzle 28 also needs to be adjusted. The nozzle forward can improve the atomization effect, but it will increase the tendency to block the nozzle 26.
[0072] The blowing gas source 27 uses high-pressure gas, and the most commonly used gases are nitrogen and argon. Specifically, the blowing gas source 27 is located outside the vacuum chamber 5, and the gas is sent into the vacuum chamber 5 through the conduit 30 and connected to the gas nozzle 26; the injection pressure is configured to be 0.1-30MPa, and the preferred pressure range is 0.3-3MPa. When the liquid flow 53 is formed in the guide tube 24 below the water-cooled copper crucible 10, the valve of the blowing gas source 27 is opened, so that the high-pressure gas is ejected from the nozzle 28 of the nozzle to impact the liquid flow 53, breaking the liquid into fine droplets to form an atomized beam 23, and the atomized beam 23 is cooled during the downward spraying process, and some droplets solidify into solid particles, and the atomized beam 23 forms a liquid-solid two-phase state.
[0073] Combination Figure 8-9 As shown in 12-13, the curing device 5 of this embodiment is a device that receives the atomized beam 23 and solidifies it into a solid deposition layer 31 and forms it into a blank 32 that meets geometric requirements, and is installed below the curing and molding area 8 and the atomizing area nozzle 26 of the vacuum chamber 5. The curing device 5 includes a base member 33, a base lifting mechanism 34 and a molding drive mechanism 35.
[0074] Specifically, the base member 33 is located below the nozzle 26 and faces the atomizing beam 23. It is made of metal material, mostly copper material; in order to speed up the cooling speed, water cooling can be passed through the base member 33. The base lifting mechanism 34 is installed below the vacuum chamber 5, and its lifting rod 36 passes through the bottom of the vacuum chamber 5 through the vacuum seal to extend into the vacuum chamber 5 to support the base member 33, which has the function of adjusting the distance between the base member 33 and the nozzle 26. By changing the distance between the base member 33 and the nozzle 26, the atomizing beam 23 can achieve different strokes before contacting the base member 33, obtain different degrees of temperature drop, and change the ratio of solid / liquid particles in the atomizing beam 23. Among them, increasing the distance can increase the proportion of solid particles. The molding drive mechanism 35 drives the base member 33 to move or rotate, so that the blank obtains different required shapes and sizes.
[0075] It is worth noting that for different forms of blanks, such as rod blanks, plate blanks or tube blanks, the solidification device 4 has different structural configurations:
[0076] Attached Figure 8 The structure of the curing device 4 for preparing the rod blank is shown. The base member 33 is plate-shaped. According to the requirements of the cross-sectional shape of the rod blank, the plate-shaped base member 33 adopts a circular plate, a square plate, a rectangular plate or other plate-shaped devices. Among them, the base lifting mechanism 34 and the forming drive mechanism 35 are combined into one mechanism, and are installed under the vacuum chamber 5, which has the functions of lifting and rotating the plate-shaped base member 33; the lifting rod 36 extends from the bottom of the chamber into the vacuum chamber 5 and combines with the plate-shaped base member 33. The lifting action of the lifting rod 36 not only has the function of adjusting the distance between the plate-shaped base member 33 and the nozzle 26, but also has the function of making the rod blank obtain the required length. As the height of the plate-shaped base member 33 is lowered, the length of the rod blank increases; the function of the rotation of the plate-shaped base member 33 is to make the deposition process of the atomized beam 23 on the surface of the plate-shaped base member 33 more uniform.
[0077] It should be noted that, in conjunction with the Figure 1 In order to prepare a rod blank with a larger width, a crucible moving mechanism 16 is required. Its function is to drive the water-cooled copper crucible 10 to move back and forth, so that the liquid flow flowing out of the liquid flow hole 17 moves back and forth, and the atomization beam 23 formed by the liquid flow 53 produces a reciprocating scanning effect, thereby increasing the area of the deposition layer 31 and improving the uniformity of the deposition layer.
[0078] Attached Fig. 9 The structure of the curing device 4 for preparing the slab is shown, the base member 33 includes a base plate 37 and a track plate 38, wherein the base plate 37 is a plate-shaped device whose width and length meet the slab size requirements; the track plate 38 is arranged on the bottom surface of the base plate 37, and a track 39 is arranged at the bottom of the track plate 38 to limit the moving track of the base plate 37. The lifting rod 36 of the base lifting mechanism 34 installed under the vacuum chamber 5 extends from the bottom of the chamber into the vacuum chamber 5, and its top end is engaged with the track 39 at the bottom of the track plate 38. The molding drive mechanism 35 is installed on the side of the base plate 37 along the length direction outside the vacuum chamber 5, and its first drive rod 40 extends into the vacuum chamber 5 in the horizontal direction through the chamber wall through the vacuum dynamic seal, and is combined with the edge of the track plate 38.
[0079] Therefore, before atomization begins, the substrate lifting mechanism 34 first raises the track disc 38 and the substrate plate 37 to a height suitable for injection, and then makes the first driving rod 40 of the forming drive mechanism 35 engage with the end of the substrate plate 37, and pushes the front section of the substrate plate 37 to the bottom of the nozzle 26; after atomization begins, when the deposition layer 31 is formed at the front end of the substrate plate 37 and the thickness reaches the requirement of the slab, the forming drive mechanism 35 slowly pulls the track disc 38, so that the substrate plate 37 moves in the direction of the forming drive mechanism 35, and the length of the slab 41 gradually increases until the slab covers the entire substrate plate 37, forming a complete slab 41. During the movement of the substrate plate 37, the top end of the lifting rod 36 is always engaged with the track 39, maintaining the supporting effect of the lifting rod 36 on the substrate plate 37.
[0080] It is worth mentioning that please refer to Figure 10-11 For slabs with a larger width, the track plate 38 is required to move the base plate 37 along the length direction of the base plate 37 (hereinafter referred to as "longitudinal"), and the base plate 37 is also required to move back and forth along the width direction of the base plate 37 (hereinafter referred to as "lateral") . To this end, the track 39 under the track plate 38 should be configured in a zigzag or bow shape. Therefore, during the spraying process, the track plate 38 moves back and forth along the lateral direction with the base plate 37 while moving longitudinally, forming a zigzag movement trajectory; or first move laterally along the base plate 37, then move a certain distance longitudinally, then move in the opposite width direction, and then move a certain distance longitudinally, forming an arched movement trajectory.
[0081] Preferably, Fig.12 As shown, in order to realize the above-mentioned moving trajectory, in addition to setting the molding drive mechanism 35 on the side of the vacuum chamber 5 along the length direction of the base plate 37, a transverse drive mechanism 42 is also set on the side of the vacuum chamber 5 along the width direction of the base plate 37, which drives the track plate 38 to move through the second transversely moving drive rod 43; the molding drive mechanism 35 and the transverse drive mechanism 42 operate according to the set program to enable the base plate 37 to achieve the required moving trajectory.
[0082] It is understandable that, combined with Figure 2 As shown, when making a slab with a larger width, it is not necessary to set up the lateral drive mechanism 42 separately. The crucible moving mechanism 16 can be used to make the water-cooled copper crucible 10 move back and forth while the base plate 37 moves longitudinally, so that the liquid flow flowing out of the liquid flow hole 17 moves back and forth, and the atomization beam 23 formed by the liquid flow 53 produces a lateral reciprocating scanning effect on the base plate 37, thereby increasing the width of the deposition layer.
[0083] Attached Fig.13The structure of a curing device 4 for preparing a tube blank is shown, wherein a base member 33 is configured as a cylindrical core rod 44, and its diameter is designed according to the inner diameter of a tube blank 45 to be produced; a lifting rod 36 of a base lifting mechanism 34 is located below the core rod 44 to support the core rod, and its joint portion has a structure that allows the core rod 44 to move and rotate on its surface; a forming drive mechanism 35 is installed on the outside of the side wall of a vacuum chamber 5 along the length direction of the core rod, and its first driving rod 40 extends into the vacuum chamber 5 through a vacuum seal to be combined with the end of the core rod, and the forming drive mechanism 35 has the function of driving the core rod to rotate and move in a direction (longitudinal) away from the nozzle 26.
[0084] Therefore, before the atomization process is started, the core rod 44 is raised to a suitable height by using the lifting rod 36, the end of the core rod is fixed by the end of the first driving rod 40, and the end of the core rod is pushed to a suitable position under the nozzle 26; after the injection process is started, the driving mechanism is started to rotate the core rod so that the atomized beam formed by the injection forms a cylindrical deposition layer with uniform thickness along the surface of the core rod. After the thickness of the deposition layer reaches the thickness requirement of the tube blank 45, the driving mechanism is used to drive the core rod to move slowly in the direction away from the nozzle, and the moving speed is based on the thickness that the deposition layer can achieve; the injection and molding process continues until a tube blank 45 with a length that meets the requirements is formed on the core rod.
[0085] The auxiliary device of this embodiment includes a cooling system and a control system. The cooling system provides cooling and propulsion for the water-cooled copper crucible 10 and the induction coil 11, the nozzle 26, the base member 33, the vacuum chamber 5, the induction power supply 14 and the vacuum unit for suspension smelting; the control system provides control conditions for the smelting process, the atomization process, the solidification process, the induction power supply 14, the vacuum unit and the cooling system.
[0086] It should be noted that the density of the blank formed by the injection molding technology can be improved by hot processing processes such as forging, rolling, and extrusion. For blanks that are brittle at high temperatures, hot processing is required under the condition of three-dimensional compressive stress, such as hot isostatic pressing technology.
[0087] The present invention provides some specific embodiments to better understand the present invention:
[0088] Embodiment 1:
[0089] The suspension melting-spray forming equipment of this embodiment is used to prepare the blank of the rod material. It consists of five parts: a vacuum furnace body 1, a melting device 2, an atomizing device 3, a curing device 4 and an auxiliary device ( Figure 1 ).
[0090] The vacuum furnace body consists of a vacuum chamber 5, a vacuum unit and an argon filling system. The inner diameter of the vacuum chamber is 2000mm and the height is 2400mm. The vacuum chamber is divided into three areas from top to bottom: melting area 6, atomization area 7 and solidification molding area 8 ( Figure 1 ).
[0091] The smelting device 2 is installed in the smelting area 6 of the vacuum chamber 5, and is composed of a water-cooled copper crucible 10, an induction coil 11, a water-cooled electrode 12, a cable 13, an induction power supply 14, a crucible stand 15 and a crucible moving mechanism 16 ( Figure 2 ). The inner diameter of the water-cooled copper crucible is 240 mm. It has a petal structure, and there is a cooling water path in each petal. A liquid flow hole 17 is provided at the center of the bottom of the crucible. A crucible cover 18 is provided at the upper end of the crucible. The crucible cover is provided with a gas filling pipe 19. The gas filling pipe is combined with an outdoor argon gas source to apply pressure to the molten pool after the metal is melted, so that the molten metal is ejected from each liquid flow hole. The pressure of the argon gas is controlled to be 0.05MPa.
[0092] The induction coil 11 is a copper water-cooled solenoid arranged around the crucible. The water-cooled electrode 12 is installed in the electrode interface tube 20 of the vacuum chamber wall and is insulated from the chamber wall. The part of the electrode inside the chamber is connected to the induction coil 10, and the part outside the chamber is connected to the induction power supply 14 through the cable 13 ( Figure 2 ), the power of the power supply is 1000kW.
[0093] The crucible stand 15 is a support for installing the crucible. The induction coil is also installed on the crucible stand, but it is insulated from the crucible stand ( Figure 2 ).
[0094] The atomizing device 3 is a device for breaking up the liquid flow removed from the crucible to form an atomized beam 23. It is installed in the atomizing area 7 of the vacuum chamber 5, below the crucible 10, and is composed of a guide tube 24, a guide tube heater 25, a gas nozzle 26, and a blowing gas source 27. Figure 3 ). The upper end of the copper electromagnetic flow guide tube 24 with a petal structure is inserted into the liquid flow hole 17 of the crucible, and the inner diameter is 8 mm. An annular induction coil 25 is arranged outside the flow guide tube. A Laval type nozzle 26 is arranged around the flow guide tube 24, and the spray angle 29 is selected to be 45°.
[0095] The blowing gas 27 is argon, which is sent into the vacuum chamber through the conduit 30 and connected to the gas nozzle 26. The injection pressure is controlled at 5MPa. When the liquid flow is formed in the guide tube below the crucible, the valve of the blowing gas is opened to allow the high-pressure gas to be ejected from the nozzle of the nozzle to impact the liquid flow, breaking the liquid into fine droplets to form an atomized beam 23. The atomized beam cools during the downward injection process, and some droplets solidify into solid particles, and the beam becomes a liquid-solid two-phase atomized beam.
[0096] This embodiment uses a curing device 5 for preparing rods, which is installed in the curing molding area 8 of the vacuum chamber 5, below the nozzle 26 in the atomization area. The device consists of a base member 33, a base lifting and rotating mechanism 34 ( Figure 4 ). The substrate 33 is located below the nozzle and faces the atomizing beam 23. It is made of copper, has a round cross section, a diameter of 120 mm, and is cooled by water inside. The substrate lifting and rotating mechanism is installed below the vacuum chamber. Its lifting rod 36 passes through the bottom of the chamber through the vacuum seal and extends into the vacuum chamber to support the substrate plate. Its lifting function is used to adjust the distance between the substrate and the nozzle, and its rotating function is used to make the thickness of the atomized deposition layer uniform.
[0097] 100kg of nickel-based high-temperature alloy is placed in the crucible, and the power supply is turned on to heat the material. At the same time, the base plate is raised through the base lifting and rotating mechanism and is located below the nozzle. When the alloy material in the crucible is completely melted, argon gas is introduced into the crucible to eject the alloy liquid through the preheated guide tube, and at the same time, the high-pressure atomizing gas is sprayed to the liquid flow through the nozzle. The base lifting and rotating mechanism is started to rotate and descend the base plate, so that the thickness of the deposition layer formed by the atomized beam on the base surface is increased to form a rod blank. When the alloy liquid is completely ejected, a rod blank with a diameter of about 100mm and a length of about 600mm is formed on the base plate.
[0098] Embodiment 2:
[0099] This embodiment is a suspension melting-spraying molding device for preparing a blank of a plate. The basic structure of the melting device and the melting materials are the same as those in Embodiment 1 ( Figure 1 ).
[0100] One of the differences between this embodiment and embodiment 1 is that its curing molding device ( Figure 6), in this device, the substrate is composed of a substrate plate 37 and a track disk 38, wherein the width of the substrate plate is 350 mm, the length is 800 mm, and the interior is water-cooled. The track disk is mounted on the bottom surface of the substrate plate, and a linear track 39 is provided at the bottom of the disk to limit the moving trajectory of the substrate plate. The lifting mechanism 34 mounted below the vacuum chamber has a lifting rod 36 extending into the vacuum chamber from the bottom of the chamber, and its top end is engaged with the track 39 at the bottom of the track disk 38. The molding drive mechanism 35 is mounted on the side outside the vacuum chamber along the length direction of the substrate plate, and its first driving rod 40 extends into the chamber horizontally through the chamber wall through a vacuum dynamic seal and combines with the edge of the track disk. Before atomization begins, the lifting mechanism first raises the track disk and the substrate plate to a height suitable for injection, then allows the driving rod of the driving mechanism to combine with the end of the substrate, and pushes the front section of the substrate plate to the bottom of the nozzle. After atomization begins, when the deposition layer 31 is formed at the front end of the base plate and the thickness reaches the requirement of the slab, the driving mechanism slowly pulls the track plate, so that the base plate moves in the direction of the driving mechanism, and the length of the slab 41 gradually increases until the slab covers the entire base plate to form a complete slab. During the movement of the base plate 37, the top end of the lifting rod 36 is always engaged with the track 39 of the track plate, maintaining the supporting effect of the lifting rod on the base plate.
[0101] The second difference between this embodiment and the first embodiment is that the smelting device 2 is additionally provided with a crucible moving mechanism 16, which is installed outside the vacuum chamber, on the side of the slab width direction. Its crucible driving rod 21 is fixed to the crucible frame. During the atomization and molding process, while the base plate moves longitudinally, the crucible moving mechanism causes the crucible to reciprocate horizontally ( Figure 2 ), so that the liquid flow out of the liquid flow hole moves back and forth, so that the atomized beam formed by the liquid flow produces a transverse reciprocating scanning effect on the substrate plate, thereby increasing the width of the deposition layer.
[0102] When all the alloy liquid is ejected, a slab with a width of about 300 mm, a length of about 600 mm, and a thickness of about 12 mm is formed on the substrate.
[0103] Embodiment 3:
[0104] This embodiment is a suspension melting-spray forming device for preparing a pipe blank. The basic structure of the melting device and the melting materials are also basically the same as those in Embodiment 1 ( Figure 1 ).
[0105] The difference between this embodiment and embodiment 1 is that its curing and molding device is a device for preparing a tube blank ( Fig.10). In this embodiment, the base member is a cylindrical mandrel 44 with a diameter of 200 mm and water cooling inside. The lifting rod 36 of the base lifting mechanism 34 is located below the mandrel to support the mandrel, and its joint has a structure that allows the mandrel to move and rotate on its surface; the forming drive mechanism 35 is installed outside the side wall of the vacuum chamber along the length direction of the mandrel, and its first drive rod 40 extends into the chamber through the vacuum seal to connect with the end of the mandrel. This drive mechanism has the function of driving the mandrel to rotate and move in the direction away from the nozzle (longitudinal). Before the atomization process is started, the mandrel is raised to a suitable height by the lifting rod, the end of the mandrel is fixed by the end of the drive rod, and the end of the mandrel is pushed to a suitable position under the nozzle. After the injection process is started, the drive mechanism is started to rotate the mandrel, so that the atomized beam formed by the injection forms a cylindrical deposition layer with uniform thickness along the surface of the mandrel. After the thickness of the deposition layer reaches the requirement, the drive mechanism drives the mandrel to slowly move in the direction away from the nozzle. After the injection and forming process is completed, a tube blank with an inner diameter of about 120mm, a length of about 600mm, and a thickness of about 10mm is formed on the mandrel.
[0106] Although the embodiments of the present invention have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.
Claims
1. A high-end metal billet preparation device combining suspension melting and spray forming, characterized in that: It comprises a vacuum furnace body (1), a smelting device (2), an atomizing device (3) and a solidifying device (4); The vacuum furnace body (1) comprises a vacuum chamber (5), and the vacuum chamber (5) is sequentially configured from top to bottom as a smelting zone (6), an atomization zone (7) and a solidification forming zone (8); The smelting device (2) is installed in the smelting area (6), and comprises a water-cooled copper crucible (10) and an induction coil (11); the water-cooled copper crucible (10) has a petal structure, and a cooling water path is arranged in each petal; high-temperature resistant insulating material is filled between the petals; the induction coil (11) is arranged to surround the water-cooled copper crucible (10), wherein a liquid flow hole (17) is opened at the center of the bottom of the water-cooled copper crucible (10); The atomizing device (3) is installed below the atomizing zone (7) and the water-cooled copper crucible (10), and comprises a flow guide tube (24), a flow guide tube heater (25), a gas nozzle (26) and a blowing gas source (27); The guide tube (24) is installed below the bottom of the water-cooled copper crucible (10), with the upper end inserted into the liquid flow hole (17) of the water-cooled copper crucible (10) and the lower end extending downward; an annular guide tube heater (25) is arranged outside the guide tube (24); the nozzle (26) is arranged around the guide tube (24), the blowing gas source (27) is located outside the vacuum chamber (5), and the gas is sent into the vacuum chamber (5) through the conduit (30) and connected to the gas nozzle (26); The curing device (4) is installed below the curing and forming area (8) and the nozzle (26) of the atomization area, and comprises a base member (33), a base lifting mechanism (34) and a forming drive mechanism (35); The base member (33) is located below the nozzle (26) and faces the atomization beam (23); the base lifting mechanism (34) is installed below the vacuum chamber (5), and its lifting rod (36) passes through the bottom of the vacuum chamber (5) through the vacuum seal and extends into the vacuum chamber (5) to support the base member (33); the molding drive mechanism (35) drives the base member (33) to move or rotate, so that the blank can obtain different required shapes and sizes.
2. The device according to claim 1, characterized in that The smelting device (2) further comprises a crucible stand (15) and a crucible moving mechanism (16) for causing the water-cooled copper crucible (10) to reciprocate in a horizontal direction, and for causing the liquid flow (53) flowing out of the liquid flow hole (17) to reciprocate, thereby causing the atomized beam (23) formed by the liquid flow (53) to generate a reciprocating scan; The crucible stand (15) is configured as a bracket for mounting a water-cooled copper crucible (10), the induction coil (11) is also mounted on the crucible stand (15), and the induction coil (11) and the crucible stand are insulated; The crucible moving mechanism (16) is installed outside the vacuum chamber (5), and its crucible driving rod (21) is fixed to the crucible frame (15).
3. The device according to claim 1, characterized in that An induction coil (51) is arranged around the flow guide tube (24) to heat the molten metal in the flow guide tube (24) using a high-frequency electromagnetic field, and the induction coil (51) applies an electromagnetic force (52) to the molten metal to prevent the liquid flow (53) from contacting the tube wall of the flow guide tube (24); and / or, the flow guide tube (24) and the induction coil (51) surrounding it form an electromagnetic valve, and when the high-frequency power supply is cut off, the metal liquid in the flow guide tube (24) will immediately solidify to interrupt the liquid flow; The guide pipe (24) is made of a copper tube, and the guide pipe (24) is divided into a plurality of petals (46) of equal width along the length direction, a small hole (47) is provided in each petal (46) as a cooling water path, and the water paths of adjacent petals (46) are connected end to end to form an overall water path (48) of the guide pipe (24); Alternatively, the flow guide tube (24) is made of a thin copper tube (49), and the thin copper tube is repeatedly bent into a plurality of mutually parallel arched segments (50), and the plurality of arched segments (50) are then formed around a center into a cylindrical flow guide tube (24).
4. The device according to claim 1, characterized in that The base member (33) is plate-shaped, and the base lifting mechanism (34) and the molding drive mechanism (35) are combined into one mechanism, which is installed below the vacuum chamber (5) and is configured to have the functions of lifting and rotating the plate-shaped base member (33).
5. The device according to claim 1, characterized in that The base member (33) comprises a base plate (37) and a track plate (38); The base plate (37) is a plate-shaped device whose width and length meet the requirements of the plate blank size; The track plate (38) is arranged on the bottom surface of the base plate (37), and a track (39) for limiting the moving track of the base plate (37) is arranged at the bottom of the track plate (38); The lifting rod (36) extends from the bottom of the chamber into the vacuum chamber (5), and the top end thereof is engaged with the track (39) at the bottom of the track plate (38); The molding drive mechanism (35) is installed on the side surface of the base plate (37) outside the vacuum chamber (5) in the length direction, and its first drive rod (40) extends horizontally into the vacuum chamber (5) through the chamber wall via a vacuum dynamic seal and is connected to the edge of the track plate (38).
6. The device according to claim 1, characterized in that The base member (33) is configured as a cylindrical core rod (44), and the lifting rod (36) is located below the core rod (44) to support the core rod (44); The molding drive mechanism (35) is installed outside the side wall of the vacuum chamber (5) along the length direction of the core rod, and its first drive rod (40) extends into the vacuum chamber (5) through the vacuum seal to be connected with the end of the core rod, and the molding drive mechanism (35) is configured to have the function of driving the core rod to rotate and move in a direction away from the nozzle (26).
7. The device according to claim 5, characterized in that The track (39) below the track plate (38) is configured in a zigzag or arched shape; A lateral driving mechanism (42) is arranged on the side of the vacuum chamber (5) along the width direction of the base plate (37), and drives the track plate (38) to move via a second driving rod (43) that moves laterally.
8. The device according to claim 1, characterized in that A crucible cover (18) is provided at the upper end of the water-cooled copper crucible (10), and the crucible cover (18) is provided with a gas charging pipe (19) connected to an outdoor inert gas source, so that a closed space is formed in the water-cooled copper crucible (10), so as to apply gas pressure to the metal molten pool in the water-cooled copper crucible (10), pressurize the liquid flow, and control the flow rate of the liquid flow.
9. The device according to any one of claims 1 to 8, characterized in that: The angle α formed by the gas being ejected from the nozzle (28) of the nozzle (26) is referred to as the injection angle (29), wherein the injection angle (29) is configured to be 10 to 100 degrees; And / or, the injection pressure is configured to be 0.1 to 30 MPa.
10. The device according to any one of claims 1 to 8, characterized in that: The smelting device (2) also includes a water-cooled electrode (12), a cable (13) and an induction power supply (14); The water-cooled electrode (12) is installed in an electrode interface tube (20) on the wall of the vacuum chamber (5) and is insulated from the wall. The portion of the water-cooled electrode (12) inside the vacuum chamber (5) is connected to the induction coil (11), and the portion outside the vacuum chamber (5) is connected to the induction power supply (14) via a cable (13).