Vehicle door collision resisting component

By using a combination of metal substrates, continuous fiber reinforced thermoplastic material reinforced beams and staple fiber thermoplastic material connection cladding in the door collision resistance member, the problem of both protection performance and lightweight in the prior art is solved, and a higher Collision energy absorption and safety.

CN222004915UActive Publication Date: 2024-11-15KOLLER (NANJING) NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202420705317.4
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2024-04-08
Publication Date
2024-11-15
Estimated Expiration
2034-04-08

AI Technical Summary

Technical Problem

The existing door collision resistance components are difficult to take into account lightweight while improving the protection performance, and the connection stability and load transfer uniformity between metal and fiber composite materials are insufficient, resulting in limited protection performance.

Method used

A connecting cladding layer made of stamped metal substrates, pultruded continuous fiber reinforced thermoplastic material and injection moldable staple fiber reinforced thermoplastic material, is made of recesses on the substrate and The hot melt connection coating is used to achieve clamping and reinforcement beams to improve the contact surface and connection stability between materials.

Benefits of technology

Effectively utilize the tensile strength of fiber composite materials and the compressive stress tolerance of metal materials to improve the protective performance and lightweight level of door collision resistance components, improve collision energy absorption and anti-stability performance, and simplify the processing technology and reduce the weight.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222004915U_ABST
    Figure CN222004915U_ABST
Patent Text Reader

Abstract

The utility model belongs to the technical field of vehicle door safety components, and particularly relates to a vehicle door collision resisting component. The vehicle door collision resisting component comprises a base plate which can be formed through punching and is made of metal, a reinforcing beam made of a continuous fiber reinforced thermoplastic material and a connecting coating layer made of a short fiber reinforced thermoplastic material. A groove is punched in the base plate, the connecting coating layer is embedded into the groove in an injection molding mode and connected with the groove in a clamping and adhering mode through the through hole, and the connecting coating layer and the reinforcing beam are connected in a melting mode on a mutual contact interface. Therefore, all the components are stably connected, collision loads are uniformly conducted, and all the components cooperate with one another to achieve the effects of light weight and collision protection performance improvement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model belongs to the technical field of vehicle door safety components, and in particular relates to a vehicle door collision resistance component. Background Art

[0002] The increase in the use of motor vehicles and traffic congestion have led to a high rate of traffic accidents. According to surveys, side collision accidents account for about 30% of vehicle collision accidents. Limited driving space limits the thickness of car doors. At present, the yield strength and collision energy absorption effect of the metal components of car doors are poor. Side collisions cause the doors to deform and invade the driving space, thus threatening the lives of drivers and passengers. Therefore, door collision resistance components have become a research and development hotspot for automobile manufacturers, and industry standards such as "QC / T1093-2018 Passenger Car Side Door Anti-collision Bar" have been released one after another.

[0003] The main body of the current door collision resistance components is strip or tube-shaped, such as strip plates, round tubes, square tubes, and is provided with connecting parts riveted, welded or glued to the door at both ends and / or upper and lower edges. The cross-section of the round tube door collision resistance component is circular or nearly circular; the cross-section of the strip door collision resistance component is hat-shaped, U-shaped / F-shaped, M-shaped / W-shaped, and the cross-section of the square tube door collision resistance component is well-shaped (also called extrusion type). Door collision resistance components are generally made of metal materials. Door collision resistance components are usually non-detachable or detachable to the metal frame of the door in a horizontal or oblique direction. However, the door collision resistance component is limited by the thickness of the door, and it is difficult to further improve the protection performance, and further increasing the thickness of the metal material will increase the weight of the vehicle, affecting the driving performance. This has led to the yield strength and safety performance of the door collision resistance component and the limited lightweight, driving performance and driving space becoming a pair of typical technical contradictions in TRIZ theory. Concave-convex structure and hollow structure are one of the ideas to solve this technical contradiction. Known studies have found that the bending resistance of M-shaped / W-shaped door collision resistance components is better than that of tubular components. Tubular components are prone to breakage, resulting in energy absorption failure (Sun Xiaoyu, Ji Yurong, Li Na. Research on selection strategy of door anti-collision beams [J]. Shanghai Automotive, 2020(3):5; Xue Xicai. Failure of side impact door anti-collision bars and optimization of weld layout [J]. Failure Analysis and Prevention, 2021, 16(5):6.).

[0004] The use of lightweight composite materials is the second way to solve the above technical contradictions, but the materials of lightweight composite materials and metal materials are different. The connection stability, mechanics and load transfer uniformity between the two, how to effectively utilize the yield strength of lightweight composite materials, etc., have become further technical problems in the specific application scenarios of door collision resistance components. CN201810384069.7 adopts the strategy of wrapping carbon fiber with the outer layer of a metal round tube, which belongs to the metal tube outer wall fully covered with carbon fiber, and the connection stability, mechanics and load transfer uniformity are good, but it leads to increased thickness, large carbon fiber usage, and increased cost. CN201711053720.4 adopts the strategy of clamping the fiber resin composite material layer with double-layer metal plates, which has good connection stability, mechanics and load transfer uniformity, but it leads to increased thickness, large metal plates and fiber resin usage, and increased cost. And the double-layer metal structure still has the problem of large metal plate usage. CN201410574671.9 adopts the strategy of laying different unidirectional resin fiber prepreg sheets in staggered, multi-layer, and trapezoidal directions, but has high requirements for unidirectional arrangement, resulting in complicated processes. CN201510964622.0 adopts a strategy of clamping the fiber layer with a double metal plate and sealing the periphery of the double metal plate with a temperature-sensitive adhesive to limit the displacement of the fiber layer. However, the temperature-sensitive adhesive does not have the function of transferring load or impact between the metal plate and the fiber layer and is prone to aging and failure in an external environment with unfavorable temperature and humidity.

[0005] In summary, whether from the perspective of market demand or technical demand, improving the protective performance while taking into account the lightweight door collision resistance components is still a problem that needs to be further tackled in the field of door component technology. Summary of the invention

[0006] In view of the above problems, the purpose of the present invention is first to provide a door collision resistance component, specifically to provide a door collision resistance component with fiber composite materials and metal materials, so as to improve the protection performance of the door collision resistance component while taking into account lightweight, and to improve the connection stability of the fiber composite material and the metal material, and to improve the load or impact transmission uniformity between the metal material and the fiber composite material. In this way, the advantages of the high tensile strength of the fiber composite material and the strong compressive stress tolerance of the metal material are effectively utilized to synergistically improve the protection performance of the door collision resistance component.

[0007] For this, the solution adopted by the utility model is as follows:

[0008] A door collision resistance component, whose components include: a substrate made of stampable metal, a reinforcing beam made of continuous fiber reinforced thermoplastic material that can be pultruded, and a connecting coating layer made of short fiber reinforced thermoplastic material that can be injection molded; the substrate is provided with at least one groove in the extension direction; the bottom wall and / or side wall of the groove are provided with a through hole for the hot-melt connecting coating layer to pass through; the main cross-section of the reinforcing beam is one of rectangular, trapezoidal, triangular or semicircular, with a cross-sectional width of 3mm~12mm and a cross-sectional height of 5mm~20mm; the reinforcing beam and the connecting coating layer are located in the groove, the connecting coating layer is embedded in the groove and is bonded to the groove through the through hole; the connecting coating layer forms a continuous or intermittent surface contact with at least the lower surface of the reinforcing beam, and the connecting coating layer and the reinforcing beam are melt-connected at the contact surface where they contact each other.

[0009] Among them, the term "metal" includes alloys. The term "continuous fiber reinforced thermoplastic material", such as the well-known definition of fiber reinforced composite materials (Fiber Reinforced Polymer or Fiber Reinforced Plastic) in the art, belongs to a thermoplastic composite material, which is a composite material formed by winding, molding or pultrusion of reinforcing fiber materials, such as glass fiber, carbon fiber, aramid fiber, glass-carbon hybrid fiber, etc., and matrix materials. The forming process. As another example of the well-known definition of fiber reinforced materials in the art, the components of this type of continuous fiber reinforced thermoplastic material are divided into two parts: matrix and reinforcement. Continuous fibers such as glass fibers, carbon fibers, aramid fibers, etc. are reinforcements, and the continuously distributed components are the matrix, such as a polymer (thermoplastic resin) matrix. Continuous fiber reinforced thermoplastic materials (CFRTP) are a new type of thermoplastic composite materials with high strength, high rigidity, high toughness and recyclability. Compared with steel and aluminum alloys, they can have comparable strength, lighter weight and higher energy absorption capacity; compared with thermosetting composite materials, they are easier to process, environmentally friendly and recyclable. They have great application potential in lightweight automotive design and can replace some metal materials and high-end polymer materials. They are used in body structural parts and semi-structural parts such as seat backs, front-end modules, door inner panels, and bumpers. Continuous carbon fiber reinforced high-performance thermoplastic composites have the characteristics of excellent mechanical properties, low moisture absorption, chemical resistance, short molding cycle, and secondary molding. Its material strength can reach 1500MPa~2200MPa, which is greater than high-strength steel and high-strength aluminum alloy, but its weight is only 1 / 4 of steel and 1 / 2 of aluminum, thereby improving the lightweight level and collision safety of door anti-collision bars. The term short fibre reinforced thermoplastic materials, also known as "short fibre reinforced thermoplastics" (SFT), is a composite material reinforced with short fibres. As is well known in the art, short fibre reinforced thermoplastic materials are usually made into pellets, and the fiber length in the pellets is usually in the mm level, such as 0.2mm~7mm, 2mm~7mm, etc.; the reinforcement and the matrix in the pellets are irregularly mixed (while the reinforcement, i.e., the fiber, in the pellets of long fibre reinforced thermoplastic materials is arranged along the length direction of the pellets). Therefore, although the term "short" fiber is used here, it is a well-known concept in the art and will not lead to problems such as unclear scope of protection. In the utility model, the connecting coating layer plays the role of connecting the substrate and the reinforced beam, and has a lightweight feature. The fiber length in the pellets is within the well-known range, such as 0.2mm~7mm, which meets the use requirements, so it is not specifically limited here.

[0010] The term "fusion connection" means that the contact interface between the connecting coating and the reinforced beam is in a hot-melt state under the same temperature environment, thereby diffusing and fusing with each other to achieve a fusion connection, and this connection state is more solid after cooling. As for the reinforcing beam made of continuous fiber reinforced thermoplastic material and the connecting coating layer made of short fiber reinforced thermoplastic material, ordinary technicians in this field can select materials with the same or overlapping melting temperatures according to the melting temperature of the composite material matrix, so as to easily achieve the melting connection of the connecting coating layer and the contact interface of the reinforcing beam under the same temperature environment during the injection molding process. For example, among the matrix materials of continuous fiber reinforced thermoplastic material and short fiber reinforced thermoplastic material, it is known that: PA6 (nylon 6) has a melting temperature of 215°C~255°C, PA66 (nylon 66) has a melting temperature of 255°C~275°C, PA1212 (nylon 1212) has a melting temperature of 178°C~190°C, PMMA (polymethyl methacrylate) has a melting temperature of 180°C~240°C, and PC (polymethyl methacrylate) has a melting temperature of 220°C~300°C, so that the composite matrix of the reinforced beam and the composite matrix of the connecting coating layer can be selected to be PA6, or PA6 and PC respectively.

[0011] Among them, when the main cross section of the reinforcing beam is trapezoidal, triangular or semicircular, it is obvious that in order to form a stable and highly resistant structure, ordinary technicians in the field should know that the bottom side (trapezoid), bottom (triangle) or straight part (semicircle) of the trapezoidal, triangular or semicircular should be on the side facing the collision impact, that is, the side of the groove that is not open. When the main cross section of the reinforcing beam is trapezoidal, triangular or semicircular, under the same height and bottom width, the reinforcing beam uses less material than the rectangular cross section, and the performance of resisting collision is not significantly reduced. It is conducive to further reducing the weight of the door collision resistance component. Obviously, the term "main body" refers to the core part or main part of an object. The term "cross section" refers to the cross section along the minor axis direction of an object. Obviously, the term "semicircle" is a shape similar to a semicircle formed by the bottom side of a straight line segment and a convex arc line, and it does not have to be an absolute semicircle in the geometric sense. The length of its straight side is the cross-sectional width. Obviously, when the cross section is a trapezoid, the cross-sectional width refers to the lower bottom width of the trapezoid, that is, the longer bottom side. Obviously, the term "cross-sectional width" refers to the length in the direction parallel to the open plane of the groove; the term "cross-sectional height" refers to the length in the direction perpendicular to the open plane of the groove.

[0012] Regarding the substrate: the main body of the substrate of the utility model is a strip. Obviously, according to the Chinese definition, the strip is a description of a narrow and long shape, which refers to a narrow and long shape with slightly parallel two sides and slightly equal width. Its upper and lower edges are approximately parallel, but not strictly parallel. The two ends of the substrate can be provided with a movable and detachable or non-movable detachable mechanism connected to the metal frame of the door in a conventional manner, such as a reserved riveting hole (non-movable and detachable), a reserved welding point (non-movable and detachable), a reserved threaded connection hole (movable and detachable), etc. The width of the two ends of the substrate can be greater than the main body of the substrate, forming a dumbbell shape with wide ends and a narrow middle. Obviously, the movable and detachable or non-movable detachable mechanism can also be arranged at the upper and lower edges and / or the middle position of the substrate, etc., to increase the contact between the substrate and the metal frame of the door, and improve the dispersion and uniformity of the contact, thereby improving the bending resistance of the substrate.

[0013] Among them, the grooves arranged in the extension direction of the substrate make the main cross-section of the substrate present a hat shape, a U shape / a "J" shape, an M shape / a "W" shape, etc., so that the substrate has a compressible convex structure to improve the energy absorption and buffering effect of the substrate during a collision. Obviously, the U shape and the "J" shape, the M shape and the W shape are only description differences caused by the observation direction. Obviously, when the door collision resistance component is installed in the door, the opening of the groove faces the driver's compartment, otherwise the convex part of the cavity will lose the energy absorption and buffering effect during a collision.

[0014] Regarding the depth of the groove and the ratio of the groove depth to the width of the upper opening of the groove, conventional values ​​and ranges of the prior art may be adopted, such as the depth of the groove being 20 mm to 35 mm, and the ratio of the groove depth to the width of the upper opening of the groove being 2:1 to 2:7. In other words, the depth of the groove and the ratio of the groove depth to the width of the upper opening of the groove are conventionally selected by those skilled in the art based on the thickness limit of the vehicle door and the need for energy absorption and buffering during collision, and are not specifically limited here.

[0015] The through holes provided on the bottom wall and / or side wall of the groove can be passed through by the hot-melt connection coating layer. Under the limiting effect of the mold (for example, the through hole of the bottom wall) or the effect of gravity (for example, the through hole of the side wall), the hot-melt connection coating layer is blocked or affected by gravity after passing through the through hole, and the extension direction is changed outside the through hole, so that after cooling, a structure similar to a "nail cap" is formed to limit the connection coating layer from retracting from the through hole. In addition, the connection coating layer itself is bonded to the through hole by hot melting, so that the connection coating layer and the through hole form a "card-bonded connection". Different from the "card-bonded connection" of the traditional mechanical connection combined with additional bonding, the "card-bonded connection" of the utility model does not require additional bonding materials, and the bonding is completed while forming the card-bonded structure. Obviously, the number of the through holes can be conventionally selected by ordinary technicians in this field according to the fixed connection requirements, such as 5 to 30 through holes are respectively provided on the bottom wall and / or side wall of the groove. No specific limitation is made here. The embedding means that the connection coating layer is located in the cavity of the groove. Of course, since the connecting coating layer is a thermoplastic material with adhesiveness, it will naturally bond with the cavity of the groove after being injected into the groove in a hot melt state, and thus form a strong bond after cooling.

[0016] The term "surface contact" is a concept relative to point contact and line contact. The connection coating layer and the reinforcement beam form a surface contact, which is conducive to improving the firmness of the connection between the two and the uniformity of collision load transfer, and is more conducive to the collision energy absorption effect of the reinforcement beam. When the two form a continuous rather than discontinuous surface contact, the firmness of the connection and the uniformity of load transfer are better, and it is more conducive to improving the anti-instability performance of the reinforcement beam. Therefore, it is further preferred that the connection coating layer forms a continuous surface contact with at least the lower surface of the reinforcement beam.

[0017] Preferably, two grooves are provided in the extension direction of the substrate, so that the main cross section of the substrate is M-shaped / W-shaped. This M-shaped structure gives the substrate better anti-instability performance, and both grooves are filled with reinforcing beams and connecting cladding layers, which is more conducive to further improving lightweight and impact resistance.

[0018] Preferably, the metal of the substrate is selected to have a yield strength of 500 MPa or more; for example, one of DP steel, CP steel, QP steel, DH steel that can be cold stamped, or martensitic steel that can be hot stamped. Further preferably, the thickness of the substrate is 1.2 mm to 2 mm. Obviously, the "thickness of the substrate" refers to the thickness of the metal sheet used for the substrate. Preferably, the yield strength of the metal is 500 MPa to 1800 MPa, for example, the yield strength can be selected to be 500 MPa, 900 MPa, 1500 MPa, or 1800 MPa, etc.

[0019] For the reinforced beam:

[0020] Preferably, the continuous fiber, i.e., the reinforcement, of the reinforcement beam is selected from one of glass fiber, carbon fiber, or glass-carbon mixed fiber; further preferably, the product form of the continuous fiber is selected from at least one of continuous yarn, unidirectional tape, or unidirectional cloth. Preferably, the thermoplastic material, i.e., the matrix of the reinforcement beam is selected from at least one of polyamide material, polymethyl methacrylate material, and polycarbonate material; further preferably, the polyamide material is selected from at least one of PA6, PA66, and PA1212. Obviously, the main cross-sectional shape, size, and orientation of the reinforcement beam should match the groove of the substrate. The main cross-sectional thickness and size of the reinforcement beam are allowed to vary instead of having the cross-sectional size of each part being exactly the same.

[0021] For the connection coating:

[0022] Preferably, the short fiber of the connecting coating layer, i.e., the reinforcement, is selected from one of glass fiber and carbon fiber. The thermoplastic material of the connecting coating layer, i.e., the matrix, is selected from one of polyamide material, polymethyl methacrylate material, and polycarbonate material. Further preferably, the polyamide material is selected from at least one of PA6, PA66, and PA1212.

[0023] Preferably, the weight fraction of the short fibers in the short fiber reinforced thermoplastic material is 10% to 50%.

[0024] Preferably, the groove is provided with a cavity compartment separated by a connecting coating layer. Obviously, the cavity compartment does not have to be closed, and the outer opening is more convenient for processing and molding, which can be easily realized by using a mold during the hot melt injection molding process of the connecting coating layer, for example, the side facing the driving space is in an open state. Obviously, the cavity compartment can be separated and formed in a variety of ways: for example, the cavity compartment can be formed by a depression inside the connecting coating layer itself, that is, it is only separated and enclosed by the connecting coating layer; the cavity compartment can also be enclosed by the connecting coating layer and the side walls of the groove and / or the reinforcing beam. This situation can be divided into: the cavity compartment is only enclosed by the connecting coating layer and the groove; the cavity compartment is only enclosed by the connecting coating layer and the side walls of the reinforcing beam; the cavity compartment is enclosed by the connecting coating layer and the side walls of the groove and the reinforcing beam. This situation can be further divided into: the cavity compartment is formed by the connecting coating layer and the side walls of the groove and the reinforcing beam as the four side walls of the cavity compartment (having 4 side walls, 1 for the groove side, 1 for the reinforcing beam side, and 2 for the connecting coating layer side), for example, a part of the connecting coating layer is distributed between the side walls of the groove and the reinforcing beam in the form of parallel lines (the angle between the parallel lines and the side walls of the groove is not equal to 180 degrees), dividing the space between the side walls of the groove and the side walls of the reinforcing beam into rectangular or diamond-shaped cavity compartments; the cavity compartment is formed by the connecting coating layer and the side walls of the groove and the reinforcing beam respectively, for example, the connecting coating layer is distributed between the side walls of the groove and the reinforcing beam in the form of V-shaped, W-shaped, Y-shaped or X-shaped broken lines, so that it can be respectively enclosed with the side walls of the groove and the reinforcing beam to form cavity compartments of various shapes such as triangles, trapezoids, pentagons, hexagons, etc.

[0025] Obviously, the shape of the cavity compartment can be diverse, and multiple shapes can exist at the same time, for example, the top view shape of the cavity compartment is at least one of a triangle, a trapezoid, a rectangle, a rhombus, a hexagon, a circle, an ellipse, and a semicircle. Obviously, each groove can be provided with a number of cavity compartments, such as 1 to 200 cavity compartments, and for example 30 to 70 cavity compartments, so as to further improve the weight reduction effect and maintain the anti-instability performance of the reinforcement beam. When only a small number of cavity compartments are provided in one groove, it is obvious that the lightweight effect can be taken into account by increasing the area of ​​a single cavity compartment. The setting of the cavity compartment can further reduce the weight of the connecting coating layer to exert the weight reduction effect. And because the connecting coating layer and the groove are bonded and stuck, and the connecting coating layer and the reinforcement beam are in surface contact and molten connection, the setting of the cavity compartment does not significantly affect the connection stability between different parts of the door collision resistance component.

[0026] As a preferred solution, the cavity compartment is formed by the connecting coating layer and the side walls of the groove and the reinforcing beam. For example, a part of the connecting coating layer is distributed between the groove and the side walls of the reinforcing beam in the form of parallel lines (the angle between the parallel lines and the side walls of the groove is not equal to 180 degrees), and the space between the side walls of the groove and the side walls of the reinforcing beam is divided into rectangular or diamond-shaped cavity compartments. As another preferred solution, the cavity compartment is formed by the connecting coating layer and the side walls of the groove and the reinforcing beam respectively. For example, a part of the connecting coating layer is distributed between the side walls of the groove and the reinforcing beam in the form of a V-shaped, W-shaped, Y-shaped or X-shaped broken line, so that it can be respectively surrounded by the side walls of the groove and the reinforcing beam to form a cavity compartment of various shapes such as a triangle, trapezoid, pentagon, hexagon, etc. Preferably, in the side walls of the cavity compartment, the wall thickness of the connecting coating layer located between the side walls of the groove and the reinforcing beam is 2.5mm~7mm. The term "connecting coating layer between the groove and the side wall of the reinforcing beam" is distinguished from the connecting coating layer below the reinforcing beam; the term "wall thickness" refers to the thickness between the two side surfaces along the length direction of the base plate.

[0027] Obviously, when the connecting coating layer and the side wall of the reinforcing beam are enclosed to form a cavity compartment, the connecting coating layer will naturally form at least intermittent surface contact with the side wall of the reinforcing beam. For example, the two-to-two connection positions (i.e., the angle positions) of the outer wall of the cavity compartment are in surface contact, and there may be no surface contact at positions other than the two-to-two connection positions, so the surface contact at this time is "intermittent". Of course, at this time, the size of the cavity compartment can also be reduced by forming a continuous surface contact between the connecting coating layer and the side wall of the reinforcing beam (i.e., except for the angle position, the connecting coating layer also overlaps and contacts with the side wall of the reinforcing beam).

[0028] Regarding the overall structure of the door collision resistance member:

[0029] Preferably, the volume of the connecting coating layer accounts for 40% to 90% of the volume of the groove. Properly increasing the volume percentage of the coating layer in the groove (ie, the filling rate) can further improve the collision energy absorption function of the door collision resistance component while ensuring the requirement of lightweight.

[0030] Further preferably, in the door collision resistance member, the ratio of the total weight of the connecting cladding layer and the reinforcing beam to the weight of the substrate is 1:1.5 to 1:6. A person skilled in the art may also adopt other weight ratios according to the requirements of lightweighting by adjusting the amount of the connecting cladding layer.

[0031] In general, the utility model adopts the strategy of punching grooves on a metal substrate to improve the collision energy absorption effect of the substrate itself and reduce the risk of bending failure (i.e., instability); further, in the groove, a reinforcing beam and a connecting coating layer made of fiber-reinforced composite materials with similar melting temperatures, high strength, and light weight are used to achieve an effective and stable connection between the substrate and the reinforcing beam, and at the same time, the collision load borne by the substrate is effectively and evenly transferred to the reinforcing beam, thereby making full use of the respective performance advantages of the reinforcing beam, which has high tensile strength and can withstand tensile stress, and the substrate and the groove, which can withstand compressive stress and have buffering performance. While meeting the lightweight requirements and not increasing the thickness of the door, the collision energy absorption and protective effect of the door collision resistance component are improved. Among them, the reinforcing beam made of continuous fiber-reinforced composite materials has the advantage of convenient processing because it can be pultruded; the connecting coating layer made of short fiber-reinforced thermoplastic material has the advantage of convenient processing because it can be plasticized and then injection molded.

[0032] The method for preparing the above-mentioned door collision resistance component comprises the following steps:

[0033] Substrate stamping: Take the substrate sheet and punch out a groove along the length direction of the substrate;

[0034] Initial forming of the reinforced beam: the continuous fibers are pulled out and immersed in the liquid thermoplastic material for the reinforced beam, the soaked continuous fibers are polymerized and formed, and then cut into the required length; or the continuous fibers pre-impregnated with the thermoplastic material for the reinforced beam are directly pulled out, preheated and softened, polymerized and formed, and then cut into the required length;

[0035] Reinforcement beam shaping: After the initial shaping, the reinforcement beam is heated and softened, transferred to a shaping mold that meets the groove shape characteristics for shaping, and taken out after cooling.

[0036] Coating of the connection coating layer: clean the stamped substrate, put the substrate and the shaped reinforcement beam into the injection mold, plasticize the short fiber reinforced thermoplastic material particles and inject them into the mold cavity, pressurize the short fiber reinforced thermoplastic material to be injection-molded into the groove, pass through the through hole of the groove, and melt-connect with the reinforcement beam at the interface of mutual contact; keep the pressure and cool to shape, so as to form a connection coating layer, and the connection coating layer is bonded to the through-hole card, so as to realize that the reinforcement beam, the groove of the substrate and the connection coating layer are connected into a whole, and the finished product is demoulded.

[0037] The continuous fiber reinforced thermoplastic material capable of pultrusion and the short fiber reinforced thermoplastic material capable of injection molding involved in the utility model can both adopt materials available on the market in the prior art, such as short fiber reinforced thermoplastic plastics, continuous fiber reinforced thermoplastic resins, etc.

[0038] Beneficial effects of the utility model:

[0039] (1) The reinforcement beam is made of high-strength continuous glass fiber, carbon fiber or glass-carbon hybrid fiber composite material, which is stronger than common metals and has a large elastic range, and has better elasticity than metal door collision resistance components. The strength of the continuous fiber reinforced thermoplastic composite material used can reach 1500MPa~2200MPa, but the weight is only 1 / 4 of steel and 1 / 2 of aluminum. The connecting cladding layer also uses lightweight materials, thereby improving the lightweight level and collision safety of the door anti-collision bar.

[0040] (2) Connecting the cladding layer and the reinforcing beam to fill the groove portion of the substrate can enhance the substrate's ability to resist instability and improve collision safety.

[0041] (3) Combined with the stress analysis and material characteristics of the door collision resistance component, the materials and structures are comprehensively utilized, such as the hollow design (cavity compartment) connecting the cladding layer, the mechanical transmission structure design (surface contact) connecting the cladding layer and the reinforcement beam, and the buffer structure design (groove) of the base plate. The reinforcement beam has high tensile strength and can withstand tensile stress, and the base plate groove can withstand compressive stress and buffer, giving full play to the mechanical performance advantages of each material.

[0042] (4) The fusion connection between the reinforcement beam and the connecting coating layer can be completed naturally during the injection molding process with the help of the melting and cooling process, which has the advantage of being easy to process. After cooling, the fusion connection is stable and not easy to separate, and there are no additional welding points, so the connection is firm. In addition, the fusion connection is a surface contact, but it does not require a large area of ​​additional adhesives or other mechanical connections to achieve a reliable connection between the two. The connecting coating layer is injection molded into the groove of the substrate, and with the help of through holes, it forms a double connection method that is both bonded and clamped with the substrate. There is no need for double-layer metal plate clamping, which further improves the reliable connection between the connecting coating layer and the substrate. The processing technology is simple and the connection effect is better.

[0043] (5) The installation space inside the car door is small and limited. The utility model further improves the anti-collision performance of the car door without increasing the cross-sectional height and weight of the anti-collision beam. According to the analysis results, under the same weight, the car door collision resistance component of the utility model can increase the energy absorption value of the car door collision resistance component by more than 15% or be more than 15% lighter under the same energy absorption value. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 This is a schematic diagram of the overall structure of a door collision resistance component of Embodiment 1 of the present utility model;

[0045] Figure 2 This is a schematic diagram of the structure disassembly of the door collision resistance component of Embodiment 1 of the present utility model;

[0046] Figure 3It is a cross-sectional schematic diagram of a substrate of a door collision resistance component of Embodiment 1 of the utility model;

[0047] Figure 4 It is a schematic cross-sectional view of the first groove of the door collision resistance component of the first embodiment of the utility model along the point a;

[0048] Figure 5 It is a schematic cross-sectional view of the first groove of the door collision resistance component of the first embodiment of the utility model extending from point b;

[0049] Figure 6 It is a schematic cross-sectional view of the first groove of the door collision resistance component of the first embodiment of the utility model extending from point c;

[0050] Figure 7 is a force direction analysis diagram of a door collision resistance component of Embodiment 1 of the present utility model;

[0051] Figure 8 It is a cross-sectional schematic diagram of the location of the first groove cavity compartment of the door collision resistance component of the second embodiment of the utility model;

[0052] Fig. 9 It is a cross-sectional schematic diagram of the location of the non-cavity compartment of the first groove of the door collision resistance component of Example 2 of the utility model;

[0053] Fig.10 It is a schematic diagram of the overall structure of the door collision resistance component of Embodiment 3 of the present utility model;

[0054] Fig.11 This is a manufacturing process flow chart of the vehicle door collision resistance component of the utility model;

[0055] Among them, 1 is a base plate, 11 is an end portion for fixing the base plate, 12 is a reserved riveting hole, 13 is a through hole, 21 is a first connecting coating layer, 22 is a second connecting coating layer, 23 is a melting layer, 31 is a first reinforcing beam, 32 is a second reinforcing beam, 41 is a first groove, and 42 is a second groove. DETAILED DESCRIPTION

[0056] The present invention is further described below in conjunction with the embodiments. Due to space limitations, it is difficult to list them all, and the embodiments are only illustrative examples and should not be regarded as limiting the scope of protection. Without departing from the overall concept of the present invention, similar technical solutions obtained by simple replacement / substitution and other means should also be regarded as the scope of protection of the present invention, including but not limited to: modification of the shape of the end of the substrate, modification of the number of grooves, adjustment of the shape of the reinforcing beam, adjustment of the shape and number of the cavity compartments, adjustment of the number or position of the through holes, etc.

[0057] Embodiment 1 A vehicle door collision resistance component

[0058] Please refer to the instruction manual Figure 1 To Attachment Figure 6 .

[0059] As attached Figure 1 As shown, the present embodiment provides a door collision resistance member, which is composed of a substrate 1, a first groove 41, a second groove 42, a first connection covering layer 21, a second connection covering layer 22, a first reinforcement beam 31, and a second reinforcement beam 32. The first reinforcement beam 31 and the first connection covering layer 21 are filled in the first groove 41, and the second reinforcement beam 32 and the second connection covering layer 22 are filled in the second groove 42.

[0060] As attached Figure 2 As shown, the main body of the substrate 1 is in the shape of a strip, and ends 11 for fixing the substrate are provided at both ends to facilitate the connection of the substrate 1 with the metal frame provided in the vehicle door. The width of the ends 11 for fixing the substrate is greater than the main body of the substrate 1, which can increase the contact area between the substrate 1 and the metal frame provided in the vehicle door, and improve the connection stability. The ends 11 for fixing the substrate are provided with reserved rivet holes 12, so that the substrate 1 can be connected to the metal frame provided in the vehicle door by riveting. Obviously, the reserved rivet holes 12 here can also be replaced by other structures such as reserved welding points or reserved threaded holes, so as to facilitate the welding or threaded connection between the substrate 1 and the metal frame provided in the vehicle door.

[0061] As attached Figure 2 As shown, the lengths and shapes of the first groove 41 and the second groove 42, the first connecting coating layer 21 and the second connecting coating layer 22, and the first reinforcing beam 31 and the second reinforcing beam 32 may not be completely the same. The cross-sectional dimensions of the first reinforcing beam 31 and the second reinforcing beam 32 may also be varied to adapt to the shapes and directions of the first groove 41 and the second groove 42.

[0062] As attached Figure 1 To Attachment Figure 6 As shown, the openings of the first groove 41 and the second groove 42 face the driver compartment and are formed by punching the base plate 1 in the extension direction. Figure 3 The W-shaped or M-shaped (depending on the viewing direction) is shown. The bottom wall of the first groove 41 and the second groove 42 is provided with a through hole 13 for the first connection coating layer 21 and the second connection coating layer 22 to pass through so as to form a card bonding connection.

[0063] As attached Figure 1 and attached Figure 2As shown, a portion of the first connecting coating layer 21 of the door collision resistance component is distributed in the form of a V-shaped fold line between the side wall of the first groove 41 and the side wall of the first reinforcing beam 31, playing a partitioning role. As a result, the first connecting coating layer 21 is respectively enclosed with the side wall of the first groove 41 and the side wall of the first reinforcing beam 31 to form a number of triangular and trapezoidal cavity compartments (the second groove 42 also has such a structure). The number of cavity compartments in the first groove 41 and the second groove 42 is 50 to 60. In the side wall of the cavity compartment, the wall thickness of the first connecting coating layer 21 located between the side wall of the first groove 41 and the first reinforcing beam 31 is 2.5 mm to 7 mm, for example Figure 6 In the embodiment, the wall thickness of the first connection coating layer 21 in the left cavity of the first groove 41 is preferably 5 mm.

[0064] Due to the existence of the cavity compartment, in order to clearly show the positional relationship between the first connection coating layer 21 and the first groove 41 and the first reinforcing beam 31 (which can represent the position and connection relationship between the second connection coating layer 22 and the second groove 42 and the second reinforcing beam 32), a first groove 41 extension is provided. Figure 1 For cross-sectional schematic diagrams of point a (i.e., the upper vertex of the triangular cavity compartment formed by the first connecting cladding layer 21 and the first reinforcing beam 31), point b (i.e., the right vertex of the triangular cavity compartment formed by the first connecting cladding layer 21 and the first reinforcing beam 31), and point c (i.e., the waist midpoint of the triangular cavity compartment formed by the first connecting cladding layer 21 and the first reinforcing beam 31), please see the attached Figure 4 To Attachment Figure 6 . Figure 4 It can be seen that when a cross section is made at point a, the first connection coating layer 21 is in contact with a side wall of the first groove 41; it is in contact with the lower surface of the first reinforcement beam 31 and there is a molten layer 23; Figure 5 It can be seen that when a cross section is made at point b, the first connecting coating layer 21 does not contact the side wall of the first groove 41; it is connected to the side and lower surface of the first reinforcing beam 31 and both have a molten layer 23; Figure 6It can be seen that when the cross section is made at point c, the first connection coating layer 21 is not in contact with the side wall of the first groove 41, and has two contact connections with the bottom wall of the first groove 41, including the connection at the position of the through hole 13; it is connected to the lower surface of the first reinforcement beam 31 and has a molten layer 23. That is, in the cross-sectional view of each point, the first connection coating layer 21 is in surface contact with the lower surface of the first reinforcement beam 31 (i.e., forming a continuous surface contact), while the first connection coating layer 21 is in intermittent surface contact with the side of the first reinforcement beam 31. This surface contact connection improves the connection stability of the first connection coating layer 21, the second connection coating layer 22 and the first reinforcement beam 31, the second reinforcement beam 32. Furthermore, when there are cavity compartments, there are continuous surface contacts between the first connection coating layer 21 and the second connection coating layer 22 and the lower surfaces of the first reinforcement beam 31 and the second reinforcement beam 32, respectively, and discontinuous surface contacts between the first connection coating layer 21 and the second connection coating layer 22 and the side surfaces of the first reinforcement beam 31 and the second reinforcement beam 32, respectively, which are more conducive to improving the anti-instability performance of the first reinforcement beam 31 and the second reinforcement beam 32. Furthermore, the first connection coating layer 21 and the second connection coating layer 22 support the first groove 41 and the second groove 42 from the inside to the full depth, which also improves the anti-instability performance of the substrate 1.

[0065] As attached Figures 4 to 6 As shown in FIG. 1 , the bottom wall of the first groove 41 is provided with a through hole 13. When the hot-melt first connection coating layer 21 is embedded in the first groove 41 by injection molding, the first connection coating layer 21 in a hot-melt state partially passes through the through hole 13 and is inserted into the substrate 1. A baffle is provided at the bottom of the substrate 1 or the excess first connection coating layer 21 protruding from the through hole 13 is flattened when the injection molding is completed but not completely solidified to form the first connection coating layer 21 as shown in FIG. Figures 4 to 6 The nail cap-shaped snap-on structure shown. Obviously, since the first connection coating layer 21 and the second connection coating layer 22 are adhesive, after hot melt solidification, the first connection coating layer 21, the second connection coating layer 22 and the through holes 13 of the first groove 41 and the second groove 42 are both snap-on and adhesive, so it is called a snap-on connection. This structure can improve the connection stability between the first connection coating layer 21, the second connection coating layer 22 and the first groove 41 and the second groove 42, and the process is simple.

[0066] As attached Figures 4 to 6 As shown, the main cross-section of the first reinforcing beam 31 and the second reinforcing beam 32 is rectangular, and the cross-sectional width can be 3mm~12mm, and the cross-sectional height can be 5mm~20mm. Here, the cross-sectional width is preferably 8mm, and the cross-sectional height is 15mm. Figure 2 As shown in the disassembly diagram, the first reinforcing beam 31 and the second reinforcing beam 32 are in a strip shape, but the cross-sectional dimensions do not have to be completely consistent, but rather match the properties of the first groove 41 and the second groove 42.

[0067] The depth of the first groove 41 and the second groove 42 of the door collision resistance member can be 20 mm to 35 mm, and the ratio of the depth of the first groove 41 and the second groove 42 to the width of the upper open part can be 2:1 to 2:7. Here, the depth of the first groove 41 and the second groove 42 is preferably 27 mm. Here, the ratio of the depth of the first groove 41 and the second groove 42 to the width of the upper open part is preferably 2:5.

[0068] The substrate 1 of the door collision resistance component is made of a metal that can be stamped. The metal is selected from a metal material with a yield strength of 500MPa or more, such as a yield strength of 900MPa, 1500MPa or 1800MPa, such as DP steel, CP steel, QP steel, DH steel that can be cold stamped, or martensitic steel that can be hot stamped. The thickness of the substrate 1 can be selected from 1.2mm to 2mm. Here, the thickness of the substrate 1 is preferably 1.5mm.

[0069] The first reinforcing beam 31 and the second reinforcing beam 32 of the door collision resistance component are made of continuous fiber reinforced thermoplastic material that can be pultruded, and the continuous fiber can be selected from one of glass fiber, carbon fiber or glass-carbon mixed fiber; the product form of the continuous fiber can be selected from one of continuous yarn, unidirectional tape or unidirectional cloth. The thermoplastic material can be selected from one of polyamide material (such as one of PA6, PA66, PA1212), polymethyl methacrylate material, and polycarbonate. For example, the continuous fiber reinforced thermoplastic material is a glass fiber unidirectional tape pre-impregnated with PA6.

[0070] The first connecting covering layer 21 and the second connecting covering layer 22 of the vehicle door collision resistance component are made of injection moldable short fiber reinforced thermoplastic material, and the short fiber can be selected from glass fiber short fiber or carbon fiber short fiber; the thermoplastic material can be selected from polyamide material (such as one of PA6, PA66, and PA1212), polymethyl methacrylate material, and polycarbonate. The weight fraction of the short fiber in the short fiber reinforced thermoplastic material can be selected to be 10% to 50%. Here, the weight fraction of the short fiber in the short fiber reinforced thermoplastic material is preferably 30%.

[0071] The first connection coating layer 21 and the second connection coating layer 22 of the vehicle door collision resistance component may occupy 40% to 90% of the volume of the corresponding first groove 41 or the second groove 42, so as to improve the collision energy absorption effect of the vehicle door collision resistance component. Here, it is preferred that the first connection coating layer 21 and the second connection coating layer 22 occupy 60% of the volume of the corresponding first groove 41 or the second groove 42.

[0072] The vehicle door collision resistance member may have a total weight ratio of the connected cladding layer and the reinforcement beam to the weight of the substrate of 1:1.5 to 1:6. Preferably, the total weight ratio of the connected cladding layer and the reinforcement beam to the weight of the substrate is 1:1.97.

[0073] The force direction of the collision resistance component of this door is shown in the appendix of the manual. Figure 7 ,like Figure 7 As shown, when a collision occurs, the direction of the impact force is toward the open direction of the first groove 41 or the second groove 42, that is, inside the driving space. The raised portion of the first groove 41 or the second groove 42 bears the impact force, absorbs energy by deformation, and resists collision damage. Since the first connecting coating layer 21 and the second connecting coating layer 22 form surface contact with the first reinforcing beam 31 and the second reinforcing beam 32 respectively, and are connected to the first groove 41 or the second groove 42, the impact force can be evenly transmitted to the first reinforcing beam 31 and the second reinforcing beam 32. The material of the first reinforcing beam 31 and the second reinforcing beam 32 has the advantage of high tensile strength, and the impact bearing performance of the substrate 1 can be improved by means of tensile stress, giving full play to the mechanical property advantages of each material, and jointly playing the role of lightweighting and improving protective performance.

[0074] Embodiment 2 A vehicle door collision resistance component

[0075] This embodiment provides a door collision resistance member, which is different from the first embodiment in that its cavity compartment is formed by a concave structure provided in the connecting cladding layer, and the top view of the cavity compartment is a rectangle. Figure 8 The schematic cross-sectional view of the location of the cavity compartment of the first groove 41 of the door collision resistance component (which can represent the first groove 42), the instruction manual appendix Fig. 9 The cross-sectional view of the non-cavity compartment of the first groove 41 of the door collision resistance member (which can represent the first groove 42 ) is shown. The depressions on the left and right sides of the first reinforcement beam 31 located at the lower side are the cavity compartments.

[0076] Compare with Figure 4 -Attached Figure 6 With attached Figure 8 and attached Fig. 9 The cross section of the hollow compartment of the first groove 41 or the second groove 42 of the door collision resistance member is rectangular, and the top view is rectangular. Since the cross section is rectangular and the top view is rectangular, the cross-sectional view at the location of the hollow compartment and the location of the non-hollow compartment can represent the contact connection relationship between the first connection coating layer 21 and the first groove 41 and the first reinforcement beam 31. Figure 8 and attached Fig. 9 It can be seen that the first connecting covering layer 21 of the door collision resistance component is in contact and connected with both side walls of the first groove 41 (and is in continuous surface contact), is in continuous surface contact with the lower surface of the first reinforcing beam 31, and is in continuous surface contact with the left and right side surfaces of the first reinforcing beam 31.

[0077] The contact surface between the first connecting coating layer 21 and the first groove 41 of the door collision resistance component is larger than that of the door collision resistance component of Example 1, which is beneficial to enhancing the anti-instability performance of the first groove 41 and the substrate 1 through the filling effect of the first connecting coating layer 21.

[0078] Embodiment 3 A door collision resistance member

[0079] This embodiment provides a door collision resistance member, which is different from the first embodiment in that at least part of its cavity compartments are rhombus-shaped (rhombus-shaped when viewed from above). For example, a part of the second connecting coating layer 22 is distributed between the second groove 42 and the side wall of the second reinforcing beam 32 in the form of parallel lines (the angle between the parallel lines and the groove side wall is about 30 degrees to 60 degrees), dividing the space between the second groove 42 and the side wall of the second reinforcing beam 32 into rectangular or rhombus-shaped cavity compartments.

[0080] As attached Fig.10 As shown, in the middle part of the second groove 42 of the door collision resistance member, the second connection covering layer 22 is distributed in the form of parallel lines (the angle between the parallel lines and the groove side wall is about 60 degrees), dividing the space between the second groove 42 and the side wall of the second reinforcement beam 32 into diamond-shaped cavity compartments. Other features (including the wall thickness of the first connection covering layer 21 and the second connection covering layer 22, etc.) are the same as those of Example 1.

[0081] Embodiment 4 A vehicle door collision resistance component

[0082] The present embodiment provides a door collision resistance component, which differs from the first embodiment in that the first connection covering layer 21 and the second connection covering layer 22 distributed in the form of a V-shaped fold line between the side wall of the first groove 41 and the side wall of the first reinforcing beam 31 and between the side wall of the second groove 42 and the side wall of the second reinforcing beam 32 are higher than the first reinforcing beam 31 and the second reinforcing beam 32, so that during the injection molding process, the first connection covering layer 21 and the second connection covering layer 22 can also form intermittent surface contact with the upper surfaces of the first reinforcing beam 31 and the second reinforcing beam 32 respectively.

[0083] Reference Figure 5 When the first reinforcing beam 31 of the door collision resistance member is fused with the first connection coating layer 21, the connection firmness of the first connection coating layer 21 to the first reinforcing beam 31 is further improved, and the anti-instability performance of the first reinforcing beam 31 is reduced.

[0084] Example 5 Preparation process of vehicle door collision resistance component

[0085] Please refer to the appendix of the manual for the preparation process of the door collision resistance component. Fig.11The process includes the following steps: substrate stamping, reinforcement beam initial forming, reinforcement beam shaping, and connection and cladding of the cladding layer:

[0086] Substrate stamping: Take the substrate sheet and punch out a groove along the length direction of the substrate;

[0087] Initial forming of the reinforced beam: the continuous fibers are pulled out and immersed in the liquid thermoplastic material for the reinforced beam, the soaked continuous fibers are polymerized and formed, and then cut into the required length; or the continuous fibers pre-impregnated with the thermoplastic material for the reinforced beam are directly pulled out, preheated and softened, polymerized and formed, and then cut into the required length;

[0088] Reinforcement beam shaping: After the initial shaping, the reinforcement beam is heated and softened, transferred to a shaping mold that meets the groove shape characteristics for shaping, and taken out after cooling.

[0089] Coating of the connection coating layer: clean the stamped substrate, put the substrate and the shaped reinforcement beam into the injection mold, plasticize the short fiber reinforced thermoplastic material particles and inject them into the mold cavity, pressurize the short fiber reinforced thermoplastic material to be injection-molded into the groove, pass through the through hole of the groove, and melt-connect with the reinforcement beam at the interface of mutual contact; keep the pressure and cool to shape, so as to form a connection coating layer, and the connection coating layer is bonded to the through-hole card, so as to realize that the reinforcement beam, the groove of the substrate and the connection coating layer are connected into a whole, and the finished product is demoulded.

[0090] Specifically, for the preparation of reinforced beams, taking continuous carbon fiber reinforced PA6 as an example, the reinforced beams can be prepared by the following steps:

[0091] (1) Pulling the continuous carbon fiber out of the creel, the pulling action is controlled by the pulling system of the composite material pultrusion equipment;

[0092] (2) The guide plate collects the continuous carbon fibers into bundles and then guides them into the injection mold;

[0093] (3) The mold is preheated to 150° C., and the continuous carbon fiber enters the injection mold, where liquid PA6 prepolymer liquid is injected to immerse the continuous carbon fiber in the PA6 prepolymer liquid;

[0094] (4) The continuous carbon fiber soaked in PA6 prepolymer liquid leaves the injection mold and enters the polymerization section of the mold so that the material reacts and polymerizes in the mold to form a reinforced beam;

[0095] (5) Cooling and solidification, cutting the solidified product into required lengths by cutting tools to obtain a preliminarily formed reinforced beam.

[0096] After the reinforcement beam is pultruded, it is a straight structure with equal cross-section. In order to match the reinforcement beam with the groove structure and direction, secondary shaping is required. The specific steps are as follows:

[0097] (6) heating and softening the preliminarily formed reinforced beam, and the heating method may be thermal convection heating or infrared radiation heating;

[0098] (7) The softened material is transferred to a molding die for secondary molding or shaping.

[0099] (8) After cooling, take out the shaped reinforced beam.

[0100] When the continuous carbon fiber unidirectional tape of pre-impregnated PA6 is used as the starting point of the process, the pre-impregnated unidirectional tape can be pulled out from the creel; it enters the forming mold and is collected into bundles. After the material softens, it is gathered, heated, and initially formed in the mold; it is cooled and cut into the required length, and then reshaped to finalize the shape.

[0101] Example 6 CAE (Computer Simulation Analysis) Comparison of the Protection Performance of Door Collision Resistance Components

[0102] 1. The vehicle door collision resistance component of the utility model

[0103] The same preferred door collision resistance component structure as in Example 1 is adopted: the metal material of the substrate is DP980 steel, there are two grooves, the groove depth is 27 mm, the continuous fiber for the reinforcing beam is carbon fiber, the thermoplastic material for the reinforcing beam is PA6, the short fiber for the connecting coating layer is carbon fiber, the thermoplastic material for the connecting coating layer is PA6, the volume of the connecting coating layer accounts for 60% of the volume of the groove, and the ratio of the total weight of the connecting coating layer and the reinforcing beam to the weight of the substrate is 1:1.97.

[0104] 2. Comparison of door collision resistance components

[0105] Double groove strip metal plate (M-shaped cross section) with the same metal material and weight as in Part 1 of this embodiment. That is, strength comparison under the same weight.

[0106] 3. Comparison results

[0107] According to the analysis guidelines such as the "Automobile Crash Simulation Analysis Specifications", CAE analysis is carried out under the same analysis conditions.

[0108] The collision energy absorption value of the vehicle door collision resistance component of the utility model is increased by 15% compared with the comparative vehicle door collision resistance component.

Claims

1. A door collision resistance member, It is characterized in that The door collision resistance component includes: a substrate made of stampable metal, a reinforcing beam made of continuous fiber reinforced thermoplastic material that can be pultruded, and a connecting coating layer made of short fiber reinforced thermoplastic material that can be injection molded; the substrate is provided with at least one groove in the extension direction; the bottom wall and / or side wall of the groove are provided with a through hole for the hot-melt connecting coating layer to pass through; the main cross-section of the reinforcing beam is one of rectangular, trapezoidal, triangular or semicircular, with a cross-sectional width of 3mm~12mm and a cross-sectional height of 5mm~20mm; the reinforcing beam and the connecting coating layer are located in the groove, the connecting coating layer is embedded in the groove and is bonded to the groove through the through hole; the connecting coating layer forms a continuous or intermittent surface contact with at least the lower surface of the reinforcing beam, and the connecting coating layer and the reinforcing beam are melt-connected at the contact surface where they contact each other.

2. The door collision resistance member according to claim 1, It is characterized in that Two grooves are arranged in the extension direction of the substrate.

3. The door impact resistance member according to claim 1, It is characterized in that The groove is provided with a cavity compartment separated by a connecting cladding layer; the cavity compartment is formed by a recessed structure provided in the connecting cladding layer itself, or is enclosed by the connecting cladding layer and the side wall of the groove and / or the reinforcing beam.

4. The door impact resistance member according to claim 3, It is characterized in that The cavity compartment is formed by the connecting cladding layer, the groove and the side wall of the reinforcing beam; in the side wall of the cavity compartment, the wall thickness of the connecting cladding layer located between the groove and the side wall of the reinforcing beam is 2.5 mm to 7 mm.

5. The door impact resistance member according to claim 1, It is characterized in that The metal of the substrate is selected from DP steel, CP steel, QP steel, DH steel, and martensitic steel.

6. The door impact resistance member according to claim 1, It is characterized in that The thickness of the substrate is 1.2 mm to 2 mm.

7. The door impact resistance member according to claim 1, It is characterized in that The continuous fiber of the reinforcement beam is selected from one of glass fiber, carbon fiber and glass-carbon mixed fiber; the thermoplastic material of the reinforcement beam is selected from one of polyamide material, polymethyl methacrylate material and polycarbonate material.