Semi-insulating GaN micro-groove type neutron detector filled with 6LiF

By filling the 6LiF neutron conversion material in the GaN microtrench neutron detector, the problems of insufficient ray energy absorption and low neutron detection efficiency of GaN materials are solved, and higher detection efficiency and energy resolution are achieved.

CN222070841UActive Publication Date: 2024-11-26JIANGXI YUHONGJIN MATERIAL TECHNOLOGY CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202420427945.0
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2024-03-06
Publication Date
2024-11-26
Estimated Expiration
2034-03-06

AI Technical Summary

Technical Problem

The detection efficiency and energy resolution of GaN-based nuclear radiation detectors are limited because the radiation energy cannot be fully absorbed by GaN materials. After the traditional neutron detector covers the neutron conversion layer on the surface, the secondary charged particles have limited range and cannot be completely Absorption leads to low neutron detection efficiency.

Method used

Design a semi-insulated GaN micro-trench neutron detector filled with 6LiF, using semi-insulated GaN self-supporting substrate and combined mask layer to form a micro-trench structure, depositing Si3N4 passivation layer and Schottky contact metal The electrode is filled with 6LiF neutron conversion material to increase the contact area of ​​neutron reaction and improve detection efficiency.

Benefits of technology

Through high-quality GaN materials and microtrench structure, the neutron detection efficiency and energy deposition rate are improved, the probability of neutron reaction products entering the GaN materials is increased, and the charge collection efficiency and the overall performance of the detector are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222070841U_ABST
    Figure CN222070841U_ABST
Patent Text Reader

Abstract

The utility model discloses a semi-insulating GaN micro-groove type neutron detector filled with 6LiF, which comprises a semi-insulating GaN self-supporting substrate, a combined mask layer or a photoresist mask layer, a Si3N4 passivation layer, a micro-groove structure, a front Schottky contact metal electrode, a back ohmic contact metal electrode and a 6LiF neutron conversion layer material filled on the front, neutrons are incident from the Schottky contact metal electrode on the front surface; in the neutron detection process, the contact area of the GaN material and the neutron conversion layer is greatly increased through the micro-groove structure on the front face, and therefore the probability that charged particles emitted in an isotropic mode enter a semiconductor material can be effectively increased; the thickness of the semi-insulating GaN self-supporting substrate is 200-400 [mu] m, it can be guaranteed that secondary charged particles generated in the neutron detection process can completely lose energy in a GaN material, and the detection efficiency is greatly improved; in addition, the third-generation semiconductor GaN has excellent physical and chemical characteristics such as wide forbidden band and high threshold energy, so that the GaN shows more excellent performance in severe environments such as high temperature, high pressure and intense radiation compared with Si, GaAs and other materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the technical field of semiconductor radiation detection devices, in particular to a filling 6 Semi-insulating GaN micro-trench neutron detector based on LiF. Background Art

[0002] Compared with first- and second-generation semiconductor materials such as Si and GaAs, GaN, as the third-generation wide bandgap semiconductor material, has a much larger bandgap width (3.39 eV) than Si and GaAs, and has a large potential threshold energy. In addition, its physical and chemical properties are extremely stable, which makes GaN material have great advantages and application prospects in high temperature, high pressure and strong radiation environments.

[0003] Due to the limitations of the GaN material epitaxial process, GaN films epitaxially grown using metal organic chemical vapor deposition (MOCVD) are generally thin, usually not exceeding 10μm, while the range of α particles in GaN is generally more than 10μm, resulting in the radiation energy not being well absorbed by the GaN material, thereby limiting the detection efficiency and energy resolution of GaN-based nuclear radiation detectors.

[0004] For traditional semiconductor neutron detectors, in order to achieve neutron detection, the solution is usually to deposit a neutron conversion layer on the surface of the semiconductor device. Its working principle is to coat the neutron conversion layer on the surface of the semiconductor detector. When neutron detection is performed, the neutron reacts with the neutron conversion layer and produces secondary charged particles with a certain energy. Then, the indirect detection of neutrons is achieved through the detection and analysis of the secondary charged particles. In order to increase the probability of neutron capture, thickening the neutron coating layer is the simplest and most commonly used method. However, simply covering the surface of the detector with a thick layer of neutron conversion layer may not effectively improve the neutron detection efficiency. Instead, it may make the secondary charged particles unable to pass through the neutron conversion layer due to their limited range, resulting in them not being completely absorbed by the semiconductor detector, thereby limiting the semiconductor detector's detection efficiency for neutrons. Utility Model Content

[0005] The technical problem solved by the utility model is to provide a filling 6 A LiF semi-insulating GaN micro-groove neutron detector is provided to solve the problem of limited neutron detection efficiency in the above-mentioned background technology.

[0006] The technical problem solved by the utility model is achieved by the following technical solutions:

[0007] A filling 6The invention discloses a semi-insulating GaN micro-groove type neutron detector of LiF, comprising a semi-insulating GaN self-supporting substrate, a combination mask layer or a photoresist mask layer is deposited on the semi-insulating GaN self-supporting substrate, a micro-groove structure is etched on the semi-insulating GaN self-supporting substrate deposited with the combination mask layer or the photoresist mask layer, and Si is deposited on the surface of the micro-groove structure. 3 N 4 Passivation layer, using photolithography and RIE dry etching to etch away part of the Si 3 N 4 The passivation layer is used as the front Schottky contact metal area, and then Ni / Au is deposited in the front Schottky area in sequence by electron beam evaporation to form the front Schottky metal electrode, and Ti / Al / Ti / TiN is deposited in sequence on the back of the semi-insulating GaN self-supporting substrate by magnetron sputtering coating process to form the back ohmic metal electrode; finally, 6 LiF neutron conversion material is filled into the front micro-grooves for neutron reaction, and neutrons are incident from the front Schottky metal electrode.

[0008] Furthermore, the resistivity of the semi-insulating GaN self-supporting substrate is greater than 1×10 12 Ω·cm, thickness range is 200~450μm, dislocation density is <1×10 6 cm -2 .

[0009] Furthermore, when a photoresist mask layer is deposited on a semi-insulating GaN self-supporting substrate, the thickness of the photoresist mask layer is 9 to 12 μm; the width of the groove after etching is 10 to 30 μm, the depth is 5 to 50 μm, the two sides of the groove wall are not perpendicular, the ratio of the groove wall width to the groove width is ≤1:1, and decreases with the increase of etching depth.

[0010] Further, when a combined mask layer is deposited on a semi-insulating GaN self-supporting substrate, the combined mask layer includes a Ni metal mask layer, a Si 3 N 4 The mask layer and the photoresist mask layer, wherein the thickness of the Ni metal mask layer is 200-300nm, and the thickness of the Si 3 N 4 The thickness of the mask layer is 600-800nm, and the thickness of the photoresist mask layer is 9-12μm; after etching, the groove is rectangular, the width of the groove is 10-30μm, the depth is 5-50μm, and the ratio of the groove wall width to the groove width is 1:1.

[0011] Further, the Si 3 N 4 The thickness of the passivation layer is 200-400 nm.

[0012] Furthermore, the thickness of Ni in the front Schottky contact metal electrode is 50-100 nm, and the thickness of Au is 100-200 nm.

[0013] Furthermore, the thickness of the bottom layer Ti in the back ohmic contact metal electrode is 6-20 nm, the thickness of the second layer Al is 120-200 nm, the thickness of the third layer Ti is 200-500 nm, and the thickness of the top layer TiN is 50-100 nm.

[0014] Further, the 6 The LiF neutron conversion material is in the form of irregular powder. Beneficial Effects

[0015] The semi-insulating GaN substrate in the utility model is a third-generation wide bandgap semiconductor material. Due to its excellent physical and chemical properties such as wide bandgap and high threshold energy, GaN has more stable performance than Si, GaAs and other materials in harsh environments such as high temperature, high pressure, and strong radiation;

[0016] In the utility model, the semi-insulating GaN material is a high-quality GaN self-supporting substrate 1 with a thickness of 200-400 μm, which can ensure that the secondary charged particles generated during the neutron detection process can have a higher energy deposition rate in the GaN material, greatly improving the detection efficiency;

[0017] The two different etching mask layers in the utility model will have different effects on the subsequent dry etching of the micro-groove structure; the three-layer combination mask of Ni plus Si3N4 plus photoresist is used, because the uppermost Si3N4 plus photoresist mask layer is thick enough, and the bottom metal Ni protects the step edge, so that the step edge after etching is flat and the groove wall is vertical; only the photoresist is used as a mask, because the positive photoresist used is in a positive trapezoidal shape after photolithography, as the etching depth increases, the side wall of the groove after etching becomes more inclined, and the micro-groove as a whole is also in a positive trapezoidal shape;

[0018] In the utility model, since the secondary charged particles generated by the reaction of neutrons and the conversion material are isotropically emitted, after the micro-groove structure is formed on the front side, the 6 The contact area between the LiF neutron conversion layer and the detector increases the probability that the reaction products of neutrons and the neutron conversion layer enter the GaN material.

[0019] The utility model uses a semi-insulating GaN substrate with a high resistivity and a Schottky contact metal electrode deposited on the front side, so that the reverse leakage current of the detector can be kept at a low level. After the reverse bias voltage is applied, the Schottky barrier height is effectively increased, the depletion region is widened, and the probability of charged particles losing energy in the depletion region is increased, which will generate more electron-hole pairs, thereby improving the charge collection efficiency and neutron detection efficiency of the detector. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a structural schematic diagram of a combined mask layer in a preferred embodiment 1 of the utility model;

[0021] Figure 2 This is a schematic diagram of the structure of a preferred embodiment 1 of the utility model;

[0022] Figure 3 This is a schematic diagram of the structure of a preferred embodiment 2 of the present utility model; DETAILED DESCRIPTION

[0023] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below with reference to specific illustrations.

[0024] Example 1: See Figure 1 and Figure 2 The invention comprises a semi-insulating GaN self-supporting substrate 1, a Ni metal mask layer 2, and a Si 3 N 4 Mask layer 3, photoresist mask layer 4, micro-groove structure 5, Si 3 N 4 Passivation layer 6, front Schottky contact metal electrode 7, back ohmic contact metal electrode 8, 6 LiF neutron conversion material 9, the specific preparation method is as follows:

[0025] First, select the resistivity>1.0×10 12 Ω·cm, thickness range is 200~450μm, dislocation density is <1×10 6 cm -2 The semi-insulating GaN self-supporting substrate 1 was placed in acetone, anhydrous ethanol, and deionized water for ultrasonic cleaning for 10 minutes to remove organic matter on the surface; then placed in SPM (mass ratio H 2 SO:H 2 O 2 :H 2 O=1:1:3) solution, control the temperature to 100℃, soak for 5min to remove inorganic dirt on the surface; then put in HCl:H 2 O (mass ratio 1:1) for 120s to remove the surface oxide layer; finally, the substrate is blown dry with high-purity nitrogen to complete the surface cleaning of the front side of the substrate.

[0026] After the surface is cleaned, a Ni metal mask layer 2 is deposited on the semi-insulating GaN self-supporting substrate 1 using an electron beam evaporation coating process, and then a Si layer is grown using PECVD. 3 N 4After depositing two layers of hard mask, a photoresist mask layer 4 is formed on the surface by photolithography, wherein the thickness of the Ni metal mask layer is 200-300nm, and the Si 3 N 4 The thickness of the mask layer 3 is 600-800 nm, and the thickness of the photoresist mask layer is 9-12 μm; finally, RIE and IBE are used to respectively remove the Si 3 N 4 The Ni and metal Ni are removed cleanly, and the upper photoresist is retained, finally forming Ni+Si 3 N 4 +The three-layer combination mask of photoresist completes the mask layer deposition work.

[0027] Micro-groove etching is performed using an ICP etcher. Due to the protection of the underlying Ni metal mask layer 2 and the Si 3 N 4 The sacrifice of mask layer 3 makes the groove rectangular after ICP etching, with a width of 10-30 μm, a depth of 5-50 μm, and a ratio of the groove wall width to the groove width of 1:1; after the dry etching, the film is immersed in a stripping solution (NMP-80°C), BOE (6:1) and SPM solution for 30 min, 16 min and 5 min respectively, to remove the remaining photoresist and Si after etching. 3 N 4 and Ni are removed completely; finally, after soaking in TMAH (25% / 80°C) solution for 30 minutes, the etching of the micro groove 5 is completed.

[0028] Then PECVD is used to grow Si on the micro-groove surface. 3 N 4 Passivation layer 6, Si 3 N 4 The thickness of the passivation layer 6 is 200-400 nm. The Schottky contact window is left on the micro-groove surface by photolithography, and then a combination of dry etching and wet etching is used to first use RIE dry etching to etch the 150-180 nm thick Si 3 N 4 , use BOE wet etching to remove the remaining Si 3 N 4 Remove cleanly and complete the window opening work of Schottky contact metal.

[0029] Finally, Ni / Au is deposited in the Schottky region in sequence using an electron beam evaporation coating process, wherein the thickness of Ni is 50-100 nm and the thickness of Au is 100-200 nm, so as to form a front Schottky contact metal electrode 7; Ti / Al / Ti / TiN is deposited in sequence on the back side using a magnetron sputtering coating process, wherein the thickness of the bottom layer Ti is 6-20 nm, the thickness of the second layer Al is 120-200 nm, the thickness of the third layer Ti is 200-500 nm, and the thickness of the top layer TiN is 50-100 nm, so as to form a back ohmic contact metal electrode 8; finally, a filling method combining ultrasound and centrifugation is used to fill the 6 LiF neutron conversion material 9 is filled into the micro groove 5 to perform neutron reaction, and neutrons are incident from the front Schottky metal electrode; 6 LiF neutron conversion material is in irregular powder form. Ultrasonic technology is used to fill it. 6 LiF is evenly dispersed in alcohol, and then the neutron detector to be filled is fixed at the bottom of the reagent container. 6 The reagent container is filled with alcohol containing LiF neutron conversion material, and then centrifugal technology is used to spin the LiF neutron conversion material at high speed. 6 The LiF neutron conversion material is filled into the micro grooves, wherein the centrifuge speed is 3000 r / min, the time is 2.5 min, and the centrifugation is repeated 10 to 20 times to ensure the compactness of the neutron filling material.

[0030] Example 2: See Figure 3 As shown, the difference from Example 1 is that after the surface cleaning is completed, only photoresist is used as a mask layer, and only the photolithography process needs to be performed on the front side of the semi-insulating GaN substrate 1. The thickness of the photoresist mask layer is 9 to 12 μm; the width of the groove after etching is 10 to 30 μm, the depth is 5 to 50 μm, the two sides of the groove wall are not vertical, the ratio of the groove wall width to the groove width is ≤1:1, and decreases with the increase of the etching depth.

Claims

1. A filling 6 LiF semi-insulating GaN micro-trench neutron detector, characterized in that, The invention comprises a semi-insulating GaN self-supporting substrate (1), wherein a combined mask layer or a photoresist mask layer is deposited on the semi-insulating GaN self-supporting substrate (1), a micro-groove structure (5) is etched on the semi-insulating GaN self-supporting substrate (1) deposited with the combined mask layer or the photoresist mask layer, a Si3N4 passivation layer (6) is deposited on the surface of the micro-groove structure (5), a part of the Si3N4 passivation layer (6) is etched away by photolithography and RIE dry etching to form a front-side Schottky contact metal region, and then Ni / Au is sequentially deposited on the front Schottky region by an electron beam evaporation process to form a front Schottky metal electrode (7), and Ti / Al / Ti / TiN is sequentially deposited on the back of the semi-insulating GaN self-supporting substrate (1) by a magnetron sputtering coating process to form a back-side ohmic metal electrode (8); finally, 6 LiF neutron conversion material is filled into the front micro-grooves for neutron reaction, and neutrons are incident from the front Schottky metal electrode.

2. The neutron detector according to claim 1, characterized in that The resistivity of the semi-insulating GaN self-supporting substrate (1) is greater than 1×10 12 Ω·cm, thickness range is 200~450μm, dislocation density is <1×10 6 cm -2 .

3. The neutron detector according to claim 1, characterized in that When a photoresist mask layer (4) is deposited on a semi-insulating GaN self-supporting substrate (1), the thickness of the photoresist mask layer is 9 to 12 μm; after etching, the width of the groove is 10 to 30 μm, the depth is 5 to 50 μm, the two sides of the groove wall are not perpendicular, the ratio of the groove wall width to the groove width is ≤1:1, and decreases with increasing etching depth.

4. The neutron detector according to claim 1, characterized in that When a combined mask layer is deposited on a semi-insulating GaN self-supporting substrate (1), the combined mask layer comprises, from bottom to top, a Ni metal mask layer, a Si3N4 mask layer (3) and a photoresist mask layer, wherein the thickness of the Ni metal mask layer is 200-300 nm, the thickness of the Si3N4 mask layer (3) is 600-800 nm, and the thickness of the photoresist mask layer is 9-12 μm; after etching, the groove is rectangular, the width of the groove is 10-30 μm, the depth is 5-50 μm, and the ratio of the groove wall width to the groove width is 1:

1.

5. The neutron detector according to claim 1, characterized in that The thickness of the Si3N4 passivation layer (6) is 200-400 nm.

6. The neutron detector according to claim 1, characterized in that The thickness of Ni in the front Schottky contact metal electrode is 50 to 100 nm, and the thickness of Au is 100 to 200 nm.

7. The neutron detector according to claim 1, characterized in that The thickness of the bottom Ti layer in the back ohmic contact metal electrode (8) is 6-20 nm, the thickness of the second Al layer is 120-200 nm, the thickness of the third Ti layer is 200-500 nm, and the thickness of the top TiN layer is 50-100 nm.

8. The neutron detector according to claim 1, characterized in that described 6 The LiF neutron conversion material is in the form of irregular powder.

Citation Information

Cited By

  • Method and device for filling neutron conversion material in semiconductor microstructure groove

    CN119451286A

  • Method and device for filling neutron conversion material in semiconductor microstructure trenches

    CN119451286B