Composite board and rail transit floor
By using thermoplastic resin honeycomb structure and foam filling design in composite panels, combined with continuous fiber reinforced layer and aluminum alloy surface layer, the problem of poor mass and durability of composite panels is solved, achieving higher mechanical properties and better Lightweight, suitable for high load and anti-aging needs of rail transit floors.
Patent Information
- Application Number
- CN202323490701.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-19
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2033-12-19
AI Technical Summary
The existing composite panels are heavier in rail transit floors and have poor durability, making it difficult to meet the requirements of long-term use.
Designed with composite panels including thermoplastic resin honeycomb structure and thermoplastic foam. The surface of the honeycomb structure is free of holes. The reinforcement layer is composed of continuous fiber reinforced thermoplastic resin. It is combined through hot melt cooling to increase the interface bonding force, and aluminum is used in the surface layer. Alloys and alumina materials.
It improves the mechanical properties and durability of composite panels, reduces overall quality, enhances interface bonding, avoids stratification problems, and meets the high load and anti-aging performance requirements of rail transit floors.
Smart Images

Figure CN222080300U_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of composite panels, and in particular to a composite panel and a rail transit floor. Background Art
[0002] Rail transit floor is an important load-bearing component inside rail transit vehicles. Its function is to bear the weight of passengers or cargo, and also to withstand the vibration and impact during the operation of the vehicle. Therefore, rail transit floor needs to have high load-bearing capacity and durability, as well as good anti-slip, fireproof, sound insulation and other properties.
[0003] Rail transit floors are usually made of composite panels, the materials and structures of which need to be designed and strictly manufactured to ensure their safety and reliability.
[0004] Composite panels usually use a composite structure of a middle aluminum honeycomb, an upper aluminum panel, and a lower aluminum panel, and are made into floors with frame profiles and embedded parts or connectors set therebetween. However, aluminum alloy is heavy, and the bonding force between the layers of the composite panel is linear contact bonding, which is difficult to meet the durability requirements of long-term use.
[0005] Therefore, it is necessary to develop a new composite board and rail transit floor. Utility Model Content
[0006] An embodiment of the present disclosure provides a composite board, comprising: a core layer, comprising: at least one layer of honeycomb structure, the material of the honeycomb structure comprising thermoplastic resin; thermoplastic foam filled in the honeycomb structure; a surface layer, located on opposite sides of the core layer, bonded and fixed to the core layer, the material of the surface layer comprising metal.
[0007] In some embodiments, the core layer includes two layers of honeycomb structures, and the honeycomb holes of the two layers of honeycomb structures are staggered with each other.
[0008] In some embodiments, the material of the honeycomb structure includes: one or more of polypropylene, polyethylene terephthalate and nylon.
[0009] In some embodiments, the thermoplastic foam includes one or more of polypropylene foam, polyethylene terephthalate foam and nylon foam.
[0010] In some embodiments, the material of the honeycomb structure includes: one or both of polypropylene or polyethylene terephthalate; and the thermoplastic foam is polypropylene foam.
[0011] In some embodiments, the honeycomb structure has a thickness of 3 to 300 mm.
[0012] In some embodiments, the core layer further includes: a reinforcement layer bonded to at least one side of the honeycomb structure and located between the honeycomb structure and the surface layer, and the material of the reinforcement layer includes continuous fiber reinforced thermoplastic resin.
[0013] In some embodiments, the thickness of the reinforcement layer is 0.5 mm to 2 mm.
[0014] In some embodiments, the composite board further includes: a thermoplastic film layer, located on opposite sides of the core layer and bonded to the core layer and the surface layer respectively.
[0015] In some embodiments, the surface layer includes: a main body layer, the material of the main body layer includes aluminum alloy; and a treatment layer located on the surface of the main body layer, the material of the treatment layer includes aluminum oxide.
[0016] In some embodiments, the thickness of the surface layer is 0.3 mm to 1 mm.
[0017] In some embodiments, the composite board has at least one of the following properties: i) the peel strength between the surface layer and the core layer is above 150 N·cm / cm; ii) the peel strength between the two surface layers is above 110 N·cm / cm; iii) the compressive strength of the composite board is above 4.5 MPa; iv) the tensile strength of the composite board is above 5.5 MPa; v) the bending strength of the composite board is above 40 MPa.
[0018] An embodiment of the present disclosure further provides a rail transit floor, comprising: any of the above-mentioned composite panels; a frame, which is fittedly arranged on at least one side of the core layer, and the material of the frame is metal or fiber-reinforced thermoplastic resin.
[0019] In some embodiments, the frame is made of aluminum alloy, and an oxide layer is formed on the surface of the frame.
[0020] In some embodiments, the frame is made of short glass fiber reinforced polyethylene terephthalate resin, and the honeycomb structure is made of polyethylene terephthalate resin.
[0021] Compared with the prior art, the technical solution of the embodiment of the present disclosure has the following beneficial effects:
[0022] The core layer of the embodiment of the present invention has a honeycomb structure filled with thermoplastic foam, and the surface of the honeycomb structure presents a hole-free surface, thereby increasing the contact area between the honeycomb structure and the surface layer or the reinforcement layer, thereby increasing the interface bonding strength, being less likely to have delamination problems, and increasing durability of use.
[0023] The core layer of the embodiment of the present disclosure is a thermoplastic resin honeycomb structure filled with thermoplastic foam. Compared with the traditional aluminum honeycomb structure, it has a lighter weight and good mechanical properties.
[0024] The core layer of the embodiment of the present disclosure includes two or more honeycomb structures, and the honeycombs between adjacent layers of the honeycomb structures are staggered. Compared with the single-layer honeycomb structure with the same thickness, the multi-layer honeycomb structure has better mechanical properties, especially a higher concentrated load, and can be used in scenarios with high requirements for concentrated loads.
[0025] The reinforcement layer of the embodiment of the present disclosure further enhances the mechanical properties of the composite plate, can reduce the thickness of the surface layer of the metal material, and thus reduce the overall mass of the composite plate; since the material of the reinforcement layer includes continuous fiber reinforced thermoplastic resin, the honeycomb structure and thermoplastic foam of the core layer are both thermoplastic materials, the reinforcement layer and the core layer are easy to process and bond, and have good bonding properties.
[0026] The rail transit floor of the embodiment of the present disclosure has good load-bearing performance, can meet the use requirements of the rail transit floor, and has a lighter weight than the traditional aluminum honeycomb floor. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Other features and advantages of the present disclosure will be better understood through the following detailed description of the optional embodiments in conjunction with the accompanying drawings, in which the same reference numerals represent the same or similar components, wherein:
[0028] Figure 1 A schematic structural diagram of a composite plate according to an embodiment of the present disclosure is shown;
[0029] Figure 2 A schematic structural diagram of a core layer according to an embodiment of the present disclosure is shown. DETAILED DESCRIPTION
[0030] Embodiments of the present disclosure are described in detail below, and examples of the embodiments are shown in the accompanying drawings. In the accompanying drawings, the same or similar reference numerals represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present disclosure, and cannot be understood as limiting the present disclosure.
[0031] Unless otherwise defined, the technical terms or scientific terms used herein shall have the usual meanings understood by persons with ordinary skills in the field to which the present disclosure belongs. In the description of the present disclosure, it should be understood that the terms "center", "longitudinal", "lateral", "upper", "lower", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present disclosure and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation to the present disclosure.
[0032] In order to solve the problems of heavy weight and poor durability of existing composite panels, the embodiments of the present disclosure provide a composite panel, a rail transit floor and a preparation method thereof. The technical solutions of the embodiments of the present disclosure are described in detail below in conjunction with the accompanying drawings.
[0033] Figure 1 A schematic structural diagram of a composite plate according to an embodiment of the present disclosure is shown; Figure 2 : shows a schematic diagram of the structure of the core layer according to an embodiment of the present disclosure; to more clearly show the structure of the composite board of the embodiment of the present disclosure, Figure 1 and Figure 2 The structural diagrams shown in the figure are all exploded views. Figure 1 and Figure 2 The embodiment of the present disclosure provides a composite board 1, the composite board 1 comprising: a core layer 11; and surface layers 12 located on opposite sides of the core layer 11; the core layer 11 and the surface layer 12 are bonded and fixed. The core layer 11 comprises: at least one layer of honeycomb structure 111 and thermoplastic foam 112, the material of the honeycomb structure 111 comprises thermoplastic resin, and the thermoplastic foam is filled in the honeycomb structure 111.
[0034] The core layer 11 of the embodiment of the present disclosure is a thermoplastic resin honeycomb structure 111 filled with thermoplastic foam 112 , which has a lighter weight and good mechanical properties compared to an aluminum honeycomb structure.
[0035] Since the honeycomb structure 111 is filled with thermoplastic foam 112, the surface of the honeycomb structure 111 is a non-porous surface, which increases the surface area of the honeycomb structure 111 compared to the honeycomb structure not filled with thermoplastic foam, thereby increasing the interface bonding force between the honeycomb structure 111 and other layers, making it less likely to have delamination problems, thereby increasing the service life of the composite board 1. The mechanical properties of the honeycomb structure 111 filled with thermoplastic foam 112 are further enhanced, thereby enhancing the overall mechanical properties of the composite board 1.
[0036] In some embodiments, the material of the honeycomb structure 111 of the embodiments of the present disclosure includes: one or more of polypropylene (PP), polyethylene terephthalate (PET) and nylon (PA).
[0037] In some embodiments, the thermoplastic foam 112 of the embodiments of the present disclosure includes: one or more of polypropylene (PP) foam, polyethylene terephthalate (PET) foam and nylon (PA) foam.
[0038] The honeycomb structure 111 and the thermoplastic foam 112 may be made of the same or different thermoplastic polymers. In some embodiments, the material of the honeycomb structure 111 includes one or both of polypropylene or polyethylene terephthalate, and the thermoplastic foam 112 is polypropylene foam.
[0039] In order to increase the flame retardant performance of the composite board 1, in some embodiments, the material of the honeycomb structure 111 is a flame retardant modified thermoplastic resin; in some embodiments, the material of the honeycomb structure 111 is a homopolymer polypropylene modified with a nitrogen-phosphorus flame retardant, and the compression strength of the honeycomb structure is above 4Mpa and the density is 150kg / m 3 about.
[0040] In order to increase the flame retardant performance of the composite board 1 , in some embodiments, the thermoplastic foam 112 is a flame retardant modified thermoplastic foam; in some embodiments, the thermoplastic foam 112 is polypropylene modified with a nitrogen-phosphorus flame retardant.
[0041] In some embodiments, the honeycomb structure 111 includes: a plurality of honeycomb walls; a plurality of honeycomb holes, each of which is formed between the plurality of honeycomb walls, and the thermoplastic foam 112 is filled in the honeycomb holes.
[0042] In some embodiments, the thickness of the honeycomb wall of the honeycomb structure 111 is 0.3 mm to 0.6 mm.
[0043] In some embodiments, the diameter of the honeycomb holes of the honeycomb structure 111 is 6 mm to 9 mm, and the thermoplastic foam 112 is filled in the honeycomb holes; in some embodiments, the thermoplastic foam 112 fills all the honeycomb holes.
[0044] In some embodiments, the opening direction of the honeycomb holes of the honeycomb structure 111 faces the surface layer 12 .
[0045] The thickness of the honeycomb structure 111 can be obtained by cutting according to the needs of actual application. In some embodiments, the thickness of the honeycomb structure 111 is 3 to 300 mm; in some embodiments, the thickness of the honeycomb structure 111 is 4 to 50 mm; in some embodiments, the thickness of the honeycomb structure 111 is 15 to 30 mm.
[0046] In some embodiments, the core layer 11 includes a two-layer honeycomb structure, and the honeycomb holes of the two-layer honeycomb structure are staggered, which has better mechanical properties, especially higher concentrated loads, compared with a single-layer honeycomb structure of the same thickness, and can be applied to scenes with high requirements for concentrated loads. In some embodiments, the core layer 11 includes a three-layer honeycomb structure, and the honeycombs between adjacent layers of the honeycomb structure are staggered, so as to have better mechanical properties, especially higher concentrated loads.
[0047] Continue to refer Figure 2 In some embodiments, the composite board 1 further comprises: a reinforcement layer 113, which is bonded to at least one side of the honeycomb structure 111 and is located between the honeycomb structure 111 and the surface layer 12. In some embodiments, the reinforcement layer 113 is bonded to both opposite sides of the honeycomb structure 111.
[0048] In some embodiments, the material of the reinforcement layer 113 includes continuous fiber reinforced thermoplastic resin, and the continuous fiber can be one or more of glass fiber, plant fiber, and carbon fiber; the thermoplastic resin includes: one or more of polypropylene (PP) resin, polyethylene terephthalate (PET) resin, polyamide (PA) resin, polyphenylene sulfide (PPS) resin and polyetheretherketone (PEEK) resin.
[0049] The reinforcing layer 113, the honeycomb structure 111 and the thermoplastic foam 112 are all made of thermoplastic materials, and are combined into a whole by hot-melt cooling, and have high interface strength. In some embodiments, the reinforcing layer 113, the honeycomb structure 111 and the thermoplastic foam 112 are made of the same thermoplastic resin; in some embodiments, the reinforcing layer 113 is made of continuous fiber reinforced polypropylene resin, the honeycomb structure 111 is made of polypropylene, and the thermoplastic foam 112 filled in the honeycomb structure 111 is polypropylene foam. The polypropylene material is melted by heat during the molding process, and has good interface bonding after cooling.
[0050] Compared with thermosetting plastics, thermoplastics have better recyclability, reduce the impact on the environment, and are conducive to the conservation and utilization of resources.
[0051] In some embodiments, the thickness of the reinforcement layer 113 is 0.5 mm to 2 mm, for example 0.5 mm, 0.8 mm, 1 mm, 1.5 mm, 2 mm, and the like.
[0052] The reinforcement layer 113 of the embodiment of the present disclosure further enhances the mechanical properties of the composite plate and can reduce the thickness of the surface layer 12 of the metal material, thereby reducing the overall mass of the composite plate 1 while ensuring the mechanical properties.
[0053] Continue to refer Figure 1In some embodiments, the composite board 1 further includes a thermoplastic film layer 13 , which is located on opposite sides of the core layer 11 and is bonded to the core layer 11 and the surface layer 12 respectively, that is, the core layer 11 and the surface layer 12 are bonded and fixed by the thermoplastic film layer 13 .
[0054] In some embodiments, the thermoplastic film layer 13 includes: a film carrier; and modified layers bonded to both sides of the film carrier.
[0055] In some embodiments, the material of the adhesive film carrier is a thermoplastic resin, specifically but not limited to, an ethylene-propylene-based resin; the adhesive film carrier can withstand high temperatures above 100°C.
[0056] In some embodiments, the material of the modified layer can be a thermoplastic resin modified with maleic anhydride and polyolefin elastomer to improve the bonding strength and toughness with the metal; further, it can be a thermoplastic resin modified with an antioxidant to enhance the antioxidant ability; it should be noted that the specific modification is selected according to actual needs, and is only used as an example here, and does not constitute a limitation to the technical solution of the present disclosure.
[0057] In some embodiments, the material of the modified layer is ethylene propylene based resin modified with maleic anhydride, polyolefin elastomer and antioxidant.
[0058] In some embodiments, the total thickness of the two modified layers is 20% to 30% of the thickness of the adhesive film carrier.
[0059] Compared with traditional polyurethane glue which is prone to powdering and stratification after long-term use, the thermoplastic film layer 13 of the embodiment of the present invention is used to bond the core layer 11 and the surface layer 12, has good bonding effect and stability, can meet the requirements of moisture and heat / salt spray resistance, and has good toughness and strong fatigue resistance.
[0060] Continue to refer Figure 1 In some embodiments, the surface layer 12 of the composite board 1 includes: a body layer and a treatment layer located on the surface of the body layer.
[0061] In some embodiments, the material of the body layer includes aluminum alloy, and the material of the handle layer includes aluminum oxide.
[0062] In some embodiments, the treatment layer is formed by oxidation treatment of the surface of the surface layer 12 . The treatment layer is closer to the core layer 11 than the body layer. The treatment layer has better bonding force with the thermoplastic resin than the body layer.
[0063] In some embodiments, the thickness of the surface layer 12 is 0.3 mm to 1 mm, and the thickness of the treatment layer is 0.015 mm to 0.02 mm.
[0064] The composite board 1 of the embodiment of the present disclosure has at least one of the following properties:
[0065] i) The peel strength between the surface layer and the core layer is above 150N·cm / cm;
[0066] ii) The peel strength between the two surface layers is above 110N·cm / cm;
[0067] iii) The flat compressive strength of the composite board is above 4.5MPa;
[0068] iv) The tensile strength of the composite plate is above 5.5MPa;
[0069] v) The flexural strength of the composite plate is above 40MPa.
[0070] In some embodiments, according to the national standard "GB / T 1457-2022 Sandwich structure roller peel strength test method", the peel strength between the surface layer 12 and the core layer 11 of the composite panel 1 is above 150N·cm / cm; according to the procedure D4 in Appendix D of the national standard "GB / T35489-2017 Adhesive Aging Conditions Guide", a 4-week cycle is performed. After the aging cycle, the composite panel has no problems such as degeneration, cracking, deformation, and delamination, and the peel strength between the surface layer 12 and the core layer 11 is still above 150N·cm / cm.
[0071] In some embodiments, according to the national standard "GB / T 1457-2022 Sandwich structure roller peel strength test method", the peel strength between the two surface layers 12 is above 110N·cm / cm; according to the procedure D4 in Appendix D of the national standard "GB / T 35489-2017 Adhesive Aging Conditions Guide", a 4-week cycle is performed. After the aging cycle, the composite board has no problems such as degeneration, cracking, deformation, and delamination. The peel strength between the two surface layers 12 is tested to be above 95N·cm / cm.
[0072] In some embodiments, according to the national standard "GB / T 1453-2022 Test method for flat compression performance of sandwich structures or cores", the flat compression strength of the composite panel 1 is above 4.5 MPa; according to the procedure D4 in Appendix D of the national standard "GB / T 35489-2017 Guide to Aging Conditions of Adhesives", a 4-week cycle is performed. After the aging cycle, the composite panel has no problems such as degeneration, cracking, deformation, and delamination. The flat compression strength of the tested composite panel 1 is above 4.4 MPa.
[0073] In some embodiments, according to the national standard "GB / T 1452-2018 Test Method for Flat Tensile Strength of Sandwich Structures", the flat tensile strength of the composite plate 1 is above 5.5 MPa; according to the procedure D4 in Appendix D of the national standard "GB / T35489-2017 Guide to Aging Conditions of Adhesives", a 4-week cycle is performed. After the aging cycle, the composite plate has no problems such as degeneration, cracking, deformation, and delamination. The flat tensile strength of the tested composite plate 1 is above 5.0 MPa.
[0074] In some embodiments, according to the national standard "GB / T 1456-2021 Test Method for Bending Performance of Sandwich Structures", the bending strength of the composite plate 1 is above 40 MPa; according to the procedure D4 in Appendix D of the national standard "GB / T35489-2017 Guide to Aging Conditions of Adhesives", a 4-week cycle is performed. After the aging cycle, the composite plate has no problems such as degeneration, cracking, deformation, and delamination. The bending strength of the tested composite plate 1 is above 33 MPa.
[0075] In some embodiments, the surface density of the composite board 1 is 9.0-9.3 kg / m 2 .
[0076] For the aluminum honeycomb composite panel formed by the commonly used aluminum honeycomb panel and the aluminum panels on both sides thereof, its surface density is about 11.5, the peel strength between the honeycomb core layer and the aluminum panel is about 50N·cm / cm, the peel strength between the two layers of aluminum panels is about 50N·cm / cm, the flat compression strength of the aluminum honeycomb composite panel is about 4.0MPa, the flat tensile strength is about 3.5MPa, and the bending strength is about 28MPa.
[0077] As described above, the composite panel 1 of the embodiment of the present disclosure has good mechanical properties and anti-aging properties, and is lighter in weight and has better mechanical properties than conventional aluminum honeycomb composite panels.
[0078] In order to facilitate the installation and fixation of the composite board 1 of the embodiment of the present disclosure, in some embodiments, a frame is provided to fix the composite board 1 in a specific position. Figure 1 The frame 2 is arranged on at least one side of the core layer 11, and the material of the frame 2 is metal or fiber-reinforced thermoplastic resin. In some embodiments, the frame 2 is arranged on all sides of the core layer 11, and the shape of the frame 2 matches the shape of the core layer 11 so as to completely fit and bond the core layer 11.
[0079] In some embodiments, the material of the frame 2 is aluminum alloy, which has good supporting performance and rigidity, good nail holding force, and high dimensional stability; in some embodiments, an oxide layer is formed on the surface of the frame 2, and the oxide layer can be formed by oxidizing and sandblasting the surface of the frame 2, thereby increasing the bonding area of the frame 2; in some embodiments, the thickness of the frame 2 is 0.015mm~0.02mm.
[0080] In some embodiments, the frame 2 is made of fiber-reinforced thermoplastic resin. Both the frame 2 and the core layer 11 are made of thermoplastic resin and are hot-melt-bonded into a whole. The frame 2 and the core layer 11 have stable interface properties.
[0081] In some embodiments, the material of the frame 2 is short glass fiber reinforced polyethylene terephthalate resin, the material of the honeycomb structure 111 is polyethylene terephthalate resin, and the material of the reinforcement layer 113 is continuous glass fiber reinforced polyethylene terephthalate resin. Therefore, the frame 2 has excellent hot-melt adhesion with the honeycomb structure 111 and the reinforcement layer 113, and forms a whole after hot-melt cooling, and has strong interface bonding strength.
[0082] To facilitate installation and fixation of the composite panel 1 , in some embodiments, the thickness of the frame 2 matches the thickness of the core layer 11 ; in some embodiments, the thickness of the frame 2 matches the thickness of the composite panel 1 .
[0083] In some embodiments, the composite panel 1 and the frame 2 are installed on a plate-like structure or a beam-like structure, for example, they are installed and used as a floor.
[0084] It should be noted that a fixing structure may be provided on the frame 2 to fix the composite board 1 at a specific position. The fixing structure may be a hole, a snap-fit structure, etc., and may be designed according to actual needs, and is not limited here.
[0085] An embodiment of the present disclosure further provides a rail transit floor, comprising: any of the above composite panels; a frame, which is fittedly arranged on at least one side of the core layer, and the material of the frame is metal or fiber-reinforced thermoplastic resin.
[0086] The composite board and the frame are the same as those described in any of the above embodiments and will not be described again here.
[0087] Figure 1 The exploded view of the structure of the rail transit floor of the embodiment of the present disclosure is also shown. Figure 1 In some embodiments, the frame 2 is adhesively disposed on the side of the core layer 11, and the thickness of the frame 2 is the same as the thickness of the core layer 11; one side of the thermoplastic film layer 13 is bonded to the core layer 11 and the frame 2, and the other side is bonded to the surface layer 12.
[0088] In some embodiments, the core layer 11 includes a honeycomb structure 111 , a thermoplastic foam 112 filling honeycomb pores of the honeycomb structure 111 , and a reinforcement layer 113 bonded to a surface of the honeycomb structure 111 .
[0089] The shape of the rail transit floor in the embodiment of the present disclosure can be prepared according to actual application needs and is not limited here.
[0090] Since the core layer 11, the thermoplastic film layer 13 and the surface layer 12 are in surface contact, the contact area is large, and since the core layer 11 and the thermoplastic film layer 13 are both thermoplastic resins, they are heat-fused together during processing, have good interface bonding strength, and are not easy to delaminate.
[0091] Due to the filling of the thermoplastic foam 112 , the honeycomb structure 111 and the thermoplastic foam 112 are in surface contact with the reinforcement layer 113 , with a large contact area and strong interface bonding force. Moreover, they are both thermoplastic resins and are heat-fused into one, which further enhances the overall mechanical strength.
[0092] The rail transit floor of the embodiment of the present disclosure can withstand 10 people / m 2 (60kg per person) load. 4-point support, floor support spacing 600mm×300mm (rectangular support, support block size 100mm×50mm, spacing is the distance between the support points), deflection is no more than 1mm.
[0093] The rail transit floor of the embodiment of the present disclosure is subjected to a floor point load test according to ISO4586 standard. A ball weighing 324g±5.0g and having a diameter of 42.8mm±0.2mm is dropped from 0.8m. No cracks are visible on the floor and the diameter of the pits is less than 10mm.
[0094] The rail transit floor of the embodiment of the present disclosure should be able to withstand a vertical load of 6 kN per square meter, 300 mm 2 It can withstand a vertical load of 2kN on an area basis without any permanent deformation or indentation, and has good static load performance.
[0095] The rail transit floor of the embodiment of the present disclosure can be applied to transportation vehicles such as trains, subways, light rails, trams, and maglev trains.
[0096] An embodiment of the present disclosure also provides a method for preparing a rail transit floor, which is used to prepare the rail transit floor described in any of the above embodiments, and the preparation method includes: providing two surface layers, two film layers and a core layer; sequentially laying the surface layer, the film layer, the core layer and the frame, the film layer, and the surface layer, heating and compounding them, and then cooling them to form the rail transit floor.
[0097] In some embodiments, the method for forming the core layer includes: placing a thermoplastic foaming blank for forming a thermoplastic foam on the lower surface of a mold, and then placing a thermoplastic resin having a honeycomb structure into the mold; closing the mold, and adjusting the mold closing pressure to 12 MPa;
[0098] The mold is heated to 140°C to 150°C, supercritical carbon dioxide gas is injected to fully impregnate the thermoplastic foaming blank, then cooled to the foaming temperature of the thermoplastic foaming blank 130°C to 140°C, and the pressure is quickly released at a speed of 1 to 3 MPa / s to form thermoplastic foam and fill the honeycomb structure formed by the thermoplastic resin.
[0099] In some embodiments, the core layer further includes a reinforcement layer. Correspondingly, the method for forming the core layer further includes: providing a honeycomb structure filled with thermoplastic foam and two reinforcement layers, wherein the material of the reinforcement layer includes a continuous fiber reinforced thermoplastic resin; sequentially laying the reinforcement layer, the honeycomb structure, and the reinforcement layer, heating and compounding, and then cooling to form the core layer. In some embodiments, the reinforcement layer, the honeycomb structure, and the reinforcement layer are sequentially laid and fed into a continuous Teflon belt conveyor or a steel belt conveyor for compounding, the gap of the compounding machine is set according to the thickness requirements, and the composite is firstly hot compounded, and then cooled to form.
[0100] In some embodiments, the thermoplastic resin forming the honeycomb structure is polypropylene or polyethylene terephthalate, and the thermoplastic foaming stock for forming the thermoplastic foam is polypropylene.
[0101] In some embodiments, the reinforcing layer, the honeycomb structure and the thermoplastic foam are made of the same thermoplastic resin material, for example, polypropylene resin. During processing, the resin is thermally melted into a whole without interface stratification.
[0102] In some embodiments of the preparation method of the embodiment of the present disclosure, the preparation method further comprises: after forming the core layer, layering is performed according to the layering structure of the surface layer, the thermoplastic film layer, the frame + the core layer, the thermoplastic film, and the surface layer, and the layering is performed in a continuous Teflon belt conveyor or a steel belt conveyor at one time for compounding. The gap of the compounding machine is set according to the product thickness requirements, and the thermal compounding is performed first and then cooled to obtain the desired rail transit floor.
[0103] In some embodiments of the method for preparing the rail transit floor of the embodiments of the present disclosure, the surface layer, the thermoplastic film layer, and the reinforcement layer may be sequentially layered to form a composite panel, and then the composite panel, the honeycomb structure filled with thermoplastic foam, and the composite panel may be sequentially layered to form the rail transit floor.
[0104] In a specific embodiment, the preparation method comprises:
[0105] 1) Preparing a honeycomb structure filled with thermoplastic foam: placing a PP foaming blank on the lower surface of a mold, and then placing a PET honeycomb structure into the mold; closing the mold, and adjusting the mold closing pressure to 12 MPa; heating the mold to 140° C. to 150° C., injecting supercritical carbon dioxide gas to fully impregnate the PP foaming blank, then cooling the mold to 135° C., and then rapidly releasing the pressure at a rate of 2 MPa / s to form a PP foam-filled PET honeycomb structure with a thickness of 26 mm;
[0106] 2) Preparation of composite panels: Lay layers of 0.5 mm aluminum plate, thermoplastic film layer, and 0.5 mm thick continuous glass fiber reinforced PET coil, heat to 250-280°C, and then cool to 0-10°C. The steel belt machine composite gap is 1 mm, and the production speed is 4 m / min to obtain a 1 mm thick composite panel. Prepare two composite panels.
[0107] 3) Finished product preparation: Lay the composite panel with a thickness of 1mm, the short glass fiber reinforced PET resin profile with a thickness of 25mm + the honeycomb structure filled with 26mm thermoplastic foam, and the composite panel with a thickness of 1mm, and put them into the steel belt machine for compounding at one time; compounding speed: 2m / min, heating temperature: 240-250℃, cooling temperature: 5-10℃. The height setting of the compounding machine: 27mm. Cut and carve online according to the size requirements to obtain the final product.
[0108] The preparation method of the embodiment of the present disclosure can realize continuous batch production. Glass fiber reinforced thermoplastic resin within 2 mm can be continuously unwound, and aluminum plate of 0.5 to 1 mm can also be continuously unwound. Continuous production can be achieved on a continuous laminating machine.
[0109] The present disclosure is further described below through specific embodiments.
[0110] Example
[0111] Test Method Description
[0112] Peel strength between the surface layer and the core layer: tested according to GB / T 1457-2022 Sandwich structure roller peel strength test method;
[0113] Peel strength between two surface layers: tested according to GB / T 1457-2022 Sandwich structure roller peel strength test method;
[0114] Flat compression strength of composite panels: tested according to GB / T 1453-2022 Test method for flat compression performance of sandwich structures or cores;
[0115] The horizontal tensile strength of the composite plate: tested according to GB / T 1452-2018 Test method for horizontal tensile strength of sandwich structures;
[0116] Bending strength of composite panels: tested according to GB / T 1456-2021 Test method for bending properties of sandwich structures;
[0117] Oxygen index: tested according to GB / T8924-2005 Test method for combustion performance of fiber reinforced plastics;
[0118] Sound insulation performance: tested according to GB / T19889.3-2005 Sound insulation measurement of acoustic buildings and building components;
[0119] Static load: 6kN vertical load per square meter, and 300mm 2 The requirements are met if there is no permanent deformation or indentation under the condition of a vertical load of 2kN on the area.
[0120] Example 1
[0121] 1) Preparation of honeycomb structure filled with thermoplastic foam: First, place the PP foam blank into the lower surface of the mold, and then add a 150kg / m 3 Homopolymer PP honeycomb is placed in the mold and locked; the temperature is set at about 145℃, supercritical carbon dioxide gas is injected to fully impregnate the PP blank, and the temperature is lowered to 135℃, the foaming temperature of the PP blank, and the press pressure is quickly released. The PP blank begins to foam, and the PP density is 60kg / m 3 , filling the PP honeycomb holes by itself. The obtained PP honeycomb structure filled with PP foam is then sawed, and the slice thickness is 15.8mm. The surface density of the honeycomb structure filled with thermoplastic foam is 3.4kg / m 2 .
[0122] 2) Preparation of the core layer: According to the layered structure of 1mm thick continuous glass fiber reinforced PP layer, thermoplastic foam filled honeycomb structure, and 1mm thick continuous glass fiber reinforced PP layer, it is sent to a continuous Teflon belt conveyor for compounding. The compounding speed is 1.5m / min, the heating temperature is 220℃, and the cooling temperature is 5℃. The height setting of the compounding machine is 17mm. The core layer is cut online according to the required length and width. The thickness of the core layer is 17mm, and the surface density is 6.4kg / m 2 .
[0123] 3) Preparation of rail transit floor: Lay the floor in the following structure: 0.5mm thick aluminum alloy plate, 0.15mm thick thermoplastic film layer, 16.7mm thick aluminum profile frame + 17mm thick core layer, 0.15mm thick thermoplastic film layer, 0.5mm thick aluminum alloy plate, and enter the continuous Teflon belt conveyor at one time. Lamination speed: 1.5m / min, heating temperature: 220-230℃, cooling temperature: 5-10℃. Lamination machine height setting: 18mm. Cut online according to size requirements, and finally engrave according to drawing requirements to obtain the floor. Floor thickness: 18mm.
[0124] 4) The prepared composite board was subjected to performance tests, and the test results were recorded in Table 1.
[0125] Comparative Example 1
[0126] An aluminum honeycomb floor is used as a comparative example. The thickness of the aluminum alloy upper surface plate of the aluminum honeycomb floor is 2 mm, the thickness of the lower surface is 1 mm, the thickness of the honeycomb core layer is 15 mm, and the total thickness of the aluminum honeycomb floor is 18 mm. The performance of the aluminum honeycomb floor is tested, and the test results are recorded in Table 1.
[0127] Table 1 Performance test results
[0128]
[0129] According to the test results in Table 1, the floor prepared in Example 1 has better mechanical properties than the industry requirements and meets the conditions for use. In addition, compared with the traditional aluminum honeycomb floor in Comparative Example 1, the rail transit floor of the present disclosure has better mechanical properties, flame retardant properties and sound insulation properties, and is lighter in weight.
[0130] The above is only an exemplary embodiment used to illustrate the principle of the present disclosure, and is not intended to limit the scope of protection of the present disclosure. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present disclosure, and these modifications and improvements are also within the scope of protection of the present disclosure.
Claims
1. A composite board, characterized in that: include: The core layer comprises: at least one honeycomb structure, wherein the material of the honeycomb structure comprises a thermoplastic resin; and thermoplastic foam is filled in the honeycomb structure; The surface layer is located on two opposite sides of the core layer and is bonded and fixed to the core layer. The material of the surface layer includes metal.
2. The composite panel according to claim 1, characterized in that: The core layer comprises two layers of honeycomb structures, and the honeycomb holes of the two layers of honeycomb structures are staggered with each other.
3. The composite panel according to claim 1, characterized in that: The material of the honeycomb structure includes: polypropylene, polyethylene terephthalate, or nylon.
4. The composite panel according to claim 1, characterized in that: The thermoplastic foam includes polypropylene foam, polyethylene terephthalate foam, or nylon foam.
5. The composite panel according to claim 1, characterized in that: The material of the honeycomb structure includes: polypropylene or polyethylene terephthalate; the thermoplastic foam is polypropylene foam.
6. The composite panel according to claim 1, characterized in that: The thickness of the honeycomb structure is 3 to 300 mm.
7. The composite panel according to claim 1, characterized in that: The core layer further comprises: a reinforcement layer, which is bonded to at least one side of the honeycomb structure and is located between the honeycomb structure and the surface layer. The material of the reinforcement layer comprises continuous fiber reinforced thermoplastic resin.
8. The composite panel according to claim 7, characterized in that: The thickness of the reinforcement layer is 0.5 mm to 2 mm.
9. The composite panel according to claim 1, characterized in that: Also includes: Thermoplastic adhesive film layers are located on two opposite sides of the core layer and are bonded to the core layer and the surface layer respectively.
10. The composite panel according to claim 1, characterized in that: The surface layer comprises: A body layer, wherein the material of the body layer comprises aluminum alloy; The processing layer is located on the surface of the main layer, and the material of the processing layer includes aluminum oxide.
11. The composite panel according to claim 7, characterized in that: The thickness of the surface layer is 0.3 mm to 1 mm.
12. The composite panel according to any one of claims 1 to 11, characterized in that: The composite panel has at least one of the following properties: i) the peel strength between the surface layer and the core layer is above 150N·cm / cm; ii) the peel strength between the two surface layers is greater than 110 N·cm / cm; iii) the flat compressive strength of the composite plate is above 4.5 MPa; iv) the tensile strength of the composite plate is above 5.5 MPa; v) The flexural strength of the composite plate is above 40 MPa.
13. A rail transit floor, characterized in that: include: The composite panel as claimed in any one of claims 1 to 12; A frame is fitted on at least one side of the core layer, and the frame is made of metal or fiber-reinforced thermoplastic resin.
14. The rail transit floor according to claim 13, characterized in that: The frame is made of aluminum alloy, and an oxide layer is formed on the surface of the frame.