Detection device for membrane electrode catalyst layer
By using a resistance measuring device and an adjustable electrode fixture in a constant temperature and humidity box, the speed, flexibility and losslessness of the catalytic layer detection in the prior art is solved, and the catalytic layer of the electrolytic water film electrode is realized. Fast and accurate detection.
Patent Information
- Application Number
- CN202420274805.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-04
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2034-02-04
AI Technical Summary
The prior art cannot quickly, flexibly and without loss in quality detection of the electrolytic water-film electrode catalytic layer, and cannot adapt to the diversity of the catalytic layer size. The commonly used surface resistance testing methods are not suitable for the detection of membrane electrode catalytic layer.
A detection device including a constant temperature and humidity chamber and a test device is designed. The test device includes a resistance measuring device, an adsorption table and an electrode fixture. The electrode fixture has an adjustable distance and corrosion-resistant coating, and the catalytic layer is directly measured through an ohmmeter. Plane resistance ensures consistency and accuracy of the measurement environment.
The rapid screening, flexible detection and non-destructive detection of the catalytic layer are achieved, ensuring the accuracy of measurement and product consistency, and avoiding damage to the catalytic layer.
Smart Images

Figure CN222087629U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of hydrogen production by electrolysis of water, in particular to a detection device for a membrane electrode catalytic layer. Background Art
[0002] Low-cost, low-emission green hydrogen production is one of the important challenges facing the hydrogen energy industry. Under the premise of not increasing carbon emissions, solving the problem of hydrogen sources is a prerequisite for the development of the hydrogen energy industry. Among the many hydrogen production technologies, proton exchange membrane water electrolysis is considered to be one of the promising water electrolysis hydrogen production technologies because of its advantages of no pollution, high efficiency, high safety, simple structure, stable performance and long life. The membrane electrode catalyst layer is regarded as the "heart" of the fuel cell stack.
[0003] In the catalyst layer of the membrane electrode for water electrolysis, the anode coating accounts for more than half of the cost of the entire membrane electrode. Reducing the anode catalyst loading is an important means to reduce costs. It is worth noting that the quality of the catalyst layer must be guaranteed while reducing the loading, and the planar resistance of the coating is one of the key indicators for measuring the uniformity and consistency of the planar catalyst coating. It indirectly reflects the quality and performance of the catalyst coating and is also an important tool for quality control and optimization of the catalyst layer of the membrane electrode for water electrolysis hydrogen production.
[0004] At present, the commonly used methods for measuring the planar resistance of coatings include impedance spectroscopy and four-probe measurement. However, these conventional test methods cannot quickly test the quality of the catalyst layer in actual processes. Secondly, they cannot adapt to the diversity of catalyst layer sizes. Finally, they cannot carry out non-destructive testing of the catalyst layer. Therefore, these methods cannot be used as conventional characterization methods for catalyst coatings.
[0005] In summary, the prior art has the following problems:
[0006] (1) In most relevant literature reports, the plane resistance measurement of the catalyst layer coating for membrane electrode is not taken seriously. The catalyst layer is mainly detected by microscopic means such as scanning electron microscopy, and there is a lack of macroscopic detection to quickly and preliminarily screen the catalyst layer of the membrane electrode for hydrogen electrolysis;
[0007] (2) Most devices cannot accommodate the diversity of catalyst layer sizes;
[0008] (3) The currently commonly used surface resistance test method is not suitable for non-destructive testing of the catalytic layer of the membrane electrode used for hydrogen electrolysis. Utility Model Content
[0009] In order to overcome the deficiencies of the prior art, the utility model provides a detection device for a membrane electrode catalyst layer, which solves the problem that the prior art cannot perform a rapid preliminary screening of the catalyst layer of a membrane electrode for hydrogen electrolysis.
[0010] The technical solution adopted by the utility model to solve the above problems is:
[0011] A detection device for a membrane electrode catalyst layer comprises a constant temperature and humidity chamber and a testing device arranged in the constant temperature and humidity chamber.
[0012] As a preferred technical solution, the testing device includes a resistance measuring device.
[0013] As a preferred technical solution, the testing device also includes an adsorption platform for placing the catalytic layer.
[0014] As a preferred technical solution, an insulating coating is provided on the surface of the adsorption platform.
[0015] As a preferred technical solution, the testing device also includes an electrode wire and an electrode fixture arranged outside the side of the adsorption platform where the catalyst layer is placed, and the resistance measuring device is electrically connected to the electrode fixture through the electrode wire.
[0016] As a preferred technical solution, the electrode fixture includes an end body, and the end body is provided with a connection terminal for electrically connecting to the resistance measuring device.
[0017] As a preferred technical solution, the electrode fixture also includes a coating laid on the surface of the end body.
[0018] As a preferred technical solution, the coating is an iridium coating, a platinum coating or a gold coating.
[0019] As a preferred technical solution, there are two electrode fixtures, and the distance between the two electrode fixtures can be adjusted.
[0020] As a preferred technical solution, the resistance measuring device is an ohmmeter.
[0021] Compared with the prior art, the utility model has the following beneficial effects:
[0022] (1) The utility model directly measures the surface resistance data between the two ends of the catalyst layer and compares it with the reference value data to realize rapid screening of the catalyst layer produced in batches;
[0023] (2) The utility model can flexibly detect catalyst layers of various sizes by simply replacing an electrode fixture that is consistent with the width of the catalyst layer;
[0024] (3) The utility model uses the pressure generated by the electrode's own weight as the stable pressure during the electrode testing process, and the pressure will not damage the catalytic layer; and the electrode surface has a corrosion-resistant precious metal coating, and the coating will not damage the catalytic layer;
[0025] (4) The utility model ensures the accuracy of measurement by controlling the environment in which the catalytic layer is measured to be consistent. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic diagram of the structure of the utility model;
[0027] Figure 2 A schematic diagram of measuring the catalytic layer using a test device;
[0028] Figure 3 for Figure 2 A top view of
[0029] Figure 4 It is a structural schematic diagram of the electrode fixture;
[0030] Figure 5 This is a graph showing the relationship between electrode distance and measured resistance in Example 3.
[0031] Marks in the accompanying drawings and their corresponding names: 1. Constant temperature and humidity chamber, 2. Testing device, 10. First glove operation port, 11. Second glove operation port, 21. Ohmmeter, 22. Electrode wire, 23. Adsorption table, 24. Catalytic layer, 25. Electrode fixture, 251. Plating layer, 252. Terminal body, 253. Wiring terminal. DETAILED DESCRIPTION
[0032] The present invention will be further described in detail below in conjunction with the embodiments and drawings, but the implementation manner of the present invention is not limited thereto.
[0033] Example 1
[0034] like Figures 1 to 5 As shown, the utility model discloses a detection device for a membrane electrode catalyst layer, through which the electrolytic water catalyst layer can be detected quickly, flexibly, non-destructively and accurately.
[0035] A detection device for a membrane electrode catalyst layer, comprising a constant temperature and humidity chamber 1, the constant temperature and humidity chamber can provide a stable test environment, thereby ensuring the accuracy of the test results; the constant temperature and humidity chamber also includes a first glove operation port 10 and a second glove operation port 11, through which the glove operation ports are used to perform measurement operations (the operator extends both hands into the constant temperature and humidity chamber from the first glove operation port 10 and the second glove operation port 11 to perform the measurement operation), which can prevent the external environment from polluting the catalyst layer; and also includes a test device 2, through which the surface resistance of the catalyst layer is measured; the test device 2 includes an ohmmeter 21, which is used to directly measure the catalyst layer between two electrodes (this embodiment uses a substrate with a substrate). The test device 2 also includes an adsorption platform 23, which can keep the catalytic layer in a planar state, and the surface of the adsorption platform 23 is provided with an insulating coating to ensure that the test result is accurate; the test device 2 also includes an electrode fixture 25, the width of the electrode fixture is consistent with the width of the catalytic layer, and the pressure generated by its own weight will not damage the catalytic layer, thereby realizing non-destructive testing of the catalytic layer, the outer layer of the electrode fixture is a coating 251, and the coating 251 is one of iridium, platinum, and gold. Due to its extremely strong corrosion resistance, the coating will not damage the catalytic layer during the measurement process; the electrode fixture also includes an end body 252 and a terminal 253 connected to an ohmmeter.
[0036] The test steps include, first, placing the catalyst layer in a constant temperature and humidity chamber, setting the temperature to 25°C and the humidity to 50%, and maintaining it in this state for 24 hours, so that the internal state of the catalyst layer remains consistent. Then, enter the constant temperature and humidity chamber through the glove port, operate the adsorption table, and use vacuum adsorption to make the catalyst layer for membrane electrode flatly adsorbed on the adsorption table; finally, enter the constant temperature and humidity chamber through the glove port and move the electrode fixture to the edge of the catalyst layer, so that the distance between the two electrode fixtures is fixed to the width of the catalyst layer, and the electrode fixture is connected to the ohmmeter 21 through the electrode line 22, and the plane resistance of the catalyst layer between the two electrodes is directly measured. In this way, the surface resistance of the catalyst layer produced in batches is measured, and the catalyst layer is quickly screened by comparing the deviation of the measurement result with the reference value; the width of the electrode fixture is consistent with the width of the catalyst layer, and the pressure generated by its own weight will not cause damage to the catalyst layer. The constant temperature and humidity chamber can control the test environment of the catalyst coating to be consistent, and at the same time, it can prevent the catalyst layer from adhering to dust and other debris in the air, thereby avoiding its impact on the performance of the catalyst layer for membrane electrode. The device can also measure the resistance R of different electrode fixtures at a distance x. x , the goodness of fit R2 is obtained by using the linear fitting method, and the accuracy of the test is judged by the value of R2.
[0037] Example 2
[0038] like Figures 1 to 5As shown, as a further optimization of Example 1, based on Example 1, this embodiment also includes the following technical features:
[0039] A method for rapidly screening anode catalyst layers of the same batch during production comprises the following steps:
[0040] S1: Prepare slurry according to 1 g of catalyst, 15 g of ultrapure water, 15 g of ethanol, and 0.25 g of resin.
[0041] S2: Six anode coatings with the same loading and an area of 5.5*5.5 cm were prepared on the PTFE substrate material using ultrasonic spraying.
[0042] S3: The prepared catalytic layer is placed in a constant temperature and humidity chamber for 24 hours, with the temperature fixed at 25° C. and the humidity at 50%.
[0043] S4: Using the test device of the utility model, the distance between the two electrodes was adjusted to be fixed at 55 mm, and the test was performed. The results are shown in the following table:
[0044] Under this condition, the reference surface resistance of most catalyst layers is 145±3Ω. The results show that the measured resistance of the catalyst layer No. 2 is 118.34Ω, and the measured resistance of the catalyst layer No. 7 is 110.60Ω. The test values of the catalyst layer No. 2 and the catalyst layer No. 7 deviate from the reference value by more than 10%. To ensure the consistency of the product, the catalyst layer No. 2 and the catalyst layer No. 7 are considered unqualified and will not enter the next step of membrane electrode preparation. That is, the catalyst layer can be quickly screened using this device.
[0045] Table 1 Surface resistance measurement results of different anode catalyst layers
[0046] Serial number Measuring resistance / (Ω) Filter results 0(PTFE) insulation - 1 148.08 √ 2 118.34 × 3 144.62 √ 4 145.08 √ 5 142.18 √ 6 144.67 √ 7 110.60 ×
[0047] Example 3
[0048] like Figures 1 to 5 As shown, as a further optimization of Example 1, based on Example 1, this embodiment also includes the following technical features:
[0049] A method for quantitatively testing the surface resistance of a catalyst layer comprises the following steps:
[0050] S1: Prepare slurry according to 1 g of catalyst, 15 g of ultrapure water, 15 g of ethanol, and 0.35 g of resin.
[0051] S2: An anode coating with an area of 100*100 mm was prepared on a PTFE substrate material by ultrasonic spraying.
[0052] S3: The prepared catalytic layer is placed in a constant temperature and humidity chamber for 24 hours, with the temperature fixed at 25° C. and the humidity at 50%.
[0053] S4: Using the device of the utility model, the distance between the two electrodes was adjusted to 9, 28, 47, and 66 mm, and the test results were shown in Table 2. By plotting the relationship between the measured resistance R and the electrode distance x, as shown in the attached figure, Figure 5 shown.
[0054] S5: Using a scanning electron microscope to test the cross section of the catalyst layer, it is found that the thickness t of the anode catalyst layer is about 10 μm.
[0055] S6: Test the membrane electrode obtained by transferring the catalyst layer at a temperature of 60°C, a water flow rate of 200 mL / min, and a current density of 2 A / cm 2 In this case, the corresponding voltage is 1.950V, which is within the reference value range of 1.93±0.05V.
[0056] First, under this test condition, the linear fitting between the electrode distance and the measured resistance is R2 = 0.9973, indicating that the surface resistance measurement of the catalyst layer using this device has considerable accuracy. In addition, the performance of the membrane electrode prepared using the catalyst layer after the test is consistent with the benchmark value, indicating that the test will not cause damage to the catalyst layer; finally, the resistance per unit width of the coating dR is obtained by linear fitting. x / dx=7.6579Ω / mm, then the resistivity of the 100*100mm coating surface can be approximated as R plane =dR x / dx×d×t=7.6579Ω / mm*19mm*0.01mm=1.45Ω.mm. In the later stage, the relationship between surface resistance and electrochemical performance can be established through a large amount of test data, thereby achieving the function of predicting membrane electrode performance.
[0057] Table 2 Test results
[0058]
[0059] As described above, the utility model can be implemented well.
[0060] The above is only a preferred embodiment of the utility model and does not limit the utility model in any form. According to the technical essence of the utility model, within the spirit and principles of the utility model, any simple modification, equivalent replacement and improvement made to the above embodiment still falls within the protection scope of the technical solution of the utility model.
Claims
1. A detection device for a membrane electrode catalyst layer, characterized in that: It comprises a constant temperature and humidity chamber (1) and a testing device (2) arranged in the constant temperature and humidity chamber (1); The testing device (2) comprises a resistance measuring device, an adsorption platform (23) for placing a catalyst layer, an electrode wire (22), and an electrode fixture (25) arranged outside a side of the adsorption platform (23) where the catalyst layer is placed, wherein the resistance measuring device is electrically connected to the electrode fixture (25) via the electrode wire (22).
2. A detection device for a membrane electrode catalyst layer according to claim 1, characterized in that: The surface of the adsorption platform (23) is paved with an insulating coating.
3. A detection device for a membrane electrode catalyst layer according to claim 1, characterized in that: The electrode fixture (25) comprises an end body (252), and a connection terminal (253) for electrically connecting to a resistance measuring device is provided on the end body (252).
4. A detection device for a membrane electrode catalyst layer according to claim 3, characterized in that: The electrode fixture (25) further comprises a coating (251) laid on the surface of the end body (252).
5. A detection device for a membrane electrode catalyst layer according to claim 4, characterized in that: The plating layer (251) is an iridium plating layer, a platinum plating layer or a gold plating layer.
6. The detection device for membrane electrode catalyst layer according to claim 1, characterized in that: There are two electrode jigs (25), and the distance between the two electrode jigs (25) can be adjusted.
7. A detection device for a membrane electrode catalyst layer according to any one of claims 1 to 6, characterized in that: The resistance measuring device is an ohmmeter (21).