Glass packaging structure and laminated glass

By performing ultrasonic immersion welding technology on the glass glaze layer of vacuum glass and combining with the intermediate solder layer, the problem that the temperature of the existing vacuum glass edge packaging material exceeds the resistance temperature of the laminated glass film when used at high temperature is solved, and the problem of the temperature of the laminated glass film when used is achieved is achieved. The low-temperature and high-strength combination of glass and solder and the airtightness of the vacuum cavity are suitable for the production of laminated vacuum glass.

CN222119098UActive Publication Date: 2024-12-06FUYAO HIGH PERFORMANCE GLASS TECH (FUJIAN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202420881335.8
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2024-04-25
Publication Date
2024-12-06
Estimated Expiration
2034-04-25

AI Technical Summary

Technical Problem

When used at high temperatures, the temperature of the existing vacuum glass edge packaging materials exceeds the temperature of the laminated glass film, resulting in insufficient packaging strength and poor vacuum long-term effectiveness, which is particularly difficult to be suitable for the production of laminated vacuum glass.

Method used

Using a glass encapsulation structure consisting of glass glaze layer, ultrasonic immersion solder layer and intermediate solder layer, the glass glaze layer with pores is sintered on the glass surface, and the ultrasonic immersion solder technology is used to make the solder enter the pores, forming a strong bond, allowing Low melting point solder is used and suitable for processing of laminated vacuum glass.

Benefits of technology

The low-temperature and high-strength combination of glass and solder is achieved, the airtightness of the vacuum cavity is ensured, and the production cost is reduced. It is suitable for the processing of laminated vacuum glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222119098U_ABST
    Figure CN222119098U_ABST
Patent Text Reader

Abstract

The utility model provides a glass packaging structure and laminated glass. The glass packaging structure comprises a first glass glaze layer, a first dip soldering layer, a middle solder layer, a second dip soldering layer and a second glass glaze layer which are arranged in sequence, the first glass glaze layer has a pore structure, and the first dip soldering layer infiltrates the pore structure of the first glass glaze layer; the second glass glaze layer is provided with a pore structure, and the second dip soldering layer infiltrates the pore structure of the second glass glaze layer. The utility model further provides laminated glass which comprises a first glass substrate and a second glass substrate, and the glass packaging structure is arranged between the first glass substrate and the second glass substrate. The glass glaze layer of the glass packaging structure is of a porous structure, the dip soldering layer can be immersed into pores of the glass glaze layer, tight combination of the glass glaze layer and the dip soldering layer is achieved, welding flux and the glass substrate can be indirectly and tightly welded through the dip soldering layer and the glass glaze layer, and the air tightness of the vacuum cavity is guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to a glass packaging structure and laminated glass, belonging to the technical field of glass preparation. Background Art

[0002] Vacuum glass is a glass deep-processing product that is obtained by sealing two pieces of flat glass, evacuating the gap and sealing the exhaust holes, which has the properties of heat insulation, sound insulation and noise reduction, lightness and anti-condensation. The gap between the two pieces of vacuum glass is generally no more than 0.3mm, and there are tiny support columns between the two pieces of glass. The tiny support columns are used to support the glass plates on both sides to prevent the two pieces of glass from bending and deforming significantly due to negative pressure. The diameter of the tiny pillars is generally controlled between 0.2-0.5mm, and the gap between the support columns is generally controlled to be around 30mm-40mm.

[0003] There are three types of existing edge packaging materials for vacuum glass:

[0004] 1) Organic packaging materials, such as epoxy resin glue, polyvinyl chloride, polyamide series resin, triethanolamine, UV organic materials and organic-inorganic composite materials;

[0005] 2) Glass packaging materials: such as vanadate low melting point glass, phosphate low melting point glass, and bismuthate low melting point glass powder.

[0006] 3) Metal packaging materials, such as indium alloy, Kovar alloy, aluminum alloy, silver paste, etc.

[0007] However, the above edge packaging materials have the following problems respectively:

[0008] 1) When using organic packaging materials, the glass and organic matter can be bonded together at a lower temperature. However, it is difficult for organic packaging vacuum glass to maintain a long-term effective vacuum degree. This is because at room temperature of 25°C, the vapor pressure of organic matter is generally greater than 1.0×10 -2 Pa will volatilize or decompose in the vacuum glass, and the trace gas produced will reduce the vacuum degree in the vacuum chamber, resulting in the failure of the thermal insulation and heat preservation of the vacuum glass.

[0009] 2) When using glass packaging materials, although the glass material has good chemical and physical compatibility with the glass plate, the packaging temperature of environmentally friendly lead-free glass packaging materials is generally greater than 400°C. Even if lead glass packaging materials are used, the packaging temperature can only be reduced to about 300°C, which is far higher than the tolerance temperature of the film in laminated glass (about 115-135°C); therefore, glass packaging materials can only be used to make tempered vacuum glass, but cannot be used to make laminated vacuum glass.

[0010] 3) When metal packaging materials are used, the packaging temperature of Kovar alloy is generally 1420-1455°C; the packaging temperature of aluminum and aluminum alloy is above 500°C; and the packaging temperature of silver paste is generally above 450°C; although the melting point of indium alloy can be as low as below 135°C, the bonding strength of this low-melting-point indium alloy is weak and cannot resist the edge stress of vacuum glass, which will cause structural collapse. Therefore, indium alloy with a melting point above 150°C is generally used. This temperature also exceeds the tolerance temperature of the film in laminated glass, which is about 115-135°C; therefore, metal packaging materials can only be used to make tempered vacuum glass, but not laminated vacuum glass.

[0011] Generally speaking, metal materials and inorganic silicate glass materials have poor adhesion, and it is impossible to simply bond low-fusion metal to the glass surface, unless special interface treatment is taken between the metal and the glass to allow the two to bond seamlessly and achieve an airtight sealing effect. As described below, when metal and glass need to have a certain strength of connection, this behavior is called mutual "infiltration", that is, at the connection between the metal and the glass, the two are infiltrated and mixed with each other to form a disordered metal-glass material mixture structure, rather than a simple metal layer and glass layer structure with a clear interface, so that a certain connection strength can be achieved.

[0012] In order to achieve the wetting effect of the metal solder layer and the glass layer, the metal packaging of traditional vacuum glass generally uses metal paste to sinter a metallization layer on the glass surface (mostly silver paste is used for sintering). However, the cost of silver paste is high, resulting in the high market price of vacuum glass. In addition, the welding effect of the silver paste sintered layer and the low melting point alloy (such as indium tin alloy) with a melting point below 150°C is not good. After hot-melt welding, the two only show physical contact. After pulling them apart with force, a clear silver paste layer and a low melting point alloy layer can be seen. Therefore, the silver paste sintered layer must be matched with a suitable metal solder, which is generally a high-temperature metal solder. In addition to sintering the metallization layer, ultrasonic welding equipment is also used to pre-plate a metallization layer on the glass surface (mostly tin alloy is used). However, the pre-plated metallization layer of the ultrasonic welding equipment has a weak bonding force with the glass surface. The ultrasonic pre-plated metallization layer can be scraped off the glass surface in pieces by a blade. Therefore, although the cost of the ultrasonic pre-plated metallization layer is reduced, the durability is poor and it is impossible to maintain a long-term vacuum seal.

[0013] Therefore, in view of the technical shortcomings of the above-mentioned vacuum glass edge packaging, it is necessary to innovatively develop a new vacuum glass edge packaging solution to resolve the contradiction between laminated vacuum glass and edge packaging temperature, packaging strength, and long-term vacuum after packaging. Utility Model Content

[0014] In order to achieve the above technical problem, the purpose of the utility model is to provide a glass packaging structure, which is based on a glass glaze layer and can provide good support for the combination of glass and solder.

[0015] To achieve the above object, the utility model first provides a glass packaging structure, wherein the glass packaging structure comprises a first glass glaze layer, a first dip solder layer, an intermediate solder layer, a second dip solder layer and a second glass glaze layer which are arranged in sequence;

[0016] The first glass glaze layer has a pore structure, and the first dip solder layer infiltrates the pore structure of the first glass glaze layer;

[0017] The second glass glaze layer has a porous structure, and the second solder dip layer wets the porous structure of the second glass glaze layer.

[0018] In the above-mentioned glass packaging structure, the glass glaze layer can be made by sintering glass powder doped with organic resin and metal oxide on the surface of the original glass substrate (sintering temperature is 300-900°C). After the glass powder is sintered, the organic resin component will be burned off, thereby forming a glass glaze layer with fine pores on the surface.

[0019] In the above-mentioned glass packaging structure, preferably, the first solder dip layer and the second solder dip layer are ultrasonic solder dip layers respectively. The ultrasonic solder dip layer is formed on the surface of the glass glaze layer by ultrasonic soldering with solder (metal solder or alloy solder). Since the glass glaze layer has fine pores, under the action of ultrasonic waves, the bubbles in the fine pores burst and overflow, and the solder enters the pores, thereby realizing the ultrasonic solder dip layer infiltrating the glass glaze layer to form a strong bond. Since the ultrasonic wave has a small action range and a short time on the glass surface, the allowable action temperature can be higher than the film tolerance temperature of the laminated glass (generally 135°C). The temperature of the ultrasonic wave is set according to the melting point of the solder, and is generally greater than / equal to the melting point of the solder.

[0020] In the above glass packaging structure, preferably, the first solder dip layer is made of silver-indium alloy solder, aluminum alloy solder, tin solder or tin alloy solder, wherein the tin alloy solder includes indium-tin alloy, tin-bismuth alloy, etc., preferably indium-tin alloy solder.

[0021] In the above glass packaging structure, preferably, the second soldering layer is made of silver-indium alloy solder, aluminum alloy solder, tin solder or tin alloy solder, wherein the tin alloy solder includes indium-tin alloy, tin-bismuth alloy, etc., preferably indium-tin alloy solder.

[0022] In the above glass packaging structure, preferably, the width of the first solder dip layer is less than 10 mm, and the width of the second solder dip layer is less than 10 mm.

[0023] In the above glass packaging structure, preferably, the intermediate solder layer is formed by a metal solder wire, a metal solder sheet, an alloy solder wire or an alloy solder sheet.

[0024] In the above glass packaging structure, preferably, the material of the middle solder layer is metal solder and / or alloy solder with a hot melting temperature ≤150°C.

[0025] Traditional metal brazing directly metallizes the glass surface. To achieve a strong bond between the metallized layer and the glass, high temperature sintering (greater than 500°C) must be used. If ultrasonic metal dip soldering is used directly on the glass surface, although the metal solder can be spread on the glass surface, it will peel off with a slight scrape. The utility model provides a glass glaze layer and metallizes the surface of the glass glaze layer to achieve a strong bond between the metallized layer and the glass in a low temperature environment.

[0026] The utility model also provides a laminated glass, which comprises a first glass substrate and a second glass substrate, wherein: the above-mentioned glass packaging structure is arranged between the first glass substrate and the second glass substrate.

[0027] In the above-mentioned laminated glass, preferably, the first glass substrate is a soda-lime glass plate, a high-aluminum glass plate, a medium-aluminum glass plate or a borosilicate glass plate.

[0028] In the above-mentioned laminated glass, preferably, the second glass substrate is a soda-lime glass plate, a high-aluminum glass plate, a medium-aluminum glass plate or a borosilicate glass plate.

[0029] In the above-mentioned laminated glass, preferably, at least one of the first glass substrate and the second glass substrate is a laminated glass, that is, the laminated glass provided by the present invention can be a laminated glass.

[0030] In the above laminated glass, preferably, a sealant is provided on the outside of the glass packaging structure, and the sealant is provided in the area between the outside of the glass packaging structure and the first glass plate and the second glass plate to seal this space.

[0031] In the above-mentioned laminated glass, preferably, the laminated glass is hollow glass or vacuum glass. The laminated glass of the utility model is provided with an intermediate chamber. Preferably, when the intermediate chamber is filled with air, the laminated glass is hollow glass; when the intermediate chamber is in a vacuum state, the laminated glass is vacuum glass, that is, the intermediate chamber of the laminated glass is a vacuum chamber, that is, the laminated glass is vacuum glass. When the intermediate chamber of the laminated glass is a vacuum chamber and the glass plate is a laminated glass, the laminated glass is a laminated vacuum glass. Specifically, the intermediate chamber can be evacuated by opening an exhaust port on the glass plate, and the exhaust port is sealed after evacuation.

[0032] The laminated glass of the present invention can be prepared by the following methods:

[0033] Pre-treating the surface of the glass plate to be used as a glass substrate, including cleaning, etc., to remove residual oil and other organic matter;

[0034] Placing glass powder doped with organic resin and metal oxide on the surface of a first glass substrate and sintering (sintering temperature is 300-900° C.) to form a first glass glaze layer with a porous structure on the surface, and repeating this step to form a second glass glaze layer on the surface of a second glass substrate;

[0035] Placing solder (metal solder or alloy solder) on the surface of the first glass glaze layer, and then performing ultrasonic dip soldering to form a first dip solder layer, and repeating this step to form a second dip solder layer on the surface of the second glass glaze layer;

[0036] The solder of the intermediate solder layer (e.g., metal solder wire / sheet / foil, alloy solder wire / sheet / foil) is disposed on the surface of the first dip solder layer, and then the two glass substrates are joined so that the dip solder layer regions of the two glass substrates are relatively aligned. When preparing vacuum glass, a micro-pillar is placed in the vacuum chamber region of the glass substrate, and then the two glass substrates are joined;

[0037] After the two glass substrates are pressed together with external force, the solder of the middle solder layer is hot-melted (hot-melting temperature ≤ 150°C) in normal pressure air / vacuum negative pressure / inert gas atmosphere. The melted solder of the middle solder layer forms an middle solder layer, which is tightly connected to the dip solder layer on the glass substrate to form an airtight structure, thereby completing the glass packaging. When preparing vacuum glass, the vacuum glass is evacuated after being combined, the evacuation port is sealed, and a sealant is applied.

[0038] If tempered vacuum glass is produced, the sintering of the glass glaze layer can be carried out before the tempering process, or glass powder with the same melting point as the tempering temperature can be used to sinter the glass glaze layer on the glass surface while tempering; if laminated vacuum glass is produced, the glass glaze layer must be sintered first, and then the glass is assembled according to the traditional laminated process.

[0039] The technical solution provided by the utility model can solve the technical difficulties in the existing laminated glass (especially vacuum glass) packaging, and bring the following technical effects:

[0040] 1. The glass glaze layer has a simple composition and a wide range of raw materials. It can be tightly integrated with the glass plate. At the same time, the glass glaze layer has a porous structure, and the dip solder layer can be immersed in the pores of the glass glaze layer to achieve a tight combination of the glass glaze layer and the dip solder layer. The solder and the glass substrate can be indirectly welded tightly through the dip solder layer and the glass glaze layer to ensure the airtightness of the vacuum cavity.

[0041] 2. The glass glaze layer and the solder layer form a strong bond mainly through porous bite, so the glass glaze layer can be matched with a dip solder layer made of solder of any composition. For example, the same solder as the middle solder layer can be selected to maintain the consistency of the composition of the dip solder layer and the middle solder layer to achieve the best welding effect.

[0042] 3. The presence of glass glaze layer and solder dip layer allows the use of low melting point solder for metal edge sealing (melting point below 135°C), which is suitable for the processing of laminated vacuum glass. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a schematic diagram of the structure of the vacuum glass provided in Example 1.

[0044] Figure 2 This is a schematic diagram of the arrangement of the first glass glaze layer in Example 1.

[0045] Figure 3 This is a schematic diagram of the arrangement of the second glass glaze layer and the second dip solder layer in Example 1.

[0046] Figure 4 This is a schematic diagram of the arrangement of the alloy solder wire in Example 1.

[0047] Description of main figures:

[0048] The first glass substrate 11, the second glass substrate 12, the first glass glaze layer 21, the second glass glaze layer 22, the first dip solder layer 31, the second dip solder layer 32, the middle solder layer 4, the middle chamber 5, the stainless steel support column 6, the edge sealing protective glue 7, and the alloy solder wire 8. DETAILED DESCRIPTION

[0049] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the utility model, the technical solution of the utility model is now described in detail below, but it should not be understood as limiting the applicable scope of the utility model.

[0050] Example 1

[0051] This embodiment provides a vacuum glass, the structure of which is as follows: Figure 1 shown.

[0052] The vacuum glass has the following structure:

[0053] The first glass substrate 11 and the second glass substrate 12 are both ordinary soda-lime glass with a thickness of 4 mm;

[0054] The first glass glaze layer 21 and the second glass glaze layer 22 have a width of not less than 5 mm and a film thickness of 10-25 μm. The distance between the first glass glaze layer 21 and the edge of the first glass substrate 11 is ≤2 mm, and the distance between the second glass glaze layer 22 and the edge of the second glass substrate 12 is ≤2 mm.

[0055] The first dip soldering layer 31 and the second dip soldering layer 32 are made of In 52 Sn 48 The solder has the same width as the glass glaze layer, a thickness of about 0.1 mm, and a distance of 2 mm from the edge of the glass plate; the first dip solder layer 31 and the second dip solder layer 32 respectively wet the pore structure of the first glass glaze layer 21 and the pore structure of the second glass glaze layer 22, such as Figure 2 As shown;

[0056] An intermediate solder layer 4 is provided between the first solder dip layer 31 and the second solder dip layer 32. The intermediate solder layer 4 is formed of an alloy solder wire. The alloy solder wire is a continuous and complete structure, with the head and tail overlapping or welded together, and an intermediate chamber 5 is formed between the first solder dip layer 31 and the second solder dip layer 32. The diameter of the alloy solder wire is 1 mm.

[0057] The middle chamber 5 is a vacuum chamber, and a stainless steel support column 6 is arranged in the middle of the middle chamber 5;

[0058] Edge sealing protective glue 7 is provided on the side of the vacuum glass.

[0059] The vacuum glass of this embodiment is prepared in the following manner:

[0060] 1. After washing and drying the two pieces of glass, use a plasma treatment device to further clean the glass surface to remove residual oil and other organic matter (one of the pieces has an exhaust port), and use them as the first glass substrate 11 and the second glass substrate 12 respectively.

[0061] 2. A circle of glass glaze raw material is printed on the edge of the first glass substrate 11 and the second glass substrate 12 by screen printing, with a width of about 10 mm and a wet film thickness of 20 μm-30 μm; a glass ink layer is sintered on the glass surface by conventional automotive glass sintering / tempered / semi-tempered process (pre-baking at 100° C.-150° C. for 60 s-600 s, sintering temperature at 550-770° C. for 90-300 s) to form a first glass glaze layer 21 (such as Figure 2 As shown, the distance between the first glass glaze layer 21 and the edge of the first glass substrate 11 is 0 mm) and the second glass glaze layer 22; wherein, the glass glaze raw materials are mixed by the following components in a certain proportion: glass powder (wt%, >60%), copper chromium spinel (wt%, 10%-15%) and water-based ink oil (including water-based resin, additives, water, etc., no residue at high temperature; wt%, <20%), and the sum of the contents of the three components is 100%.

[0062] 3. The exposed glass glaze layer and the basic surface of the glass to be combined on one side of the vacuum chamber are subjected to plasma surface treatment to make the product clean and improve the effect and strength of ultrasonic dip welding.

[0063] 4. Place the first glass substrate 11 and the second glass substrate 12 (with the glass glaze layer facing upward) flat on a silicone electric heating blanket for preheating at a temperature of 60°C.

[0064] 5. Keep the preheating temperature (60°C) and use ultrasonic infiltration equipment to infiltrate In52Sn48 solder on the surface of the first glass glaze layer 21 and the second glass glaze layer 22 to form a first dip solder layer 31 and a second dip solder layer 32 (such as Figure 3 As shown), and connected head to tail to form an ultrasonic metal dip soldering circle, wherein the width of the dip soldering layer is the same as the width of the glass glaze layer, and the thickness is about 0.1mm; the parameters of the ultrasonic infiltration equipment are: ultrasonic frequency 40KHZ, ultrasonic power 100 watts, temperature 180℃, and heating power 200 watts.

[0065] 6. Wipe the surface of the first dip solder layer 31 and the second dip solder layer 32 with a dust-free cloth dipped in saturated oxalic acid solution to remove the surface oxide layer; at the same time, wipe the low melting point alloy solder wire of In52Sn48 with a dust-free cloth dipped in saturated oxalic acid solution to remove the surface oxide layer; and use anhydrous alcohol to clean the oxalic acid remaining on the surface of the first dip solder layer 31, the second dip solder layer 32 and the solder wire.

[0066] 7. Place a 1 mm diameter In52Sn48 low melting point alloy solder wire (the surface oxide layer has been removed by using oxalic acid) inside one of the first dip solder layer 31 and the second dip solder layer 32, that is, alloy solder wire 8 (such as Figure 4 As shown), it is a continuous and complete structure, with the head and tail overlapping / welded together, and an intermediate solder layer 4 is formed through backlog, and stainless steel support columns 6 (i.e., edge stainless steel support columns) are evenly placed 2-4 mm away from the solder. The size of the stainless steel support columns 6 is 0.57 (diameter) × 0.3 mm (height), and the interval between the stainless steel support columns 6 is 10 mm.

[0067] 8. Stainless steel support columns 6 are evenly placed in the vacuum glass cavity surrounded by the solder wire. The size of the stainless steel support columns 6 is 0.57 (diameter) × 0.3 mm (height), and the interval between the stainless steel support columns is 30 mm.

[0068] 9. Align the solder-dip layer areas of the two glass substrates and join them together, and apply a force of 0.3-0.6MPa on the edge of the glass substrate to tightly connect the two glass substrates, the glass glaze layer, the solder-dip layer, the solder wire, and the edge stainless steel support column together; while maintaining the edge force, melt the solder at normal pressure at 130°C (hold the temperature for 20 minutes) to achieve a dense connection between the middle solder layer, the solder-dip layer, the glass glaze layer, and the glass substrate.

[0069] 10. Vacuum the glass and seal the vacuum port.

[0070] 11. Finally, polyurethane glue is applied on the periphery of the edge-sealing metal solder as the edge-sealing protective glue 7 to complete the complete edge-sealing of the vacuum glass.

[0071] The packaging structure provided by the utility model pre-sets a separate, non-dense structure (i.e., pore structure) of the glass glaze layer, and allows the solder to enter the non-dense structure of the glass glaze layer through ultrasonic dip soldering, rather than entering the glass surface. In this way, the dip soldering layer can form a close bond with the glass glaze layer, thereby improving the bonding strength and air tightness. Moreover, since the glass glaze layer contains glass components, it can also form a good bond with the glass plate.

Claims

1. A glass packaging structure, characterized in that: The glass packaging structure comprises a first glass glaze layer, a first dip solder layer, an intermediate solder layer, a second dip solder layer and a second glass glaze layer which are arranged in sequence; The first glass glaze layer has a pore structure, and the first dip solder layer infiltrates the pore structure of the first glass glaze layer; The second glass glaze layer has a porous structure, and the second dip solder layer wets the porous structure of the second glass glaze layer.

2. The glass packaging structure according to claim 1, characterized in that: The first solder dip layer and the second solder dip layer are ultrasonic solder dip layers respectively.

3. The glass packaging structure according to claim 1, characterized in that: The material of the first dip soldering layer is silver-indium alloy solder, aluminum alloy solder, tin solder or tin alloy solder; The material of the second solder dip layer is silver-indium alloy solder, aluminum alloy solder, tin solder or tin alloy solder.

4. The glass packaging structure according to claim 1, characterized in that: The middle solder layer is formed by metal solder wire, metal solder sheet, alloy solder wire or alloy solder sheet.

5. The glass packaging structure according to claim 4, characterized in that: The material of the middle solder layer is metal solder and / or alloy solder with a hot melting temperature of ≤150°C.

6. A laminated glass comprising a first glass substrate and a second glass substrate, characterized in that: The glass packaging structure according to any one of claims 1 to 5 is disposed between the first glass substrate and the second glass substrate.

7. The laminated glass according to claim 6, characterized in that: The first glass substrate is a soda-lime glass plate, a high-aluminum glass plate, a medium-aluminum glass plate or a borosilicate glass plate; The second glass substrate is a soda-lime glass plate, a high-aluminum glass plate, a medium-aluminum glass plate or a borosilicate glass plate.

8. The laminated glass according to claim 6, characterized in that: At least one of the first glass substrate and the second glass substrate is laminated glass.

9. The laminated glass according to claim 6, characterized in that: A sealant is provided on the outer side of the glass packaging structure.

10. The laminated glass according to claim 6, characterized in that: The laminated glass is hollow glass or vacuum glass.