Glass plate and methods for processing a glass plate
A glass plate with laser-scanned edges forming a diffraction grating on the outer edge addresses the visibility issue, enhancing handling and design aesthetics through structural colors.
Patent Information
- Application Number
- DE112014006072
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2014-12-17
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2034-12-17
AI Technical Summary
Glass plates are difficult to handle due to the lack of visibility at their outer edges, making it challenging to grasp and manipulate them accurately.
A glass plate design featuring an outer edge with an adjacent surface intersecting a principal plane at an obtuse angle, created by laser scanning, which forms a diffraction grating with Wallner lines and a surface roughness of less than 100 nm, enhancing visibility through structural colors.
The design improves edge visibility and provides a visually appealing appearance with changing colors under different angles, facilitating easier handling and aesthetic appeal.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
NAME OF THE INVENTION: GLASS SHEET AND METHOD FOR PROCESSING A GLASS SHEET TECHNICAL AREA
[0001] The present invention relates to a glass plate and a method for processing a glass plate. STATE OF THE ART
[0002] After cutting to a desired size, a glass plate can be beveled. The beveled glass plate It has an adjacent surface on an outer edge that intersects a principal plane at an obtuse angle. (See, for example, patent document 1). Patent document 2 describes a laser beam processing device and a Laser beam processing method. Patent document 3 describes a processing method for glass using a laser and a Device for this purpose. Patent document 4 describes a chamfering process for a brittle substrate. DOCUMENTS OF THE STATE OF THE TECHNOLOGY PATENT DOCUMENTS Patent document 1: JP 2008 - 93 744 A Patent document 2: JP 2007- 21 548 A Patent document 3: JP 2002- 241 141 A Patent Document 4: CN 1 01 386 466 A SUMMARY OF THE INVENTION PROBLEM TO BE SOLVED BY THE INVENTION
[0003] Since a glass plate is transparent, it is difficult to visually identify an outer edge of the glass plate. A problem arises in that if it is difficult to visually identify the outer edge of the glass plate, it can be problematic for a For a worker carrying the glass and, for example, trying to hold the outer edge of the glass plate, it is difficult to hold a piece of glass that is difficult to grip. The position is difficult to discern, making the glass plate difficult to handle.
[0004] The present invention was made with regard to the problem described above and a The main object of the present invention is to provide a glass plate that offers excellent visibility of a has an outer edge. MEANS TO SOLVE THE PROBLEM
[0005] According to one aspect of the present invention, a glass plate is provided which is at least partially has an outer edge and an adjacent surface that intersects a principal plane at an obtuse angle, wherein the adjacent surface is a cutting plane, which is created by extending a crack by generating a tensile stress formed by scanning with a laser beam along at least part of an outer edge of the glass plate is, and the adjacent surface forms a diffraction grating that includes at least one Wallner line and a stop- line includes, and an arithmetic mean roughness Ra, as described in JIS B0601, of the adjacent surface less than or equal to 100 nm. ADVANTAGEOUS EFFECT OF THE INVENTION
[0006] According to one aspect of the present invention, a glass plate can be provided which has an excellent Visibility of an outer edge. BRIEF DESCRIPTION OF THE DRAWINGS Fig. 1 is a cross-sectional view of a glass plate according to an embodiment of the present invention, Fig. 2 is a top view of the glass plate from Fig. 1. Fig. 3 is a side view showing a laser processing method of the glass plate according to Example 1, Fig. 4 is a top view showing the direction of scanning with a laser beam in relation to the glass plate of Fig. 3 shows, Fig. 5 is a side view showing the state of the glass plate after laser processing as described in Fig. 3 and Fig. 4. shows, Fig. 6 is a side view showing the state of the glass plate from Fig. 5 after a load has been applied. has been Fig. 7 is a micrograph of a first adjacent surface of the glass plate shown in Fig. 6. Fig. 8 is a micrograph of a second adjacent surface of the glass plate, which is shown in Fig. 6. Fig. 9 is a top view showing the direction of scanning with a laser beam in relation to the glass plate. Example 2 shows, Fig. 10 is a side view showing the state of the glass plate after the laser processing of Fig. 9. Fig. 11 is a side view showing the state of the glass plate from Fig. 10 after a load has been applied. has been exercised, and Fig. 12 is a micrograph of a first adjacent surface of the glass plate shown in Fig. 11. EXECUTIONAL FORMS FOR IMPLEMENTING THE INVENTION
[0007] An embodiment for implementing the present invention is described below with reference to the The drawings are described. Each drawing contains identical or corresponding symbols. The corresponding configurations are assigned, and therefore the descriptions are omitted. In the following... The description implies "-", which represents a range of numbers, a range containing numerical values before and after the The number range is included.
[0008] Fig. 1 is a cross-sectional view of a glass plate according to the embodiment of the present invention. Fig. 2 is a top view of the glass plate.
[0009] The glass plate 10 is used, for example, as a window glass for a vehicle, a window glass for a building, a substrate for a display or a cover glass for a display. The glass plate 10 can, for example, be made of soda-lime glass, be made of alkali-free glass or chemically tempered glass. After applying a chemical In the hardening process, the chemically hardened glass is used, for example, as cover glass.
[0010] In Fig. 1, the glass plate 10 is a flat plate, however, the glass plate 10 can be a curved plate. The shape of the glass plate 10 is not specifically restricted, although the shape of the glass plate 10 could, for example, be rectangular. It can be trapezoidal, circular, or elliptical in shape. The thickness of the glass plate 10 depends on a The application of the glass plate 10 is appropriately adjusted and the thickness of the glass plate 10 is, for example, from 0.01 cm to 2.5 cm.
[0011] The glass plate 10 comprises a first principal plane 11 and a second principal plane 12 and the glass plate 10 comprises at least on part of an outer edge a first adjacent surface 13, a second adjacent surface 14 and an edge surface 15. The first principal plane 11 and the second principal plane 12 are parallel to each other. The first The adjacent surface 13 intersects the first principal plane 11 at an obtuse angle. The second adjacent Surface 14 intersects the second principal plane 12 at an obtuse angle. The edge surface 15 is perpendicular to the first. The first adjacent surface 13 connects the main plane 11 and the second main plane 12 and the edge surface 15. and the second adjacent surface 14. Since the first adjacent surface 13 and the second adjacent Since surface 14 is identically formed, the first adjacent surface 13 is described by way of example.
[0012] The first adjacent surface 13 is a cutting plane formed by extending a crack. has been. During the cutting of the glass plate 10, the first adjacent surface 13 is formed. Since a Since chamfering is not required, processing time can be reduced and processing costs lowered.
[0013] The first adjacent surface 13 is a cutting plane which is scanned with a laser beam along at least part of the outer edge of the glass plate 10 is formed. Scanning with a laser beam is used in this process. for a shift in the position at which the laser beam is directed. Since a structural color is visible, A cutting plane created by a laser beam exhibits excellent visibility and design possibilities.
[0014] In particular, as shown in Fig. 2, the first adjacent surface 13 forms a diffraction grating which at least one of which comprises a Wallner line and a stop line. A "Wallner line" is a striped line that indicates the direction of crack extension. A "stop line" is a striped line that indicates a This indicates a temporary halt to the extension of a crack. The Wallner line and the stop- The line is referred to as a line that indicates a state of crack elongation.
[0015] Since the first adjacent surface 13 forms a diffraction grating that reflects at least one of the Wallner line and the The stop line is present when visible light, such as sunlight, is incident due to diffraction and the Interference of light makes a structural color visible. Consequently, the visibility of the outer edge of the glass plate 10 improved. Furthermore, since different colors are visible, a favorable design can be achieved because the color the structural color changes depending on the viewing angle.
[0016] Preferably, a plurality of lines representing the state of crack elongation are arranged along the outer edge of the glass plate 10 arranged, while the lines are separated by intervals are separated. By arranging them in this way, if the intervals (distances) between the lines are 16 are identical, compared to a case where lines 16 are in a direction perpendicular to the outer edge of the glass plate 10 are arranged, namely in a case where the lines 16 are in a plate thickness direction of the glass plate 10 When arranged, a larger number of lines 16 are formed. Consequently, diffraction and interference occur. of the light more frequently, so there is a tendency for the structural color to be visible.
[0017] The lines 16 may not extend over the entire circumference of the outer edge of the glass plate 10. formed and lines 16 can be formed in a section of the outer edge.
[0018] The spacing P of the lines 16 is, for example, from 0.1 µm to 1000 µm. If the spacing P of the lines 16 is within the In the area described above, there is a tendency for diffraction and interference of the A structural color appears under visible light. The spacing P of the lines 16 is preferably from 0.2 µm to 500 µm. µm and larger, preferably from 0.5 µm to 300 µm.
[0019] The spacing P of the lines 16 is determined, for example, by counting the number of lines 16 in a length range of 1000 µm. measured along the outer edge of the glass plate on a micrograph.
[0020] It should be noted that if the spacing of the lines 16 is the same as the spacing compared to In the case of an irregular distance, diffraction and interference of light occur, so that visibility and The design can be improved.
[0021] The fact that the distance is an identical distance means that both the minimum value of the Distance as well as the maximum value of the distance in a range of ± 15% of an average value of the Distance as a reference point.
[0022] It should be noted that in at least one part of the diffraction grating formed by the lines 16, The lines 16 can be arranged at identical intervals. In an area where the lines 16 are aligned with the Since they are arranged at identical distances, there is a tendency for diffraction and interference of the Light can occur, so that visibility and design can be improved.
[0023] The lines 16 can be designed such that when the lines 16 are in a direction perpendicular to the The lines 16 are curved in the first principal plane 11 and the second principal plane 12. The curved A line can be divided into two components that are perpendicular to each other. Consequently, there is an angular range at which the Diffraction and interference of light occur, magnified compared to a case where lines 16 are formed in this way The advantage is that they are straight lines, so the structural color is visible over a wider angle range.
[0024] It should be noted that the first adjacent surface 13 can be designed such that an angle which between the first adjacent surface 13 and the first principal plane 11, exceeds 135 degrees. By forming this angle, it can be ensured that a step is created at the boundary between the first adjacent Surface 13 and the first main layer 11 are less perceptible. Furthermore, the tactile sensation becomes smooth. The angle is preferably greater than or equal to 150 degrees. Furthermore, the first adjacent surface 13 is designed such that that it is a flat surface, so that when the first adjacent surface 13 is considered in cross-section The first adjacent surface 13 is a straight line. However, the first adjacent surface 13 can be such that... It must be designed so that it is a curved surface, so that when the first adjacent When surface 13 is viewed in cross-section, the first adjacent surface 13 is an arc.
[0025] The surface roughness Ra (the arithmetic mean roughness value Ra, which is defined in JIS B0601 of the Japanese industrial standard) (as described) the first adjacent surface 13 is less than or equal to 100 nm. If the surface roughness If Ra is less than or equal to 100 nm, a sufficient degree of sparkle is achieved and a glittering effect is produced. A design can be obtained that differs from the design described above based on the structural Color varies. The surface roughness Ra is preferably less than or equal to 50 nm, and preferably more. less than or equal to 30 nm. [Examples] [Example 1]
[0026] In Example 1, the glass plate shown in Figures 5 to 8 was obtained by the processing method, as shown in Figures 3 and 4. Figure 3 is a side view illustrating the laser processing method of the A glass plate as shown in Example 1. Figure 4 is a top view showing one direction of scanning with a laser beam. Referring to the glass plate shown in Fig. 3, Fig. 5 is a side view showing the state of the glass plate after the Laser processing is shown in Figures 3 and 4. Figure 6 is a side view showing a state Figure 5 shows the result after a load has been applied to the glass plate. Figure 7 is a micrograph of the first adjacent surface of the glass plate, shown in Fig. 6. Fig. 8 is a micrograph of the second adjacent surface of the glass plate, shown in Fig. 6. In Fig. 7 and Fig. 8, a line is shown that forms a The condition of the elongation of a crack is shown, highlighted.
[0027] In Example 1, the glass plate 10A was treated using a laser beam 20 passing through the glass plate 10A. the first main plane 11A passes through to the second main plane 12A, is locally heated, and the irradiation position of the Laser beam 20 was varied. Glass plate 10A was a glass plate with a thickness of 2.8 mm (from ASAHI GLASS). CO., LTD. (soda-lime glass manufactured by CO., LTD.) was used. A Yb fiber laser was used as the light source 22 of the laser beam 20. (wavelength 1070 nm) was used and the laser beam 20 was directed perpendicularly onto the first principal plane 11A. -1 The absorption coefficient (Σ) of the glass plate 10A with respect to the laser beam 20 was 0.57 cm and the internal The permeability was 85%. Internal permeability is a permeability in a case where it is assumed that... It is determined that no reflection occurs on the first principal plane 11A. The beam shape on the first principal plane 11A was... The laser beam 20 forms a circular shape with a diameter of 0.5 mm. A condenser lens 25 collects the The laser beam 20 was installed between the light source 22 and the glass plate 10A. The focus position of the condenser lens 25 was a position that was 11.48 mm away from the first principal plane 11A in the direction of the light source 22, and the The convergence angle was 2.5 degrees. The output power of light source 22 was 440 W. Sampling with the Laser beam 20 was directed at a speed of 70 mm / second parallel to the two parallel edges of the four edges The procedure was carried out on glass plate 10A, which had a trapezoidal shape as shown in Fig. 4. An initial crack was found in An edge that cuts the two parallel edges at an angle was formed beforehand with a file. The initial A crack formed at the point where irradiation with laser beam 20 began. The scanning direction of the laser beam 20 was relative to a tangent line of an outer edge of the glass plate 10A at the The position at which the laser beam 20 was first directed was inclined. Since at the position to which the When laser beam 20 was directed at the target, a tensile stress was generated, which was achieved by varying the position to which the When laser beam 20 was applied, the crack was extended starting from the initial crack as the starting point.
[0028] In Example 1, a continuous oscillation laser was used as the Yb fiber laser.
[0029] Furthermore, in Example 1, as shown in Fig. 3, a first cooling nozzle 28 was used to spray a cooling gas. to the first main level 11A of the glass plate 10A and a second cooling nozzle 29 for spraying a cooling gas onto the second Main plane 12A is used, so that at the position where the laser beam 20 was directed, a high Tensile stress was generated. The center line of the first cooling nozzle 28 and the center line of the second cooling nozzle 29 were measured with aligned with the optical axis of the laser beam 20. Each of the first cooling nozzle 28 and the second cooling nozzle 29 had a circular ejection opening with a diameter of 1 mm, formed a gap of 15 mm with the glass plate 10A and injected the cooling gas at a flow rate of 30 liters / minute. Compressed air was used as the cooling gas.
[0030] The glass plate 10A was moved relative to the light source 22, the first cooling nozzle 28 and the second cooling nozzle 29, so that the crack was extended from the initial crack as its starting point. As a result, the first adjacent surface 13, which intersects the first principal plane 11A at an obtuse angle, and the second adjacent surface 14, which intersects the second principal plane 12A at an obtuse angle, formed simultaneously as shown in Fig. 5. It is assumed that the reason for the first adjacent The reason surface 13 and the second adjacent surface 14 were formed was that the scanning direction of the The laser beam 20 (the X-direction in Fig. 4) was inclined with respect to the outer edge of the glass plate 10A at the position where the laser beam 20 was initially applied. Afterwards, a bending load was applied to the glass plate. 10A was applied and the glass plates 10 and 10B were joined by forming the edge surface 15 to connect the first adjacent surface 13 and the second adjacent surface 14 are obtained as shown in Fig. 6.
[0031] The surface roughness Ra of the glass plate 10 was determined using a surface roughness measuring device. (SURFCOM200DX2, manufactured by TOKYO SEIMITSU CO., LTD.) measured. The measurement conditions are below. described. Limit value >c: 0.08 mm Limit ratio <c / >s: 30 Measuring speed: 0.03 mm / s Rating length: 0.4 mm
[0032] In the first adjacent surface 13, the line 16, which represents the state of the crack extension, as can be seen in Fig. 7 As shown. When sunlight was shone onto the first adjacent surface 13, diffraction caused and the interference of the light made a structural color visible, so that a glass plate was obtained which had a The outer edge exhibited excellent visibility. Furthermore, various colors were visible, as the color of the structural color changed depending on the viewing angle, so that a glass plate was obtained which had a It exhibited excellent design. Lines 16, which represented the state of the crack's extension, were along one edge of the glass plate 10 was arranged, while the lines 16 were separated by intervals. When the glass plate 10 was in When viewed from a direction perpendicular to the main plane of the glass plate 10, each line 16 was curved. The shape of the Line 16 represents a time-dependent variation in the position of the crack tip during laser scanning. Each line 16 had an end section 16a on the side of the first main level 11 behind an end section 16b. the side of edge surface 15 in the scanning direction of the laser beam. It is evident from this that the crack originates from an internal Section of the glass plate 10A was extended in the direction of the surface, instead of extending from the first main plane 11A of the to extend glass plate 10A in the depth direction. According to the inventors' knowledge, there is a tendency such that if a crack spreads from an inner section of glass plate 10A in the direction of a The surface extends, line 16 appears, representing the state of crack elongation. On the first The distance between lines 16 and the adjacent surface 13 was 58.8 µm and the surface roughness Ra was 4.0 nm. The spacing of lines 16 was identical. If the spacing of lines 16 is identical, then there is a A tendency for diffraction and interference of light to occur, compared to a case an irregular spacing, and visibility and design can be improved.
[0033] On the second adjacent surface 14 was the line 16, which indicated the state of the crack extension. This is visible, as shown in Fig. 8. When sunlight shines onto the second adjacent surface 14 Due to diffraction and interference of light, a structural color became visible, so that a glass plate was obtained, which showed excellent visibility of the outer edge. Furthermore, various colors were visible, because the color of the structural color changed depending on the viewing angle, so that a glass plate was obtained, which exhibited an excellent design. Line 16, which shows the state of the crack extension. The lines were arranged along one edge of the glass plate 10, while the lines 16 were separated by intervals. When the glass plate 10 was viewed in a direction perpendicular to the main plane of the glass plate 10, every line 16 curved. The shape of line 16 represents a time-dependent variation in the position of the crack tip during the Scanning with the laser. In each line 16 there was an end section 16c on the side of the second principal plane 12. behind an end section 16d on the side of the edge surface 15 in the scanning direction of the laser beam. From this, It was evident that the crack extended from an inner section of glass plate 10A in the direction of the surface, instead of extending from the second main plane 12A of the glass plate 10A in the depth direction. On the second On the adjacent surface 14, the distance between lines 16 was 58.8 µm and the surface roughness Ra was 5.0 nm. The spacing of lines 16 was identical. If the spacing of lines 16 is identical, then there is a A tendency for diffraction and interference of light to occur, compared to a case an irregular spacing, and visibility and design can be improved.
[0034] It should be noted that the embodiment shows an example in which the distance is identical The distance is, however, the lines 16 can be formed with an irregular distance. [Example 2]
[0035] Fig. 10 is a top view showing a scanning direction of a laser beam with respect to a glass plate in Example 2. Figure 11 shows a side view depicting the state after a load has been applied to the glass plate in Figure 10. has been exercised. Fig. 12 is a micrograph of the first adjacent surface of the glass plate, which is shown in Fig. Figure 11 is shown. In Figure 12, a line representing a state of crack elongation is highlighted.
[0036] In Example 2, as shown in Fig. 10, the front and back surfaces of the glass plate 10A were compared. with example 1. The glass plate 10A was scanned using a laser beam 20 passing through the glass plate. 10A passes from the first main level 11A to the second main level 12A, is locally heated, and the The irradiation position of the laser beam 20 was varied. A glass plate with a thickness of 2.8 mm was used as glass plate 10A. mm (a soda-lime glass manufactured by ASAHI GLASS CO., LTD.) was used. The light source 22 of the laser beam 20 was... a Yb fiber laser (wavelength 1070 nm) was used and the laser beam 20 was directed perpendicularly onto the first principal plane 11A irradiated. The absorption -1 The coefficient (Δ) of the glass plate 10A with respect to the laser beam 20 was 0.57 cm and the internal transmittance was 85%. On the first principal plane 11A, the beam shape of the laser beam 20 was a circular shape with a diameter of 0.5 mm. The condenser lens 25 for collecting the laser beam 20 was located between the light source 22 and the glass plate. 10A installed. The focus position of the condenser lens 25 was a position that was from the first principal plane 11A in the direction The light source 22 was 9.06 mm away, and the convergence angle was 6.3 degrees. The output power of the Light source 22 had a power of 100 W. The scanning with laser beam 20 was performed at a speed of 10 mm / second. parallel to the two parallel edges of the four edges of the glass plate 10A, which had a trapezoidal shape as shown in Fig. 9 As shown, the procedure was carried out. An initial crack was made in an edge that obliquely intersects the two parallel edges. Formed beforehand with a file. The initial crack was created in a position where radiation exposure was expected. The process began with the laser beam 20. The scanning direction of the laser beam 20 was relative to a tangent line of a The outer edge of the glass plate 10A is inclined at the position where the laser beam 20 was first directed. Since a tensile stress was generated at the position onto which the laser beam 20 was directed, by varying the position onto which the laser beam 20 was directed, the crack starting from the initial crack as the starting point extended.
[0037] In Example 2, unlike in Example 1, a pulse oscillation laser was used as the Yb fiber laser. Pulse width was set to 200 µs and repetition frequency was set to 400 Hz.
[0038] Furthermore, in Example 2, unlike in Example 1, the first cooling nozzle 28 and the second cooling nozzle 29, which are located in As shown in Fig. 3, only the first cooling nozzle 28 is used and the second cooling nozzle 29 is not used. The center line of the first cooling nozzle 28 was in the scanning direction of the laser beam with respect to the optical axis of the The laser beam 20 was tilted backwards by 45 degrees. The first cooling nozzle 28 had a circular ejection opening with a A diameter of 1 mm was created, forming a gap of 10 mm with the glass plate 10A, and the cooling gas was injected with a Flow rate of 10 liters / minute. Compressed air was used as the cooling gas.
[0039] The glass plate 10A was moved relative to the light source 22 and the first cooling nozzle 28, so that the crack starting from the initial crack, it was extended. As a result, the first adjacent Surface 13, which intersects the first principal plane 11A at an obtuse angle, and the second adjacent Surface 14, which intersects the second principal plane 12A at an obtuse angle, are formed simultaneously, as it as shown in Fig. 10. A bending load was then applied to glass plate 10A and the glass plates 10 and 10B were formed by creating the edge surface 15 to connect the first adjacent surface 13 and the second adjacent surface 14, as shown in Fig. 11.
[0040] In Example 2, the line 16, which represents the extension state of the first adjacent surface 13, was located on the first adjacent surface 13. The crack is visible, as shown in Fig. 12. When sunlight hits the first adjacent surface 13 When light was shone on it, a structural color became visible due to diffraction and interference of the light, so that A glass plate was obtained that offered excellent visibility of the outer edge. Furthermore, various Colors were visible because the color of the structural color changed depending on the viewing angle, so that a A glass plate was obtained, which had an excellent design. Lines 16, which indicate the state of the extension of the The cracks were arranged along one edge of the glass plate 10, while the lines 16 were separated by intervals. were. When the glass plate 10 was viewed in a direction perpendicular to the main plane of the glass plate 10, each Line 16 curved. In each Line 16 there was an end section 16a on the side of the first main level 11 in front of a End section 16b on the side of the edge surface 15 in the scanning direction of the laser beam. From this it can be seen that the The crack extended from the first main plane 11 in the depth direction of the glass plate 10A. Furthermore, on the first Adjacent surface 13, the distance between lines 16 was 25 µm. The distance between lines 16 was identical. If the distance between lines 16 is identical, there is a tendency for diffraction and an interference of the light occurs, compared to a case of an irregular distance, and the Visibility and design can be improved.
[0041] It should be noted that in a case where a pulse oscillation laser is used as the light source of a The laser beam is used by varying at least one of its pulse widths and repetition frequencies. The spacing of lines 16 can be adjusted. The spacing of lines 16 can be adjusted during scanning with the laser. will be changed.
[0042] Additionally, for a case in which a pulse oscillation type laser is used as the light source of a laser beam will be the reproducibility of the spacing of the lines 16 that are to be formed len, compared to a case where a continuous oscillation laser is used, is advantageous, so that The desired visibility and design on the outer edge of the glass plate are always maintained. can.
[0043] Above, embodiments of the glass plate have been described. However, the present invention is not limited to the The embodiments described above are limited, and various modifications and improvements are possible. within the scope described in the patent claims.
[0044] For example, the glass plate 10 includes at least on a part of the outer edge both the first adjacent Surface 13 as well as the second adjacent surface 14; however, it is sufficient if the glass plate 10 at least one of them. For example, the glass plate 10 can encompass the first adjacent surface 13 and The glass plate 10 cannot encompass the second adjacent surface 14. In this case, the edge surface 15 can The second main plane 12 can be cut perpendicularly. Alternatively, the glass plate 10 can cut the second adjacent surface 14. encompass and the glass plate 10 cannot encompass the first adjacent surface 13. In this case, the The edge surface 15 intersects the first principal plane 11 perpendicularly.
[0045] Furthermore, the glass plate 10 comprises at least a part of its outer edge the edge surface 15, which is perpendicular to the first principal plane 11 and the second principal plane 12. However, the shape of the edge surface 15 is not special. restricted. For example, the edge surface 15 can be an arc surface instead of a flat surface.
[0046] Furthermore, the glass plate 10 can be a flat plate or a curved plate and the glass plate 10 can any ornamental glass with a rough pattern formed on the surface, wired glass, which is comprising a metal mesh or metal conduits or wires, a film-coated glass in which a functional film, such as an anti-reflective film (AR film), is applied to the surface of a laminated glass and be tempered glass.
[0047] Furthermore, the method for producing the glass plate 10 is not limited to the one shown in Fig. 3 and Fig. 4. The procedure is limited. For example, in Fig. 3 and Fig. 4, at the position where the irradiation of the The laser beam 20 begins to trace the outer edge of the glass plate 10 into a straight line; the outer edge of the However, glass plate 10 can have a curved shape. The first adjacent surface 13 and the second Adjacent surface 14 can be obtained as long as the scanning direction (the X-direction in Fig. 4) of the The laser beam 20 is inclined with respect to the tangent line of the outer edge of the glass plate 10A at the position where it is inclined with the irradiation of the laser beam 20 begins. In addition, there is a requirement to obtain the first adjacent surface 13 and the second adjacent surface 14 a method in which a laser beam, which is exhibits an asymmetric cross-sectional shape or an asymmetric intensity distribution on the cross-section, which The glass plate 10A is irradiated. For example, by inserting a shielding plate in the middle of the The beam path of the laser beam results in a laser beam that has an asymmetrical cross-sectional shape or a exhibits an asymmetric intensity distribution across the cross-section. In a case where this laser beam is used... will be, even if the scanning direction of the laser beam 20 is not in relation to the tangent line of the The outer edge of the glass plate 10A is inclined at the position where the laser beam 20 is first directed. The first adjacent surface 13 and the second adjacent surface 14 are formed simultaneously. Furthermore According to Fig. 3 and Fig. 4, the first adjacent surface 13 and the second adjacent surface 14 are formed simultaneously by the laser beam 20; however, only one of the first adjacent surfaces 13 can be formed. and the second adjacent surface 14 are formed. In addition, Figures 3 and 4 show both the The first cooling nozzle 28 as well as the second cooling nozzle 29 are used; however, one or both of the first may be used. Cooling nozzle 28 and the second cooling nozzle 29 should not be used.
[0048] The present application is based on and claims priority of Japanese patent application No. 2013- 273330, which was submitted on December 27, 2013. DESCRIPTION OF REFERENCE MARKS 10 glass plate 11 First Main Level 12 Second Main Level 13 First adjacent surface 14 Second adjacent surface 15 edge area 16. Line representing the state of a crack extension 20 laser beam 22 Light source 28 First cooling nozzle Second cooling nozzle 29
Claims
1. Glass plate, comprising an adjacent surface that intersects a principal plane at an obtuse angle, the adjacent surface is present at least on part of an outer edge, wherein the adjacent surface is a cutting plane formed by extending a crack by creating a Tensile stress by scanning with a laser beam along at least a part of an outer edge of the glass plate has been formed, the adjacent surface forms a diffraction grating having at least one of a Wallner line and a stop line, and an arithmetic mean roughness Ra, which is described in JIS B0601, of the adjacent surface is less than or equal to 100 nm.
2. Glass plate according to claim 1, wherein the at least one of the Wallner line and the stop line is arranged along at least a part of an outer edge of the glass plate.
3. Glass plate according to claim 1 or 2, wherein when the glass plate is in a direction perpendicular to the main plane is considered, at least one of the Wallner line and the stop line is curved.
4. Glass plate according to one of claims 1 to 3, wherein at least a part of the diffraction grating consists of at least one of the Wallner lines, which are arranged at an identical distance, or the stop lines, which are arranged at an identical are arranged at a distance.
5. A method for processing a glass plate, comprising: a step of forming, in the glass plate, an adjacent surface which is a principal plane of the glass plate in a obtuse angle, by locally heating the glass plate by irradiating a laser beam, and by Moving a position at which the laser beam is irradiated, wherein the adjacent surface is a cutting plane formed by extending a crack by creating a Tensile stress by scanning with a laser beam along at least a part of an outer edge of the glass plate has been formed, the adjacent surface forms a diffraction grating having at least one of a Wallner line and a stop line, and an arithmetic mean roughness Ra, which is described in JIS B0601, of the adjacent surface is less than or equal to 100 nm.
6. A method for processing a glass plate, comprising: a step of simultaneously forming, in the glass plate, a first adjacent surface having a first principal plane the glass plate at an obtuse angle, and a second adjacent surface forming a second Main plane of the glass plate at an obtuse angle, by locally heating the glass plate by irradiation a laser beam, and by shifting a position at which the laser beam is irradiated, wherein each of the first adjacent surface and the second adjacent surface is a cutting plane defined by a extension of a crack, each of the first adjacent surface and the second adjacent surface forms a diffraction grating comprising at least one of a Wallner line and a stop line, and a arithmetic mean roughness Ra, which is described in JIS B0601, of the adjacent surface less than or equal to 100 nm.
Citation Information
Patent Citations
Chamfering method for brittle substrate
CN101386466A
Working method for glass by means of laser and device therefor
JP2002241141A
Laser beam machining apparatus and laser beam machining method
JP2007021548A
Rotary grinding wheel
JP2008093744A
CN000101386466A
Cited By
Cover glass and display device
DE112017002734T5
Method for processing brittle-hard materials
US12544861B2