Combination of piezoelectric and magnetostrictive materials to obtain a magnetoelectric composite material exhibiting self-polarizing behavior
A composite material with specific layer thicknesses and bonding methods achieves self-polarization and high magnetoelectric output, addressing the need for external magnetic fields in implantable devices and enhancing deformation efficiency.
Patent Information
- Application Number
- FR2023003015
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-04
AI Technical Summary
Existing magnetoelectric composites rely on external magnetic fields for polarization, which limits their application in implantable medical devices due to the need for continuous field application, and conventional laminar composites with thin nickel layers fail to achieve sufficient deformation of piezoelectric materials.
A composite material is developed with specific layer thicknesses of magnetostrictive and piezoelectric materials, including nickel layers of 1 to 50 pm and piezoelectric layers of less than 1 mm, bonded using sputtering growth to achieve self-polarization and significant deformation, eliminating the need for external magnetic fields.
The composite material achieves a high magnetoelectric output of -100 V/(cm Oe) in the -100-400 kHz regime, facilitating efficient self-polarized magnetoelectric devices without lead or rare earths, and reduces structural fatigue through strong physical bonding.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Title of the invention: Combination of piezoelectric and magnetostrictive materials for obtaining a magnetoelectric composite material exhibiting self-polarizing behavior
[0001] The present invention relates to the field of laminar composite materials comprising a piezoelectric substrate associated with layers of magnetostrictive materials.
[0002] Bibliographic references in the following text are noted in this way in the description text: [] ; and listed in the reference table. Prior art
[0003] Magnetoelectric (ME) composites open up possibilities in various engineering fields for designing sensors, transducers, filters, and other devices based on the change in electrical polarization induced by an excitation magnetic field (direct ME effect) or by the change in M (magnetization) induced by an excitation electric field (inverse ME effect). For example, the possibility of harvesting electrical energy from an external excitation magnetic field for use in integrated medical devices is particularly interesting [1].
[0004] The term “magnetoelectric”, used hereafter by its acronym “ME”; defines the ability of a material to vary its state of magnetization under the action of an electric field and to vary its state of electric polarization under the action of a magnetic field, generally composed of a static polarization component and a small signal dynamic component.
[0005] Furthermore, the use of a micro-energy source ME to power a sensor in the biomedical field through the human body is known. This application is feasible by employing a small-signal dynamic magnetic field operating in a frequency range where there is no absorption by the human body (approximately 100 kHz) [2].
[0006] ME devices incorporating laminar composites made of ferroelectric (FE) materials (e.g., BaTiO3, Pb(Zr, Ti)O3, Pb(Mg, Nb)O3, PbTiO3) bonded to ferromagnetic (FM) and magnetostrictive materials (e.g., CoFe2O4, Terfenol-D, Galfenol) leading to effective cross-coupling via intense elastic mechanical deformation upon application of a magnetic field, i.e., magnetoelastic coupling, are common [3]. Self-polarization conditions are difficult to achieve, but they allow ME composites to become independent of the static component of the excitation magnetic field.
[0007] The term “magnetostrictive” defines a material exhibiting a magnetostriction property, which characterizes the ability of a material to deform according to the orientation of its magnetization, for example under the influence of a magnetic field.
[0008] The term “self-bias” defines the ability to obtain a usable magnetoelectric coefficient without the need to impose an external continuous magnetic field, which greatly simplifies the technology of ME devices and facilitates their use for implantable medical device purposes.
[0009] Due to their magnetic properties, nickel (Ni) films are good candidates for magneto-elastic actuation by coupling with substrates that exhibit structural anisotropy in the plane parallel to the surfaces, such as LiNbO3. Nickel films are usually composed of randomly distributed crystals (so-called polycrystalline film). However, magnetization and magnetostriction curves can exhibit anisotropic behavior when an extensive (positive) or compressive (negative) external stress is applied along the x and y directions of the plane. An example of controlling the magnetic anisotropy of nickel films deposited on LiNbO3 is known from document [4].However, the nickel layers in [4] are too thin, at most 100 nm, to induce sufficient deformation of the LiNbO3 bearing the nickel layers on its faces by applying an external magnetic excitation field. Indeed, the Ni layers are deposited using a laboratory technique well-suited to the study of very thin films (electron beam evaporation), which therefore does not allow for sufficient deformation. Description of the invention
[0010] To overcome the drawbacks of the aforementioned prior art, the present invention relates to a composite material, comprising the stacking of layers one on top of the other in the following order: • a first layer comprising a magnetostrictive material with a thickness of 1 to 50 pm; • a second layer comprising a piezoelectric material less than 1 mm thick; and • a third layer comprising said magnetostrictive material with a thickness of 1 to 50 pm.
[0011] The inventors have shown entirely by chance that the combination of such layers in these thickness ranges makes it possible to obtain sufficient deformation of the piezoelectric material by the magnetoelectric material under self-polarization conditions. Such a composite material incorporating relatively thick magnetostrictive layers inducing significant longitudinal deformations of the piezoelectric layer makes it possible to obtain a high ME output (-100 V / (cm Oe)). in the -100-400 kHz range.
[0012] Advantageously, the magnetostrictive material is selected from the following materials: nickel (Ni), iron (Fe), metallic alloys comprising Ni, metallic alloys comprising Fe, Fe-based oxides and cobalt (Co)-based oxides, such as CoFe2O4.
[0013] Advantageously, the piezoelectric material is selected from materials comprising at least one of the elements chosen from N (nitrogen), Fe, Nb (niobium), Bi (bismuth), Li (lithium), Ti (titanium), Ba (barium), Pb (lead), Al (aluminium), Mg (magnesium), O (oxygen) and Zn (zinc); preferably, selected from LiNbO3, ZnO, BaTiO3, BiFeO3, LiTaO3, a lead zirconate titanate (PZT), a magnesium lead niobate - lead titanate (PMN-PT), or even aluminium nitride (AIN).
[0014] The inventors have shown that materials incorporating such stacks, for example Ni / LiNbO3 / Ni, make it possible to consider efficient self-polarizing magnetoelectric devices without lead and rare earth elements. The sputtering growth of these trilayers ensures a tight and strong physical bond between the magnetostrictive layers and the piezoelectric material. This is an advantage over conventional laminar composites, in which the magnetostrictive layers are bonded to the piezoelectric material using epoxy, making the composites susceptible to structural fatigue and material aging. In the case of Ni / LiNbO3 / Ni, the residual stresses are due to the mismatch in the coefficient of thermal expansion of Ni and LiNbO3, which, in turn, induces significant magnetic anisotropy and consequently a self-polarizing effect of the composite material
[11] .
[0015] PZTs, being lead zirconate titanoates, are chemical compounds with the formula PbZrxTiiXO3 (0 < x < 1) and are perovskite-structured ceramics. PZTs can be of the type PZT-5A, PZT-5H, or PZT-5J.
[0016] PMN-PT, being lead magnesium niobate - lead titanate, are compounds of formula xPb(Mgi / 3Nb2 / 3)O3-(lx)PbTiO3 (0 < x < 1), such as for example those described in article [5].
[0017] Aluminium nitride of formula AIN, whose IUP name AC is azanylidynealumane, is identified by a CAS number: 24304-00-5.
[0018] Advantageously, the piezoelectric material is selected from 36° Y-cut LiNbO3; 163° Y-cut LiNbO3; Y-cut LiNbO3; Y-cut LiTaO3; 36° Y-cut LiTaO3 and 163° Y-cut LiTaO3, and preferably from 36° Y-cut LiNbO3; 163° Y-cut LiNbO3; 36° Y-cut LiTaO3 and 163° Y-cut LiTaO3. The inventors have demonstrated that the crystalline orientation of the substrate, in particular 36° Y-cut and 163° Y-cut, induces anisotropic residual stress spontaneously in the magnetoelectric layers upon cooling after growth, as evidenced by X-ray diffraction and magnetometry measurements, described in the experimental section that follows.
[0019] The cut angle of the LiNbO3 crystal and that of LiTaO3 are defined with respect to an orthonormal coordinate system (X,Y,Z) which we define as follows: the Z direction is parallel to the ternary rotation axis present in these two crystals (space group R3c) [Wong, KK (2002). Properties of Lithium Niobate. London, United Kingdom: INSPEC. p. 8. ISBN 0-85296-799-3.] The lattice is defined by the usual basis vectors of a Bravais lattice of the hexagonal crystal family: (a, b, c), with c parallel to Z. We define X and Y as the two directions perpendicular to Z such that X is parallel to the vector a and Y is perpendicular to X. Consequently, the so-called Y-cut indicates that the crystal is cut with the Y axis parallel to the normal to the surface. The 163° Y-cut indicates that the crystal is cut at the plane rotated 163° relative to the Y plane around the X axis (counterclockwise rotation).The 36° Y-cut indicates that the crystal is cut at the plane rotated 36° with respect to the Y plane around the X axis (counterclockwise rotation). Advantageously, the thickness of each layer containing the magnetostrictive material is 5 to 35 pm.
[0020] Advantageously, the thickness of the layer comprising the piezoelectric material is from 100 to 500 pm.
[0021] The present invention also relates to a method of manufacturing the composite material according to the invention comprising at least one step of depositing one of the selected layers between the first and third layers designated as thin layers, onto the second layer designated as substrate, implementing the sputtering technique.
[0022] Advantageously, the manufacturing process according to the present invention comprises the following steps: a- cleaning the surfaces of the substrate, preferably chosen from a double-sided polished LiNbO3 plate, in an ultrasonic bath with acetone, then with isopropanol; b- introducing the substrate into a sputtering deposition apparatus;
[0023] c- once a vacuum is established, perform in-situ plasma surface cleaning of the aforementioned substrate in the growth frame; and d- Spray a thin layer of magnetostrictive material, preferably a Ni film, at a pressure of 10⁻³ to 10⁻¹ mbar, with a power of 100 to 1000 W (i.e., between 1 W / cm² and 13 W / cm²). The temperature applied to the substrate during this magnetostrictive material deposition step can vary from ambient temperature up to 600°C.
[0024] e- repeat steps b-, c- and d- previously described on the opposite face of the LiNbO3 plate.
[0025] Advantageously, the cathode sputtering apparatus is an SCM400 frame, comprising a magnetron, formerly marketed by the Alcatel company. The mode used is an RF mode (13.56 MHz) under Ar gas.
[0026] Advantageously, the Ni sputtering in steps d- and e- is carried out while maintaining a bare surface, preferably 0.5 to 1.5 mm wide, on the edges of the LiNbO3 substrate plate. The objective being that the two opposite faces do not short-circuit after the Ni depositions.
[0027] The present invention also relates to a magnetoelectric transducer comprising the composite material according to the invention, and a magnetic field source.
[0028] The present invention also relates to the use of a magneto-electric transducer according to the invention, for obtaining a potential difference between the first and third layers comprising the magnetostrictive material by applying a small dynamic magnetic field in the direction of the planes of the layers at a frequency of 100 to 400 kHz. This dynamic magnetic field has a sufficiently low amplitude to maintain a linear approximation. This is the case here because the magnetic field has an amplitude of 1 Oe = 0.1 mT and the response of the magnetostrictive material is linear.
[0029] The present invention also relates to a magnetoelectric device comprising a magnetoelectric transducer according to the invention, for generating an electric voltage without applying a continuous, so-called static, magnetic field. Such behavior of the device is attributed to so-called self-bias phenomena.
[0030] Such a device can be advantageously used to power electronic microsystems for monitoring deformations in construction infrastructure, or in the medical field, used in a medical implant.
[0031] The present invention is also described in the detailed description that follows, with reference to the experimental part which details certain embodiments by means of examples, given only by way of illustration and which should not be considered limiting, and the figures briefly described in the part that follows. Brief description of the figures
[0032] [Fig.l] - the [Fig.l] represents illustrations of the different sections of the single-crystal substrate LiNbO3;
[0033] [Fig.2] - [Fig.2] represents the XRD diagrams of the deposited nickel films (Cu target with a monochromator wavelength X = 1.54 Â);
[0034] [Fig. 3] - [Fig. 3] represents the characterization of the Ni / LiNbO3 / Ni trilayer with magnetic fields applied along the x or y axes
[0035] [Fig.4] - [Fig.4] represents an ME resonance measurement performed to de- to determine the electromechanical resonance (EMR) frequency of each sample in their two directions in the plane; two different cuts of LiNbO3 are studied: (YX1) 36° (a) and (YX1) 163° (b);
[0036] [Fig.5] - the [Fig.5] represents the ME coefficient as a function of the HDC for the Ni / (YX1) 36° Y-cut LiNbO3 / Ni and Ni / (YX1) 36° Y-cut LiNbO3 / Ni samples in the x and y directions, the measurements are carried out at the electromechanical resonance frequency (EMR) of each sample;
[0037] [Fig.6] - the [Fig.6] represents the magnetization of Nickel films in a three-layer sample and in the free state;
[0038] [Fig.7] - Figure 7 represents the ME hysteresis loops and (dM2 / dH)-H curves three-layered samples;
[0039] [Fig.8] - [Fig.8] represents the VSM magnetization cycles measured at different temperatures in both directions of a Ni / (YX1) 36° Y-cut LiNbO3 / Ni trilayer. ; and
[0040] [Fig.9] - [Fig.9] represents the XRD diagrams in the plane of the (311) Ni peak from a sample incorporating the (YX1) 36° Y-cut LiNbO3 (target Cu without monochromator, X of K_a= 1.5419 Â). Experimental Section
[0041] Materials and methods Within the framework of the invention, the diffractometer implemented for X-ray diffraction is a multi-configuration 5-circle rotating anode "Smartlab®" Rigaku diffractometer, suitable for thin films enabling grazing incidence diffraction and other high-resolution measurements.
[0042] Two commercial single-crystal LiNbO3 substrates (supplied upon specific request from NEYCO®) polished on two faces, Y-cut at 36° – “36° Y-cut” (20x5x0.1 mm³) and Y-cut at 163° – “163° Y-cut” (10x5x0.1 mm³) were used to deposit thick polycrystalline Ni films on each face by RF magnetron sputtering. A high-purity Ni target (Ni > 99.95%) was used. The “a” axis is identified by the (210) peak of the single-crystal LiNbO3 substrates using in-plane X-ray diffraction (XRD). It is observed that the “a” axes of the two LiNbO3 substrates are parallel to their x (length) directions. As shown in [Fig. 1], the 36° Y-cut and the 163° Y-cut can also be designated as (YX1) 36° and (YX1) 163° respectively according to the IEEE | ANSI / IEEE Std 176-1987 An American National Standard IEEE Standard on Piezoelectricity, 74].Prior to deposition, the LiNbO3 substrates were chemically cleaned (ultrasonic bath with first acetone then isopropanol) before being introduced into the sputtering deposition machine, and the surfaces of the substrates were cleaned in situ using a plasma. of argon. Nickel films with a thickness of 5 to 35 µm were deposited on both surfaces under a pressure of 10⁻¹ mbar with a power output between 100 and 500 W. The limiting vacuum of the sputtering chamber was 10⁷ mbar. Deposition was performed under an argon atmosphere, at room temperature or at 200°C. The distance between the target and the substrate support was 65 mm. A 1 mm gap was maintained between the edges of the LiNbO₃ substrate and the edges of the nickel film to prevent short-circuiting the deposited nickel films. Both surfaces of the same sample were assumed to be symmetrical, with the same amount of Ni.
[0043] The XRD patterns of the deposited nickel films (arbitrary side) of the two samples are shown in [Fig. 2], and compared to the pattern of the reference polycrystalline Ni target. The nickel films deposited on the LiNbO3 substrate are polycrystalline. Results and discussion
[0044] Characterization of magnetoelectric (ME) behavior
[0045] As shown in [Fig. 1], the ME behaviors of the Ni / LiNbO3 / Ni samples are characterized in the so-called LT mode, where the external magnetic field is applied longitudinally in the direction of the x or y plane, and the output electric voltage is polarized transversely in the z direction. According to studies published in [6-7], the ME coefficient aE is mainly determined by the transverse piezoelectric constants d_31AP, thus the (YX1) 36° and (YX1) 163° cuts are chosen with high values [8], i.e. d_31AP ~ 18 pC / N for the first and d_31AP ~ -20 pC / N for the second respectively, favoring the ME effect along the x and y directions of the experimental setup, respectively (see [Fig. 3]).
[0046] The characterization of the ME coefficient was performed using the same setup as described in [2]. A 100-turn copper coil was used to apply a small harmonic magnetic signal Hac of 1 Oe = 0.1 mT RMS. This field was driven by an alternating current from a Rohde & Schwarz® HM8150 arbitrary waveform generator. Simultaneously, a static magnetic field of HDC polarization was superimposed in the same direction as Hac by fixing the distance "d" between two blocks of permanent magnets mounted on a movable rail and previously calibrated with a gaussmeter at the center of the copper coil. The ME samples were inserted into the center of the coil to apply the superimposed magnetic field during the characterization of the ME coefficient. They were mounted in a sample holder made of plastic plates printed by a 3D printer and two separate conducting wires.Plastic plates were used to align the length or width direction of the ME samples with the applied magnetic field; the wires were made electrically contacted with the Ni films on both sides of the ME sample. Then the ME output voltage (VME) was measured. generated between the Ni layers of an ME sample is measured using a Keysight® MSO7054A digital oscilloscope. From these results, the ME coefficient aE is obtained using formula (A) where tp is the thickness of the piezoelectric substrate:
[0047] [FORMULA A] 6'?.- “ / t
[0048] In order to clearly study the ME aE behavior as a function of the HDC value of the Ni / LiNbO3 / Ni samples, the Hac frequency is fixed close to the electromechanical resonance frequency (EMR) of each sample to obtain a significant magnitude of the output voltage VME. This frequency or EMR is calculated using the following equation according to formula (B) [9], where l is the length of the piezoelectric substrate, y is the average Young's modulus, and p is the average volume density of the ME composite.
[0049] [FORMULA B] ^0 = V 21
[0050] The measurements are shown in [Fig. 4]: the first harmonics obtained are approximately 160 kHz and 320 kHz for the samples with the (YX1) 36° substrate, 20 mm long, and the (YX1) 163° substrate, 10 mm long, respectively [9]. The electromechanical resonance (EMR) frequency corresponding to the maximum of the V ME is identified by ME voltage measurements performed by sweeping the frequency of the Hac signal. Next, the characterization of the ME coefficient is performed by sweeping the H DC first from -710 Oe = -71 mT to 710 Oe = 71 mT, then from 71 to -71 mT. The direction of HDC is changed by permuting the permanent magnets in the position of Hdc ≈ 0 mT (see [Fig. 4]).
[0051] As shown in [Fig. 5], each measurement exhibits a maximum ME response to the optimal polarization magnetic field, Hbias. It is noted that the values of Hbias in the x direction are much lower than those in the y direction, where x is parallel to the al axis in the trigonal system of LiNbO3 and y is the axis perpendicular to x, in the plane: for the Ni / (YX1) 36° Y-cut LiNbO3 / Ni, Hbias is equal to ±37 Oe = ± 3.7 mT and ±149 Oe = ± 14.9 mT in the x and y directions, respectively. For the Ni / (YX1) 163° Y-cut LiNbO3 / Ni, Hbias is equal to ±106 Oe = ± 10.6 mT and ±238 Oe = ±23.8 mT in the x and y directions, respectively.
[0052] In [Fig. 5] (Figures 5a and 5b), a "self-polarized" behavior is shown for Hac parallel to the x-direction. Interestingly, at HDC = 0, aE is at 94.20% of Its maximum value for the sample grown on substrate (YX1) is 36° LiNbO3, and at 80% for the one grown on substrate (YX1) 163° LiNbO3. Furthermore, the self-bias behavior is strongly reduced in the y direction, where the aE values are less than 40% of their maximum values.
[0053] Measurement of magnetic anisotropies: role played by the LiNbO3 substrate
[0054] In what follows, we relate the ME response of our devices to the intrinsic magnetic properties of Ni films and we show the important role played by the LiNbO3 substrate. To this end, magnetic hysteresis loops are collected using a vibrating sample magnetometer (VSM) available on a Physical Property Measurement System (PPMS) from Quantum Design®.
[0055] The magnetization (M) was measured at 300 K as a function of the HDC from 2 kOe = 200 mT to 500 Oe = 50 mT (step = 10 Oe = 1 mT), then from 500 Oe = 50 mT to -500 Oe = -50 mT with high precision (step = 2 Oe = 0.2 mT), then from -500 Oe = -50 mT to -2 kOe = -200 mT, and finally a repetition in reverse. A precise determination of the coercive field was attempted during these measurements. Before mounting each sample, an oscillating field from 10 kOe = 1 T to zero was applied to reduce the residual magnetic field in the solenoid to less than 5 Oe = 0.5 mT.
[0056] The samples were laser-cut into 5 x 5 mm² pieces to fit the VSM sample holder. After measuring the magnetization of the trilayer sample, self-supporting nickel films whose magnetization had been measured by VSM were isolated. As shown in [Fig. 6], anisotropic magnetization behavior is observed in the trilayer samples, with higher remanence and a weaker saturation field in the x direction compared to the y direction. Interestingly, the anisotropy is greater in the trilayer samples than in the isolated Ni films. The anisotropy is significantly reduced in the self-supporting films, indicating the important role played by the residual stress imposed by the substrate. This allows us to deduce that the LiNbO3 substrates induce anisotropic internal stress and a consequent magnetic anisotropy.
[0057] Relationship between magnetic anisotropies and ME
[0058] In order to relate the magnetic anisotropy to the anisotropic ME response, we compare the M(H) cycles with the field dependence aE. Indeed, the ME coupling combines piezomagnetic and piezoelectric effects, both of which are assumed to be linear
[10] . The ME coefficient can be written as the product of the gradients of the piezomagnetic and piezoelectric effects: aE = / dS xdD / dT xdE jdtyxdS / dH , where T is the stress, D is the displacement field, E is the electric field, and S is the strain. Thus, the magnetic field dependence of the ME coefficient is such that gF oc 35 / dH — dÀjdH, where 2 is the deformation due to magnetostriction. Since A. M2^ finally the relation obtained by the inventors is aE dM2 / dH as relation linking the ME response and the magnetization.
[0059] As shown in [Fig.7], we find a good agreement between the dependence of H on (dM2 / dH) and the ME hysteresis loop (permutation of the sign of a_E at antiresonances), attesting that the ME anisotropy behavior reflects the magnetic anisotropy of the nickel films in contact with the LiNbO3 substrates.
[0060] Origin of magnetic anisotropies and ME
[0061] The results presented in this section show that the origin of the magnetic anisotropy lies in the difference between the coefficient of thermal expansion (CTE) of Ni and that of LiNbO3. The thicknesses of the two Ni layers are 1 µm each, and that of the LiNbO3 substrate is 100 µm. Similar effects were observed for Ni thicknesses of 35 µm. Indeed, the samples are heated during deposition due to plasma exposure and the deposition temperature imposed on the substrate, and then cooled to room temperature (300 K) after the sputtering growth procedure. Thus, the nickel films of the three-layer samples are subject to residual stresses m related to the effects of thermal expansion, i.e., the very general formula ar, ij — Ce, ijkl {as - af )kl ziT , where as and a / are respectively the coefficients of thermal expansion of the LiNbO3 substrate and the Ni film, AT the difference between the ambient temperature and the temperature during the sputtering deposition process, and Ce, ijkl is the elastic tensor of the nickel film. The experiments presented below investigate the biaxial (residual) stress in the plane, induced in the nickel films, i.e., xx and 55. Since the CTE of the LiNbO3 substrate in the x direction is higher than the CTE of nickel, as shown in Table 1 (as - af > 0), a negative (compressive) residual stress develops during cooling of the sample. On the other hand, the coefficient of thermal expansion of the LiNbO3 substrate in the y direction is lower than the CTE of nickel, as shown in Table 1 (“5-af < 0”) leading to a positive residual (extensional) stress under cooling conditions.Thus, the residual stress is anisotropic at room temperature, leading to the observed magnetic anisotropy. Indeed, the order of magnitude of the residual stress can be estimated by considering an AT of -100 K due to the growth procedure and a Young's modulus of nickel Ce = 207 GPa. It turns out that the expected residual stress, ar, will be on the order of 50 MPa, with opposite signs in the x and y directions.
[0062] [Tables 1] a in the direction xa in the direction [K1] y [K1] Nickel 13x106 13x106 (YX1) 36° LiNbO3 15.4X106 10.23X106 (YX1) 163° LiNbO3 15.4X106 10.9X106 Table 1: CTE of nickel af and LNO substrates as
[0063] Probe stress-induced magnetic anisotropy by magnetic and structural measurements
[0064] The inventors also carried out the following experiments in order to determine the most suitable conditions for obtaining the ideal deformation induced by phenomena related to magnetic anisotropy.
[0065] MfH curves) at different temperatures:
[0066] Figure 8 shows the magnetization cycles measured by VSM in the x and y directions as a function of temperature. It appears that the magnetization cycles are strongly temperature-dependent in the y direction: the magnetic remanence is higher at 400 K than at 200 K. In the x direction, a high remanence is found at all probed temperatures. This indicates that the residual stress is released by heating, leading to more isotropic magnetic behavior at 400 K. This behavior is consistent with that observed in Figure 6, where the magnetization cycles of the self-supporting films are significantly altered in the y direction compared to the cycles measured for the same layer when it was still in contact with the substrate.
[0067] Determination of residual stresses by the X-ray diffraction method
[0068] The existence of residual stresses is confirmed by a direct and quantitative determination of the changes in the atomic spacing of the nickel film by XRD phi-scan along the x and y directions. We compare the atomic spacing corresponding to peak (311), d311, in the nickel film deposited on LiNbO3 with the free nickel film after removal from the substrate. As shown in [Fig. 9], by fitting the measured peaks (311) using the Pseudo-Voigt function, the value of d311 can be estimated in the x and y directions. The measured negative (positive) change in atomic spacing indicates a negative (positive) residual stress in x (y).
[0069] [Tables2] Neither in trilayer Nor isolated Neither in trilayer Nor isolated (x direction) (x direction) (y direction) (y direction) 20 [degree] 93.0401 93.0127 92.9828 93.0318 dsn [Â] 1.0625 1.0627 1.0630 1.0626 Change -0.0002 0.0004 of atomic space [Â] Table 2. Estimation of the variation in atomic spacing References
[0070] The following table 3 lists the references cited previously in the text: [Tables 3] 1 M. Paluszek, D. Avirovic, Y. Zhou, S. Kundu, A. Chopra, R. Montague, S. Priya, Compos. Magnetoelectrics, 2015, 297-327. 2 K. Malleron, A. Gensbittel, H. Talleb, Z. Ren, Microe-electronics Journal Volume 88, June 2019, 184-189 3 Xianfeng Liang, Huaihao Chen, and Nian X., SunMater 9, 2021 ,041114 4 Mathew, A. Scott, Press. Joum. Of Magnetism and Magnetic Mat. 566, 2023, 170314 5 loan Alexandru Ivan, Joël Agnus, Pierre Lambert. Sensors and Actuators A-Physical, Y1J, 2012, 37-47 6 Y. Zhou, S. Chul Yang, DJ Apo, D. Maurya, S. Priya, Appl. Phys. Eett.2W2, 101, 232905 7 F. Yang, YM Wen, P. Li, M. Zheng, LX Bian, Sensors and Actuators A : Physical2QQ8, 141, 129 8 Wang Yuea,, Jiang Yi-jian, Optical Materials 23, 2003, 2003-49 GG Wan, ZY Li, Y. Wang, M. Zeng, GH Wang, J.-M. Liu , Appl. Phys. On II.2005. 86, 202504 10 Yan, YK, Y. Zhou, and S. Priya. 2013. “Giant Self-Biased Magnetoelectric Coupling in Co-fired Textured Layered Composites.” Applied Physics Letters 102 (5):052907. doi: 10.1063 / 1.4791685. 11 Orpita Saha; Erik Andersen; Shad Roundy Wireless Power Transfer by Self-biased Magnetoelectric Laminate for Biomédical Implants, 2021IEEE 20th International Conférence on Micro and Nanotechnology for Power Génération and Energy Conversion Applications (PowerMEMS) p.36.
Claims
Claims
1. Composite material comprising stacking the layers on top of each other in the following order: - a first layer comprising a magnetostrictive material with a thickness of 1 to 50 pm; - a second layer comprising a piezoelectric material with a thickness of less than 1 mm; and - a third layer comprising said magnetostrictive material with a thickness of 1 to 50 pm.
2. A composite material according to claim 1, wherein the magnetostrictive material is selected from Ni, Fe, metal alloys comprising Ni, metal alloys comprising Fe, Fe-based oxides and Co-based oxides.
3. A composite material according to claim 1 or 2, wherein the piezoelectric material is selected from materials comprising at least one of the elements selected from N, Fe, Nb, Bi, Li, Ti, Ba, Pb, Al, Mg, O and Zn.
4. Composite material according to one of claims 1 to 3, wherein the piezoelectric material is selected from 36° Y-cut LiNbO3; 163° Y-cut LiNbO3; Y-cut LiNbO3; Y-cut LiTaO3; 36° Y-cut LiTaO3 and 163° Y-cut LiTaO3.
5. Composite material according to one of claims 1 to 4, wherein the thickness of each layer comprising the magnetostrictive material is 5 to 35 pm.
6. Composite material according to one of claims 1 to 5, wherein the thickness of the layer comprising the piezoelectric material is 100 to 500 pm.
7. Magnetoelectric transducer comprising the composite material according to one of claims 1 to 6, and a magnetic field source.
8. Use of a magnetoelectric transducer according to claim 7, for obtaining a potential difference between the first and third layers comprising the magnetostrictive material by applying a dynamic magnetic field of small amplitude in the direction of the planes of the layers at a frequency of 100 to 400 kHz.
9. Magnetoelectric device comprising a magnetoelectric transducer according to claim 7, for generating electrical voltages without applying a constant so-called static magnetic field.