Method and system for continuously executing ammonia decomposition and carbon monoxide generation
The integration of ammonia decomposition and carbon monoxide production in a single system with countercurrent flow reactors addresses inefficiencies in existing methods, enhancing gas production yield and reducing energy consumption.
Patent Information
- Application Number
- JP2023038400
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-13
- Publication Date
- 2024-09-27
AI Technical Summary
Existing methods for ammonia decomposition and carbon monoxide production require separate reactors for ammonia decomposition and reverse water gas shift reactions, leading to inefficiencies and high energy consumption.
A method and system that integrates ammonia decomposition and carbon monoxide production by using a single system with moving bed reactors, where metal/metal oxide materials are circulated between reactors in countercurrent flow, allowing continuous ammonia decomposition and carbon monoxide production.
This approach integrates ammonia decomposition and carbon monoxide production in a single system, reducing energy consumption and improving gas production yield by enhancing equilibrium conversion and producing a continuous stream of gaseous products.
Smart Images

Figure 2024129293000007 
Figure 2024129293000013 
Figure 2024129293000010
Abstract
Description
[Technical field]
[0001] The present invention relates to a method and system for continuously decomposing ammonia and producing carbon monoxide. [Background technology]
[0002] H2 is a component of synthesis gas (a mixture of hydrogen and carbon monoxide gases), which is a key intermediate in the production of chemicals and fuels from carbon dioxide (CO2), e.g., in methanol synthesis and the Fischer-Tropsch process. Ammonia (NH3) offers advantages over molecular hydrogen as an energy vector because it can be more easily liquefied, transported, and stored using existing infrastructure. Traditionally, NH3 is split into H2 and N2 at the point of consumption. Such splitting is a catalytic reaction shown in reaction (A) below. NH3 → 0.5N2 + 1.5H2(A) This reaction results in a mixture of unconverted NH3 with H2 and N2. Separation of H2 gas from NH3 and N2 gas requires complex processes with high energy consumption.
[0003] Patent document 1, which is a document related to a patent application (hereinafter abbreviated as "patent document"), discloses a system and method for converting fuel such as ammonia using a metal oxide supported on a carrier. In this system and method, a first reactor is used to reduce a primary metal oxide in the first reactor to produce a reduced metal or reduced metal oxide, and a second reactor is used to oxidize at least a portion of the reduced metal or reduced metal oxide transferred from the first reactor to regenerate the primary metal oxide. When the fuel is NH3, not only the ammonia decomposition reaction but also the reduction of the metal oxide by H2 generated from NH3 occurs, and a mixture of N2, H2, and H2O is produced in the first reactor. Then, in the second reactor, pure H2 is produced from H2O using the reduced metal oxide. This reduces the energy loss for separating N2 and H2 compared to the conventionally used ammonia pyrolysis that forms one mixed stream containing unconverted NH3, H2, and N2.
[0004] To produce synthesis gas using NH3 as a hydrogen source, the decomposition of NH3 is followed by a series of gas separation processes to produce the desired H2 product free of N2 gas, and then the H2 product and CO2 are subjected to a reverse water gas shift (hereinafter often abbreviated as "RWGS") reaction (reaction (B)) to produce carbon monoxide (CO) and HO. CO2+H2→CO+H2O (B) Therefore, the production of synthesis gas using NH3 requires several processes including the decomposition of NH3 and the RWGS reaction. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2017 / 205638 Summary of the Invention [Problem to be solved by the invention]
[0006] In the system disclosed in Patent Document 1, only H2 gas is produced in the second reactor. Therefore, in order to produce synthesis gas, the RWGS reaction for producing CO gas must be carried out separately from the ammonia decomposition reaction. [Means for solving the problem]
[0007] In view of the above problems, a first aspect of the present invention is the following method for continuously carrying out ammonia decomposition and carbon monoxide production. [1] A method for continuously carrying out ammonia decomposition and carbon monoxide production, comprising: 1) moving the metal / metal oxide material in a direction opposite to the flow of the NH3 gas in a first reactor, thereby contacting the continuous flow of NH3 gas with the oxidized metal / metal oxide material to convert the metal / metal oxide material to a reduced state while producing HO gas and N2 gas; 2) continuously transferring the reduced metal / metal oxide material to a second reactor while continuously withdrawing gaseous products including HO gas and N gas from the first reactor; 3) contacting the continuous flow of oxidized gas with the reduced metal / metal oxide material in a second reactor by moving the metal / metal oxide material in a direction opposite to the flow direction of the oxidized gas to convert the metal / metal oxide material back to its oxidized state while producing a reduced gas, the oxidized gas being CO2 gas or a mixture of CO2 gas and HO gas, and the reduced gas being CO gas or a mixture of CO gas and H2 gas; 4) continuously transferring oxidized metal / metal oxide material to the first reactor while continuously withdrawing gaseous products, including reduced gas, from the second reactor; 5) Steps 1) to 4) are repeated continuously. The method includes: [2] The method according to [1] above, wherein each of the first reactor and the second reactor is a moving bed reactor, and the metal / metal oxide material is a moving bed in the moving bed reactor. [3] The method according to [1] above, wherein the metal / metal oxide material is an iron oxide material. [4] The method according to the above [3], wherein the reaction temperatures in both the first and second reactors are 700°C to 750°C.
[0008] A second aspect of the present invention is the following system for carrying out the above-described method for continuous ammonia decomposition and carbon monoxide production. [5] A system for carrying out the method according to [1] above, Metal / metal oxide materials, a first reactor having a first metal / metal oxide material inlet, a first metal / metal oxide material outlet, a gas inlet for supplying NH3 gas, and a gas outlet for withdrawing a gaseous product comprising H2O and N2 gas; and a second reactor having a second metal / metal oxide material inlet, a second metal / metal oxide material outlet, a gas inlet for supplying the oxidized gas, and a gas outlet for withdrawing gaseous products including the reduced gas; The oxidized gas is CO2 gas or a mixture of CO2 gas and H2O gas, and the reduced gas is CO gas or a mixture of CO gas and H2 gas, a metal / metal oxide material is disposed within the first reactor and the second reactor; a first metal / metal oxide material outlet of the first reactor is connected to a second metal / metal oxide material inlet of the second reactor, and a second metal / metal oxide material outlet of the second reactor is connected to a first metal / metal oxide material inlet of the first reactor, thereby forming a circuit allowing circulation of the metal / metal oxide material between the first and second reactors; a gas inlet for supplying NH3 gas and a gas outlet for withdrawing gaseous products including HO and N2 gas are provided at a position that allows gas to flow in a direction opposite to the direction of movement of the metal / metal oxide material in the first reactor; A system comprising a gas inlet for supplying an oxidized gas and a gas outlet for withdrawing gaseous products including a reduced gas, the gas inlet and the gas outlet being positioned to allow gas flow in a direction opposite to the direction of movement of the metal / metal oxide material within the second reactor. [6] The system of [5] above, wherein each of the first reactor and the second reactor is a moving bed reactor, and the metal / metal oxide material is a moving bed in the moving bed reactor. [7] The system described in [5] above, wherein the metal / metal oxide material is an iron oxide material. [8] The method according to the above [7], wherein the reaction temperatures in both the first and second reactors are 700°C to 750°C. Effect of the Invention
[0009] The present invention provides a method and system for integrating NH decomposition into the RWGS reaction, which allows for continuous production of H gas from NH and CO gas from CO using a single system, providing further process intensification. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic diagram illustrating an exemplary system for continuous ammonia decomposition and carbon monoxide production. [Diagram 2] 1 is a graph showing the residual NH3 concentration in the cracked gas as a function of temperature and product gas oxidation at thermodynamic equilibrium. [Diagram 3] FIG. 2 is a design diagram of a process of the present invention carried out at a temperature of 750° C. using an Fe—O compound as the metal / metal oxide material. [Figure 4] 1 is a graph showing the reduction kinetics of granular Fe / MgAl2O4 with 6.95% NH3 in He. [Diagram 5] Arrhenius plot for the reduction kinetics of Fe / MgAl2O4 with 6.95% NH3 in He. [Figure 6]1 is a graph showing the dependence of NH3 decomposition on the degree of reduction X of Fe / MgAl2O4 with 6.95% NH3 in He. [Figure 7] Figure 11 is an Arrhenius plot of the decomposition kinetics for Fe / MgAl2O4 with 6.95% NH3 in He. [Figure 8] 1 is a graph showing weight change due to nitride formation as a function of temperature for powdered Fe / MgAl2O4 samples with 6.95% NH3 in He. [Figure 9] 1 is a graph showing the oxidation kinetics of powdered Fe / MgAl2O4 with 5% CO2 in He. [Figure 10] 13 is an Arrhenius plot of the oxidation kinetics of Fe / MgAl2O4 with 5% CO2 in He. [Figure 11] 1 is a graph showing the cycle stability of Fe / MgAl2O4 at a temperature of 720° C. in the presence of 5% CO2 in He for the oxidation step and 6.95% NH3 for the reduction step. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The embodiments of the present invention will now be described in detail with reference to the accompanying drawings.
[0012] 1. A method for continuously decomposing ammonia and producing carbon monoxide A first embodiment of the present invention is a method for continuously decomposing ammonia and producing carbon monoxide, comprising the steps of: 1) moving the metal / metal oxide material in a direction opposite to the flow of the NH3 gas in a first reactor, thereby contacting the continuous flow of NH3 gas with the oxidized metal / metal oxide material to convert the metal / metal oxide material to a reduced state while producing HO gas and N2 gas; 2) continuously transferring the reduced metal / metal oxide material to a second reactor while continuously withdrawing gaseous products including HO gas and N gas from the first reactor; 3) contacting the continuous flow of oxidized gas with the reduced metal / metal oxide material in a second reactor by moving the metal / metal oxide material in a direction opposite to the flow direction of the oxidized gas to convert the metal / metal oxide material back to its oxidized state while producing a reduced gas, the oxidized gas being CO2 gas or a mixture of CO2 gas and HO gas, and the reduced gas being CO gas or a mixture of CO gas and H2 gas; 4) continuously transferring oxidized metal / metal oxide material to the first reactor while continuously withdrawing gaseous products, including reduced gas, from the second reactor; 5) continuously repeating steps 1) to 4).
[0013] In step 1) of the method of the present invention, the decomposition of NH3 and the reduction of metal / metal oxide materials are carried out by contacting a continuous flow of NH3 gas with the metal / metal oxide materials in a first reactor. Here, the feed NH3 gas is fed to the reactor in a direction opposite to the direction of movement of the metal / metal oxide materials (solids). In other words, the gas (NH3 gas) is fed in a countercurrent direction to the solid flow (metal / metal oxide materials), resulting in a solid-gas counterflow. Such a solid-gas counterflow of the feed NH3 gas results in a higher gas and solid conversion rate at the reactor outlet.
[0014] In the first reactor, NH3 is decomposed into N2 and H2 according to the following reaction (A1): In the absence of oxygen, the gas conversion rate by this reaction is limited by thermodynamic equilibrium. In the first reactor, H2 produced from NH3 is oxidized to H2O by lattice oxygen released from the metal / metal oxide material in the first reactor according to the following reaction (A2): NH3 → 0.5N2 + 1.5H2 (A1) 1.5H2+1.5MeO→1.5Me+1.5H2O (A2) (In the above reactions, "Me" refers to the reduced form of the metal / metal oxide material and "MeO" refers to the oxidized form of the metal / metal oxide material).
[0015] Reaction (A2) improves the conversion of NH3 by reaction (A1). In FIG. 2, the conversion of NH3 at thermodynamic equilibrium (at 1 bar) is shown as a function of the degree of oxidation of the gas. FIG. 2 shows the residual NH3 concentration in the cracked gas as a function of temperature and oxidation of the product gas at thermodynamic equilibrium when 100% NH3 is fed to the reactor. FIG. 2 shows that at the high gas oxidation degree and high temperature required for the present invention, the residual NH3 concentration can be expected to be much less than 100 ppm. As a result, the gas conversion in the first and second reactors will be determined by the thermodynamics of the redox reaction with H2 as the reducing agent and CO2 and / or H2O as the oxidizing agent. The conversion of gases and solids in this system can then be determined by design diagrams such as those shown for Fe-O compounds in FIG. 3.
[0016] The reaction conditions for the oxidation of NH3 gas (and reduction of metal / metal oxide materials) may vary depending on the metal / metal oxide materials and reactors used, production rate, etc., but are generally the same as the reaction conditions for conventional NH3 decomposition reactions. For example, the temperature of step 1) ranges from 450°C to 1000°C, preferably from 600°C to 900°C, and more preferably from 700°C to 800°C. As explained in detail in the Examples section below, high temperatures are preferred to reduce the amount of unreacted NH3 in the gaseous product and to further prevent the formation of nitrides due to reaction between N2 and metal / metal oxide materials.
[0017] In step 2) of the method of the present invention, the reduced metal / metal oxide material is continuously transferred to the second reactor while the gaseous product containing H2O and N2 is continuously withdrawn from the first reactor. The gaseous product withdrawn from the first reactor may contain a small amount of unreacted NH3.
[0018] In step 3) of the method of the present invention, the reduction of the oxidized gas and the oxidation of the reduced metal / metal oxide material are carried out in the second reactor by contacting a continuous flow of the oxidized gas with the metal / metal oxide material. The oxidized gas is either CO2 gas or a mixture of CO2 gas and H2O gas. The CO2 gas fed to the second reactor is converted to CO gas according to the following reaction (B1), and the H2O fed to the second reactor is converted to H2 gas according to the following reaction (B2). CO2 →CO+[O] (B1). HO → H2 + [O] (B2). In this step, oxygen from CO2 and / or H2O is used to convert the metal / metal oxide material back to an oxidized state. The metal / metal oxide material oxidized in the second reactor is now capable of decomposing NH3 in the first reactor.
[0019] In this process, the feed CO2 and / or HO gas is fed to the reactor in a direction opposite to the direction of movement of the metal / metal oxide material (solids). In other words, the gas (CO2 / HO) is fed in a countercurrent direction to the solid flow (metal / metal oxide material), resulting in a solid-gas counterflow. Such a solid-gas counterflow of feed CO2 / HO results in higher gas and solid conversion at the respective reactor outlets.
[0020] The oxidized gas fed to the second reactor is either CO2 gas or a mixture of CO2 gas and H2O gas. Using CO2 gas alone as the oxidized gas results in the production of a reduced gas that is CO gas.
[0021] Using a mixture of CO2 and HO gases as the oxidized gas results in the production of a mixture of CO and H2 gases as the reduced gases, i.e., synthesis gas. For example, if HO and CO2 are used in a 2:1 molar ratio, the resulting gas will contain H2 and CO in approximately a 2:1 ratio, which is useful for downstream synthesis of methanol.
[0022] Alternatively, the oxidized gas fed to the second reactor can be H2O alone. When only H2O is fed to the second reactor, the net reaction is the decomposition of NH3. Nevertheless, this method has an advantage over the conventional decomposition of NH3 because a gaseous product containing H2 gas is obtained separately from N2 gas.
[0023] The reaction conditions for the reduction of CO2 / H2O (and oxidation of metal / metal oxide materials) may vary depending on the metal / metal oxide materials and reactors used, production rates, etc., but are generally the same as the reaction conditions for converting CO2 to CO in conventional chemical looping processes for RWGS. Chemical looping processes for RWGS are techniques in which the RWGS reaction is carried out in two separate half-reactions, namely the conversion of H2 to H2O and the conversion of CO2 to CO, with oxygen being transported between the two half-reactions as lattice oxygen of the metal or metal oxide material. For example, the temperature of step 3) is in the range of 450°C to 1000°C, preferably 600°C to 900°C, more preferably 700°C to 800°C. Furthermore, the reaction conditions of step 3) may be the same or different from the reaction conditions of step 1).
[0024] In step 4) of the method of the present invention, the oxidized metal / metal oxide material is continuously transferred to the first reactor while a gaseous product comprising reduced gas is continuously withdrawn from the second reactor. The gaseous product withdrawn from the second reactor may contain unreacted CO2 and / or HO along with the produced CO and / or H2.
[0025] In step 5), steps 1) to 4) are repeated continuously. There is no particular limitation on the number of times steps 1) to 4) are repeated. Steps 1) to 4) can be repeated until a desired amount of product is obtained or until the metal / metal oxide material is inactivated.
[0026] As is evident from steps 1)-4) above, the metal / metal oxide material is circulated between the first and second reactors while being converted from an oxidized to a reduced state and vice versa. Such circulation of the metal / metal oxide material allows the metal / metal oxide material to be used for an extended period of time without inactivation and provides sufficient oxygen to the reaction system. Furthermore, the method of the present invention increases the gas production yield by improving the equilibrium conversion and producing a continuous flow of gaseous products.
[0027] The reactor used in the present invention can be a moving bed reactor capable of realizing countercurrent solid-gas flow, or a multi-stage fluidized bed reactor capable of achieving near countercurrent solid-gas flow. The reactor used in step 1) and the reactor used in step 3) can be the same or different, although the use of two moving bed reactors is preferred to generate a continuous flow of product gas. The reactors used to carry out the process of the present invention are described in more detail below in connection with the system of the present invention.
[0028] The metal / metal oxide material used in the method of the present invention is any metal- or metal oxide-containing material (or the metal or metal oxide itself) that can be used as a catalyst for the decomposition of NH3.
[0029] Metal / metal oxide materials for use in the method of the invention may be selected using design diagrams. As an example, FIG. 3 shows a design diagram for an Fe-O compound at a temperature of 750° C. Similar design diagrams can be generated for different candidate metal / metal oxide materials and used to select metal / metal oxide materials for use in the method of the invention. Details regarding the use of design diagrams are described in more detail in connection with the system of the invention.
[0030] The metal / metal oxide material may be a metal or metal oxide combined with a support material. The support material is used to prevent sintering and gradual loss of activity during use of the metal / metal oxide material. For example, in the examples below, Fe is combined with MgAl2O4 as the support material.
[0031] The inventors conducted experiments using Fe / MgAl2O4 as a metal / metal oxide material, and verified the reduction kinetics (Figures 4 and 5), decomposition kinetics (Figures 6 and 7), nitride formation (Figure 8), CO generation (Figures 9 and 10), and cycle stability (Figure 11) of Fe / MgAl2O4. As a result of the verification, it was found that the method using this material can achieve high gas conversion in both the first reactor (i.e., decomposition of NH3 and oxidation of H2) and the second reactor (i.e., production of CO by RWGS) while achieving the production of N2-free gas without permanent gas separation.
[0032] Furthermore, the inventors have found that the prevention of nitride formation in step 1) is important to achieve good performance of the method. In step 1) of the method of the present invention, N2 is generated by decomposition of NH3, and the generated N2 can react with metal / metal oxide materials in the reactor to form nitrides. Such nitrides are detrimental to the performance of the process because they can carry atomic nitrogen from the first reactor to the second reactor, which can contaminate the gaseous product obtained from the second reactor.
[0033] In the present invention, the formation of nitrides was observed using the weight loss of the metal / metal oxide material. Specifically, when the reduction of the material in NH3 is completed, the reaction gas is switched from the NH3 / He mixture to He only, and the nitrides that may have formed during exposure to NH3 naturally decompose, resulting in a weight loss. This weight loss as a function of temperature thus represents the amount of nitrides formed during the reaction.
[0034] If the metal / metal oxide material is Fe, the iron nitride is Fe x N can be formed in the first reactor and transported to the second reactor. As shown in Figure 8, at about 540°C, almost all of the iron in the material is in the form of Fe2N, while at temperatures above 700°C, the formation of undesirable nitrides is suppressed to a large extent. Therefore, in the present invention, when the metal / metal oxide material is an iron oxide material, the reaction temperature is preferably in the range of 700°C to 750°C, with 750°C being most preferred.
[0035] 2. System for Continuous Reverse Water-Gas Shift Reaction A second embodiment of the present invention is a system for carrying out the method of the present invention for continuously performing ammonia decomposition and carbon monoxide production. The system comprises: Metal / metal oxide materials, a first reactor having a first metal / metal oxide material inlet, a first metal / metal oxide material outlet, a gas inlet for supplying NH3 gas, and a gas outlet for withdrawing gaseous products comprising HO gas and N2 gas; and a second reactor having a second metal / metal oxide material inlet, a second metal / metal oxide material outlet, a gas inlet for supplying the oxidized gas, and a gas outlet for withdrawing gaseous products including the reduced gas; The oxidized gas is CO2 gas or a mixture of CO2 gas and H2O gas, and the reduced gas is CO gas or a mixture of CO gas and H2 gas, a metal / metal oxide material is disposed within the first reactor and the second reactor; a first metal / metal oxide material outlet of the first reactor is connected to a second metal / metal oxide material inlet of the second reactor, and a second metal / metal oxide material outlet of the second reactor is connected to a first metal / metal oxide material inlet of the first reactor, thereby forming a circuit allowing circulation of the metal / metal oxide material between the first and second reactors; a gas inlet for supplying NH3 gas and a gas outlet for withdrawing gaseous products including HO and N2 gas are provided at a position that allows gas to flow in a direction opposite to the direction in which the metal / metal oxide material moves in the first reactor; The system includes a gas inlet for supplying the oxidized gas and a gas outlet for withdrawing gaseous products including the reduced gas, located in a position that allows gas to flow in a direction opposite to the direction of movement of the metal / metal oxide material within the second reactor.
[0036] The system of the present invention will now be described with reference to FIG. 1, which is a schematic diagram of a representative system for continuously carrying out the decomposition of ammonia and the production of carbon monoxide.
[0037] The system of the present invention includes a first reactor 10 for the decomposition of NH3 (and reduction of metal / metal oxide materials) and a second reactor 20 for the production of CO (and also oxidation of metal / metal oxide materials). Any gas-solid reactor that achieves or approximates a countercurrent solid-gas flow can be used in the system of the present invention. For example, the reactor can be a moving bed reactor capable of achieving a countercurrent solid-gas flow, or a staged fluidized bed reactor capable of achieving an approximate countercurrent flow. The first reactor 10 and the second reactor 20 can be the same or different, but the use of two moving bed reactors is preferred to produce a continuous flow of product gas.
[0038] The first reactor 10 has a first metal / metal oxide material inlet 11, a first metal / metal oxide material outlet 12, a gas inlet 13 for supplying NH3 gas, and a gas outlet 14 for withdrawing gaseous products including H2O and N2 gas. The metal / metal oxide material 30 forms a moving bed in the reactor. To achieve a solid-gas countercurrent state or a state close to it in the reactor, the flow direction of the feed gas is opposite to the moving direction of the moving bed. Thus, in a typical system, the gas inlet 13 is installed near the metal / metal oxide material outlet 12, and the gas outlet 14 is installed near the metal / metal oxide material inlet 11. The gas inlet 13 is connected to an ammonia gas source for supplying NH3 gas to the reactor. The gas outlet 14 can be connected to a storage vessel for storing the gaseous products containing N2 gas, H2O gas, and unreacted NH3 gas. Alternatively, the gaseous products can be supplied to an apparatus for separating N2, H2O, and NH3. The separated NH3 gas can be returned to the ammonia gas source and then fed to the first reactor 10 through the gas inlet 13.
[0039] The second reactor 20 has a second metal / metal oxide material inlet 21, a second metal / metal oxide material outlet 22, a gas inlet 23 for feeding the oxidized gas, and a gas outlet 24 for withdrawing the gaseous product containing the reduced gas. The metal / metal oxide material 30 forms a moving bed in the reactor. The flow direction of the feed gas is opposite to the moving direction of the moving bed to achieve a countercurrent solid-gas flow condition or a condition close to the countercurrent solid-gas flow condition in the reactor. Thus, in a typical system, the gas inlet 23 is installed near the metal / metal oxide material outlet 22, and the gas outlet 24 is installed near the metal / metal oxide material inlet 21.
[0040] In the present invention, the oxidized gas fed to the second reactor is either CO2 gas or a mixture of CO2 gas and H2O gas. Using CO2 gas alone as the oxidized gas produces CO gas as the reduced gas, and using a mixture of CO2 gas and H2O gas as the oxidized gas produces a mixture of CO gas and H2 gas, i.e., synthesis gas, as the reduced gas. Alternatively, the oxidized gas fed to the second reactor can be H2O alone. When only H2O is fed to the second reactor, the net reaction is the decomposition of NH3. Nevertheless, this method has an advantage over the conventional decomposition of NH3, since a gaseous product containing H2 gas is obtained separately from N2 gas.
[0041] The gas inlet 23 is connected to a gas source for supplying CO2 and / or H2O to the reactor, and the gas supplied to the second reactor 20 contains CO2 and / or H2O. The gas outlet 24 may be connected to a storage vessel for storing the gaseous product containing CO and / or H2 and unreacted CO2 and / or H2O. Alternatively, the gaseous product may be supplied to a device for separating unreacted CO2 and / or H2O, and the separated CO2 gas may be returned to the source of oxidized gas and then supplied to the second reactor 20 via the gas inlet 23.
[0042] The first reactor 10 and the second reactor 20 are connected to each other to form a circuit. Specifically, the first metal / metal oxide material outlet 12 of the first reactor 10 is connected to the second metal / metal oxide material inlet 21 of the second reactor 20, and the second metal / metal oxide material outlet 22 of the second reactor 20 is connected to the first metal / metal oxide material inlet 11 of the first reactor 10, and the metal / metal oxide material 30 in the reactor, i.e. the moving bed, is circulated between the two reactors.
[0043] The metal / metal oxide material used in the process of the present invention is any metal- or metal oxide-containing material (or the metal or metal oxide itself) that can be used as a catalyst in the decomposition of NH3.
[0044] Metal / metal oxide materials for use in the process of the present invention can be selected using a design diagram, taking into account the equipment of the reaction system. As an example, FIG. 3 shows a design diagram for an Fe-O compound at a temperature of 750° C. In FIG. 3, the “reducer” is the first reactor of the present invention, and the “oxidizer” is the second reactor of the present invention. FIG. 3 shows that the reaction system used in the process of the present invention is subject to the following limitations: 1) As solids (metal / metal oxide materials) are fed from the first reactor to the second reactor, the solids conversion at the bottom of the first reactor needs to be the same as the solids conversion at the top of the second reactor. 2) Conversely, the solids conversion at the top of the second reactor must be the same as the solids conversion at the bottom of the first reactor. 3) At no time during operation of the system should the operating line extend into a thermodynamically unpermissible region. 4) The slopes of the run lines in the first and second reactors can be selected independently since the corresponding solid-gas flow ratios are adjustable.
[0045] What operating line is considered optimal depends on the process requirements. The optimization can be for the gas conversion and also for the solids conversion in either the first or second reactor or both. Higher solids conversion reduces the amount of solids that must be circulated between the reactors. The desired operating line can be determined graphically, by a series of empirical rules or by rigorous numerical optimization. The operating line shown here was obtained by optimizing the gas conversion in both reactors.
[0046] The metal / metal oxide material may be a metal or metal oxide combined with a support material. The support material is used to prevent sintering and gradual loss of activity during use of the metal / metal oxide material. For example, in the following examples, Fe is combined with MgAl2O4 as the support material.
[0047] Through experiments using Fe / MgAl2O4 as the metal / metal oxide material, the inventors found that the system of the present invention using this material is capable of achieving high gas conversion in both the first reactor (i.e., decomposition of NH3) and the second reactor (i.e., production of CO by RWGS), and production of N2-free gas without permanent gas separation. Furthermore, the inventors determined the reaction conditions suitable for preventing nitride formation in the first reactor by measuring the weight loss of the metal / metal oxide material (FIG. 8). Thus, in the present invention, when the metal / metal oxide material is an iron oxide material, the reaction temperature is preferably in the range of 700°C to 750°C, and most preferably 750°C.
[0048] The present invention will now be described in detail with reference to examples, but the following examples should not be construed as limiting the present invention. EXAMPLES
[0049] Example 1 Decomposition of ammonia and production of carbon monoxide using Fe-O compounds as metal / metal oxide materials
[0050] (1) Preparation of metal / metal oxide materials Fe-O compounds were prepared for use as metal / metal oxide materials.
[0051] Granular Fe / MgAl2O4 was produced from fine powders of Fe2O3 (50 wt%, Sigma-Aldrich, USA) and MgAl2O4 (50 wt%, Baikowski, France). First, the powders were thoroughly mixed in an Eirich EL1 high shear mixer. Then, deionized water was gradually added to the mixture as a binder to build the granular material. To impart mechanical stability to the resulting granular material, it was dried and calcined at 1250 °C for 3 h. Finally, the calcined granules were sieved to a size range of 250-500 μm. To eliminate the effect of initial passivation due to sintering of the material during the redox cycles, three cycles of complete reduction in H2 followed by complete oxidation in CO2 were performed. The resulting material was then used for the experiments either as is (referred to as "granular") or after fine grinding in a pestle and mortar (referred to as "powdered") with NH3.
[0052] The experiments were carried out in a setup for coupled thermogravimetry / quadrupole mass spectrometry (TG / QMS method) in order to simultaneously determine the NH3 decomposition kinetics from the QMS signal and the redox kinetics from the TG signal. A differential balance (STA2500, Netzsch, Germany) was used to minimize the effects of gas switching and buoyancy on the TG signal. Quantitative QMS data were obtained by careful calibration of the QMS (403 Aeolos Quadro, Netzsch, Germany) with pure gases. The crucible was filled to the brim with inert ZrO2 spheres, the sample was placed on top and a high flow rate (400 ml N / min) and a small sample size of approximately 8 mg to minimize the effects of mass transport limitations on the kinetic measurements.
[0053] (2) Reduction kinetics The reduction of Fe3O4 to Fe can proceed directly or indirectly. The direct route gives H2O and N2 as gaseous products (Equation (1)). NH3+0.375Fe3O4→0.5N2+1.5H2O+1.125Fe (1)
[0054] This reduction of Fe3O4 can also occur indirectly, where gaseous H2 is first produced by decomposition of NH3, and then the H2 is oxidized by the lattice oxygen of the solid iron oxide. No pathway can be discerned from the experiments performed in this study. The reduction rate can be well described by a first-order reaction model. Figure 4 shows the reduction kinetics of granular Fe / MgAl2O4 with 6.95% NH3 in He, the solid line shows the model result obtained from Eq. (2) below.
[0055] The rate equation for the reduction reaction with NH3 is given by the factor X, which represents the dependence on the solid conversion or degree of reduction, the reactant concentration C NH3 and the reaction temperature T. X=0 indicates the fully oxidized state before the sample is reduced by NH3, and X=1 indicates the reduced state after the sample is exposed to NH3.
[0056] In the first order reaction model, we obtain:
number
[0057] The Arrhenius plot for the reduction kinetics of Fe / MgAl2O4 with 6.95% NH3 in He is shown in Figure 5. Figure 5 shows the temperature dependence with a clear mechanism change observable at about 560-600 °C. At lower temperatures, high activation energies of about 91 kJ mol-1 and 82 kJ mol-1 were observed for the granular and powdered materials, respectively, indicating kinetic control. At higher temperatures, very low activation energies of about 13 kJ mol-1 and 6 kJ mol-1 were observed for the granular and powdered materials, respectively. The complete kinetic parameters are provided by Figure 5.
[0058] The reaction order n was determined from concentration change experiments with granular material at T = 520°C and T = 680°C, yielding n = 0.44 for the lower temperature range and n = 0.77 for the higher temperature range.
[0059] (3) Decomposition kinetics Similar to the reduction kinetics, the rate equation for the NH3 decomposition reaction can be formulated as shown in equation (3) below.
number
[0060] The decomposition rate depends on the degree of reduction X of the material, since metallic iron is the active phase for NH3 decomposition. From simultaneous TG-QMS measurements, a good first approximation is the linear dependence of the decomposition rate on the degree of reduction X. This is shown in Figure 6, which shows the dependence of the NH3 decomposition rate on the degree of reduction X of Fe / MgAl2O4 with 6.95% NH3 in He. X is determined from the weight change by gravimetry and the decomposition rate obtained from simultaneous QMS measurements.
[0061] Reaction rate constant k crack,0 was determined from the last 10 min of NH3 exposure (X ≈ 1), when reduction was complete. The Arrhenius plot for the decomposition kinetics for Fe / MgAl2O4 with 6.95% NH3 in He is shown in Figure 7.
[0062] In Figure 7, a clear change in mechanism can be observed at about 520-560 °C. At lower temperatures, higher activation energies of about 91 kJ mol-1 and 125 kJ mol-1 are observed for granular and powdered materials, respectively, indicating kinetic control. At higher temperatures, lower activation energies of about 27 kJ mol-1 are observed. The complete kinetic parameters are provided in Figure 7.
[0063] The reaction order n was determined from concentration change experiments with granular material at T = 520°C and T = 680°C, giving n = 0.43 for the lower temperature range and n = 0.89 for the higher temperature range.
[0064] (4) Nitride formation Iron nitride, Fe x If N is formed, it is detrimental to process performance because it can carry atomic nitrogen from the first reactor (the "reducer") to the second reactor (the "oxidizer") and contaminate the desired nitrogen-free product gas.
[0065] After completion of the reduction of the metal / metal oxide material in NH3, when the reaction gas is switched from the NH3 / He mixture to He only, the nitrides that may have formed during exposure to NH3 spontaneously decompose, resulting in weight loss. Figure 8 shows the weight change due to nitride formation as a function of temperature for a powdered Fe / MgAl2O4 sample with 6.95% NH3 in He. At about 540°C, almost all the iron in the material is in the form of Fe2N. This was confirmed from the XRD patterns of the samples obtained by exposure to NH3 / He followed by quenching in NH3 / He to prevent spontaneous decomposition of the nitrides.
[0066] To avoid this undesirable nitride formation, the process should be operated at a temperature above 700°C, preferably about 750°C.
[0067] (5) CO generation For the production of CO from CO2 by oxidation of iron, a rate equation can be formulated similar to that for the reduction reaction (equation (4)).
number
[0068] Similar to the reduction kinetics, the oxidation kinetics can be well described by a first-order kinetic model. Figure 9 shows the oxidation kinetics of powdered Fe / MgAl2O4 with 5% CO2 in He. The solid line shows the model results obtained from equation (4) above.
[0069] The corresponding Arrhenius plot is shown in Figure 10. The apparent activation energy of the powder sample was 55.8 kJ mol-1. On the other hand, the apparent activation energy of the granular material was 32.5 kJ mol-1, significantly lower than that of the powder sample. This indicates the existence of some degree of intra-particle mass transfer resistance, which needs to be taken into account in process and material design.
[0070] (6) Cycling stability Fifteen cycling experiments consisting of decomposition and reduction in NH3, followed by oxidation in CO2 were performed to determine the cycling stability of the material. The experiments used Fe / MgAl2O4, with the oxidation step performed with 5% CO2 in He and the reduction step with 6.95% NH3, both at a temperature of 720 °C. The relative rates for the 15 cycles are shown in Figure 10. No discernible activation trend was observed from Figure 10, thus indicating that the reaction was stable.
[0071] (7) Summary of results It was found that the production of N2-free gas without permanent gas separation was feasible, and the suitable operating temperature of Fe / MgAl2O4 was in the range of about 700°C to 750°C. In this temperature range, high gas conversion was achieved and the deleterious formation of iron nitrides was prevented.
[0072] Example 2 Use of a mixture of H2O and CO2 gases in the second reactor The decomposition of ammonia and the production of carbon monoxide were carried out in substantially the same manner as in Example 1, except that a mixture of H2O and CO2 in a molar ratio of 2:1 was used as the oxidized gas instead of CO2 gas.
[0073] When a mixture of H2O gas and CO2 gas was used as the oxidized gas, the reduced gas produced in the second reactor was a mixture of H2 gas and CO gas. Since the molar ratio of H2O gas to CO2 gas in the oxidized gas was 2:1, the molar ratio of H2 and CO in the reduced gas was about 2:1. The reduced gas thus produced was useful for the downstream synthesis of methanol. [Industrial Applicability]
[0074] The present invention provides a method and system for integrating the NH decomposition process with the RWGS reaction, allowing for the continuous production of H gas from NH and CO gas from CO using a single system, providing further process intensification. [Explanation of symbols]
[0075] 10 First Reactor 11 First metal / metal oxide material inlet 12 First metal / metal oxide material outlet 13 Gas inlet 14 Gas outlet 20 Second Reactor 21 Second metal / metal oxide material entrance 22 Second metal / metal oxide material outlet 23 Gas inlet 24 Gas outlet 30 Metal / Metal Oxide Materials
Claims
1. 1. A process for continuously carrying out ammonia decomposition and carbon monoxide production, comprising: 1) In a first reactor, NH 3 The NH 3 A continuous flow of gas is contacted with the metal / metal oxide material in an oxidized state to convert the metal / metal oxide material to a reduced state while H 2 O gas and N 2 Generates gas, 2) from the first reactor, 2 O gas and N 2 continuously transferring the reduced metal / metal oxide material to a second reactor while continuously withdrawing gaseous products including a gas; 3) contacting the continuous flow of oxidized gas with the metal / metal oxide material in a reduced state in the second reactor by moving the metal / metal oxide material in a direction opposite to the flow direction of the oxidized gas to convert the metal / metal oxide material back to an oxidized state while producing a reduced gas, the oxidized gas producing CO 2 Gas or CO 2 Gas and H 2 and the reduced gas is a mixture of CO gas or CO gas and H 2 It is a mixture with gas, 4) continuously transferring the oxidized metal / metal oxide material to the first reactor while continuously withdrawing gaseous products from the second reactor, the gaseous products including the reduced gas; 5) Steps 1) to 4) are repeated continuously; The method includes:
2. 10. The method of claim 1, wherein each of said first reactor and said second reactor is a moving bed reactor, and said metal / metal oxide material is a moving bed in said moving bed reactor.
3. The method of claim 1 , wherein the metal / metal oxide material is an iron oxide material.
4. The method of claim 3, wherein the reaction temperatures of the first and second reactors are both between 700°C and 750°C.
5. A system for carrying out the method of claim 1, comprising: Metal / metal oxide materials, a first metal / metal oxide material inlet; a first metal / metal oxide material outlet; and a NH 3 a gas inlet for supplying gas; 2 O and N 2 a gas outlet for withdrawing a gaseous product comprising a gas; and a second reactor having a second metal / metal oxide material inlet, a second metal / metal oxide material outlet, a gas inlet for supplying the oxidized gas, and a gas outlet for withdrawing gaseous products including the reduced gas; Including, The oxidized gas is CO 2 Gas or CO 2 Gas and H 2 and the reduced gas is a mixture of CO gas or CO gas and H 2 It is a mixture with gas, the metal / metal oxide material is disposed within the first reactor and the second reactor; the first metal / metal oxide material outlet of the first reactor is connected to the second metal / metal oxide material inlet of the second reactor, and the second metal / metal oxide material outlet of the second reactor is connected to the first metal / metal oxide material inlet of the first reactor, thereby forming a circuit allowing circulation of the metal / metal oxide material between the first and second reactors; NH 3 The gas inlet for supplying gas and H 2 O and N 2 a gas outlet for withdrawing the gaseous products including a gas; the gas inlet for supplying the oxidized gas and the gas outlet for withdrawing the gaseous products including the reduced gas are located in a position that allows gas to flow in a direction opposite to a direction of movement of the metal / metal oxide material within the second reactor.
6. 6. The system of claim 5, wherein each of said first reactor and said second reactor is a moving bed reactor, and said metal / metal oxide material is a moving bed in said moving bed reactor.
7. The system of claim 5 , wherein the metal / metal oxide material is an iron oxide material.
8. The method of claim 7, wherein the reaction temperatures of the first and second reactors are both between 700°C and 750°C.
Citation Information
Patent Citations
Production of carbon monoxide
JP1994279012A
Production of carbon monoxide
JP1996245211A
Catalyst for producing carbon monoxide, manufacturing method of the same, and production method of carbon monoxide using the same
JP2021045726A
Chemical looping systems for conversion of low- and no-carbon fuels to hydrogen
US20190119107A1
Chemical looping systems for conversion of low- and no-carbon fuels to hydrogen
WO2017205638A1
Cited By
Method and apparatus for producing hydrogen from an ammonia feedstock
GB2703723A
Oxygen-deficient perovskite-type metal oxide, and oxygen storage material, oxygen adsorption / desorption device, oxygen concentrator, oxygen adsorption / desorption method, oxygen concentrator, and chemical reaction execution method using the same.
JP2026180570A
Method and apparatus for producing hydrogen from an ammonia feedstock
WO2026099584A1