Positive electrode active material particle, method for manufacturing positive electrode active material particle, and lithium ion battery

Spherical Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O 2 particles, produced through ion exchange, enhance the rate characteristics and capacity of lithium ion batteries by reducing reaction and diffusion resistance.

JP2024132511AActive Publication Date: 2024-10-01TOYOTA JIDOSHA KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023043303
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-10-01
Estimated Expiration
2043-03-17

AI Technical Summary

Technical Problem

Positive electrode active materials with an O2 type structure in lithium ion batteries have room for improvement in rate characteristics and capacity.

Method used

The development of positive electrode active material particles with an O2 type structure, composed of Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O 2, where 1.0

Benefits of technology

The resulting particles exhibit excellent rate characteristics and capacity due to reduced reaction resistance and diffusion resistance, with improved lithium ion conduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132511000001_ABST
    Figure 2024132511000001_ABST
Patent Text Reader

Abstract

To disclose a positive electrode active material particle having the O2-type structure, and having excellent rate characteristics and capacity.SOLUTION: A positive electrode active material particle of the present disclosure has the O2-type structure, has a spherical shape and has a chemical composition represented by LiaNabMnx-pNiy-qCoz-rMp+q+rO2 (wherein 1.0<a<1.30, 0≤b≤0.20, x+y+z=1, and 0≤p+q+r≤0.15, and M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application discloses positive electrode active material particles, a method for producing positive electrode active material particles, and a method for producing a lithium ion battery. [Background technology]

[0002] A positive electrode active material having an O2 type structure is known for a lithium ion battery. As disclosed in Patent Document 1, a positive electrode active material having an O2 type structure is obtained by ion-exchanging at least a part of Na in a Na-containing transition metal oxide having a P2 type structure with Li. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-186937 A Summary of the Invention [Problem to be solved by the invention]

[0004] There is room for improvement in the rate characteristics and capacity of the positive electrode active material having the O2 type structure. [Means for solving the problem]

[0005] The present application discloses the following aspects as means for solving the above problems. <Aspect 1> Positive electrode active material particles, It has an O2 structure. Li a Na b Mn x-p Ni y-q Co z-r M p+q+rO2 (where 1.0 < a < 1.30, 0 ≤ b ≤ 0.20, x + y + z = 1, and 0 ≤ p + q + r ≤ 0.15, and M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W), and spherical, cathode active material particles. <Aspect 2> The cathode active material particles of Aspect 1, wherein the particle surface is composed of a plurality of crystallites, cathode active material particles. <Aspect 3> A method for manufacturing cathode active material particles, comprising: obtaining Na-containing transition metal oxide particles having a P2-type structure, and contacting the Na-containing transition metal oxide particles with an ion exchange material to replace at least a part of the Na in the Na-containing transition metal oxide particles with Li to obtain Li-containing transition metal oxide particles having an O2-type structure. The ion exchange material contains lithium hydroxide and a lithium salt. Manufacturing method. <Aspect 4> The manufacturing method of Aspect 3, wherein the Na-containing transition metal oxide particles are spherical, and the Li-containing transition metal oxide particles are spherical. Manufacturing method. <Aspect 5> The manufacturing method of Aspect 3 or 4, wherein the Na-containing transition metal oxide particles are Na c Mn x-p Ni y-q Co z-r M p+q+r O2 (0 < c < 0.70, x + y + z = 1, and 0 ≤ p + q + r ≤ 0.15, and M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W), having a chemical composition represented by Manufacturing method. <Aspect 6> In the production method according to any one of aspects 3 to 5, Obtaining precursor particles; coating the surface of the precursor particles with a Na salt to obtain coated particles; and and calcining the coated particles to obtain the Na-containing transition metal oxide particles. Manufacturing method. <Aspect 7> The method of manufacturing of embodiment 6, and coating 40% or more by area of ​​the surface of the precursor particles with the Na salt to obtain the coated particles. The precursor particles are spherical. Manufacturing method. <Aspect 8> A lithium ion battery having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, The positive electrode active material layer includes the positive electrode active material particles according to embodiment 1 or 2. Lithium-ion battery. Effect of the Invention

[0006] The positive electrode active material particles of the present disclosure have excellent rate characteristics and capacity. [Brief description of the drawings]

[0007] [Figure 1] FIG. 2 is a SEM photograph showing an example of the external shape of a positive electrode active material particle. [Diagram 2] 1 shows an example of a flow of a method for producing positive electrode active material particles. [Diagram 3] 1 shows an example of a flow of a method for producing Na-containing transition metal oxide particles having a P2 type structure. [Figure 4] 1 illustrates a schematic diagram of an example of the configuration of a lithium ion battery. [Diagram 5] 1 shows an example of firing conditions for obtaining Na-containing transition metal oxide particles having a P2 type structure. [Figure 6A] FIG. 2 is a SEM photograph showing the external shape of the positive electrode active material particles according to Example 1. [Figure 6B]It is a SEM photograph showing the external appearance shape of the positive electrode active material particles according to Example 2. [Figure 6C] It is a SEM photograph showing the external appearance shape of the positive electrode active material particles according to Comparative Example 1. [Figure 6D] It is a SEM photograph showing the external appearance shape of the positive electrode active material particles according to Comparative Example 2. [Figure 6E] It is a SEM photograph showing the external appearance shape of the positive electrode active material particles according to Reference Example 1. [Figure 7] It shows the X-ray diffraction pattern of the positive electrode active material particles. [Figure 8A] It shows the first charge-discharge curve of the cell according to Example 1. [Figure 8B] It shows the first charge-discharge curve of the cell according to Example 2. [Figure 8C] It shows the first charge-discharge curve of the cell according to Comparative Example 1. [Figure 8D] It shows the first charge-discharge curve of the cell according to Comparative Example 2. [Figure 8E] It shows the first charge-discharge curve of the cell according to Reference Example 1. [Figure 9] It shows the rate characteristics of each cell.

Mode for Carrying Out the Invention

[0008] 1. Positive Electrode Active Material Particles FIG. 1 shows an example of the external appearance shape of the positive electrode active material particles according to one embodiment. The positive electrode active material particles according to one embodiment have an O2-type structure and contain Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O2 (where 1.0 < a < 1.30, 0 ≦ b ≦ 0.20, x + y + z = 1, and 0 ≦ p + q + r ≦ 0.15, and M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W), and are spherical.

[0009] 1.1 Crystal structure of positive electrode active material particles The positive electrode active material particles according to an embodiment have at least an O2 type structure (belonging to space group P63mc) as a crystal structure. The positive electrode active material particles may have an O2 type structure and a crystal structure other than the O2 type structure. Examples of the crystal structure other than the O2 type structure include a T♯2 type structure (belonging to space group Cmca) formed when Li is deintercalated from the O2 type structure and an O6 type structure (belonging to space group R-3m, with a c-axis length of 2.5 nm or more and 3.5 nm or less, typically 2.9 nm or more and 3.0 nm or less, different from the O3 type structure also belonging to space group R-3m). The positive electrode active material particles may have an O2 type structure as a main phase, or may have a crystal structure other than the O2 type structure as a main phase. The crystal structure of the positive electrode active material particles as a main phase may change depending on the charge / discharge state.

[0010] The positive electrode active material particles according to one embodiment may be a single crystal consisting of one crystallite, or may be a polycrystal having a plurality of crystallites. As shown in FIG. 1, the surface of the positive electrode active material particles may be composed of a plurality of crystallites. When the surface of the positive electrode active material particles has a plurality of crystallites, a grain boundary is present on the surface of the positive electrode active material particles. Here, the grain boundary may be an inlet and an outlet of intercalation. That is, when the positive electrode active material particles have a plurality of crystallites on their surface, the effect of increasing the number of inlets and outlets for intercalation to reduce the reaction resistance, the effect of shortening the distance traveled by lithium ions to reduce the diffusion resistance, the effect of reducing the absolute amount of expansion and contraction during charging and discharging to make it difficult for cracks to occur, and the like can be expected.

[0011] The size of the crystallite constituting the positive electrode active material particle according to one embodiment may be large or small, but the smaller the crystallite size, the more the grain boundaries, and the more likely the above-mentioned advantageous effects are to be exhibited. For example, if the diameter of the crystallite constituting the positive electrode active material particle is less than 1 μm, higher performance is likely to be obtained. The "crystallite" and "diameter of the crystallite" can be obtained by observing the surface of the positive electrode active material particle with a scanning electron microscope (SEM) or a transmission electron microscope (TEM). That is, when the surface of the positive electrode active material particle is observed and a closed region surrounded by grain boundaries is observed, the region is regarded as a "crystallite". The maximum Feret diameter of the crystallite is obtained and regarded as the "diameter of the crystallite". If the particle is made of a single crystal, the particle itself can be said to be a single crystallite, and the maximum Feret diameter of the particle is the "diameter of the crystallite". Alternatively, the diameter of the crystallite can be obtained by EBSD or XRD. For example, the crystallite diameter can be determined from the half-width of the diffraction line in the XRD pattern based on the Scherrer formula. When the crystallite diameter of the positive electrode active material particles is less than 1 μm as determined by any of the methods, the positive electrode active material particles are likely to exhibit higher performance.

[0012] The crystallites of the positive electrode active material particles according to one embodiment may have a first surface exposed on the particle surface, and the first surface may be planar. The surface of the positive electrode active material particles may have a structure in which a plurality of planes are connected. When producing the positive electrode active material particles, the crystallites are allowed to grow on the surface of the particles until one crystallite and another crystallite are connected to each other, whereby it is easy to obtain crystallites having a planar first surface.

[0013] 1.2 Chemical composition of positive electrode active material particles The positive electrode active material particles according to one embodiment include Li a Na b Mn x-p Ni y-q Co z-r M p+q+rIt has a chemical composition represented by O2. Here, 1.00 < a < 1.30, 0 ≤ b ≤ 0.20, x + y + z = 1, and 0 ≤ p + q + r ≤ 0.15. Also, M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. Conventionally, the cathode active material particles having an O2-type structure had a Li composition ratio of 1.00 or less (a above is 1.00 or less), and there was room for improvement in terms of capacity. In contrast, the cathode active material particles of the present disclosure have an O2-type structure and a Li composition ratio exceeding 1.00 (a above exceeds 1.00), and have excellent capacity (as described above, both the conventional cathode active material particles and the cathode active material particles of the present disclosure may include other crystal structures together with the O2-type structure). Such cathode active material particles containing an excessive amount of Li can be produced by a new method by the present inventor. The method for producing the cathode active material particles will be described later.

[0014] In the above chemical composition, a may be greater than 1.00, 1.02 or more, 1.04 or more, 1.06 or more, 1.08 or more, 1.10 or more, 1.12 or more, 1.14 or more, or 1.16 or more, and may be 1.30 or less, 1.28 or less, 1.26 or less, 1.24 or less, 1.22 or less, or 1.20 or less. In the above chemical composition, b may be 0 or more, 0.01 or more, 0.02 or more, or 0.03 or more, and may be 0.20 or less, 0.15 or less, or 0.10 or less. In the above chemical composition, x may be 0 or more, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, or 0.60 or less. In the above chemical composition, y may be 0 or more, 0.10 or more, or 0.15 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. In the above chemical composition, z may be 0 or more, 0.10 or more, 0.20 or more, or 0.25 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.35 or less. Many M do not contribute to charge and discharge. In this respect, by having p+q+r be 0.15 or less, a high charge and discharge capacity is easily ensured. p+q+r may be 0.10 or less, 0.05 or less, or 0. The composition of O is approximately 2, but is not necessarily exactly 2.0 and is variable.

[0015] 1.3 Shape of positive electrode active material particles The positive electrode active material particles according to one embodiment are spherical. When spherical positive electrode active material particles are included in the positive electrode active material layer of the lithium ion secondary battery, the growth of the crystallites is easily suppressed and the crystallites are easily made small, compared with the case where non-spherical positive electrode active material particles (e.g., plate-shaped particles) are included. That is, when the positive electrode active material particles are spherical, the reaction resistance is reduced by the reduction in the crystallite size, and the diffusion resistance inside the active material is easily reduced. Furthermore, it is considered that the degree of curvature is reduced by the spheroidization, and the lithium ion conduction resistance in the layer constituting the positive electrode active material layer is reduced. As a result, the spherical positive electrode active material particles are likely to have excellent rate characteristics compared with non-spherical positive electrode active material particles. Such spherical positive electrode active material particles can be manufactured by a new method by the present inventor. The manufacturing method of the positive electrode active material particles will be described later. In addition, "spherical" means that the circularity is 0.80 or more. The circularity of the positive electrode active material particles may be 0.81 or more, 0.82 or more, 0.83 or more, 0.84 or more, 0.85 or more, 0.86 or more, 0.87 or more, 0.88 or more, 0.89 or more, or 0.90 or more. The circularity of the positive electrode active material particles is 4πS / L 2 Here, S is the orthogonal projection area of ​​the particle, and L is the perimeter of the orthogonal projection image of the particle. The circularity of the positive electrode active material particles can be determined by observing the appearance or the above-mentioned cross-sectional shape of the particles with a scanning electron microscope (SEM), a transmission electron microscope (TEM), or an optical microscope.

[0016] The positive electrode active material particles according to an embodiment may be solid particles, hollow particles, or particles having voids. When the positive electrode active material particles are hollow particles or particles having voids, it is considered possible to fill the hollow or voids with liquid. For example, the electrolyte solution is distributed not only on the outer surface of the positive electrode active material particles but also inside, and the contact area between the particles and the electrolyte solution is likely to increase.

[0017] 1.4 Positive electrode active material particle size The size of the positive electrode active material particles according to an embodiment is not particularly limited. For example, the diameter D of the positive electrode active material particles according to an embodiment may be 0.1 μm or more and 10 μm or less, 0.5 μm or more and 8.0 μm or less, or 1.0 μm or more and 6.0 μm or less. The diameter D of the positive electrode active material particles refers to the circle-equivalent diameter when the appearance or cross-sectional shape of the positive electrode active material particles is observed by SEM or the like. When there are multiple positive electrode active material particles, the diameter D of the positive electrode active material particles is the number average value of the circle-equivalent diameter of each of the multiple positive electrode active material particles.

[0018] 2. Method for producing positive electrode active material particles Positive electrode active material particles containing excess Li can be produced, for example, by the following method. As shown in Fig. 2, a method for producing positive electrode active material particles according to one embodiment includes obtaining Na-containing transition metal oxide particles having a P2 type structure (step S1), and contacting the Na-containing transition metal oxide particles with an ion exchange material to replace at least a portion of the Na in the Na-containing transition metal oxide particles with Li, thereby obtaining Li-containing transition metal oxide particles having an O2 type structure (step S2). Here, the ion exchange material contains lithium hydroxide and a lithium salt.

[0019] 2.1 Process S1 In step S1, Na-containing transition metal oxide particles having a P2 type structure are obtained. Here, the shape of the Li-containing transition metal oxide particles having an O2 type structure is determined by the shape of the Na-containing transition metal oxide particles having a P2 type structure. In a manufacturing method according to an embodiment, the Na-containing transition metal oxide particles are spherical, and the Li-containing transition metal oxide particles are spherical. That is, when manufacturing Li-containing transition metal oxide particles having an O2 type structure and being spherical, it is preferable to obtain Na-containing transition metal oxide particles having a P2 type structure and being spherical in step S1.

[0020] The Na-containing transition metal oxide particles having a P2 type structure can be produced, for example, by the method shown in Fig. 3. That is, the production method according to one embodiment includes obtaining precursor particles (step S11), coating the surfaces of the precursor particles with a Na salt to obtain coated particles (step S12), and calcining the coated particles to obtain Na-containing transition metal oxide particles having a P2 type structure (step S13).

[0021] 2.1.1 Process S11 In step S11, precursor particles are obtained. Here, the precursor particles may be a salt containing at least one transition metal element selected from Mn, Ni, and Co. The precursor particles may be, for example, at least one of carbonate, sulfate, nitrate, acetate, and hydroxide. Specifically, the precursor particles may be a salt represented by MeCO3 (Me is at least one transition metal element selected from Mn, Ni, and Co), a salt represented by MeSO4, a salt represented by Me(NO3)2, a salt represented by Me(CH3COO)2, or a compound represented by Me(OH)2. These may be hydrates. In addition to the transition metal element Me, the precursor particles may also contain at least one element M selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W.

[0022] The precursor particles may be spherical. The definition of "spherical" is as described above. When the precursor particles are spherical, the shape of the Na-containing transition metal oxide particles or the Li-containing transition metal oxide particles (positive electrode active material particles) may also be spherical. The size of the spherical precursor particles is not particularly limited. The spherical precursor particles can be obtained by a solution method such as a coprecipitation method or a sol-gel method. Specifically, in the case of the coprecipitation method, an aqueous solution of MeSO4 and an aqueous solution of Na2CO3 are prepared, and each aqueous solution is dropped and mixed to obtain a precipitate. The precipitate is a spherical precursor particle represented by MeCO3. A carbonate containing Me and M may be obtained as the precursor particle by dissolving a sulfate of M in the aqueous solution of MeSO4.

[0023] 2.1.2 Process S12 In step S12, the surface of the precursor particle is coated with a Na salt to obtain a coated particle. The manufacturing method according to an embodiment may include coating 40% or more of the surface of the precursor particle with a Na salt to obtain a coated particle. Here, the precursor particle may be spherical. When the precursor particle is spherical and the coverage rate of the Na salt with respect to the precursor particle is 40% or more, spherical P2 type particles or spherical O2 type particles are easily obtained. The coated particle may be obtained by coating 50% or more, 60% or more, or 70% of the surface of the precursor particle with a Na salt. Examples of the Na salt include carbonates and nitrates.

[0024] There are various methods for coating the surface of the precursor particles with a Na salt. When spherical O2 type positive electrode active material particles are finally obtained, for example, a rolling fluidized coating method or a spray drying method may be adopted. That is, a coating solution in which a Na salt is dissolved is prepared, and the coating solution is brought into contact with the entire surface of the precursor particles, or the coating solution is dried after the contact. By adjusting the coating conditions (temperature, time, number of times, etc.), for example, 40 area % or more of the surface of the precursor particles can be coated with a Na salt. According to the findings of the present inventor, when the coverage rate of the Na salt is small, when the coated particles are fired, P2 type crystals tend to grow abnormally on the surface of the coated particles, and while plate-shaped Na-containing transition metal oxide particles are obtained, it is difficult to obtain spherical Na-containing transition metal oxide particles. When the coverage rate of the Na salt is large, when the coated particles are fired, the crystallites of the P2 type crystals can be made small, and the shape of the coated particles tends to become spherical corresponding to the shape of the precursor particles. The amount of Na salt coated on the coated particles may be sufficient to obtain a P2 type structure (a sufficient amount of Na is doped).

[0025] 2.1.3 Process S13 In step S13, the coated particles are fired to obtain Na-containing transition metal oxide particles having a P2 type structure. The Na-containing transition metal oxide particles may be plate-shaped or spherical, but as described above, spherical particles tend to exhibit better performance. When the Na-containing transition metal oxide particles are plate-shaped, the O2 type positive electrode active material obtained thereafter is also plate-shaped. On the other hand, when the Na-containing transition metal oxide particles are spherical, the O2 type positive electrode active material obtained thereafter is also spherical.

[0026] The firing temperature in step S13 may be any temperature at which the P2 type structure is formed. If the firing temperature is too low, Na doping is not performed and it is difficult to obtain the P2 type structure. On the other hand, if the firing temperature is too high, the O3 type structure is likely to be formed instead of the P2 type structure. The firing temperature may be, for example, 700°C or more and 1100°C or less, or 800°C or more and 1000°C or less.

[0027] The firing time in step S13 may be appropriately adjusted according to the shape of the desired Na-containing transition metal oxide particles. As described above, when the coverage rate of the Na salt in the coated particles is small, when the coated particles are fired, P2 type crystals tend to grow abnormally on the surface of the coated particles, and plate-shaped Na-containing transition metal oxide particles are easily obtained. On the other hand, when the coverage rate of the Na salt in the coated particles is large, when the coated particles are fired, small P2 type crystals tend to be formed on the surface of the particles, and one P2 type crystallite and another P2 type crystallite are connected to each other to grow the P2 type crystals along the surface of the particles, thereby obtaining spherical Na-containing transition metal oxide particles. If the firing time is too short, Na doping is not performed and the desired P2 type structure is not obtained. On the other hand, if the firing time is too long, the P2 type structure grows excessively, resulting in plate-shaped particles. As far as the inventors have confirmed, when the firing time is from 30 minutes to 3 hours, spherical Na-containing transition metal oxide particles are likely to be obtained, and when the firing time is longer than this, plate-shaped Na-containing transition metal oxide particles are likely to be obtained.

[0028] The firing atmosphere in step S13 is not particularly limited, and may be, for example, an oxygen-containing atmosphere such as air atmosphere, or an inert gas atmosphere.

[0029] The Na-containing transition metal oxide particles obtained through the above steps S11 to S13 may contain, as constituent elements, at least one transition metal element selected from Mn, Ni, and Co, Na, and O. In particular, when the constituent elements contain at least Na, Mn, at least one of Ni and Co, and O, and especially when the constituent elements contain at least Na, Mn, Ni, Co, and O, the performance of the positive electrode active material particles is likely to be further improved. The Na-containing transition metal oxide particles contain Na c Mn x-p Ni y-q Co z-r M p+q+rIt may have a chemical composition represented by O2. Here, 0 < c < 0.70, x + y + z = 1, and 0 ≤ p + q + r ≤ 0.15. Also, M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. When the Na-containing transition metal oxide particles have such a chemical composition, the P2-type structure is more likely to be maintained. In the above chemical composition, c may be greater than 0, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, or 0.60 or more. In the above chemical composition, x may be 0 or more, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, or 0.60 or less. In the above chemical composition, y may be 0 or more, 0.10 or more, or 0.15 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. In the above chemical composition, z may be 0 or more, 0.10 or more, 0.20 or more, or 0.25 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.35 or less. Many of M do not contribute to charge and discharge. In this regard, when p + q + r is 0.15 or less, a high charge and discharge capacity is likely to be ensured. p + q + r may be 0.10 or less, 0.05 or less, or 0. In the composition of O, it is approximately 2, but it is not necessarily exactly 2.0 and is indefinite.

[0030] 2.2 Process S2 In Process S2, by bringing the above Na-containing transition metal oxide particles into contact with an ion exchange material, at least a part of the Na in the Na-containing transition metal oxide particles is replaced with Li to obtain Li-containing transition metal oxide particles having an O2-type structure. Here, the ion exchange material contains lithium hydroxide and a lithium salt.

[0031] Ion exchange includes, for example, a method using an aqueous solution containing a lithium salt and a method using a molten lithium salt. From the viewpoint that the P2 type structure is easily broken by the penetration of water and from the viewpoint of crystallinity, the method using a molten lithium salt is preferred among the above two methods. That is, the Na-containing transition metal oxide particles having the above-mentioned P2 type structure and the lithium salt are mixed, and then heated to a temperature equal to or higher than the melting point of the lithium salt, and the molten lithium salt is brought into contact with the Na-containing transition metal oxide particles, so that at least a part of the Na in the Na-containing transition metal oxide particles can be replaced with Li by ion exchange.

[0032] Here, in step S2, it is important to use lithium hydroxide together with the lithium salt as the ion exchange material. By using a Li source with a high Li concentration during ion exchange, the ion exchange reaction can be promoted, and the Li composition ratio in the Li-containing transition metal oxide particles having an O2 type structure exceeds 1.0 (the above a exceeds 1.0). By using lithium hydroxide together with the lithium salt, such an effect can be easily obtained.

[0033] In step S2, the type of lithium salt constituting the ion exchange material is not particularly limited. In one embodiment, the lithium salt constituting the ion exchange material may contain at least one lithium halide selected from lithium chloride, lithium bromide, and lithium iodide. In particular, when lithium chloride is used, better performance is likely to be ensured. In one embodiment, the lithium salt constituting the ion exchange material may contain lithium nitrate. In one embodiment, the lithium salt constituting the ion exchange material may be a mixed salt of the lithium halide and lithium nitrate. Lithium halide and lithium nitrate have low melting points, and therefore ion exchange can be performed at a lower temperature.

[0034] In step S2, the ratio of lithium hydroxide and lithium salt contained in the ion exchange material is not particularly limited. In the ion exchange material according to one embodiment, the ratio of lithium hydroxide to the total (100 mol%) of lithium hydroxide and lithium salt may be 10 mol% to 90 mol%, 20 mol% to 80 mol%, 40 mol% to 75 mol%, 50 mol% to 70 mol%, or 55 mol% to 65 mol%. This lowers the melting point of the ion exchange material, making it more optimal as an ion exchange material. In the ion exchange material according to one embodiment, the molar ratio of lithium hydroxide may be higher than the molar ratio of lithium salt. In step S2, the ion exchange material may be composed of only lithium hydroxide and lithium salt, or may contain some optional component in addition to lithium hydroxide and lithium salt.

[0035] In step S2, the ion exchange temperature may be, for example, above the melting point of the ion exchange material and below 600°C, below 500°C, below 400°C, or below 300°C. If the ion exchange temperature is too high, the stable phase O3 structure is likely to be generated instead of the O2 structure. On the other hand, from the viewpoint of shortening the time required for ion exchange, the temperature in ion exchange is preferably as high as possible. The ion exchange time is not particularly limited, but may be, for example, 10 minutes to 10 hours, 30 minutes to 7 hours, or 1 hour to 5 hours. As far as the present inventors have confirmed, the positive electrode active material particles having the O2 crystal structure are more likely to be produced appropriately at an ion exchange temperature of 270°C to 320°C and an ion exchange time of 1 hour to 8 hours.

[0036] 3. Lithium-ion battery The positive electrode active material particles of the present disclosure may be employed as a positive electrode active material of a lithium ion battery. FIG. 4 shows a schematic configuration of a lithium ion battery 100 according to an embodiment. As shown in FIG. 4, the lithium ion battery 100 has a positive electrode active material layer 20, an electrolyte layer 30, and an anode active material layer 40. The positive electrode active material layer 20 has the positive electrode active material particles of the present disclosure. In the lithium ion battery 100, at least one of the positive electrode active material layer 20, the electrolyte layer 30, and the anode active material layer 40 may contain a solid electrolyte. Furthermore, the lithium ion battery 100 may be a solid-state battery. A solid-state battery refers to a battery in which an electrolyte having carrier ion conductivity is mainly composed of a solid electrolyte. However, a liquid component may be included in a part of the battery. Alternatively, the lithium ion battery 100 may be an all-solid-state battery that does not substantially contain a liquid component. Alternatively, the lithium ion battery 100 may be a liquid-based battery that contains an electrolytic solution. 4, the lithium ion battery 100 may include a positive electrode current collector 10 in contact with the positive electrode active material layer 20. The lithium ion battery 100 may also include a negative electrode current collector 50 in contact with the negative electrode active material layer 40.

[0037] 3.1 Positive electrode current collector The positive electrode collector 10 may be any of those generally used as a positive electrode collector for lithium ion batteries. The positive electrode collector 10 may have at least one shape selected from a foil, a plate, a mesh, a punched metal, and a foam. The positive electrode collector 10 may be made of a metal foil or a metal mesh. In particular, a metal foil is excellent in terms of ease of handling. The positive electrode collector 10 may be made of a plurality of foils. Examples of metals constituting the positive electrode collector 10 include at least one selected from Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, V, Mg, Pb, Ge, In, Sn, Zr, and stainless steel. In particular, from the viewpoint of ensuring oxidation resistance, the positive electrode collector 10 may contain Al. The positive electrode collector 10 may have some kind of coating layer on its surface for the purpose of adjusting resistance, etc. For example, the positive electrode collector 10 may have a carbon coating layer. The positive electrode collector 10 may be a metal foil or a substrate plated or vapor-deposited with the above-mentioned metal. When the positive electrode collector 10 is made of a plurality of metal foils, some layer may be present between the plurality of metal foils. The thickness of the positive electrode collector 10 is not particularly limited. For example, it may be 0.1 μm or more and 1 mm or less, the lower limit may be 1 μm or more, and the upper limit may be 100 μm or less.

[0038] 3.2 Cathode active material layer The positive electrode active material layer 20 includes at least the positive electrode active material particles of the present disclosure as the positive electrode active material. The positive electrode active material layer 20 may also include an electrolyte. The electrolyte may be a solid electrolyte, a liquid electrolyte, or a combination of a solid electrolyte and a liquid electrolyte. The positive electrode active material layer 20 may also include one or both of a conductive assistant and a binder. The positive electrode active material layer 20 may also include an electrolyte, and one or both of a conductive assistant and a binder. The positive electrode active material layer 20 may also include an electrolyte, a conductive assistant, and a binder. The positive electrode active material layer 20 may also include various additives. The contents of the positive electrode active material, electrolyte, conductive assistant, binder, and the like in the positive electrode active material layer 20 may be appropriately determined according to the desired performance. For example, the content of the positive electrode active material (the total of the positive electrode active material particles of the present disclosure and other positive electrode active materials) may be 40% by mass or more, 50% by mass or more, or 60% by mass or more, and may be 100% by mass or less, or 90% by mass or less, with the entire positive electrode active material layer 20 (total solid content) being 100% by mass. The shape of the positive electrode active material layer 20 is not particularly limited, and may be, for example, a sheet-like positive electrode active material layer 20 having a substantially flat surface. The thickness of the positive electrode active material layer 20 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.

[0039] 3.2.1 Cathode active material The positive electrode active material layer 20 may contain only the positive electrode active material particles of the present disclosure as the positive electrode active material. Alternatively, the positive electrode active material layer 20 may contain, in addition to the positive electrode active material particles of the present disclosure, a different type of positive electrode active material (other positive electrode active material). From the viewpoint of further enhancing the effect of the technology of the present disclosure, the content of the other positive electrode active material in the positive electrode active material layer 20 may be small. For example, the content of the positive electrode active material derived from the positive electrode active material particles of the present disclosure may be 50% by mass or more and 100% by mass or less, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, 95% by mass or more and 100% by mass or less, or 99% by mass or more and 100% by mass or less, based on the total positive electrode active material contained in the positive electrode active material layer 20 being 100% by mass.

[0040] As the other positive electrode active material, any of those known as positive electrode active materials for lithium ion batteries can be adopted. Among the known active materials, a material with a relatively noble potential (charge / discharge potential) for absorbing and releasing lithium ions can be used as the positive electrode active material, and a relatively base material can be used as the negative electrode active material. The other positive electrode active material may be, for example, at least one selected from various lithium-containing compounds, elemental sulfur, sulfur compounds, and the like. The lithium-containing compound as the positive electrode active material may be a lithium-containing oxide containing at least one element M, Li, and O. The element M may be, for example, at least one selected from Mn, Ni, Co, Al, Mg, Ca, Sc, V, Cr, Cu, Zn, Ga, Ge, Y, Zr, Sn, Sb, W, Pb, Bi, Fe, and Ti, or at least one selected from the group consisting of Mn, Ni, Co, Al, Fe, and Ti. More specifically, the lithium-containing oxide may be lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium nickel manganese oxide, lithium cobalt manganese oxide, lithium nickel cobalt manganese oxide (Li 1±α Ni x Co y Mn z O 2±δ(For example, 0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1)), a spinel-based lithium compound (Li 1+x Mn 2-x-y M y O4 (where M is one or more selected from Al, Mg, Co, Fe, Ni, and Zn), such as a hetero-element substituted Li-Mn spinel with a composition represented by etc.), lithium nickel cobalt aluminum oxide (for example, Li 1±α Ni p Co q Al r O 2±δ (For example, p + q + r = 1)), lithium titanate, lithium metal phosphate (such as LiMPO4, where M is one or more selected from Fe, Mn, Co, and Ni), etc. may be at least one selected from. Other cathode active materials may include a lithium-containing oxide containing at least one of Ni, Co, and Mn, Li, and O as constituent elements. Alternatively, other cathode active materials may include a lithium-containing oxide containing at least one of Ni, Co, and Al, Li, and O as constituent elements. Only one type of other cathode active material may be used alone, or two or more types may be used in combination.

[0041] The shape of the other cathode active material may be a general shape as a cathode active material of a lithium-ion battery. The other cathode active material may be, for example, particulate. The other cathode active material may have voids and may be, for example, porous or hollow. The other cathode active material may be primary particles or secondary particles aggregated from a plurality of primary particles. The average particle diameter D50 of the other cathode active material may be, for example, 1 nm or more and 500 μm or less, the lower limit may be 5 nm or more or 10 nm or more, and the upper limit may be 100 μm or less, 50 μm or less, or 30 μm or less. Incidentally, the average particle diameter D50 is the particle diameter (median diameter) at the integrated value of 50% in the volume-based particle size distribution determined by the laser diffraction / scattering method.

[0042] 3.2.2 Protective Layer An ion-conductive protective layer may be formed on the surface of the positive electrode active material (the positive electrode active material particles of the present disclosure, other positive electrode active materials). That is, the positive electrode active material layer 20 may include a complex of the positive electrode active material and the protective layer, and at least a part of the surface of the positive electrode active material in the complex may be covered with the protective layer. This makes it easier to suppress, for example, the reaction between the positive electrode active material and other battery materials (such as the sulfide solid electrolyte described later). The ion-conductive protective layer may include various ion-conductive compounds. The ion-conductive compound may be, for example, at least one selected from ion-conductive oxides and ion-conductive halides.

[0043] The ion conductive oxide may contain, for example, at least one element selected from B, C, Al, Si, P, S, Ti, La, Zr, Nb, Mo, Zn, and W, Li, and O. The ion conductive oxide may be an oxynitride containing N. More specifically, the ion conductive oxide may be Li3BO3, LiBO2, Li2CO3, LiAlO2, Li4SiO4, Li2SiO3, Li3PO4, Li2SO4, Li2TiO3, Li4Ti5O 12 , Li2Ti2O5, Li2ZrO3, LiNbO3, Li2MoO4, Li2WO4, LiPON, Li2O-LaO2, Li2O-ZnO2, etc. The ion-conductive oxide may be one in which some elements are substituted with various doping elements.

[0044] The ion conductive halide may be, for example, at least one of various compounds exemplified as the halide solid electrolyte described later. The ion conductive halide may include, for example, at least one element selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sn, Al, Sc, Ga, Bi, Sb, Zr, Hf, Ti, Ta, Nb, W, Y, Gd, Tb and Sm, at least one halogen element selected from the group consisting of Cl, Br, I and F, and Li. The ion conductive halide may include at least one element selected from the group consisting of Ti, Al, Gd, Ca, Zr and Y, at least one element selected from the group consisting of Cl, Br, I and F, and Li. The ion conductive halide may also include at least one element selected from the group consisting of Ti and Al, at least one element selected from the group consisting of Cl, Br, I and F, and Li. The ion conductive halide may also be, for example, a complex halide of Li, Ti, Al and F.

[0045] The coverage (area ratio) of the protective layer with respect to the surface of the positive electrode active material may be, for example, 70% or more, 80% or more, or 90% or more. The thickness of the protective layer may be, for example, 0.1 nm or more and 100 nm or less, with a lower limit of 1 nm or more and an upper limit of 20 nm or less.

[0046] 3.2.3 Electrolytes The positive electrode active material layer 20 may contain an electrolyte. The electrolyte that may be contained in the positive electrode active material layer 20 may be a solid electrolyte, a liquid electrolyte, or a combination of a solid electrolyte and a liquid electrolyte.

[0047] 3.2.3.1 Solid electrolyte As the solid electrolyte, a solid electrolyte known for lithium ion batteries may be used. The solid electrolyte may be an inorganic solid electrolyte or an organic polymer electrolyte. In particular, the inorganic solid electrolyte has excellent ion conductivity and heat resistance. Examples of the inorganic solid electrolyte include an oxide solid electrolyte, a sulfide solid electrolyte, and an ion-bonded inorganic solid electrolyte. Among the inorganic solid electrolytes, the sulfide solid electrolyte, and among them, the sulfide solid electrolyte containing at least Li, S, and P as constituent elements, have high performance. Alternatively, among the inorganic solid electrolytes, the ion-bonded solid electrolyte, and among them, the solid electrolyte containing at least Li, Y, and a halogen (at least one of Cl, Br, I, and F) as constituent elements, have high performance. The solid electrolyte may be amorphous or crystalline. The solid electrolyte may be particulate. The average particle diameter (D50) of the solid electrolyte may be, for example, 10 nm or more and 10 μm or less. The average particle diameter D50 in the present application is the particle diameter (median diameter) at an integrated value of 50% in the volume-based particle size distribution obtained by a laser diffraction / scattering method. The ionic conductivity of the solid electrolyte at 25° C. is, for example, 1×10 -5 S / cm or more, 1×10 -4 S / cm or more, or 1×10 -3 The solid electrolyte may have a specific surface area of ​​100 nm or more and may have a specific surface area of ​​100 nm or more.

[0048] The oxide solid electrolyte is lithium lanthanum zirconate, LiPON, Li 1+X Al X Ge 2-X It may be one or more selected from (PO4)3, Li-SiO-based glass, Li-Al-SO-based glass, etc. In addition, when an oxide solid electrolyte is combined with a liquid electrolyte, ion conductivity can be improved.

[0049] The sulfide solid electrolyte may be a glass-based sulfide solid electrolyte (sulfide glass), a glass ceramic-based sulfide solid electrolyte, or a crystalline sulfide solid electrolyte. The sulfide glass is amorphous. The sulfide glass may have a glass transition temperature (Tg). In addition, when the sulfide solid electrolyte has a crystalline phase, examples of the crystalline phase include a Thio-LISICON type crystalline phase, a LGPS type crystalline phase, and an Argyrodite type crystalline phase.

[0050] The sulfide solid electrolyte may contain, for example, Li element, X element (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and S element. The sulfide solid electrolyte may further contain at least one of O element and halogen element. The sulfide solid electrolyte may contain S element as a main component of anion element.

[0051] Examples of sulfide solid electrolytes include Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-GeS2, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-P2S5-LiI-LiBr, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-ZmSn (where m and n are positive numbers, and Z is Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, and Li2S-SiS2-Li x MO y (wherein x and y are positive numbers, and M is any one of P, Si, Ge, B, Al, Ga, and In).

[0052] The composition of the sulfide solid electrolyte is not particularly limited. For example, xLi2S·(100 - x)P2S5 (70 ≤ x ≤ 80), yLiI·zLiBr·(100 - y - z)(xLi2S·(1 - x)P2S5) (0.7 ≤ x ≤ 0.8, 0 ≤ y ≤ 30, 0 ≤ z ≤ 30), etc. may be mentioned. Alternatively, the sulfide solid electrolyte may have a composition represented by the general formula: Li 4-x Ge 1-x P x S4 (0 < x < 1). In the above general formula, at least a part of Ge may be substituted with at least one of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. In the above general formula, at least a part of P may be substituted with at least one of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. In the above general formula, a part of Li may be substituted with at least one of Na, K, Mg, Ca, and Zn. In the above general formula, a part of S may be substituted with a halogen (at least one of F, Cl, Br, and I). Alternatively, the sulfide solid electrolyte may be Li 7-a PS 6-a X a (X is at least one of Cl, Br, and I, and a is a number of 0 or more and 2 or less). a may be 0, or may be greater than 0. In the latter case, a may be 0.1 or more, may be 0.5 or more, and may be 1 or more. Also, a may be 1.8 or less, may be 1.5 or less.

[0053] The ion-bonded solid electrolyte may contain at least one element selected from the group consisting of, for example, Mg, Ca, Sr, Ba, Zn, Sn, Al, Sc, Ga, Bi, Sb, Zr, Hf, Ti, Ta, Nb, W, Y, Gd, Tb and Sm. These elements may generate cations in water. The ion-bonded solid electrolyte material may further contain, for example, at least one halogen element selected from the group consisting of Cl, Br, I and F. These elements may generate anions in water. The ion-bonded solid electrolyte may contain at least one element selected from the group consisting of Gd, Ca, Zr and Y, at least one element selected from the group consisting of Cl, Br, I and F, and Li. The ion-bonded solid electrolyte may contain Li and Y, and at least one element selected from the group consisting of Cl, Br, I and F. More specifically, the ionic solid electrolyte may contain Li, Y, Cl, and Br, or may contain Li, Ca, Y, Gd, Cl, and Br, or may contain Li, Zr, Y, and Cl. More specifically, the ionic solid electrolyte may be Li3YBr2Cl4, Li 2.8 Ca 0.1 Y 0.5 Gd 0.5 Br2Cl4 and Li 2.5 Y 0.5 Zr 0.5 Cl6.

[0054] The ionically bonded solid electrolyte may be a halide solid electrolyte. The halide solid electrolyte has excellent ion conductivity. Examples of the halide solid electrolyte include those represented by the formula (1): Li α M β X γ (A) It may have a composition represented by the following. Here, α, β, and γ are each independently a value greater than 0, M is at least one selected from the group consisting of metal elements other than Li and metalloid elements, and X is at least one selected from the group consisting of Cl, Br, and I. Note that the "metalloid element" may be at least one selected from the group consisting of B, Si, Ge, As, Sb, and Te. Also, the "metal element" may include (i) all elements contained in Groups 1 to 12 of the periodic table (excluding hydrogen) and (ii) all elements contained in Groups 13 to 16 of the periodic table (excluding B, Si, Ge, As, Sb, Te, C, N, P, O, S, and Se). The metal element can form an inorganic compound with a halide ion and become a cation.

[0055] In formula (A), M may contain Y (i.e., yttrium). The halide solid electrolyte containing Y is Li a Me b Y c It may have a composition represented by X6 (where a + mb + 3c = 6, c > 0, Me is at least one selected from the group consisting of metal elements and metalloid elements other than Li and Y, and m is the valence of Me). Me may be at least one selected from the group consisting of, for example, Mg, Ca, Sr, Ba, Zn, Sc, Al, Ga, Bi, Zr, Hf, Ti, Sn, Ta, and Nb.

[0056] The halide solid electrolyte may have a composition represented by formula (A1): Li 6-3d Y d X6. In formula (A1), X is one or more elements selected from the group consisting of Cl, Br, and I. d may satisfy 0 < d < 2, or d = 1. The halide solid electrolyte may have a composition represented by formula (A2): Li 3-3δ Y 1+δ Cl6. In formula (A2), 0 < δ ≦ 0.15 may hold. The halide solid electrolyte may have a composition represented by formula (A3): Li 3-3δ Y 1+δIt may have a composition represented by Br6. In formula (A3), 0 < δ ≦ 0.25 may be satisfied. The halide solid electrolyte has the formula (A4): Li 3-3δ+a Y 1+δ-a Me a Cl 6-x-y Br x I y and may have a composition represented by. In formula (A4), Me may be at least one selected from the group consisting of Mg, Ca, Sr, Ba, and Zn. In formula (A4), for example, -1 < δ < 2, 0 < a < 3, 0 < (3 - 3δ + a), 0 < (1 + δ - a), 0 ≦ x ≦ 6, 0 ≦ y ≦ 6, and (x + y) ≦ 6 are satisfied. The halide solid electrolyte has the formula (A5): Li 3-3δ Y 1+δ-a Me a Cl 6-x-y Br x I y and may have a composition represented by. In formula (A5), Me may be at least one selected from the group consisting of Al, Sc, Ga, and Bi. In formula (A5), -1 < δ < 1, 0 < a < 2, 0 < (1 + δ - a), 0 ≦ x ≦ 6, 0 ≦ y ≦ 6, and (x + y) ≦ 6 may be satisfied. The halide solid electrolyte has the formula (A6): Li 3-3δ-a Y 1+δ-a Me a Cl 6-x-y Br x I y and may have a composition represented by. In formula (A6), Me may be at least one selected from the group consisting of Zr, Hf, and Ti. In formula (A6), -1 < δ < 1, 0 < a < 1.5, 0 < (3 - 3δ - a), 0 < (1 + δ - a), 0 ≦ x ≦ 6, 0 ≦ y ≦ 6, and (x + y) ≦ 6 may be satisfied. The halide solid electrolyte has the formula (A7): Li 3-3δ-2a Y 1+δ-a Me a Cl 6-x-y Br x I yIn formula (A7), Me may be at least one selected from the group consisting of Ta and Nb. In formula (A7), -1<δ<1, 0 <a<1.2、0<(3-3δ-2a)、0<(1+δ-a)、0≦x≦6、0≦y≦6、かつ、(x+y)≦6であってもよい。

[0057] The ionically bonded solid electrolyte may be a complex hydride solid electrolyte. The complex hydride solid electrolyte may be composed of Li ions and complex ions containing H. The complex ion containing H may have, for example, an element M containing at least one of a nonmetallic element, a semimetallic element, and a metallic element, and H bonded to the element M. In addition, the complex ion containing H may have the element M as a central element and H surrounding the element M bonded to each other via a covalent bond. In addition, the complex ion containing H may be (M m H n ) α- In this case, m is any positive number, and n and α can be any positive number depending on m and the valence of the element M. The element M may be a nonmetallic element or a metallic element capable of forming a complex ion. For example, the element M may contain at least one of B, C, and N as a nonmetallic element, or may contain B. Also, for example, the element M may contain at least one of Al, Ni, and Fe as a metallic element. In particular, when the complex ion contains B or contains C and B, higher ionic conductivity is likely to be ensured. Specific examples of complex ions containing H include (CB9H 10 ) - , (C.B. 11 H 12 ) - , (B 10 H 10 ) 2- , (B 12 H 12 ) 2- , (BH4) - , (NH2) - , (AlH4) - , and combinations thereof. In particular, (CB9H 10 ) - , (C.B. 11H 12 ) - In other words, the complex hydride solid electrolyte may contain Li, C, B, and H.

[0058] 3.2.3.2 Liquid electrolyte The liquid electrolyte (electrolytic solution) is a liquid containing lithium ions as carrier ions. The electrolytic solution may be an aqueous electrolytic solution or a non-aqueous electrolytic solution. The composition of the electrolytic solution may be the same as that of the electrolytic solution of a lithium ion secondary battery known in the art. The electrolytic solution may be a solution in which a lithium salt is dissolved in water or a non-aqueous solvent. Examples of the non-aqueous solvent include carbonate-based solvents. Examples of the carbonate-based solvent include fluoroethylene carbonate (FEC), ethylene carbonate (EC), dimethyl carbonate (DMC), and propylene carbonate (PC). Examples of the lithium salt include LiPF6, LiTFSI, and LiFSI.

[0059] 3.2.4 Conductive additives Examples of the conductive assistant that may be included in the positive electrode active material layer 20 include carbon materials such as vapor grown carbon fiber (VGCF), acetylene black (AB), ketjen black (KB), carbon nanotubes (CNT), and carbon nanofibers (CNF); and metal materials such as nickel, titanium, aluminum, and stainless steel. The conductive assistant may be, for example, particulate or fibrous, and the size is not particularly limited. Only one type of conductive assistant may be used alone, or two or more types may be used in combination.

[0060] 3.2.5 Binders Examples of binders that can be included in the positive electrode active material layer 20 include butadiene rubber (BR)-based binders, butylene rubber (IIR)-based binders, acrylate butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, polytetrafluoroethylene (PTFE)-based binders, polyimide (PI)-based binders, etc. Only one type of binder may be used alone, or two or more types may be used in combination.

[0061] 3.2.6 Other The positive electrode active material layer 20 may contain various additives in addition to the above-mentioned components, such as a dispersant and a lubricant.

[0062] The positive electrode active material layer 20 can be manufactured by applying a known method. For example, the positive electrode active material layer 20 can be easily formed by, for example, dry or wet molding a positive electrode mixture containing the positive electrode active material particles and the like of the present disclosure. The positive electrode active material layer 20 may be molded together with the positive electrode current collector 10, or may be molded separately from the positive electrode current collector 10.

[0063] 3.3 Electrolyte layer The electrolyte layer 30 is disposed between the positive electrode active material layer 20 and the negative electrode active material layer 40. The electrolyte layer 30 includes at least an electrolyte. The electrolyte layer 30 may include one or both of a solid electrolyte and a liquid electrolyte (electrolytic solution), and may further include a binder and various additives. The content of the electrolyte and the binder in the electrolyte layer 30 is not particularly limited. Alternatively, the electrolyte layer 30 may have a separator or the like for holding the electrolytic solution and preventing contact between the positive electrode active material layer 20 and the negative electrode active material layer 40. The thickness of the electrolyte layer 30 is not particularly limited, and may be, for example, 0.1 μm or more and 2 mm or less, the lower limit may be 1 μm or more, and the upper limit may be 1 mm or less.

[0064] The electrolyte layer 30 may be composed of one layer or may be composed of multiple layers. For example, the electrolyte layer 30 may include a first layer arranged on the positive electrode active material layer 20 side and a second layer arranged on the negative electrode active material layer 40 side, and the first layer may include the first electrolyte, and the second layer may include the second electrolyte. The first electrolyte and the second electrolyte may be different from each other. The first electrolyte and the second electrolyte may each be at least one selected from the above-mentioned oxide solid electrolyte, sulfide solid electrolyte, and ionic solid electrolyte. For example, the first layer may include an ionic solid electrolyte, and the second layer may include at least one of an ionic solid electrolyte and a sulfide solid electrolyte.

[0065] The electrolyte contained in the electrolyte layer 30 may be appropriately selected from those exemplified as electrolytes that may be contained in the positive electrode active material layer 20 (solid electrolytes and / or liquid electrolytes). The binder that may be contained in the electrolyte layer 30 may also be appropriately selected from those exemplified as binders that may be contained in the positive electrode active material layer 20. Each of the electrolytes and binders may be used alone or in combination of two or more. The separator may be any separator that is normally used in secondary batteries, and examples of the separator include those made of resins such as polyethylene (PE), polypropylene (PP), polyester, and polyamide. The separator may have a single layer structure or a multilayer structure. Examples of the multilayer separator include a separator with a two-layer structure of PE / PP, or a separator with a three-layer structure of PP / PE / PP or PE / PP / PE. The separator may be made of a nonwoven fabric such as a cellulose nonwoven fabric, a resin nonwoven fabric, or a glass fiber nonwoven fabric.

[0066] 3.4 Negative electrode active material layer The negative electrode active material layer 40 includes at least a negative electrode active material. The negative electrode active material layer 40 may also include an electrolyte, a conductive assistant, a binder, various additives, and the like. The content of each component in the negative electrode active material layer 40 may be appropriately determined according to the target battery performance. For example, the content of the negative electrode active material may be 40 mass% or more, 50 mass% or more, 60 mass% or more, or 70 mass% or more, or 100 mass% or less, less than 100 mass%, 95 mass% or less, or 90 mass% or less, based on the entire solid content of the negative electrode active material layer 40 being 100 mass%. Alternatively, the negative electrode active material and optionally the electrolyte, the conductive assistant, and the binder may be included in a total amount of 85 volume% or more, 90 volume% or more, or 95 volume% or more, based on the entire negative electrode active material layer 40 being 100 volume%, and the remainder may be voids or other components. The shape of the negative electrode active material layer 40 is not particularly limited, and may be, for example, a sheet having a substantially flat surface. The thickness of the negative electrode active material layer 40 is not particularly limited, and may be, for example, 0.1 μm or more and 2 mm or less, with a lower limit of 1 μm or more, 10 μm or more, or 30 μm or more, and an upper limit of 1 mm or less, 500 μm or less, or 100 μm or less.

[0067] 3.4.1 Negative electrode active material The negative electrode active material contained in the negative electrode active material layer 40 can be any of those known as negative electrode active materials for lithium ion batteries. Of the known active materials, various materials can be used that have a potential (charge / discharge potential) at which a predetermined carrier ion is absorbed and released that is lower than the above-mentioned positive electrode active material. The negative electrode active material may be at least one selected from, for example, silicon-based active materials such as Si, Si alloys, and silicon oxide; carbon-based active materials such as graphite and hard carbon; various oxide-based active materials such as lithium titanate; metallic lithium, lithium alloys, and the like. Only one type of negative electrode active material may be used alone, or two or more types may be used in combination. The shape of the negative electrode active material may be any shape that is common as a negative electrode active material for lithium ion batteries. For example, the negative electrode active material may be in the form of particles. The negative electrode active material particles may be primary particles, or may be secondary particles formed by agglomeration of a plurality of primary particles. The average particle diameter (D50) of the negative electrode active material particles may be, for example, 1 nm or more and 500 μm or less, with a lower limit of 5 nm or more or 10 nm or more and an upper limit of 100 μm or less, 50 μm or less, or 30 μm or less. Alternatively, the negative electrode active material layer 40 may be made of a sheet-like (foil-like, film-like) active material such as lithium foil.

[0068] 3.4.2 Other The electrolyte that can be contained in the negative electrode active material layer 40 may be appropriately selected from those exemplified as the electrolyte that can be contained in the above-mentioned positive electrode active material layer 20 (solid electrolytes and / or liquid electrolytes). The conductive assistant that can be contained in the negative electrode active material layer 40 may be appropriately selected from those exemplified as the conductive assistant that can be contained in the above-mentioned positive electrode active material layer 20. The binder that can be contained in the negative electrode active material layer 40 may be appropriately selected from those exemplified as the binder that can be contained in the above-mentioned positive electrode active material layer 20. Each of the electrolyte, conductive assistant, and binder may be used alone or in combination of two or more kinds.

[0069] The negative electrode active material layer 40 may contain various additives in addition to the above-mentioned components, such as a dispersant and a lubricant.

[0070] The negative electrode active material layer 40 can be manufactured by applying a known method. For example, the negative electrode active material layer 40 can be easily formed by forming a negative electrode mixture containing the above-mentioned various components in a dry or wet manner. The negative electrode active material layer 40 may be formed together with the negative electrode current collector 50, or may be formed separately from the negative electrode current collector 50.

[0071] 3.5 Negative electrode current collector The negative electrode current collector 50 may be any of those generally used as negative electrode current collectors for lithium ion batteries. The negative electrode current collector 50 may be in the form of a foil, a plate, a mesh, a punched metal, or a foam. The negative electrode current collector 50 may be a metal foil or a metal mesh, or may be a carbon sheet. In particular, metal foil is excellent in terms of ease of handling. The negative electrode current collector 50 may be made of a plurality of foils or sheets. Examples of metals constituting the negative electrode current collector 50 include at least one selected from Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, V, Mg, Pb, Ge, In, Sn, Zr, and stainless steel. In particular, from the viewpoint of ensuring reduction resistance and being difficult to alloy with lithium, the negative electrode current collector 50 may contain at least one metal selected from Cu, Ni, and stainless steel. The negative electrode collector 50 may have some kind of coating layer on its surface for the purpose of adjusting the resistance, etc. For example, the negative electrode collector 50 may have a carbon coating layer. The negative electrode collector 50 may be an aluminum foil having a carbon coating layer. The negative electrode collector 50 may also be a metal foil or a base material on which the above metal is plated or vapor-deposited. When the negative electrode collector 50 is made of a plurality of metal foils, some kind of layer may be present between the plurality of metal foils. The thickness of the negative electrode collector 50 is not particularly limited. For example, it may be 0.1 μm or more and 1 mm or less, the lower limit may be 1 μm or more, and the upper limit may be 100 μm or less.

[0072] 3.6 Other configurations The lithium ion battery 100 may have a general configuration as a battery in addition to the above configuration. For example, a tab, a terminal, etc. The lithium ion battery 100 may have each of the above configurations housed inside an exterior body. Any known exterior body for a battery can be adopted as the exterior body. In addition, a plurality of lithium ion batteries 100 may be electrically connected and stacked in any manner to form an assembled battery. In this case, the assembled battery may be housed inside a known battery case. The lithium ion battery 100 may have other obvious configurations such as necessary terminals. The shape of the lithium ion battery 100 may be, for example, a coin type, a laminate type, a cylindrical type, a square type, etc. The lithium ion battery 100 may be a secondary battery.

[0073] 4. Manufacturing method of lithium-ion batteries The lithium ion battery 100 can be manufactured by applying a known method. For example, the lithium ion battery 100 can be manufactured as follows. However, the manufacturing method of the lithium ion battery 100 is not limited to the following method, and each layer may be formed by, for example, dry molding or the like. (1) The positive electrode active material constituting the positive electrode active material layer is dispersed in a solvent to obtain a positive electrode slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. Thereafter, the positive electrode slurry is applied to the surface of a positive electrode current collector or an electrolyte layer described later using a doctor blade or the like, and then dried to form a positive electrode active material layer on the surface of the positive electrode current collector or the electrolyte layer, thereby forming a positive electrode. Here, the positive electrode active material layer may be press-molded. (2) The negative electrode active material constituting the negative electrode active material layer is dispersed in a solvent to obtain a negative electrode slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. Thereafter, the negative electrode slurry is applied to the surface of the negative electrode current collector or the electrolyte layer described below using a doctor blade or the like, and then dried to form a negative electrode active material layer on the surface of the negative electrode current collector or the electrolyte layer, thereby forming a negative electrode. Here, the negative electrode active material layer may be press-molded. (3) The layers are laminated so as to sandwich the electrolyte layer between the negative electrode and the positive electrode, and a laminate having the negative electrode current collector, the negative electrode active material layer, the electrolyte layer, the positive electrode active material layer, and the positive electrode current collector in this order is obtained. The electrolyte layer may be obtained by, for example, molding an electrolyte mixture containing an electrolyte and a binder, or by press molding. Here, the laminate may be further press molded. Other members such as terminals are attached to the laminate as necessary. When an electrolytic solution is used, a separator may be used in the electrolyte layer. (4) The laminate is housed in a battery case and sealed to obtain a lithium-ion battery.

[0074] 5. How to increase the capacity of a lithium-ion battery The technology of the present disclosure also has an aspect of being a method for increasing the capacity of a lithium ion battery. That is, the method for increasing the capacity of a lithium ion battery of the present disclosure is characterized in that the positive electrode active material particles of the present disclosure are used in a positive electrode active material layer of the lithium ion battery.

[0075] 6. Vehicles with lithium-ion batteries As described above, when the positive electrode active material layer of a lithium ion battery is formed using the positive electrode composite of the present disclosure, an increase in the capacity of the lithium ion battery can be expected. Such a lithium ion battery can be suitably used in at least one vehicle selected from, for example, a hybrid vehicle (HEV), a plug-in hybrid vehicle (PHEV), and an electric vehicle (BEV). That is, the technology of the present disclosure also has an aspect of a vehicle having a lithium ion battery, the lithium ion battery having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, and the positive electrode active material layer contains the positive electrode active material particles of the present disclosure. EXAMPLES

[0076] As described above, one embodiment of the positive electrode active material layer, the lithium ion secondary battery, and the manufacturing method thereof of the present disclosure has been described, but the technology of the present disclosure can be modified in various ways other than the above embodiment without departing from the gist of the technology. The technology of the present disclosure will be described in more detail below with reference to examples, but the technology of the present disclosure is not limited to the following examples.

[0077] 1. Preparation of Precursor Particles MnSO4·5H2O, NiSO4·6H2O and CoSO4·7H2O were weighed out to obtain the desired composition ratio, and dissolved in distilled water to a concentration of 1.2 mol / L to obtain the first liquid. In a separate container, Na2CO3 was dissolved in distilled water to a concentration of 1.2 mol / L to obtain the second liquid. Next, 500 mL of the first and second liquids were dropped at a rate of about 4 mL / min into a reaction container that had already contained 1000 mL of pure water. After the dropwise addition, the mixture was stirred at room temperature for 1 h at a stirring speed of 150 rpm. The precipitate was washed with pure water and separated into solid and liquid using a centrifuge. The obtained precipitate was dried overnight at 120°C, crushed in a mortar, and fine particles were removed by air classification to obtain mixed salt particles (precursor particles) containing Mn, Ni and Co. The precursor particles were spherical particles with a circularity of 0.80.

[0078] 2. Preparation of Na-containing transition metal oxide particles with P2-type structure 2.1 In the case of a spherical shape (Examples 1 and 2 and Comparative Example 1) After weighing out Na2CO3 and distilled water so that the total amount was 150 g / L, the mixture was stirred with a stirrer until completely dissolved to prepare an aqueous Na2CO3 solution. The above precursor particles were mixed into the aqueous Na2CO3 solution to prepare a slurry. The Na2CO3 and the above precursor particles were dried and then mixed with Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 The mixture was mixed so as to have a composition of 0.02. The obtained slurry was dried by spray drying. Specifically, a DL410 spray dryer was used, with a slurry delivery rate of 30 mL / min, an inlet temperature of 200°C, and a circulating air volume of 0.8 m 3At a spray air pressure of 0.3 MPa, 90% of the surface area of ​​the precursor particles was coated with Na2CO3 to obtain coated particles.

[0079] The coated particles were fired in an electric furnace in an air atmosphere using an alumina crucible. Specifically, the coated particles were subjected to a "first heating step", a "pre-firing step", a "second heating step", a "main firing step", a "furnace cooling step" and an "out-of-furnace cooling step" as shown in Table 1 and FIG. 5 below. The "furnace cooling step" refers to a cooling step in an electric furnace, and the "out-of-furnace cooling step" refers to a step of cooling in the air outside the electric furnace. Thereafter, the particles were pulverized in a mortar in a dry atmosphere to obtain a Na-containing transition metal oxide (Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 The Na-containing transition metal oxide was spherical particles having a circularity of 0.82.

[0080] 2.2 In the case of plate shape (Reference Example 1 and Comparative Example 2) Na2CO3 and the above precursor particles were mixed with Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 The mixture was weighed in a dry atmosphere so as to have a composition of 02 and mixed in a mortar to obtain a mixture. The mixture was fired in an electric furnace using an alumina crucible in an air atmosphere. Specifically, the mixture was subjected to the "first heating step", "pre-firing step", "second heating step", "main firing step", "in-furnace cooling step" and "out-furnace cooling step" as shown in Table 1 and FIG. 5 below. Thereafter, the mixture was pulverized in a mortar in a dry atmosphere to obtain a Na-containing transition metal oxide (Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 O2) was obtained. The Na-containing transition metal oxide was in the form of plate-like particles.

[0081] [Table 1]

[0082] 3. Preparation of active material with O2 structure 3.1 Example 1 and Reference Example 1 LiOH and LiCl were weighed out to have a molar ratio of 65:35, and mixed with P2 type spherical particles (Example 1) or P2 type plate-like particles (Reference Example 1) in a molar ratio that was 10 times the minimum Li amount required for ion exchange to obtain a mixture. The mixture was fired at 300°C for 4 hours in an air atmosphere using an alumina crucible to obtain a fired product. The salt remaining in the fired product was washed with pure water, and solid-liquid separation was performed by vacuum filtration to obtain a precipitate. The precipitate was dried overnight at 120°C to obtain positive electrode active material particles having an O2 type structure.

[0083] 3.2 Example 2 LiOH and LiNO3 were weighed out to a molar ratio of 60:40, and mixed with P2-type spherical particles in a molar ratio that was 10 times the minimum Li amount required for ion exchange to obtain a mixture. The mixture was fired at 300°C for 1 hour in an air atmosphere using an alumina crucible to obtain a fired product. The salt remaining in the fired product was washed with pure water, and solid-liquid separation was performed by vacuum filtration to obtain a precipitate. The precipitate was dried overnight at 120°C to obtain positive electrode active material particles having an O2-type structure.

[0084] 3.3 Comparative Examples 1 and 2 LiCl and LiNO3 were weighed out to have a molar ratio of 50:50, and mixed with P2 type spherical particles (Comparative Example 1) or P2 type plate-like particles (Comparative Example 2) in a molar ratio that was 10 times the minimum Li amount required for ion exchange to obtain a mixture. Using an alumina crucible, the mixture was fired at 280°C for 1 hour in an air atmosphere to obtain a fired product. The salt remaining in the fired product was washed with pure water, and solid-liquid separation was performed by vacuum filtration to obtain a precipitate. The precipitate was dried overnight at 120°C to obtain positive electrode active material particles having an O2 type structure.

[0085] 3.4 Supplementary information on ion exchange conditions The ion exchange conditions for each of Examples 1 and 2, Comparative Examples 1 and 2, and Reference Example 1 are summarized in Table 2 below.

[0086] [Table 2]

[0087] 4. Observation of the external shape of positive electrode active material particles 6A to 6E show SEM images of the positive electrode active material particles of each of Examples 1 and 2, Comparative Examples 1 and 2, and Reference Example 1. FIG. 6A shows Example 1, FIG. 6B shows Example 2, FIG. 6C shows Comparative Example 1, FIG. 6D shows Comparative Example 2, and FIG. 6E shows Reference Example 1. As shown in FIGS. 6D and 6E, when plate-shaped P2 type particles were used, the positive electrode active material particles having an O2 type structure obtained after ion exchange were also plate-shaped. On the other hand, as shown in FIGS. 6A to 6C, when spherical P2 type particles were used, the positive electrode active material particles having an O2 type structure obtained after ion exchange were also spherical. The circularity of the positive electrode active material particles according to Example 1 was 0.83, the circularity of the positive electrode active material particles according to Example 2 was 0.81, and the circularity of the positive electrode active material particles according to Comparative Example 1 was 0.85. The plate-shaped O2 type positive electrode active material particles were substantially composed of one crystallite. On the other hand, the surface of the spherical O2 type positive electrode active material particles was composed of multiple crystallites, the diameter of the crystallites was less than 1 μm, and the crystallites had a first surface exposed on the particle surface, and the first surface was planar.

[0088] 5. Crystal structure of positive electrode active material particles X-ray diffraction measurements were performed on the positive electrode active material particles of each of Examples 1 and 2, Comparative Examples 1 and 2, and Reference Example 1. The results are shown in Fig. 7. As shown in Fig. 7, all of the positive electrode active material particles had an O2 type crystal structure.

[0089] 6. Elemental analysis of positive electrode active material particles An elemental analysis by ICP was carried out on each of the positive electrode active material particles of Examples 1 and 2, Reference Example 1, and Comparative Examples 1 and 2. The results are shown in Table 3 below.

[0090] [Table 3]

[0091] 7. Preparation of Cell for Evaluation Coin cells were produced using the positive electrode active material particles of each of Examples 1 and 2, Comparative Examples 1 and 2, and Reference Example 1. The coin cells were produced according to the following procedure. (1) Positive electrode active material particles, acetylene black (AB) as a conductive additive, and polyvinylidene fluoride (PVdF) as a binder were weighed out so that the mass ratio of positive electrode active material particles:AB:PVdF=85:10:5, and dispersed and mixed in N-methyl-2-pyrrolidone to obtain a positive electrode mixture slurry. The positive electrode mixture slurry was applied onto an aluminum foil and vacuum dried overnight at 120°C to obtain a positive electrode, which is a laminate of a positive electrode active material layer and a positive electrode current collector. (2) TDDK-217 (manufactured by Daikin Industries, Ltd.) was prepared as the electrolyte. (3) Metallic lithium foil was prepared as the negative electrode. (4) A coin cell (CR2032) was prepared using the positive electrode, electrolyte, and negative electrode.

[0092] 8.Charge / Discharge Characteristics Evaluation In a thermostatic chamber maintained at 25°C, the cells were charged at 0.1C (1C=270mA / g for Examples 1 and 2 and Reference Example 1, and 1C=220mA / g for Comparative Examples 1 and 2) in the voltage range of 2.0-4.8V, and then discharged at 0.5C, 1C, or 3C to measure the discharge capacity at each rate. The results of the initial charge / discharge curves are shown in Figures 8A to 8E. Figure 8A shows Example 1, Figure 8B shows Example 2, Figure 8C shows Comparative Example 1, Figure 8D shows Comparative Example 2, and Figure 8E shows Reference Example 1. The rate characteristics of each cell are shown in Figure 9.

[0093] 9. Evaluation Results The results shown in Table 3, FIGS. 6A to 6E, FIG. 7, FIGS. 8A to 8E, and FIG. 9 reveal the following. (1) As shown in Table 3 and FIG. 7, the positive electrode active material particles according to Examples 1 and 2 and Reference Example 1 have an O2-type structure and contain an excessive amount of Li (1.0 < a). On the other hand, the positive electrode active material particles according to Comparative Examples 1 and 2 have an O2-type structure and contain a small amount of Li (a < 0.7). For Examples 1 and 2 and Reference Example 1, since lithium hydroxide was used in combination with a lithium salt as the ion exchange material, ion exchange was promoted, and it is considered that Li-excessive positive electrode active material particles were obtained. (2) As shown in FIGS. 8A to 8E, the cells according to Examples 1 and 2 and Reference Example 1 have better initial charge capacity and initial discharge capacity than the cells according to Comparative Examples 1 and 2. The cells according to Examples 1 and 2 and Reference Example 1 are considered to have a higher initial charge capacity because the amount of Li that can be supplied to the negative electrode during the first charge is larger than that of the cells according to Comparative Examples 1 and 2. Further, when a < 0.7 as in Comparative Examples 1 and 2, it is considered that the elements whose valence changes during Li insertion (discharge) into the positive electrode active material are Ni, Mn, and Co. On the other hand, in the case of the Li-excessive positive electrode active material with 1.0 < a as in Examples 1 and 2 and Reference Example 1, it is considered that oxygen contributes in addition to Ni, Mn, and Co. Therefore, the cells according to Examples 1 and 2 and Reference Example 1 are considered to have a higher initial discharge capacity than the cells according to Comparative Examples 1 and 2. (3) As shown in FIG. 9, it can be seen that the cells according to Examples 1 and 2 have a smaller difference between the capacity at low-rate discharge and the capacity at high-rate discharge than the cells according to Reference Example 1, and can maintain a large capacity even during high-rate discharge. That is, the cells according to Examples 1 and 2 have better rate characteristics than the cells according to Reference Example 1. The spherical positive electrode active material particles according to Examples 1 and 2 (FIGS. 6A and 6B) are considered to have suppressed crystallite growth, smaller crystallites, reduced reaction resistance, and reduced diffusion resistance inside the active material compared to the plate-like positive electrode active material particles according to Reference Example 1 (FIG. 6E). Further, it is considered that the degree of bending is reduced by spheroidization, and the lithium ion conduction resistance in the layer constituting the positive electrode is reduced. As a result, it is considered that the rate characteristics are improved.

[0094] 10. Supplementary Furthermore, in the above embodiments, cathode active material particles having a specific chemical composition were exemplified. However, the chemical composition of the cathode active material particles of the present disclosure is not limited thereto. For example, the cathode active material particles may contain another element M other than Ni, Mn, and Co for the purpose of stabilizing the crystal structure or the like. The element M is as described above.

[0095] Also, in the above embodiments, the case of manufacturing the cathode active material particles at a specific ion exchange temperature and ion exchange time was exemplified. However, the ion exchange temperature and ion exchange time are not limited thereto. As far as the present inventors have confirmed, cathode active material particles having an O2-type crystal structure are more appropriately manufactured at an ion exchange temperature of 270°C or higher and 320°C or lower, and an ion exchange time of 1 hour or longer and 8 hours or shorter.

[0096] 11. Summary From the above embodiments, it can be said that the cathode active material particles satisfying the following requirements (1) to (3) have excellent rate characteristics and capacity. (1) The cathode active material particles have an O2-type structure. (2) The cathode active material particles are Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O2 (where 1.0 < a < 1.30, 0 ≤ b ≤ 0.20, x + y + z = 1, and 0 ≤ p + q + r ≤ 0.15, and M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W) and have a chemical composition represented by. (3) The cathode active material particles are spherical.

[0097] Also, from the above embodiments and reference examples, it can be said that the Li-excess type O2-type cathode active material particles can be manufactured by a method satisfying, for example, the following requirement (4). (4) A method for producing positive electrode active material particles includes obtaining Na-containing transition metal oxide particles having a P2 type structure, and contacting the Na-containing transition metal oxide particles with an ion exchange material to replace at least a portion of the Na in the Na-containing transition metal oxide particles with Li, thereby obtaining Li-containing transition metal oxide particles having an O2 type structure, wherein the ion exchange material contains lithium hydroxide and a lithium salt. [Explanation of symbols]

[0098] 100 Lithium-ion batteries 10 Positive electrode current collector 20 Cathode active material layer 30 Electrolyte layer 40 Negative electrode active material layer 50 Negative electrode current collector

Claims

1. Positive electrode active material particles, It has an O2 structure, Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O 2 (wherein 1.0<a<1.30, 0≦b≦0.20, x+y+z=1, and 0≦p+q+r≦0.15; and M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W), and It is spherical, Positive electrode active material particles.

2. The positive electrode active material particle according to claim 1 , The particle surface is composed of multiple crystallites. Positive electrode active material particles.

3. A method for producing positive electrode active material particles, comprising: Obtaining Na-containing transition metal oxide particles having a P2 type structure, and and bringing the Na-containing transition metal oxide particles into contact with an ion exchange material to replace at least a portion of the Na in the Na-containing transition metal oxide particles with Li, thereby obtaining Li-containing transition metal oxide particles having an O2 structure. the ion exchange material comprises lithium hydroxide and a lithium salt; Manufacturing method.

4. The method according to claim 3, The Na-containing transition metal oxide particles are spherical, and The Li-containing transition metal oxide particles are spherical. Manufacturing method.

5. The method according to claim 3, The Na-containing transition metal oxide particles are c Mn x-p Ni y-q Co z-r M p+q+r O 2 (wherein 0<c<0.70, x+y+z=1, and 0≦p+q+r≦0.15; and M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). Manufacturing method.

6. The method according to any one of claims 3 to 5, Obtaining precursor particles; coating the surface of the precursor particles with a Na salt to obtain coated particles; and and calcining the coated particles to obtain the Na-containing transition metal oxide particles. Manufacturing method.

7. The method according to claim 6, further comprising the steps of: and coating 40% or more by area of ​​the surface of the precursor particles with the Na salt to obtain the coated particles. The precursor particles are spherical. Manufacturing method.

8. A lithium ion battery having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, The positive electrode active material layer contains the positive electrode active material particles according to claim 1 or 2. Lithium-ion battery.

Citation Information

Patent Citations

  • Positive electrode active material for use in nonaqueous electrolyte secondary battery and method for manufacturing it

    JP2002313337A

  • Nonaqueous electrolyte secondary battery

    JP2016033887A

  • All-solid battery

    JP2019169365A

  • Positive electrode active material for nonaqueous electrolyte secondary batteries, and nonaqueous electrolyte secondary battery arranged by use thereof

    JP2014186937A