Method for manufacturing optical laminate with adhesive layer
The method of using a surface protection film to replace the release liner in optical laminate manufacturing addresses the issue of erroneous defect detection in VR goggles, ensuring high-quality production by preventing foreign matter adhesion and enhancing inspection accuracy.
Patent Information
- Application Number
- JP2023044632
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2043-03-20
AI Technical Summary
Optical laminates used in VR goggles require stricter defect control than conventional image display devices, and automated optical inspection (AOI) erroneously detects foreign matter on the release liner as defects due to adhesion, which cannot be visually identified.
A method for manufacturing optical laminates with an adhesive layer involves using a surface protection film to replace the release liner, ensuring foreign matter does not adhere to the surface during inspection, thereby preventing erroneous defect detection.
The method effectively suppresses the erroneous detection of defects during inspection, ensuring high-quality optical laminates are produced by protecting the adhesive layer with a surface protection film, thus maintaining the integrity of the manufacturing process.
Smart Images

Figure 2024134369000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a pressure-sensitive adhesive layer-attached optical laminate. [Background technology]
[0002] Image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices), are rapidly becoming widespread. In image display devices, optical members such as polarizing members and phase difference members are generally used to realize image display and to improve the performance of the image display (see, for example, Patent Document 1).
[0003] In recent years, new applications for image display devices have been developed. For example, goggles with displays (VR goggles) for realizing virtual reality (VR) have begun to be commercialized. In VR goggles, the image displayed on the display is enlarged for the viewer to view, so the optical members used in VR goggles require stricter defect management than the optical members used in conventional image display devices. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2021-103286 A Summary of the Invention [Problem to be solved by the invention]
[0005] In an optical laminate with a pressure-sensitive adhesive layer, which includes one or more optical components and has a pressure-sensitive adhesive layer on the outermost layer for bonding to adjacent components, the surface of the pressure-sensitive adhesive layer is generally protected by a release liner until it is used, and therefore the optical laminate with the release liner laminated thereon is inspected. On the other hand, as described above, for an optical laminate applied to goggles with a display, stricter defect management is required than before, and automated optical inspection (AOI) is used to detect defects of a size that cannot be visually recognized (scratches, stains, unevenness, foreign matter, etc.), for example, defects with a diameter of 80 μm or less, or for example, defects with a diameter of 50 μm or less. In this case, if a foreign matter is attached to the surface of the release liner, the foreign matter may be erroneously detected as a defect in the optical laminate with a pressure-sensitive adhesive layer in the AOI.
[0006] The present invention is directed to solving the above problems, and its main object is to provide a method for producing a pressure-sensitive adhesive layer-attached optical laminate that can suppress erroneous detection of defects in defect inspection. [Means for solving the problem]
[0007] [1] According to one aspect of the present invention, there is provided a method for producing an optical laminate with a pressure-sensitive adhesive layer, the optical laminate having an optical laminate and a pressure-sensitive adhesive layer disposed on one side thereof, the method comprising: step A of obtaining the optical laminate with a pressure-sensitive adhesive layer, in which a second release liner is disposed on the surface of the pressure-sensitive adhesive layer; and step B of inspecting the optical laminate with a pressure-sensitive adhesive layer in a state in which the second release liner is disposed on the surface of the pressure-sensitive adhesive layer, the step A comprising replacing the first release liner disposed on the surface of the pressure-sensitive adhesive layer with a release liner with a surface protective film having the second release liner and a surface protective film disposed on one side of the second release liner, and then peeling off the surface protective film. [2] In the manufacturing method of [1] above, step A may include step A-1a of preparing a first intermediate film having the pressure-sensitive adhesive layer and the first release liner disposed on the surface of the pressure-sensitive adhesive layer, step A-2a of peeling the first release liner from the first intermediate film and laminating the release liner with a surface protection film on the exposed pressure-sensitive adhesive layer to obtain a second intermediate film, step A-3a of laminating a third intermediate film on the side of the second intermediate film opposite to the side where the release liner with the surface protection film is disposed to obtain a fourth intermediate film, and step A-4a of peeling the surface protection film from the fourth intermediate film. [3] In the manufacturing method of [2] above, the first intermediate film may further have a polarizing member, and the third intermediate film may have a first λ / 4 member. [4] In the manufacturing method of [3] above, the first intermediate film may be produced by a method including preparing a laminate of the first release liner and the pressure-sensitive adhesive layer, and laminating the laminate with the polarizing member by the pressure-sensitive adhesive layer. [5] In the manufacturing method according to any one of [1] to [4] above, the peel force of the surface protection film from the second release liner (peel angle 180°, peel speed 300 mm / min) may be 0.005 N / 50 mm or more and 0.095 N / 50 mm or less. [6] In the manufacturing method according to any one of [1] to [5] above, the peel force X of the surface protection film from the second release liner (peel angle 180°, peel speed 300 mm / min) and the peel force Y of the second release liner from the pressure-sensitive adhesive layer (peel angle 180°, peel speed 300 mm / min) may satisfy the relationship of 0.2 < X / Y < 1. [7] In the manufacturing method according to any one of [1] to [6] above, the total light transmittance of the second release liner may be 80% or more. [8] In the manufacturing method according to any one of [1] to [7] above, the total light transmittance of the first release liner may be 95% or less. [9] In the manufacturing method according to any one of the above [1] to [8], the surface protective film may have a total light transmittance of 95% or less. Effect of the Invention
[0008] According to the manufacturing method of the pressure-sensitive adhesive layer-attached optical laminate according to the embodiment of the present invention, during the preparation of the pressure-sensitive adhesive layer-attached optical laminate, the first release liner protecting the pressure-sensitive adhesive layer is replaced with a release liner with a surface protective film, and only the surface protective film is peeled off and removed before inspection. This makes it possible to provide for inspection the pressure-sensitive adhesive layer-attached optical laminate in which the pressure-sensitive adhesive layer surface is protected by the second release liner to which adhesion of foreign matter is suppressed. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic diagram showing a general configuration of a display system according to an embodiment of the present invention. [Diagram 2] 2(a) and 2(b) are schematic cross-sectional views showing one example of a pressure-sensitive adhesive layer-attached optical laminate that can be used in the display system shown in FIG. 1. [Diagram 3] FIG. 2 is a schematic diagram illustrating one embodiment of step A. [Figure 4] FIG. 2 is a schematic diagram illustrating one embodiment of step A. [Diagram 5] FIG. 2 is a schematic diagram illustrating one embodiment of step B. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to these embodiments. In addition, in order to clarify the explanation, the width, thickness, shape, etc. of each part may be shown diagrammatically compared to the embodiment, but it is merely an example and does not limit the interpretation of the present invention. In addition, in this specification, "~" representing a numerical range includes the upper and lower limit numerical values, and "(meth)acrylic" means "acrylic and / or methacrylic".
[0011] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re(λ)=(nx-ny)×d, where d(nm) is the thickness of the layer (film). (3) Retardation in the thickness direction (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light of wavelength λ nm at 23° C. For example, "Rth(550)" is the retardation in the thickness direction measured with light of wavelength 550 nm at 23° C. Rth(λ) is calculated by the formula: Rth(λ)=(nx-nz)×d, where d(nm) is the thickness of the layer (film). (4) Nz coefficient The Nz coefficient is calculated by Nz=Rth / Re. (5)Angle When an angle is mentioned in this specification, the angle includes both clockwise and counterclockwise angles with respect to a reference direction. Thus, for example, "45°" means ±45°. In this specification, "substantially parallel" includes the case where the angle is within a range of 0°±10°, for example, within a range of 0°±5°, preferably within a range of 0°±3°, more preferably within a range of 0°±1°, and "substantially perpendicular" includes the case where the angle is within a range of 90°±10°, for example, within a range of 90°±5°, preferably within a range of 90°±3°, more preferably within a range of 90°±1°.
[0012] A. Display System According to one aspect of the present invention, a display system is provided. FIG. 1 is a schematic diagram showing a schematic configuration of a display system according to one embodiment of the present invention. FIG. 1 shows the arrangement and shape of each component of a display system 2. The display system 2 includes a display element 12, a reflective polarizing member 14, a first lens unit 16, a half mirror 18, a first phase difference member 20, a second phase difference member 22, and a second lens unit 24. The reflective polarizing member 14 is disposed in front of the display surface 12a side of the display element 12, and can reflect light emitted from the display element 12. The first lens unit 16 is disposed on the optical path between the display element 12 and the reflective polarizing member 14, and the half mirror 18 is disposed between the display element 12 and the first lens unit 16. The first phase difference member 20 is disposed on the optical path between the display element 12 and the half mirror 18, and the second phase difference member 22 is disposed on the optical path between the half mirror 18 and the reflective polarizing member 14. Although not shown, the display system 2 may further include an absorptive polarizing member between the reflective polarizing member 14 and the second lens portion 24 .
[0013] The display element 12 is, for example, a liquid crystal display or an organic EL display, and has a display surface 12a for displaying an image. The light emitted from the display surface 12a passes through, for example, a polarizing member 10 that may be included in the display element 12, and is converted into a first linearly polarized light.
[0014] The first phase difference member 20 includes a first λ / 4 member capable of converting a first linearly polarized light incident on the first phase difference member 20 into a first circularly polarized light. When the first phase difference member does not include any member other than the first λ / 4 member, the first phase difference member may correspond to the first λ / 4 member. In the illustrated example, a space is interposed between the first phase difference member 20 and the display element 12, but the first phase difference member 20 and the display element 12 may be provided integrally by using an optical laminate with a pressure-sensitive adhesive layer described in section B, for example.
[0015] The half mirror 18 transmits the light emitted from the display element 12 and reflects the light reflected by the reflective polarizing member 14 toward the reflective polarizing member 14. The half mirror 18 is provided integrally with the first lens portion 16.
[0016] The second phase difference member 22 includes a second λ / 4 member that can transmit light reflected by the reflective polarizing member 14 and the half mirror 18 through the reflective polarizing member 14. When the second phase difference member does not include any member other than the second λ / 4 member, the second phase difference member may correspond to the second λ / 4 member. The second phase difference member 22 may be provided integrally with the first lens portion 16.
[0017] The first circularly polarized light output from the first λ / 4 member included in the first phase difference member 20 passes through the half mirror 18 and the first lens unit 16, and is converted into the second linearly polarized light by the second λ / 4 member included in the second phase difference member 22. The second linearly polarized light output from the second λ / 4 member is reflected toward the half mirror 18 without passing through the reflective polarizing member 14. At this time, the polarization direction of the second linearly polarized light incident on the reflective polarizing member 14 is the same as the reflection axis of the reflective polarizing member 14. Therefore, the second linearly polarized light incident on the reflective polarizing member 14 is reflected by the reflective polarizing member 14.
[0018] The second linearly polarized light reflected by the reflective polarizing member 14 is converted into the second circularly polarized light by the second λ / 4 member included in the second phase difference member 22, and the second circularly polarized light output from the second λ / 4 member passes through the first lens unit 16 and is reflected by the half mirror 18. The second circularly polarized light reflected by the half mirror 18 passes through the first lens unit 16 and is converted into the third linearly polarized light by the second λ / 4 member included in the second phase difference member 22. The third linearly polarized light passes through the reflective polarizing member 14. At this time, the polarization direction of the third linearly polarized light incident on the reflective polarizing member 14 is the same as the transmission axis of the reflective polarizing member 14. Therefore, the third linearly polarized light incident on the reflective polarizing member 14 passes through the reflective polarizing member 14.
[0019] As described above, the display system 2 may include an absorption-type polarizing member (typically, an absorption-type polarizing film) in front of (the side closer to the eyes) the reflective polarizing member 14. The reflection axis of the reflective polarizing member 14 and the absorption axis of the absorption-type polarizing member may be arranged substantially parallel to each other. Thereby, the third linearly polarized light transmitted through the reflective polarizing member 14 can directly transmit through the absorption-type polarizing member. The reflective polarizing member and the absorption-type polarizing member may be laminated, for example, via an adhesive layer.
[0020] The light transmitted through the reflective polarizing member 14 passes through the second lens unit 24 and enters the user's eye 26.
[0021] For example, the absorption axis of the polarizing member 10 included in the display element 12 and the reflection axis of the reflective polarizing member 14 may be arranged substantially parallel to each other or substantially orthogonally to each other. The angle formed by the absorption axis of the polarizing member 10 included in the display element 12 and the slow axis of the first λ / 4 member included in the first retardation member 20 is, for example, 40° to 50°, may be 42° to 48°, or may be about 45°. The angle formed by the absorption axis of the polarizing member included in the display element 12 and the slow axis of the second λ / 4 member included in the second retardation member 22 is, for example, 40° to 50°, may be 42° to 48°, or may be about 45°.
[0022] The in-plane retardation Re(550) of the first λ / 4 member is, for example, 100 nm to 190 nm, may be 110 nm to 180 nm, may be 130 nm to 160 nm, or may be 135 nm to 155 nm. The first λ / 4 member preferably exhibits an inverse-dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light. The first λ / 4 member preferably satisfies the relationship of Re(450) < Re(550) < Re(650). Re(450) / Re(550) of the second λ / 4 member is, for example, 0.75 or more and less than 1, and may be 0.8 or more and 0.95 or less.
[0023] The in-plane phase difference Re(550) of the second λ / 4 member is, for example, from 100 nm to 190 nm, may be from 110 nm to 180 nm, may be from 130 nm to 160 nm, or may be from 135 nm to 155 nm. The second λ / 4 member preferably exhibits an inverse-dispersion wavelength characteristic in which the phase difference value increases according to the wavelength of the measurement light. The second λ / 4 member preferably satisfies the relationship Re(450) < Re(550) < Re(650). Re(450) / Re(550) of the second λ / 4 member is, for example, 0.75 or more and less than 1, and may be 0.8 or more and 0.95 or less.
[0024] B. Optical laminate with an adhesive layer According to another aspect of the present invention, an optical laminate with an adhesive layer is provided. The optical laminate with an adhesive layer according to an embodiment of the present invention can be used for the display system described in section A. FIGS. 2(a) and (b) are schematic cross-sectional views showing a schematic configuration of an example of the optical laminate with an adhesive layer.
[0025] The optical laminate 200a with an adhesive layer illustrated in FIG. 2(a) includes an optical laminate 100a including a polarizing member 10, a first retardation member 20, and a protective member 30 in this order, and an adhesive layer 110 disposed on the surface of the polarizing member 10 side. In the optical laminate 100a, the first retardation member 20 includes only the first λ / 4 member 20a as the retardation member. Therefore, the first retardation member 20 corresponds to the first λ / 4 member. The polarizing member 10 can correspond to the polarizing member included in the display element (for example, a liquid crystal display or an organic EL display) of the display system described in section A. Therefore, the angle formed by the absorption axis of the polarizing member 10 and the slow axis of the first λ / 4 member 20a is, as described above, for example, from 40° to 50°, may be from 42° to 48°, or may be about 45°. The polarizing member 10, the first retardation member 20, and the protective member 30 are laminated via an adhesive layer (not shown). The adhesive layer is typically an adhesive layer or a pressure-sensitive adhesive layer, and preferably a pressure-sensitive adhesive layer. The thickness of the adhesive layer is, for example, from 0.05 μm to 30 μm.
[0026] The pressure-sensitive adhesive layer-attached optical laminate 200b illustrated in FIG. 2(b) includes an optical laminate 100b including a polarizing member 10, a first phase difference member 20, and a protective member 30 in this order, and a pressure-sensitive adhesive layer 110 disposed on the polarizing member 10 side surface. The pressure-sensitive adhesive layer-attached optical laminate 200b is different from the pressure-sensitive adhesive layer-attached optical laminate 200a in that the first phase difference member 20 includes a member (so-called positive C plate) 20b whose refractive index characteristics can show the relationship nz>nx=ny in addition to the first λ / 4 member 20a. The first λ / 4 member 20a and the positive C plate 20b are typically laminated via an adhesive layer (not shown). As illustrated in the example, it is preferable that the first λ / 4 member 20a is located closer to the polarizing member 10 than the first positive C plate 20b, but the arrangement of these may be reversed.
[0027] A second release liner 320 is temporarily attached to the surface of the pressure-sensitive adhesive layer-attached optical laminates 200a, 200b on the side of the pressure-sensitive adhesive layer 110. The second release liner 320 is peeled off from the pressure-sensitive adhesive layer-attached optical laminates 200a, 200b, and the pressure-sensitive adhesive layer-attached optical laminates 200a, 200b are attached to a member constituting the display element 12 by the exposed pressure-sensitive adhesive layer 110, whereby a display system 2 in which the display element 12 and the first retardation member 20 are integrated can be obtained.
[0028] As shown in the illustrated example, a second surface protective film 360 may be further temporarily attached to the surface of the pressure-sensitive adhesive layer-attached optical laminates 200a, 200b facing the protective member 30. This makes it possible to suitably protect the surface of the pressure-sensitive adhesive layer-attached optical laminates 200a, 200b facing the protective member 30.
[0029] The thickness of the optical laminates 100a and 100b is, for example, 50 μm or more and 500 μm or less, and preferably 100 μm or more and 200 μm or less.
[0030] Hereinafter, each member constituting the pressure-sensitive adhesive layer-attached optical laminate will be specifically described.
[0031] <Polarizing materials> The polarizing member 10 is typically an absorptive polarizing member including a resin film (sometimes referred to as an absorptive polarizing film) containing a dichroic material, and may further include a protective layer on one or both sides thereof as necessary. The protective layer is typically attached to the absorptive polarizing film via any suitable adhesive layer. A typical example of the adhesive forming the adhesive layer is an ultraviolet-curing adhesive.
[0032] The crossed transmittance (Tc) of the polarizing member (absorptive polarizing film) is preferably 0.5% or less, more preferably 0.1% or less, and even more preferably 0.05% or less. The single transmittance (Ts) of the polarizing member (absorptive polarizing film) is, for example, 41.0% to 45.0%, and preferably 42.0% or more. The degree of polarization (P) of the polarizing member (absorptive polarizing film) is, for example, 99.0% to 99.997%, and preferably 99.9% or more.
[0033] The crossed transmittance, single transmittance and degree of polarization can be measured, for example, using an ultraviolet-visible spectrophotometer. The degree of polarization P can be calculated from the obtained Tp and Tc by measuring the single transmittance Ts, parallel transmittance Tp and crossed transmittance Tc using an ultraviolet-visible spectrophotometer, using the following formula. Note that Ts, Tp and Tc are Y values measured using a 2-degree visual field (C light source) according to JIS Z8701 and corrected for visibility. Polarization degree P(%)={(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100
[0034] The thickness of the absorptive polarizing film is, for example, 1 μm or more and 20 μm or less, optionally 2 μm or more and 15 μm or less, optionally 12 μm or less, optionally 10 μm or less, optionally 8 μm or less, or optionally 5 μm or less.
[0035] The absorptive polarizing film may be prepared from a single layer of resin film, or may be prepared using a laminate of two or more layers.
[0036] When preparing from a single-layer resin film, for example, an absorptive polarizing film can be obtained by subjecting a hydrophilic polymer film such as a polyvinyl alcohol (PVA)-based film, a partially formalized PVA-based film, or an ethylene-vinyl acetate copolymer-based partially saponified film to a dyeing treatment with a dichroic substance such as iodine or a dichroic dye, a stretching treatment, etc. Among them, an absorptive polarizing film obtained by dyeing a PVA-based film with iodine and uniaxially stretching it is preferable.
[0037] The dyeing with iodine is carried out, for example, by immersing the PVA film in an aqueous iodine solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching may be carried out after the dyeing treatment or while the dyeing is being carried out. Alternatively, the stretching may be followed by dyeing. If necessary, the PVA film is subjected to a swelling treatment, a crosslinking treatment, a washing treatment, a drying treatment, or the like.
[0038] Examples of the laminate produced using the laminate of two or more layers include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate. The absorptive polarizing film obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate can be produced, for example, by coating a PVA-based resin solution on the resin substrate and drying the resin substrate to form a PVA-based resin layer on the resin substrate to obtain a laminate of the resin substrate and the PVA-based resin layer; and stretching and dyeing the laminate to make the PVA-based resin layer into an absorptive polarizing film. In this embodiment, preferably, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is formed on one side of the resin substrate. The stretching typically includes immersing the laminate in an aqueous boric acid solution to stretch it. Furthermore, the stretching may further include, as necessary, stretching the laminate in air at a high temperature (for example, 95° C. or higher) before stretching in the aqueous boric acid solution. In addition, in this embodiment, the laminate is preferably subjected to a drying shrinkage treatment in which the laminate is heated while being transported in the longitudinal direction, thereby shrinking the laminate by 2% or more in the width direction. Typically, the manufacturing method of this embodiment includes subjecting the laminate to an air-assisted stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order. By introducing the auxiliary stretching, even when PVA is applied onto a thermoplastic resin, it is possible to increase the crystallinity of PVA, and to achieve high optical properties. At the same time, by increasing the orientation of PVA in advance, problems such as a decrease in the orientation or dissolution of PVA when immersed in water in the subsequent dyeing and stretching steps can be prevented, and high optical properties can be achieved. Furthermore, when the PVA-based resin layer is immersed in a liquid, the disorder of the orientation of polyvinyl alcohol molecules and the decrease in the orientation can be suppressed compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of the absorptive polarizing film obtained through treatment steps in which the laminate is immersed in a liquid, such as a dyeing treatment and an underwater stretching treatment. Furthermore, the optical properties can be improved by shrinking the laminate in the width direction through drying shrinkage treatment.The obtained laminate of resin substrate / absorptive polarizing film may be used as it is (i.e., the resin substrate may be used as a protective layer for the absorptive polarizing film), or any suitable protective layer may be laminated on the peeled surface of the resin substrate / absorptive polarizing film laminate after peeling the resin substrate from the laminate, or on the surface opposite to the peeled surface, depending on the purpose. Details of the method for producing such an absorptive polarizing film are described in, for example, JP2012-73580A and JP6470455A. The entire disclosures of these publications are incorporated herein by reference.
[0039] The protective layer is formed of any suitable film that can be used as a protective layer for an absorptive polarizing film. Specific examples of materials that are the main components of the film include cycloolefin (COP) resins such as polynorbornene resins, polyester resins such as polyethylene terephthalate (PET) resins, cellulose resins such as triacetyl cellulose (TAC), transparent resins such as polycarbonate (PC), (meth)acrylic resins, polyvinyl alcohol resins, polyamides, polyimides, polyethersulfones, polysulfones, polystyrenes, polyolefins, and acetate resins. In addition, thermosetting resins or ultraviolet curing resins such as (meth)acrylic resins, urethane resins, (meth)acrylic urethane resins, epoxy resins, and silicone resins are also included. Note that "(meth)acrylic resin" refers to acrylic resins and / or methacrylic resins. In addition, glassy polymers such as siloxane polymers are also included. In addition, the polymer films described in JP 2001-343529 A (WO01 / 37007) can also be used. The material of this film can be, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain, such as a resin composition having an alternating copolymer of isobutene and N-methylmaleimide and an acrylonitrile-styrene copolymer. The polymer film can be, for example, an extrusion molded product of the above resin composition. The materials of the resin film can be used alone or in combination.
[0040] The thickness of the protective layer is typically 100 μm or less, for example, 5 μm to 80 μm, preferably 10 μm to 50 μm, and more preferably 15 μm to 35 μm.
[0041] <First λ / 4 member> The in-plane retardation Re(550) of the first λ / 4 member 20a is, for example, 100 nm to 190 nm, may be 110 nm to 180 nm, may be 130 nm to 160 nm, or may be 135 nm to 155 nm. The first λ / 4 member preferably exhibits an inverse-dispersion wavelength characteristic in which the retardation value increases with the wavelength of the measurement light. Re(450) / Re(550) of the first λ / 4 member is, for example, 0.75 or more and less than 1, and may be 0.8 or more and 0.95 or less.
[0042] The first λ / 4 member preferably exhibits a refractive index characteristic of nx > ny ≧ nz. Here, "ny = nz" includes not only the case where ny and nz are exactly equal but also the case where they are substantially equal. Therefore, within a range that does not impair the effects of the present invention, ny < nz may occur. The Nz coefficient of the first λ / 4 member is preferably 0.9 to 3, more preferably 0.9 to 2.5, still more preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.
[0043] The first λ / 4 member is formed of any suitable material that can satisfy the above characteristics. The first λ / 4 member can be, for example, a stretched film of a resin film or an alignment cured layer of a liquid crystal compound.
[0044] Examples of the resin contained in the resin film include polycarbonate-based resins, polyester carbonate-based resins, polyester-based resins, polyvinyl acetal-based resins, polyarylate-based resins, cyclic olefin-based resins, cellulose-based resins, polyvinyl alcohol-based resins, polyamide-based resins, polyimide-based resins, polyether-based resins, polystyrene-based resins, and acrylic-based resins. These resins may be used alone or in combination. Examples of methods for combining include blending and copolymerization. When the first λ / 4 member exhibits reverse dispersion wavelength characteristics, a resin film containing a polycarbonate-based resin or a polyester carbonate-based resin (hereinafter, sometimes simply referred to as a polycarbonate-based resin) may be suitably used.
[0045] Any suitable polycarbonate-based resin can be used as the polycarbonate-based resin. For example, the polycarbonate-based resin contains a structural unit derived from a fluorene-based dihydroxy compound, a structural unit derived from an isosorbide-based dihydroxy compound, and a structural unit derived from at least one dihydroxy compound selected from the group consisting of alicyclic diol, alicyclic dimethanol, di-, tri- or polyethylene glycol, and alkylene glycol or spiro glycol. Preferably, the polycarbonate-based resin contains a structural unit derived from a fluorene-based dihydroxy compound, a structural unit derived from an isosorbide-based dihydroxy compound, a structural unit derived from an alicyclic dimethanol and / or a structural unit derived from a di-, tri- or polyethylene glycol; more preferably, it contains a structural unit derived from a fluorene-based dihydroxy compound, a structural unit derived from an isosorbide-based dihydroxy compound, and a structural unit derived from a di-, tri- or polyethylene glycol. The polycarbonate-based resin may contain a structural unit derived from another dihydroxy compound as necessary. Details of polycarbonate-based resins that can be suitably used for the first λ / 4 member and methods for forming the first λ / 4 member are described, for example, in JP 2014-10291 A, JP 2014-26266 A, JP 2015-212816 A, JP 2015-212817 A, and JP 2015-212818 A, and the descriptions in these publications are incorporated herein by reference.
[0046] The thickness of the first λ / 4 member made of a stretched resin film is, for example, 10 μm to 100 μm, preferably 10 μm to 70 μm, and more preferably 20 μm to 60 μm.
[0047] The above-mentioned liquid crystal compound alignment solidified layer is a layer in which the liquid crystal compound is aligned in a predetermined direction within the layer, and the alignment state is fixed. The "alignment solidified layer" is a concept that includes an alignment solidified layer obtained by hardening a liquid crystal monomer as described later. In the first λ / 4 member, typically, rod-shaped liquid crystal compounds are aligned in the slow axis direction of the first λ / 4 member (homogeneous alignment). Examples of rod-shaped liquid crystal compounds include liquid crystal polymers and liquid crystal monomers. The liquid crystal compound is preferably polymerizable. If the liquid crystal compound is polymerizable, the alignment state of the liquid crystal compound can be fixed by aligning the liquid crystal compound and then polymerizing it.
[0048] The alignment solidified layer of the liquid crystal compound (liquid crystal alignment solidified layer) can be formed by performing an alignment treatment on the surface of a predetermined substrate, applying a coating liquid containing a liquid crystal compound to the surface to align the liquid crystal compound in a direction corresponding to the alignment treatment, and fixing the alignment state. Any appropriate alignment treatment can be adopted as the alignment treatment. Specifically, mechanical alignment treatment, physical alignment treatment, and chemical alignment treatment can be mentioned. Specific examples of mechanical alignment treatment include rubbing treatment and stretching treatment. Specific examples of physical alignment treatment include magnetic field alignment treatment and electric field alignment treatment. Specific examples of chemical alignment treatment include oblique deposition method and photoalignment treatment. As the treatment conditions of various alignment treatments, any appropriate conditions can be adopted depending on the purpose.
[0049] The alignment of the liquid crystal compound is performed by treating the liquid crystal compound at a temperature at which the liquid crystal compound exhibits a liquid crystal phase according to the type of liquid crystal compound. By performing such temperature treatment, the liquid crystal compound takes on a liquid crystal state and is aligned according to the alignment treatment direction of the substrate surface.
[0050] In one embodiment, the alignment state is fixed by cooling the liquid crystal compound aligned as described above. When the liquid crystal compound is polymerizable or crosslinkable, the alignment state is fixed by subjecting the liquid crystal compound aligned as described above to a polymerization treatment or crosslinking treatment.
[0051] As the liquid crystal compound, any suitable liquid crystal polymer and / or liquid crystal monomer is used. The liquid crystal polymer and the liquid crystal monomer may be used alone or in combination. Specific examples of the liquid crystal compound and the method for producing the liquid crystal alignment solidified layer are described in, for example, JP 2006-163343 A, JP 2006-178389 A, and WO 2018 / 123551 A. The descriptions in these publications are incorporated herein by reference.
[0052] The thickness of the first λ / 4 member constituted by the liquid crystal alignment solidified layer is, for example, 1 μm to 10 μm, preferably 1 μm to 8 μm, more preferably 1 μm to 6 μm, and further preferably 1 μm to 4 μm.
[0053] <Positive C plate> The positive C plate 20b has a thickness direction retardation Rth(550) of preferably -50 nm to -300 nm, more preferably -70 nm to -250 nm, further preferably -90 nm to -200 nm, and particularly preferably -100 nm to -180 nm. Here, "nx=ny" includes not only the case where nx and ny are strictly equal, but also the case where nx and ny are substantially equal. The positive C plate has an in-plane retardation Re(550) of, for example, less than 10 nm.
[0054] The positive C plate may be formed of any suitable material. The positive C plate is preferably composed of a film containing a liquid crystal material fixed in homeotropic alignment. The liquid crystal material (liquid crystal compound) that can be homeotropically aligned may be a liquid crystal monomer or a liquid crystal polymer. Specific examples of such liquid crystal compounds and methods for forming a positive C plate include the liquid crystal compounds and methods for forming a retardation layer described in
[0020] to
[0028] of JP-A-2002-333642. In this case, the thickness of the positive C plate is preferably 0.5 μm to 5 μm.
[0055] <Protective materials> The protective member 30 typically includes a substrate. The substrate may be made of any appropriate film. Examples of materials that are the main components of the film that constitutes the substrate include cellulose-based resins such as triacetyl cellulose (TAC), polyester-based, polyvinyl alcohol-based, polycarbonate-based, polyamide-based, polyimide-based, polyethersulfone-based, polysulfone-based, polystyrene-based, cycloolefin-based such as polynorbornene, polyolefin-based, (meth)acrylic-based, acetate-based, and other resins. The thickness of the substrate is preferably 5 μm to 80 μm, more preferably 10 μm to 40 μm, and further preferably 15 μm to 35 μm.
[0056] The protective member preferably has a substrate and a surface treatment layer formed on the substrate. The protective member having the surface treatment layer may be arranged so that the surface treatment layer is located on the front side. Specifically, the surface treatment layer may be located on the outermost surface of the optical laminate. The surface treatment layer may have any appropriate function. Examples of the surface treatment layer include a hard coat layer, an anti-reflection layer, an anti-sticking layer, and an anti-glare layer. The protective member may have two or more surface treatment layers.
[0057] The antireflection layer is provided to prevent reflection of external light and the like. Examples of the antireflection layer include a fluororesin layer, a resin layer containing nanoparticles (typically hollow nanoparticles, e.g., hollow nanosilica particles), and an antireflection layer having a nanostructure (e.g., a moth-eye structure). The thickness of the antireflection layer is preferably 0.05 μm to 1 μm. Examples of methods for forming the resin layer include a sol-gel method, a heat curing method using an isocyanate, and an ionizing radiation curing method (typically a photocuring method) using a crosslinkable monomer (e.g., a polyfunctional acrylate) and a photopolymerization initiator. In one embodiment, the antireflection layer is provided on the outermost surface of the protective member. According to an embodiment in which the antireflection layer is provided on the outermost surface of the protective member, an excellent antireflection effect can be obtained in a display system in which a space is formed between the half mirror 18 and the first phase difference member 20.
[0058] The hard coat layer preferably has sufficient surface hardness, excellent mechanical strength, and excellent light transmittance. The hard coat layer may be formed from any suitable resin. The hard coat layer is typically formed from an ultraviolet curing resin. Examples of the ultraviolet curing resin include polyester, acrylic, urethane, amide, silicone, and epoxy resins. The thickness of the hard coat layer is, for example, 0.5 μm or more, preferably 1 μm or more, for example, 20 μm or less, preferably 15 μm or less.
[0059] <Adhesive layer> The adhesive layer 110 is composed of any appropriate adhesive. The adhesive constituting the adhesive layer 110 typically contains a (meth)acrylic polymer, a urethane polymer, a silicone polymer, or a rubber polymer as a base polymer. Preferably, the adhesive is a (meth)acrylic adhesive containing a (meth)acrylic polymer as a main component.
[0060] The (meth)acrylic polymer contains a structural unit derived from an alkyl (meth)acrylate. The content of the structural unit derived from an alkyl (meth)acrylate in the (meth)acrylic polymer is typically 50% by weight or more, for example 80% by weight or more, preferably 90% by weight or more, more preferably 93% by weight or more, and for example 100% by weight or less, preferably 98% by weight or less.
[0061] The alkyl group of the alkyl (meth)acrylate may be linear or branched. The number of carbon atoms of the alkyl group is, for example, 1 or more and 18 or less. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a 2-ethylhexyl group, a decyl group, an isodecyl group, and an octadecyl group. The alkyl (meth)acrylate may be used alone or in combination. The average number of carbon atoms of the alkyl group is preferably 3 to 10.
[0062] The (meth)acrylic polymer may contain a structural unit derived from a copolymerizable monomer polymerizable with the alkyl (meth)acrylate, in addition to the structural unit derived from the alkyl (meth)acrylate. Examples of the copolymerizable monomer include a carboxyl group-containing monomer, a hydroxyl group-containing monomer, and a nitrogen-containing monomer. The copolymerizable monomer may be used alone or in combination.
[0063] The carboxyl group-containing monomer is a compound that contains a carboxyl group in its structure and a polymerizable unsaturated double bond such as a (meth)acryloyl group or a vinyl group. Examples of the carboxyl group-containing monomer include (meth)acrylic acid, carboxyethyl (meth)acrylate, maleic acid, fumaric acid, and crotonic acid, and preferably (meth)acrylic acid. When the (meth)acrylic polymer contains a structural unit derived from a carboxyl group-containing monomer, the adhesive properties of the pressure-sensitive adhesive layer can be improved. When the (meth)acrylic polymer contains a structural unit derived from a carboxyl group-containing monomer, the content of the structural unit derived from the carboxyl group-containing monomer in the (meth)acrylic polymer is preferably 0.01% by weight or more and 10% by weight or less.
[0064] The hydroxyl group-containing monomer is a compound that contains a hydroxyl group in its structure and a polymerizable unsaturated double bond such as a (meth)acryloyl group or a vinyl group. Examples of the hydroxyl group-containing monomer include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methyl acrylate, preferably 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate, and more preferably 2-hydroxyethyl (meth)acrylate. When the (meth)acrylic polymer contains a structural unit derived from a hydroxyl group-containing monomer, the durability of the adhesive layer can be improved. When the (meth)acrylic polymer contains a structural unit derived from a hydroxyl group-containing monomer, the content ratio of the structural unit derived from the hydroxyl group-containing monomer in the (meth)acrylic polymer is preferably 0.01% by weight or more and 10% by weight or less.
[0065] Examples of the nitrogen-containing monomer include nitrogen-containing vinyl monomers and cyanoacrylate monomers. Examples of the nitrogen-containing vinyl monomer include N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, (meth)acryloylmorpholine, N-vinyl carboxylic acid amides, and N-vinylcaprolactam. Examples of the cyanoacrylate monomer include acrylonitrile and methacrylonitrile. When the (meth)acrylic polymer contains a structural unit derived from a nitrogen-containing monomer, the content ratio of the structural unit derived from the nitrogen-containing monomer in the (meth)acrylic polymer is preferably 0.01% by weight or more and 10% by weight or less.
[0066] The weight average molecular weight Mw of the (meth)acrylic polymer is, for example, 1,000,000 to 3,000,000, and preferably 1,200,000 to 2,500,000.
[0067] The content of the (meth)acrylic polymer in the pressure-sensitive adhesive is, for example, 50% by weight or more, preferably 60% by weight or more, more preferably 70% by weight or more, and even more preferably 80% by weight or more, in terms of solid content. The upper limit of the content can be, for example, 99.9% by weight or less, preferably 99.8% by weight or less.
[0068] The (meth)acrylic adhesive may contain a crosslinking agent. Representative examples of the crosslinking agent include organic crosslinking agents and polyfunctional metal chelates, and preferably organic crosslinking agents. Examples of the organic crosslinking agent include isocyanate crosslinking agents, peroxide crosslinking agents, epoxy crosslinking agents, and imine crosslinking agents, and more preferably isocyanate crosslinking agents. When the adhesive contains a crosslinking agent, the content of the crosslinking agent is usually 0.01 parts by weight or more and 15 parts by weight or less, for example 0.1 parts by weight or more and 10 parts by weight or less, based on 100 parts by weight of the (meth)acrylic polymer.
[0069] The (meth)acrylic pressure-sensitive adhesive may contain, as necessary, a solvent or various additives, such as a polymerization initiator, a polymerization catalyst, a crosslinking catalyst, a silane coupling agent, a tackifier, a plasticizer, a softener, an anti-degradation agent, a filler, a colorant, an ultraviolet absorber, an antioxidant, a surfactant, an antistatic agent, etc., within a range that does not impair the properties of the present invention.
[0070] The thickness of the pressure-sensitive adhesive layer 110 is, for example, 12 μm or more, preferably 15 μm or more, and, for example, 100 μm or less, preferably 80 μm or less.
[0071] C. Method for producing pressure-sensitive adhesive layer-attached optical laminate According to another aspect of the present invention, there is provided a method for producing a pressure-sensitive adhesive layer-attached optical laminate. According to the method for producing a pressure-sensitive adhesive layer-attached optical laminate according to an embodiment of the present invention, the pressure-sensitive adhesive layer-attached optical laminate described in section B can be suitably produced. A method for producing a pressure-sensitive adhesive layer-attached optical laminate according to an embodiment of the present invention includes the steps of: A step A of obtaining a pressure-sensitive adhesive layer-attached optical laminate in which a second release liner is disposed on the surface of the pressure-sensitive adhesive layer; and A step B of inspecting the pressure-sensitive adhesive layer-attached optical laminate in a state in which the second release liner is disposed on the surface of the pressure-sensitive adhesive layer; Including, Step A includes replacing a first release liner disposed on the surface of the pressure-sensitive adhesive layer with a release liner with a surface protective film having a second release liner and a surface protective film disposed on one side of the second release liner, and then peeling off the surface protective film. According to the manufacturing method of a pressure-sensitive adhesive layer-attached optical laminate according to an embodiment of the present invention, step A includes replacing the first release liner with the second release liner, and the second release liner can be protected with a surface protective film until immediately before step B. As a result, foreign matter adhering to the release liner surface is prevented from being erroneously detected as a defect in the pressure-sensitive adhesive layer-attached optical laminate in the inspection in step B, and a high-quality pressure-sensitive adhesive layer-attached optical laminate can be suitably manufactured. In this specification, a release liner is a film that does not itself have adhesiveness and is placed (laminated) on the surface of an adhesive layer to protect the adhesive layer, and a surface protection film is a film that has at least one adhesive surface and is attached to an adherend by means of the adhesive surface to protect the adherend.
[0072] C-1. Process A In step A, a pressure-sensitive adhesive layer-attached optical layered body is obtained in which a second release liner is disposed on the surface of the pressure-sensitive adhesive layer. FIG. In the embodiment shown in FIG. 3, step A comprises: A step A-1a of preparing a first intermediate film 410 having a pressure-sensitive adhesive layer 110 and a first release liner 310 disposed on the surface of the pressure-sensitive adhesive layer 110; A step A-2a of peeling the first release liner 310 from the first intermediate film 410 and bonding a release liner with a surface protective film 350 having a second release liner 320 and a surface protective film 330 disposed on one side of the second release liner 320 to the exposed pressure-sensitive adhesive layer 110 to obtain a second intermediate film 420; A step A-3a of laminating a third intermediate film 430 on the side of the second intermediate film 420 opposite to the side on which the release liner 350 with the surface protective film is disposed to obtain a fourth intermediate film 440; and A step A-4a of peeling the surface protective film 330 from the fourth intermediate film 440; Includes. In one embodiment, the first intermediate film and the second intermediate film may be formed in a long shape. The long second intermediate film may be cut or punched to a predetermined size before the step A-3a to form a sheet film, and then, in the step A-3a, may be laminated with the third intermediate film, which is also a sheet film. This embodiment is preferable in that when the first intermediate film has a polarizing member and the third intermediate film has a first λ / 4 member, it is easy to precisely control the axial relationship between the two. In addition, in this embodiment, foreign matter is likely to adhere to the surface protective film when cutting or punching into a sheet film, but by peeling and removing the surface protective film in the step A-4a, it is possible to suitably prevent the introduction of foreign matter into the inspection in the step B. In addition, in this specification, "long shape" means an elongated shape whose length is sufficiently long relative to the width, and includes, for example, an elongated shape whose length is 10 times or more, preferably 20 times or more, relative to the width.
[0073] C-1-1. Process A-1a In step A-1a, a first intermediate film having an adhesive layer and a first release liner disposed on the surface of the adhesive layer is prepared. As shown in FIG. 3(a), the first intermediate film 410 may have a polarizing member 10, an adhesive layer 110, and a first release liner 310 in this order. The polarizing member and the adhesive layer are as described in section B. The first intermediate film may contain other members as long as the effects of the present invention are obtained.
[0074] The first release liner 310 protects the adhesive layer 110. The first release liner 310 is formed of any suitable resin film. Specific examples of the resin that is the main component of the resin film include polyolefin, polyester, acrylic, polyamide, polyimide, polyvinyl chloride, polyvinylidene chloride, cellulose, modified cellulose, polystyrene, and polycarbonate. Examples of polyolefin include polyethylene, polypropylene, cycloolefin polymer (COP), poly-1-butene, poly-4-methyl-1-pentene, ethylene-propylene copolymer, ethylene-1-butene copolymer, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-vinyl alcohol copolymer. Examples of polyester include polyethylene terephthalate (PET), polyethylene naphthalate, and polybutylene terephthalate. Examples of polyamide include polyamide 6, polyamide 6,6, and partially aromatic polyamide. Examples of modified cellulose include triacetyl cellulose (TAC). From the viewpoint of obtaining heat resistance that can withstand the application and drying of the adhesive, the resin film preferably contains PET, COP, etc. The materials of the resin film can be used alone or in combination. In addition, the resin film may contain a filler from the viewpoint of improving heat resistance, mechanical strength, etc.
[0075] A release treatment layer may be provided on the surface of the first release liner 310 that comes into contact with the pressure-sensitive adhesive layer 110. Examples of release treatment agents that form the release treatment layer include silicone-based release treatment agents, fluorine-based release treatment agents, and long-chain alkyl acrylate-based release treatment agents. The release treatment agents may be used alone or in combination. The thickness of the release treatment layer is typically 50 nm or more and 400 nm or less.
[0076] The thickness of the first release liner 310 is typically 5 μm or more, preferably 20 μm or more, and typically 60 μm or less, preferably 45 μm or less. When a release treatment layer is provided, the thickness of the first release liner includes the thickness of the release treatment layer.
[0077] The first release liner 310 does not need to have high transparency because it is peeled off and removed before inspection. The total light transmittance of the first release liner may be, for example, 95% or less, or, for example, 90% or less or 80% or less, with no particular lower limit and, for example, 50% or more.
[0078] The peel force of first release liner 310 from adhesive layer 110 (peel angle 180°, peel speed 300 mm / min) is, for example, 0.001 N / 50 mm or more, preferably 0.004 N / 50 mm or more, and for example, 0.5 N / 50 mm or less, preferably 0.1 N / 50 mm or less.
[0079] The first intermediate film 410 can be obtained by any suitable method. In one embodiment, the first intermediate film 410 can be obtained by a method including preparing a laminate of the first release liner 310 and the adhesive layer 110, and bonding the laminate to the polarizing member 10 with the adhesive layer 110. For example, the adhesive layer 110 is formed by applying an adhesive to the first release liner 310 and drying the applied layer, and the laminate of the first release liner 310 and the adhesive layer 110 thus obtained is bonded to the polarizing member 10 with the adhesive layer 110 to obtain the first intermediate film 410. Also, for example, the adhesive layer 110 can be formed by applying an adhesive to a substrate and drying the applied layer, and the adhesive layer 110 can be formed by transferring the adhesive to the first release liner 310 and then bonding the polarizing member 10 to the first intermediate film 410.
[0080] The drying temperature of the coating layer is preferably 40°C or higher, for example 50°C or higher, 70°C or higher, 100°C or higher, or 130°C or higher, for example 200°C or lower. The drying time is, for example, 5 seconds or higher, preferably 10 seconds or higher, for example 1200 seconds or lower. When the adhesive contains a crosslinking agent, the crosslinking reaction can be sufficiently advanced during the drying. When the adhesive layer is formed by applying the adhesive to a release liner with a surface protective film, the surface protective film may be deteriorated (denatured, deformed, etc.) by heat during drying. In contrast, according to the method for producing an optical laminate with an adhesive layer according to an embodiment of the present invention, the release liner with a surface protective film is bonded to the adhesive layer separately formed on the substrate (for example, the first release liner), so that the problem of deterioration of the surface protective film does not occur.
[0081] C-1-2. Process A-2a In step A-2a, as shown in Figures 3(b) and (c), the first release liner 310 is peeled off from the first intermediate film 410, and a release liner with a surface protective film 350 having a second release liner 320 and a surface protective film 330 disposed on one side thereof is bonded to the exposed adhesive layer 110 to obtain a second intermediate film 420.
[0082] The first release liner 310 is peeled off from the first intermediate film 410 using, for example, a film peeling device. The bonding of the release liner 350 with the surface protective film is preferably performed consecutively with the peeling of the first release liner 310. By bonding the release liner with the surface protective film immediately after the peeling of the first release liner, adhesion of foreign matter to the surface of the pressure-sensitive adhesive layer can be suitably prevented.
[0083] The second release liner 320 is formed of any appropriate resin film. Specific examples of the resin that is the main component of the resin film are the same as those exemplified for the first release liner. From the viewpoint of obtaining high transparency suitable for defect inspection, it is preferable that the resin film contains COP, PET, etc. The materials of the resin film can be used alone or in combination.
[0084] The resin film preferably does not contain or substantially does not contain a filler. Such a resin film has excellent transparency and suppresses erroneous detection of defects caused by the filler. The resin film substantially does not contain a filler means that the filler content in the resin film is 0.05% by weight or less. In addition, when the resin film contains a filler, the filler is preferably a nanofiller (nanofiller means particles having a maximum length of 100 nm or less).
[0085] A release treatment layer may be provided on the surface of the second release liner 320 that comes into contact with the pressure-sensitive adhesive layer 110. The same explanation as for the first release liner can be applied to the release treatment agent that forms the release treatment layer and the thickness of the release treatment layer.
[0086] The thickness of the second release liner 320 can be explained in the same manner as for the first release liner.
[0087] Since the second release liner 320 is subjected to inspection together with the pressure-sensitive adhesive layer-attached optical laminate, it is preferable that the second release liner has excellent transparency. The total light transmittance of the second release liner is, for example, 80% or more, preferably 90% or more, more preferably 95% or more, and even more preferably 97% or more.
[0088] The peeling force of the second release liner 320 against the adhesive layer 110 (peel angle 180°, peeling speed 300 mm / min) is, for example, 0.01 N / 50 mm or more, preferably 0.02 N / 50 mm or more, more preferably 0.04 N / 50 mm or more, and for example, 0.5 N / 50 mm or less, preferably 0.2 N / 50 mm or less, more preferably 0.1 N / 50 mm or less. If the peeling force is less than 0.01 N / 50 mm, the second release liner may peel off when the surface protection film is peeled off in step A-4a. If the peeling force exceeds 0.5 N / 50 mm, the peeling workability of the second release liner may decrease when the adhesive layer-attached optical laminate is used.
[0089] The surface protection film 330 prevents foreign matter from adhering to the surface of the second release liner until the second release liner is subjected to inspection together with the pressure-sensitive adhesive layer-attached optical laminate.
[0090] The peeling force (adhesion force) of the surface protection film 330 from the second release liner 320 (peeling angle 180°, peeling speed 300 mm / min) is, for example, 0.005 N / 50 mm or more, preferably 0.007 N / 50 mm or more, more preferably 0.01 N / 50 mm or more, and, for example, 0.095 N / 50 mm or less, preferably 0.07 N / 50 mm or less, more preferably 0.05 N / 50 mm or less. If the peeling force of the surface protection film from the second release liner is less than 0.005 N / 50 mm, the surface protection film 330 may float from the second release liner 320 when the release liner 350 with the surface protection film is bonded to the pressure-sensitive adhesive layer 110 in step A-2a. If the peeling force of the surface protection film 330 from the second release liner 320 exceeds 0.095 N / 50 mm, the second release liner 320 may also be peeled off when the surface protection film 330 is peeled off in step A-4a.
[0091] The peeling force X of the surface protection film 330 from the second release liner 320 (peeling angle 180°, peeling speed 300 mm / min) and the peeling force Y of the second release liner 320 from the pressure-sensitive adhesive layer 110 (peeling angle 180°, peeling speed 300 mm / min) satisfy, for example, the relationship of 0.2 < X / Y < 1, preferably the relationship of 0.25 < X / Y < 0.7. Thereby, the problem of the surface protection film floating in step A-2a and the problem of the second release liner peeling in step A-4a can be preferably prevented.
[0092] Since the surface protection film 330 is peeled off before inspection, it does not need to have high transparency. The total light transmittance of the surface protection film may be, for example, 95% or less, or, for example, 90% or less or 80% or less, and its lower limit value is not particularly limited and may be, for example, 60% or more.
[0093] The surface protection film 330 may be, for example, a film that can be attached to an adherend by its own adhesiveness without using an adhesive or other attachment means (hereinafter, referred to as a self-adhesive film), or an adhesive film having a substrate and an adhesive layer provided on one side thereof. The self-adhesive film can favorably obtain the above-mentioned peeling force.
[0094] Typically, a polyolefin film is used as the self-adhesive film. Specifically, the self-adhesive film is preferably made of polyethylene, polypropylene, or a mixture thereof. Here, polyethylene includes ethylene homopolymers and copolymers of ethylene and other olefins. Polypropylene includes propylene homopolymers and copolymers of propylene and other olefins.
[0095] Specific examples of the polyethylene include high density polyethylene (HDPE), low density polyethylene (LDPE), and linear low density polyethylene (L-LDPE).
[0096] Examples of the other olefins include ethylene, propylene, butene, pentene, hexene, heptene, octene, nonene, and decene. Among these, ethylene, propylene, and butene are preferably used. In preparing a copolymer of ethylene or propylene and other olefins, the blending ratio of the other olefins is preferably 40 parts by weight or less, more preferably 30 parts by weight or less, and even more preferably 20 parts by weight or less, based on 100 parts by weight of the total of ethylene or propylene and other olefins.
[0097] In one embodiment, the polyolefin film preferably contains polyethylene. Specifically, the polyolefin film is preferably a polyethylene film or a mixture film of polyethylene and polypropylene. When the polyolefin film contains a mixture of polyethylene and polypropylene, the content of polyethylene is preferably 60 parts by weight or more and 97 parts by weight or less, more preferably 70 parts by weight or more, and even more preferably 80 parts by weight or more, based on 100 parts by weight of the total of polyethylene and polypropylene.
[0098] The self-adhesive film (polyolefin film) may contain other ingredients such as particles, pigments, colorants, antistatic agents, UV absorbers, antioxidants, heat stabilizers, and chlorine scavengers.
[0099] The self-adhesive film (polyolefin film) may be a single layer with a uniform composition, or may have a laminated structure of two or more layers with different compositions. Specific examples of the laminated structure include a two-layer structure of a first layer and a second layer with different compositions, and a three-layer structure of a first layer, a second layer, and a third layer. The first layer and the third layer may have substantially the same composition or may have different compositions. The self-adhesive film (polyolefin film) may be a non-stretched film or a stretched film, but is preferably a non-stretched film.
[0100] The surface roughness Ra of the self-adhesive film (surface roughness Ra before being attached to the second release liner) is, for example, 0.05 μm or more and 0.5 μm or less.
[0101] The thickness of the self-adhesive film is preferably 15 μm to 60 μm, and more preferably 20 μm to 50 μm.
[0102] Examples of materials for forming the substrate of the pressure-sensitive adhesive film include polyester-based polymers such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate; cellulose-based polymers such as diacetyl cellulose and triacetyl cellulose; polycarbonate-based polymers; (meth)acrylic polymers such as polymethyl methacrylate; and cycloolefin-based polymers such as polynorbornene. These may be used alone or in combination of two or more.
[0103] Any suitable configuration may be adopted as the adhesive constituting the adhesive layer of the adhesive film. Specific examples include acrylic adhesives, rubber adhesives, silicone adhesives, polyester adhesives, urethane adhesives, epoxy adhesives, and polyether adhesives. By adjusting the type, number, combination, and compounding ratio of monomers forming the base resin of the adhesive, as well as the compounding amount of the crosslinking agent, reaction temperature, reaction time, and the like, an adhesive having desired properties according to the purpose can be prepared. The base resin of the adhesive may be used alone or in combination of two or more. The base resin is preferably an acrylic resin (specifically, the adhesive layer is preferably composed of an acrylic adhesive). For details of the acrylic adhesive, for example, the descriptions in JP-A-2013-79360 and JP-A-2019-127526 can be referred to. The thickness of the adhesive layer is, for example, 5 μm to 30 μm, preferably 5 μm to 20 μm, and more preferably 5 μm to 15 μm.
[0104] The release liner 350 with the surface protective film can be obtained, for example, by laminating the surface protective film 330 and the second release liner 320 (for example, laminating them by roll-to-roll). When a self-adhesive film is used as the surface protective film, the peeling force of the self-adhesive film against the second release liner can be adjusted (for example, increased) by laminating the self-adhesive film and the second release liner 320 and then heating the film. The treatment temperature is, for example, 40° C. or higher, preferably 45° C. or higher, for example, 60° C. or lower, preferably 55° C. or lower. The treatment time may be any time that provides a desired peeling force, for example, 600 minutes or higher, preferably 1200 minutes or higher, for example, 48 hours or lower, preferably 36 hours or lower. The heating treatment is preferably performed in a state where pressure is applied to the release liner with the surface protective film. For example, the effect of increasing the peeling force can be suitably obtained by heating the release liner with the surface protective film wound in a roll shape.
[0105] C-1-3. Process A-3a 3(d) and (e), in step A-3a, a third intermediate film 430 is laminated on the side of the second intermediate film 420 opposite to the side on which the release liner 350 with the surface protective film is disposed, to obtain a fourth intermediate film 440. The second intermediate film and the third intermediate film are typically bonded together by an adhesive layer (e.g., a pressure-sensitive adhesive layer).
[0106] The third intermediate film 430 may have a first phase difference member 20 and a protective member 30. In the illustrated example, the third intermediate film 430 further has a second surface protective film 360 on the side opposite to the side of the protective member 30 on which the first phase difference member 20 is disposed. By the third intermediate film having the second surface protective film, the surface of the protective member side can be suitably protected. The second surface protective film may have a structure in which two or more surface protective films are laminated. As the surface protective film used for the second surface protective film, the same one as described in section C-1-2 can be used. The first phase difference member and the protective member are as described in section B. Although not illustrated, the third intermediate film may further have an adhesive layer on the side opposite to the side on which the protective member of the first phase difference member is disposed. By the third intermediate film having an adhesive layer, lamination with the second intermediate film can be easily performed. The second intermediate film having a polarizing member and the third intermediate film having a first λ / 4 member can be laminated so that the absorption axis of the polarizing member and the slow axis of the first λ / 4 member are at an angle of, for example, 40° to 50°, 42° to 48°, or approximately 45°.
[0107] The third intermediate film can be obtained by laminating each member via an adhesive layer as necessary. The order of lamination of each member is not limited. For example, the third intermediate film can be obtained by a method including laminating a first λ / 4 member and a positive C plate via an adhesive layer (e.g., an adhesive layer) to obtain a first phase difference member, and laminating a protective member on one side of the first phase difference member via an adhesive layer (e.g., a pressure-sensitive adhesive layer). If necessary, a pressure-sensitive adhesive layer may be laminated on the other side of the first phase difference member, or a second surface protective film may be attached to the surface of the protective member.
[0108] C-1-4. Process A-4a In step A-4a, as shown in FIG. 3(f), the surface protection film 330 is peeled off from the fourth intermediate film 440. This makes it possible to obtain an adhesive-layer-attached optical laminate (sometimes referred to as an "adhesive-layer-attached optical laminate of inspection configuration") 450 in which a second release liner is disposed on the surface of the adhesive layer. The adhesive-layer-attached optical laminate of inspection configuration 450 is, for example, chucked at the end and subjected to inspection. By subjecting the optical laminate to inspection immediately after peeling off the surface protection film 330, it is possible to suitably suppress the introduction of foreign matter into the inspection.
[0109] The pressure-sensitive adhesive layer-attached optical laminate 450 in the illustrated inspection configuration has the second surface protective film 360 laminated on the protective member 30 side, but may be subjected to inspection after peeling off the second surface protective film 360. When the second surface protective film 360 includes two or more surface protective films, the outer surface protective film may be peeled off and the inner surface protective film may be laminated and subjected to inspection in that state.
[0110] C-1-5. Modification of Process A The step A is not limited to the above embodiment as long as an optical laminate with a pressure-sensitive adhesive layer in which a second release liner is arranged on the surface of the pressure-sensitive adhesive layer can be obtained. For example, in the above embodiment, the third intermediate film has a first retardation member and a protective member, but an intermediate film having a first retardation member and an intermediate film having a protective member may be separately prepared and sequentially laminated on the first intermediate film.
[0111] In another embodiment, step A includes the steps of: A step A-1b of preparing a fifth intermediate film 460 having a pressure-sensitive adhesive layer-attached optical laminate 200 having an optical laminate 100 and a pressure-sensitive adhesive layer 110 disposed on one side of the optical laminate 100, and a first release liner 310 disposed on the pressure-sensitive adhesive layer 110 side surface of the pressure-sensitive adhesive layer-attached optical laminate 200; A step A-2b of peeling the first release liner 310 from the fifth intermediate film 460; A step A-3b of bonding a release liner with a surface protective film (350) having a second release liner (320) and a surface protective film (330) disposed on one side of the second release liner (320) to the pressure-sensitive adhesive layer-attached optical laminate (200) so that the second release liner (320) is in contact with the release surface to obtain a sixth intermediate film (470); and A process A-4b of peeling the surface protective film 330 from the sixth intermediate film 470; may include. In this embodiment, the pressure-sensitive adhesive layer-attached optical laminate 200 can be obtained by stacking the members in any suitable order. For example, a long polarizing member having an absorption axis in the longitudinal direction or width direction and a long first λ / 4 member having a slow axis in a direction oblique to the longitudinal direction can be used, or a long polarizing member having an absorption axis in a direction oblique to the longitudinal direction and a long first λ / 4 member having a slow axis in the longitudinal direction or width direction can be used, to prepare a pressure-sensitive adhesive layer-attached optical laminate by roll-to-roll. From the viewpoint of optimally obtaining the effects of the present invention, also in this embodiment, it is preferable that the peel force X of the surface protective film to the second release liner, the peel force Y of the second release liner to the pressure-sensitive adhesive layer, and the ratio of the peel force X to the peel force Y are within the above-mentioned ranges.
[0112] C-2.Process B In step B, the pressure-sensitive adhesive layer-attached optical laminate is inspected with the second release liner disposed on the surface of the pressure-sensitive adhesive layer. In other words, the pressure-sensitive adhesive layer-attached optical laminate 450 having the above-mentioned inspection configuration is inspected. For example, the presence or absence of defects in the pressure-sensitive adhesive layer-attached optical laminate is inspected, and the pressure-sensitive adhesive layer-attached optical laminate is judged as a good product or a defective product. The defect inspection is performed by any appropriate defect inspection device. As the defect inspection device, a known defect inspection device can be used, and preferably an automated optical inspection (AOI) device is used. Examples of documents in which the defect inspection device is described include International Publication No. 2011 / 148790, JP 2003-344302 A, JP 2011-226957 A, JP 2016-70856 A, and JP 2021-135219 A. The defect inspection may further include a visual inspection as necessary. The number of foreign matters having a diameter of 10 μm or more adhering to the surface of the second release liner of the pressure-sensitive adhesive layer-attached optical laminate in the inspection configuration is, for example, 300 or less per sheet, preferably 200 or less per sheet, and more preferably 100 or less per sheet. The size of the pressure-sensitive adhesive layer-attached optical laminate in the inspection configuration is not particularly limited, but may be, for example, 20,000 mm 2 or more, for example 50,000 mm 2 For example, 100,000 mm 2 For example, 70,000 mm 2 The following is the result.
[0113] 5, the effective inspection range on the main surface of the pressure-sensitive adhesive layer-attached optical laminate 450 in the inspection configuration is divided into a plurality of virtual areas E based on the size of the final product, and the presence or absence of defects is inspected in the plurality of virtual areas E. The size of the defects to be inspected is typically 5 μm or more and 300 μm or less, 5 μm or more and 200 μm or less, or 5 μm or more and 100 μm or less. Next, if the ratio of virtual areas E that contain defects (number of virtual areas that contain defects / total number of virtual areas × 100; hereafter referred to as the defect occupancy rate) is within a specified range, the product is judged to be good, and if it is outside the specified range, the product is judged to be defective. The upper limit of the defect occupancy is a criterion for determining whether a product is good or bad, and is, for example, 10% or less, preferably 5% or less, and the lower limit of the defect occupancy is, for example, 0% or more. When the criteria for determining whether a product is good or bad is set at the above upper limit, the proportion of final products having defects can be further reduced. Incidentally, a pressure-sensitive adhesive layer-attached optical layered body determined to be a defective product may be rejected (typically discarded).
[0114] The optical laminate with the adhesive layer that is determined to be a non-defective product in the above-mentioned inspection is sent to, for example, a punching process, where it is punched out to a predetermined size. This results in a piece of the optical laminate with the adhesive layer as a final product (more specifically, an optical laminate with the adhesive layer in a state in which the adhesive layer is protected by the second release liner). The punching is typically performed along the dividing lines of a plurality of imaginary areas in the inspection. EXAMPLES
[0115] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The thicknesses are values measured by the following measuring method. <Thickness> The thickness of 10 μm or less was measured using a scanning electron microscope (manufactured by JEOL, product name "JSM-7100F"), and the thickness of more than 10 μm was measured using a digital micrometer (manufactured by Anritsu, product name "KC-351C"). <Total light transmittance> Measurements were made using a spectrophotometer (Hitachi High-Tech Science Corporation, product name "U4100"). <Peeling force> [Release liner with surface protection film 1-4] (1-1) Peel strength of surface protective film to secondary release liner A laminate of the first release liner obtained in Production Example 6 and the adhesive layer 1 formed on one side thereof was attached and fixed to a SUS plate (SUS304BA) via the adhesive layer 1, and then the first release liner was peeled off to expose the adhesive layer 1. A release liner with a surface protective film cut to a size of 50 mm x 150 mm was attached so that the surface of the second release liner was in contact with the adhesive layer 1. Using a universal tensile tester (manufactured by Minebea Co., Ltd., product name: TCM-1kNB), the peel force was measured when the surface protective film was peeled off from the second release liner in an environment of 23°C and 65% RH at a peel speed of 300 mm / min and a peel angle of 180°. (1-2) Peel strength of second release liner from adhesive layer 1 After the measurement in (1-1) above, the peel force was measured when the second release liner was peeled from the pressure-sensitive adhesive layer 1 at a peel speed of 300 mm / min and a peel angle of 180°. [Release liner with surface protection film 5~7] (2-1) Peel strength of surface protective film to secondary release liner The release liner with the surface protective film was cut to a size of 50 mm × 150 mm, and the second release liner side was attached to a SUS plate (SUS304BA) via double-sided tape. In the same manner as in (1-1) above, the peel force (peel speed 300 mm / min, peel angle 180 degrees) when the surface protective film was peeled from the second release liner was measured. (2-2) Peel strength of second release liner from adhesive layer 1 In the same manner as in (1-1) above, the pressure-sensitive adhesive layer 1 was fixed to a SUS plate (SUS304BA), and a release liner with a surface protective film cut to a size of 50 mm × 150 mm was attached so that the surface of the second release liner was in contact with the pressure-sensitive adhesive layer 1. In the same manner as in (1-1) above, the peel force (peel speed 300 mm / min, peel angle 180 degrees) when the release liner with the surface protective film was peeled from the pressure-sensitive adhesive layer 1 was measured. <In-plane phase difference> The in-plane retardation at 23° C. was measured using a "KOBRA-WPR" manufactured by Oji Scientific Instruments.
[0116] [Production Example 1A: Release liner with surface protection film 1] A self-adhesive film (Toray Industries, Inc., "Tretec 7832C", thickness 50 μm, total light transmittance 90%) was used as the surface protection film, and a PET film with a release treatment layer (Toray Industries, Inc., "Therapeel", total light transmittance 92%) was used as the second release liner. A second release liner was laminated on one side (adhesive side) of the surface protective film under pressure bonding conditions of 23.5°C and 3.0 MPa to obtain a release liner with surface protective film 1. At this time, the second release liner was laminated so that the side opposite the release treatment layer side was the surface protective film side.
[0117] [Production Example 1B: Release liner with surface protection film 2] A release liner 2 with a surface protective film was obtained in the same manner as in Production Example 1A, except that a self-adhesive film (manufactured by Toray Industries, Inc., "Tretec 7832C", thickness 30 μm, total light transmittance 90%) was used as the surface protective film, and the long laminate obtained by laminating the surface protective film and the second release liner was wound up into a roll and heated in a heating chamber at 50°C for 24 hours.
[0118] [Production Example 1C: Release liner with surface protection film 3] A release liner 3 with a surface protective film was obtained in the same manner as in Production Example 1B, except that a self-adhesive film (manufactured by Toray Industries, Inc., "Tretec 7832C", thickness 50 μm, total light transmittance 90%) was used as the surface protective film.
[0119] [Production Example 1D: Release liner with surface protection film 4] A release liner 4 with a surface protective film was obtained in the same manner as in Production Example 1A, except that a self-adhesive film (Toray Industries, Inc., "Tretec 7832C", thickness 30 μm, total light transmittance 90%) was used as the surface protective film.
[0120] [Production Example 1E: Release Liner 5 with Surface Protection Film] As a surface protection film, an adhesive film 1 (substrate thickness 38 μm, adhesive layer thickness 20 μm, total light transmittance 89%) having a PET substrate and an acrylic adhesive layer prepared as described below was used, and a release liner 5 with a surface protection film was obtained in the same manner as in Manufacturing Example 1A, except that a second release liner was laminated on the adhesive layer surface. <Preparation of adhesive film 1> In a reaction vessel equipped with a thermometer, a stirrer, a cooler, and a nitrogen gas inlet tube, 100 parts by weight of 2-ethylhexyl acrylate (2EHA) and 4 parts by weight of hexyl acrylate as monomer components, and 0.2 parts by weight of 2,2'-azobisisobutyronitrile (AIBN) as a polymerization initiator were charged together with 150 parts by weight of ethyl acetate, and nitrogen gas was introduced while gently stirring at 23°C to perform nitrogen substitution. After that, the liquid temperature was kept at around 65°C and a polymerization reaction was carried out for 6 hours, preparing a solution of acrylic polymer A (concentration 40% by weight). The weight average molecular weight of acrylic polymer A was 530,000. Ethyl acetate was added to the solution of acrylic polymer A to dilute it to a concentration of 20% by weight. 4 parts by weight of an isocyanurate of hexamethylene diisocyanate ("Coronate HX" manufactured by Tosoh Corporation) as a crosslinking agent and 0.2 parts by weight of a surfactant ("Aqualon HS-10" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) were added to 500 parts by weight of this solution (solid content 100 parts by weight) and stirred to prepare adhesive composition A. The pressure-sensitive adhesive composition A was applied to the surface (corona-treated surface) of a substrate (PET film, manufactured by Mitsubishi Chemical Corporation, product number T100C38, thickness 38 μm) and then dried to form a pressure-sensitive adhesive layer (thickness 20 μm).
[0121] [Production Example 1F: Release liner with surface protection film 6] As a surface protection film, an adhesive film 2 having a PET substrate and an acrylic adhesive layer prepared as described below (substrate thickness 38 μm, adhesive layer thickness 5 μm, total light transmittance 89%) was used, and a release liner 6 with a surface protection film was obtained in the same manner as in Manufacturing Example 1A, except that a second release liner was laminated on the adhesive layer surface. <Preparation of adhesive film 2> In a reaction vessel equipped with a thermometer, a stirrer, a cooler and a nitrogen gas inlet tube, 96.2 parts by weight of 2-ethylhexyl acrylate (2EHA) and 3.8 parts by weight of hydroxyethyl acrylate (HEA) as monomer components, and 0.2 parts by weight of 2,2'-azobisisobutyronitrile (AIBN) as a polymerization initiator were charged together with 150 parts by weight of ethyl acetate, and nitrogen gas was introduced while gently stirring at 23°C to perform nitrogen substitution. After that, the liquid temperature was kept at around 65°C and a polymerization reaction was carried out for 6 hours to prepare a solution of acrylic polymer B (concentration 40% by weight). The weight average molecular weight of acrylic polymer B was 540,000. Ethyl acetate was added to the solution of acrylic polymer B to dilute it to a concentration of 20% by weight. 4 parts by weight of an isocyanurate of hexamethylene diisocyanate ("Coronate HX" manufactured by Tosoh Corporation) as a crosslinking agent and 3 parts by weight (solid content 0.03 parts by weight) of dibutyltin dilaurate (1% by weight solution in ethyl acetate) as a crosslinking catalyst were added to 500 parts by weight of this solution (solid content 100 parts by weight) and stirred to prepare adhesive composition B. The pressure-sensitive adhesive composition B was applied to the surface (corona-treated surface) of a substrate (PET film, manufactured by Mitsubishi Chemical Corporation, product number T100C38, thickness 38 μm) and then dried to form a pressure-sensitive adhesive layer (thickness 5 μm).
[0122] [Production Example 1G: Release liner with surface protection film 7] Release liner 7 with surface protective film was obtained in the same manner as in Production Example 1A, except that a second release liner was laminated to the corona-treated surface of a self-adhesive film (Toray Industries, Inc., "Tretec 7832C", thickness 50 μm, total light transmittance 90%) that had been corona-treated on one side.
[0123] [Production Example 2: Polarizing Film 1] A long roll of polyvinyl alcohol (PVA) resin film (manufactured by Kuraray Co., Ltd., product name "PE3000") with a thickness of 30 μm was uniaxially stretched in the longitudinal direction to 5.9 times its original size using a roll stretching machine, while simultaneously undergoing swelling, dyeing, crosslinking, and washing processes, and finally a drying process to produce an absorptive polarizing film with a thickness of 12 μm. Specifically, the film was stretched 2.2 times during the swelling treatment in pure water at 20°C. Next, the film was stretched 1.4 times during the dyeing treatment in an aqueous solution at 30°C in which the weight ratio of iodine to potassium iodide was 1:7, and the iodine concentration was adjusted so that the single transmittance of the resulting absorptive polarizing film was 45.0%. Furthermore, a two-stage crosslinking treatment was adopted, and the film was stretched 1.2 times during the first stage crosslinking treatment in an aqueous solution at 40°C in which boric acid and potassium iodide were dissolved. The boric acid content of the aqueous solution in the first stage crosslinking treatment was 5.0% by weight, and the potassium iodide content was 3.0% by weight. The film was stretched 1.6 times during the second stage crosslinking treatment in an aqueous solution at 65°C in which boric acid and potassium iodide were dissolved. The boric acid content of the aqueous solution in the second stage crosslinking treatment was 4.3% by weight, and the potassium iodide content was 5.0% by weight. The cleaning treatment was performed with an aqueous potassium iodide solution at 20° C. The aqueous solution used for the cleaning treatment had a potassium iodide content of 2.6% by weight. Finally, the film was dried at 70° C. for 5 minutes to obtain an absorptive polarizing film. A triacetyl cellulose (TAC) resin film with a hard coat layer (TAC thickness: 25 μm, HC layer thickness: 7 μm) was attached to one side of the obtained absorptive polarizing film, and a cycloolefin resin film (thickness: 13 μm) was attached to the other side as a protective layer. Specifically, the curable adhesive was applied so that the total thickness was about 1 μm, and the two were laminated using a roller. Then, UV rays were irradiated from the TAC film side to cure the adhesive. As a result, a polarizing film 1 (thickness: 57 μm) having a structure of [HC-attached TAC film / absorptive polarizing film / COP film] was obtained.
[0124] [Manufacturing example 3: λ / 4 member 1] Polymerization was carried out using a batch polymerization apparatus consisting of two vertical reactors equipped with an agitator and a reflux condenser controlled at 100° C. Bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane 29.60 parts by weight (0.046 mol), isosorbide (ISB) 29.21 parts by weight (0.200 mol), spiroglycol (SPG) 42.28 parts by weight (0.139 mol), diphenyl carbonate (DPC) 63.77 parts by weight (0.298 mol), and calcium acetate monohydrate 1.19×10 as a catalyst. -2 Weight part (6.78×10 -5 mol) was charged. After the inside of the reactor was purged with nitrogen under reduced pressure, heating was performed with a heat medium, and stirring was started when the inside temperature reached 100 ° C. 40 minutes after the start of the temperature increase, the inside temperature was reached 220 ° C., and while controlling to maintain this temperature, the pressure was reduced and 90 minutes after reaching 220 ° C., the pressure was reduced to 13.3 kPa. Phenol vapor by-produced with the polymerization reaction was led to a reflux condenser at 100 ° C., a small amount of monomer components contained in the phenol vapor were returned to the reactor, and the uncondensed phenol vapor was led to a condenser at 45 ° C. and recovered. Nitrogen was introduced into the first reactor to restore the pressure to atmospheric pressure, and the oligomerized reaction liquid in the first reactor was transferred to the second reactor. Next, the temperature increase and pressure reduction in the second reactor were started, and the inside temperature was set to 240 ° C. and the pressure to 0.2 kPa in 50 minutes. Thereafter, polymerization was allowed to proceed until the specified stirring power was reached. When the predetermined power was reached, nitrogen was introduced into the reactor to restore pressure, and the produced polyester carbonate resin was extruded into water and the strands were cut to obtain pellets.
[0125] The obtained polyester carbonate resin (pellets) was vacuum-dried at 80°C for 5 hours, and then a long resin film having a thickness of 135μm was produced using a film-forming device equipped with a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 200mm, setting temperature: 250°C), a chill roll (setting temperature: 120-130°C) and a winder. The obtained long resin film was stretched in the width direction at a stretching temperature of 143°C and a stretching ratio of 2.8 times. As a result, a stretched film (λ / 4 member 1) having a thickness of 47μm was obtained. The Re(590) of the λ / 4 member 1 was 143nm, the Re(450) / Re(550) was 0.86, and the Nz coefficient was 1.12.
[0126] [Example 4: Positive C Plate 1] A liquid crystal coating solution was prepared by dissolving 20 parts by weight of a side-chain liquid crystal polymer represented by the following chemical formula (1) (the numbers 65 and 35 in the formula indicate the mole percent of the monomer unit, and are conveniently represented as a block polymer: weight average molecular weight 5000), 80 parts by weight of a polymerizable liquid crystal exhibiting a nematic liquid crystal phase (manufactured by BASF: trade name Paliocolor LC242), and 5 parts by weight of a photopolymerization initiator (manufactured by Ciba Specialty Chemicals: trade name Irgacure 907) in 200 parts by weight of cyclopentanone. The coating solution was then applied to a PET substrate that had been subjected to a vertical alignment treatment using a bar coater, and the liquid crystal was aligned by heating and drying at 80°C for 4 minutes. The liquid crystal layer was irradiated with ultraviolet light to harden the liquid crystal layer, thereby forming a positive C plate 1 with a thickness of 4 μm and an Rth(550) of -100 nm on the substrate. [ka]
[0127] [Manufacturing Example 5: Protective Material 1] The anti-reflection layer-forming material shown below was applied to an acrylic film having a lactone ring structure and heated at 80°C for 1 minute. After heating, the coating layer was irradiated with a high-pressure mercury lamp with an integrated light intensity of 300 mJ / cm. 2The coating layer was cured by irradiating it with ultraviolet light of 1000 ohms to form an antireflection layer having a thickness of 4 μm, thereby obtaining a protective member 1 (thickness 44 μm) having a structure of [acrylic film / antireflection layer].
[0128] (Anti-reflection layer forming material) 100 parts by weight of a polyfunctional acrylate mainly composed of pentaerythritol triacrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd., trade name "Viscoat #300", solid content 100% by weight), 150 parts by weight of hollow nanosilica particles (manufactured by JGC Catalysts and Chemicals Co., Ltd., trade name "Surulia 5320", solid content 20% by weight, weight average particle diameter 75 nm), 50 parts by weight of solid nanosilica particles (manufactured by Nissan Chemical Industries, Ltd., trade name "MEK-2140Z-AC", solid content 30% by weight, weight average particle diameter 10 nm), 12 parts by weight of a fluorine-containing additive (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KY-1203", solid content 20% by weight), and 3 parts by weight of a photopolymerization initiator (manufactured by BASF, trade name "OMNIRAD907", solid content 100% by weight) were mixed. To the mixture was added a mixed solvent of TBA (tertiary butyl alcohol), MIBK (methyl isobutyl ketone) and PMA (propylene glycol monomethyl ether acetate) in a weight ratio of 60:25:15 as a dilution solvent until the total solids content was 4% by weight, and the mixture was stirred to prepare an anti-reflection layer forming material.
[0129] [Production Example 6: Adhesive Layer 1] (Acrylic Polymer 1) A monomer mixture containing 80.3 parts of butyl acrylate, 16 parts of phenoxyethyl acrylate, 3 parts of N-vinyl-2-pyrrolidone (NVP), 0.3 parts of acrylic acid, and 0.4 parts of 4-hydroxybutyl acrylate was charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Furthermore, 0.1 parts of 2,2'-azobisisobutyronitrile as a polymerization initiator was charged together with 100 parts of ethyl acetate for 100 parts of the above monomer mixture (solid content), and nitrogen gas was introduced while gently stirring to replace the nitrogen. The liquid temperature in the flask was kept at around 55°C, and a polymerization reaction was carried out for 8 hours to prepare a solution of acrylic polymer 1. The weight average molecular weight of acrylic polymer 1 was 1.5 million.
[0130] <Adhesive solution 1> An acrylic adhesive solution 1 was prepared by mixing 0.3 parts of benzoyl peroxide (BPO: Niper BMT manufactured by NOF Corporation) as a crosslinking agent with 100 parts by weight of the solid content of the acrylic polymer 1 solution.
[0131] <Adhesive layer 1> The acrylic adhesive solution 1 was applied to the release treatment layer surface of a PET film having a release treatment layer as a first release liner ("MRF38", manufactured by Mitsubishi Chemical Polyester Film Corporation, total light transmittance 86%), and dried and crosslinked at 155°C for 3 minutes to form an adhesive layer 1 with a dry thickness of 20 μm on the long first release liner.
[0132] [Example 1] A laminate of the above-mentioned adhesive layer 1 and a first release liner was roll-to-roll bonded to the COP film side of the above-mentioned polarizing film 1 to obtain a long-sized first intermediate film 1 having a structure of [first release liner / adhesive layer 1 / polarizing film 1] (Step A-1a). The first release liner was peeled off from the first intermediate film 1, and the above release liner 1 with surface protective film was laminated to the exposed adhesive layer 1 by roll-to-roll bonding so that the second release liner was on the adhesive layer 1 side. The release liner 1 with surface protective film was laminated under a nip roll pressure of 3.0 MPa. This resulted in a long second intermediate film 1 having a structure of [release liner 1 with surface protective film / adhesive layer 1 / polarizing film 1] (step A-2a). The positive C plate 1 was attached to the λ / 4 member 1 via an ultraviolet-curing adhesive (thickness after curing: 1 μm), and then the base material was peeled off and removed to obtain a retardation member 1. An acrylic pressure-sensitive adhesive layer (thickness: 15 μm) laminated on a substrate was attached to the λ / 4 member 1 side of the phase difference member 1. Next, the protective member 1 was attached to the positive C plate 1 side of the retardation member 1 via an acrylic pressure-sensitive adhesive layer (thickness: 12 μm). At this time, the protective member 1 was attached so that the acrylic film side surface of the protective member 1 faced the retardation member 1 side (in other words, so that the antireflection layer became the outermost surface). The lamination was carried out by roll-to-roll, thereby obtaining a long third intermediate film 1 having a structure of [substrate / acrylic pressure-sensitive adhesive layer / λ / 4 member 1 / positive C plate 1 / protective member 1]. The long second intermediate film 1 and the third intermediate film 1 were each punched out to a size of 371.87 mm x 236.58 mm to obtain a sheet of film. The second intermediate film 1 was punched out so that the long side direction of the sheet of film was parallel to the longitudinal direction. The third intermediate film 1 was punched out so that the long side direction was at an angle of 45° to the longitudinal direction. The substrate was peeled off from the third intermediate film 1 sheet to expose the acrylic adhesive layer, which was then attached to the polarizing member side of the second intermediate film 1 sheet. This resulted in a fourth intermediate film 1 having a configuration of [release liner with surface protective film 1 / adhesive layer 1 / polarizing film 1 / λ / 4 member 1 / positive C plate 1 / protective member 1] (step A-3a). In the fourth intermediate film 1, the angle between the absorption axis of the absorptive polarizing film and the slow axis of the λ / 4 member 1 was 45°. Next, the surface protective film was peeled off from the fourth intermediate film 1 to obtain an optical laminate with an adhesive layer 1 of the test configuration (specifically, an optical laminate with an adhesive layer having a configuration of [second release liner / adhesive layer 1 / polarizing film 1 / λ / 4 member 1 / positive C plate 1 / protective member 1]) (step A-4a).
[0133] [Example 2] An optical laminate 2 with a pressure-sensitive adhesive layer having an inspection configuration was obtained in the same manner as in Example 1, except that a release liner 2 with a surface protective film was used instead of a release liner 1 with a surface protective film.
[0134] [Example 3] An optical laminate 3 with a pressure-sensitive adhesive layer having an inspection configuration was obtained in the same manner as in Example 1, except that a release liner 3 with a surface protective film was used instead of a release liner 1 with a surface protective film.
[0135] [Example 4] An optical laminate 4 with a pressure-sensitive adhesive layer of the test configuration was obtained in the same manner as in Example 1, except that a release liner 4 with a surface protective film was used instead of the release liner 1 with a surface protective film.
[0136] [Example 5] An optical laminate 5 with a pressure-sensitive adhesive layer having an inspection configuration was obtained in the same manner as in Example 1, except that a release liner 5 with a surface protective film was used instead of the release liner 1 with a surface protective film.
[0137] [Example 6] An optical laminate 6 with a pressure-sensitive adhesive layer having an inspection configuration was obtained in the same manner as in Example 1, except that a release liner 6 with a surface protective film was used instead of the release liner 1 with a surface protective film.
[0138] [Example 7] An optical laminate 7 with a pressure-sensitive adhesive layer having an inspection configuration was obtained in the same manner as in Example 1, except that a release liner 7 with a surface protective film was used instead of the release liner 1 with a surface protective film.
[0139] [Comparative Example 1] An optical laminate C1 with a pressure-sensitive adhesive layer of the test configuration was obtained in the same manner as in Example 1, except that the second release liner was used alone instead of the release liner 1 with the surface protective film, and step A-4a was not performed.
[0140] The following evaluations were carried out on the pressure-sensitive adhesive layer-attached optical laminates 1 to 7 and C1 having the test configurations obtained in the above Examples and Comparative Examples. The evaluation results are shown in Table 1 together with the peel strength X of the surface protective film from the second release liner in each release liner with surface protective film, and the ratio (X / Y) of the peel strength X to the peel strength Y of the second release liner from the pressure-sensitive adhesive layer 1. The peel strength Y was 0.05 N / 50 mm. <Foreign matter adhesion> The surface of the second release liner of the pressure-sensitive adhesive layer-attached optical laminates 1 to 7 and C1 in the test configuration was observed with an optical microscope at a magnification of 20 times, and the number and size of foreign matter in an area of 45 mm × 50 mm was measured and evaluated according to the following criteria. The results are shown in Table 1. Good: Fewer than 10 foreign objects of 50 μm or more in size × (Fail): 10 or more foreign objects with a size of 50 μm or more <Evaluation of surface protection film lifting when replacing release liner> The same operation was carried out a total of 20 times for each of Examples 1 to 7 and Comparative Example 1, and the number of times that lifting occurred between the second release liner and the surface protective film when the first release liner was peeled off from the first intermediate film and the release liner with the surface protective film was attached to the release surface was counted and evaluated according to the following criteria. The results are shown in Table 1. 〇 (Good): No floating occurred in all 20 tests △ (Acceptable): Floating occurred in some of the 20 attempts. × (bad): Floating occurred in all 20 tests <Evaluation of peeling of secondary release liner when peeling off surface protection film> The same operation was carried out a total of 20 times for each of Examples 1 to 7 and Comparative Example 1, and the number of times that the second release liner was peeled off together when the surface protection film was peeled off from the fourth intermediate film was counted and evaluated according to the following criteria. The results are shown in Table 1. 〇 (Good): Only the surface protection film was peeled off in all 20 tests. △ (Fair): In some of the 20 tests, the second release liner peeled off together with the surface protective film. × (bad): The second release liner peeled off together with the surface protective film in all 20 tests.
[0141] [Table 1]
[0142] As shown in Table 1, during the preparation of an optical laminate with an adhesive layer of the inspection configuration, the first release liner protecting the adhesive layer is replaced with a release liner with a surface protective film, and only the surface protective film is peeled off and removed, thereby preventing foreign matter from adhering to the second release liner and, as a result, preventing erroneous detection of defects during inspection.
[0143] Furthermore, it can be seen that by adjusting the peel force X of the surface protection film to the second release liner and the ratio of this peel force X to the peel force Y of the second release liner to the adhesive layer, it is possible to suitably prevent the problem of the surface protection film lifting when replacing the first release liner with a release liner with a surface protection film attached, and the problem of the second release liner peeling when the surface protection film is peeled off.
[0144] The present invention is not limited to the above-described embodiment, and various modifications are possible. For example, the above-described embodiment may be replaced with a configuration that is substantially the same as the configuration shown in the above-described embodiment, a configuration that provides the same action and effect, or a configuration that can achieve the same purpose. [Industrial Applicability]
[0145] The method for producing a pressure-sensitive adhesive layer-attached optical laminate according to an embodiment of the present invention can be used, for example, for producing goggles with a display, such as VR goggles. [Explanation of symbols]
[0146] 2 display system, 10 polarizing member, 12 display element, 14 reflective polarizing member, 16 first lens portion, 18 half mirror, 20 first phase difference member, 22 second phase difference member, 24 second lens portion, 100 optical laminate, 110 adhesive layer, 200 optical laminate with adhesive layer, 310 first release liner, 320 second release liner, 330 surface protective film, 350 release liner with surface protective film, 410 first intermediate film, 420 second intermediate film, 430 third intermediate film, 440 fourth intermediate film, 450 optical laminate with adhesive layer of inspection configuration, 460 fifth intermediate film, 470 sixth intermediate film
Claims
1. A method for producing a pressure-sensitive adhesive layer-attached optical laminate having an optical laminate and a pressure-sensitive adhesive layer disposed on one surface of the optical laminate, comprising the steps of: A step A of obtaining the pressure-sensitive adhesive layer-attached optical laminate in which a second release liner is disposed on the surface of the pressure-sensitive adhesive layer; and A step B of inspecting the pressure-sensitive adhesive layer-attached optical laminate in a state in which the second release liner is disposed on the surface of the pressure-sensitive adhesive layer; Including, A manufacturing method in which step A includes replacing a first release liner arranged on the surface of the pressure-sensitive adhesive layer with a release liner with a surface protective film having the second release liner and a surface protective film arranged on one side of the second release liner, and then peeling off the surface protective film.
2. The step A comprises: A step A-1a of preparing a first intermediate film having the pressure-sensitive adhesive layer and the first release liner disposed on a surface of the pressure-sensitive adhesive layer; A step A-2a of peeling the first release liner from the first intermediate film and bonding the release liner with the surface protective film to the exposed pressure-sensitive adhesive layer to obtain a second intermediate film; A step A-3a of laminating a third intermediate film on the side of the second intermediate film opposite to the side on which the release liner with the surface protective film is disposed to obtain a fourth intermediate film; and A step A-4a of peeling the surface protective film from the fourth intermediate film; The method of claim 1 , comprising:
3. The first intermediate film further comprises a polarizing member, The method of claim 2 , wherein the third intermediate film comprises a first λ / 4 member.
4. preparing a laminate of the first release liner and the pressure-sensitive adhesive layer; and The method according to claim 3 , wherein the first intermediate film is produced by a method including bonding the laminate to the polarizing member via the pressure-sensitive adhesive layer.
5. The method according to claim 1 , wherein the peel force of the surface protection film from the second release liner (peel angle: 180°, peel speed: 300 mm / min) is 0.005 N / 50 mm or more and 0.095 N / 50 mm or less.
6. 2. The method according to claim 1, wherein a peel force X of the surface protective film to the second release liner (peel angle 180°, peel speed 300 mm / min) and a peel force Y of the second release liner to the pressure-sensitive adhesive layer (peel angle 180°, peel speed 300 mm / min) satisfy the relationship 0.2<X / Y<1.
7. The method according to claim 1 , wherein the second release liner has a total light transmittance of 80% or more.
8. The method of claim 1 , wherein the first release liner has a total light transmittance of 95% or less.
9. The method according to claim 1 , wherein the surface protective film has a total light transmittance of 95% or less.
Citation Information
Patent Citations
Manufacturing method of film laminate and manufacturing equipment of film laminate
JP2015047749A
Optical laminate and image display device
JP2018120119A
Substrate for surface protective film, surface protective film using the substrate, and polarizing plate with retardation layer and with surface protective film
JP2020042166A
Method for manufacturing optical laminate
JP2022164140A
Method for manufacturing optical laminate
WO2022224737A1
Cited By
Optical laminate, method for manufacturing optical film piece, and method for manufacturing display system
WO2026191554A1