Porous gel and production method thereof, as well as, gas adsorption system and gas separation system

The development of a porous gel using MOFs and size exclusion solvents addresses the trade-off between adsorption and physical properties, providing a reversible, moldable, and cost-effective solution for gas adsorption and separation.

JP2024135022AInactive Publication Date: 2024-10-04KYOTO UNIV

Patent Information

Application Number
JP2023045510
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional porous gels face a trade-off between guest adsorption properties and physical properties, with existing gels either losing viscoelasticity when converted to aerogels or maintaining physical properties at the cost of adsorption capabilities.

Method used

A new type of porous gel is developed using metal-organic frameworks (MOFs) with size exclusion solvents, where MOF particles are bonded by physical cohesive forces to form a network structure, allowing for both guest molecule adsorption and viscoelasticity, with the gel being reversible.

Benefits of technology

The porous gel maintains both guest adsorption properties and viscoelasticity, enabling applications in gas adsorption and separation systems while being moldable and cost-effective compared to MOPs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135022000001_ABST
    Figure 2024135022000001_ABST
Patent Text Reader

Abstract

To provide a novel type of physical gel having both physical characteristics as a gel and a guest absorption characteristics as a porous material.SOLUTION: A porous gel according to the present invention includes a metal organic framework having voids in its molecules and a size-exclusion solvent having a molecular size that is too large to occupy the voids. The metal organic framework is configured to adsorb at least one type of guest molecule in the voids. The metal organic framework forms a plurality of particles, and the plurality of particles are bonded to each other by physical cohesion to form a network structure. The porous gel has a storage modulus E'(ω0) that is greater than a loss modulus E''(ω0) at at least one angular frequency (ω0) under ambient conditions.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to porous gels and methods for making the same. The present disclosure also relates to gas adsorption and separation systems that include the porous gels. [Background technology]

[0002] Porous materials such as zeolites, activated carbon, and metal-organic frameworks (MOFs) have been widely studied. In particular, porous MOFs, also known as porous coordination polymers (PCPs), are expected to be used in fields such as gas adsorption and gas separation.

[0003] Porous materials are usually used in a solid state. However, the range of applications of solid materials is limited in terms of fluidity, moldability, etc. Therefore, in recent years, research on porous materials as soft materials having forms other than solid has also been conducted.

[0004] For example, Non-Patent Document 1 and Patent Documents 1 and 2 disclose techniques related to so-called porous liquids. These disclosures aim to provide liquids with permanent porosity by dispersing organic cage molecules or MOFs in a liquid phase.

[0005] However, although porous liquids are considered suitable for application to circulating or flow-type systems, they are not necessarily suitable for applications requiring moldability.

[0006] Generally, a gel is a material that has the advantages of both a liquid and a solid, and has excellent flexibility and moldability. Therefore, research is being conducted to create a gel that exhibits permanent porosity.

[0007] For example, gels containing MOFs or metal-organic polyhedra (MOPs) are disclosed in Non-Patent Documents 2 and 3. These disclosures aim to provide gels that exhibit permanent porosity.

[0008] However, these gels are inevitably transformed into aerogels through an activation step to remove the solvent or gas molecules trapped in the pores during preparation, which gives them a permanent porosity but at the expense of the gel's characteristic viscoelasticity, meaning that these gels cannot exhibit guest adsorption properties without conversion to aerogels.

[0009] Thus, the present inventors have found that it is difficult for conventional porous gels to achieve both the guest adsorption properties of a porous material (permanent porosity) and the physical properties of a gel. That is, the present inventors have found that there is a trade-off relationship in which the physical properties of a gel are sacrificed in order to obtain the guest adsorption properties of a porous material, and the guest adsorption properties of a porous material are sacrificed in order to maintain the physical properties of a gel.

[0010] In the publications shown in Non-Patent Documents 4 to 6, the present inventors reported a porous gel using MOPs cross-linked with each other by a linker. This gel has both the viscoelasticity characteristic of a gel and permanent porosity.

[0011] However, in the above-mentioned MOP gel, MOPs must be crosslinked by covalent or coordinate bonds via a linker. The formation of such a chemical gel is an irreversible reaction, and once a gel is formed, it is difficult to re-form. In addition, the production cost of MOPs is generally significantly higher than that of MOFs. [Prior art documents] [Patent documents]

[0012]

Patent Document 1

Patent document 2

Non-licensed literature

[0013] [Non-licensed document 1] Giri, N., Del Popolo, M., Melaugh, G. et al. Liquids with permanent porosity. Nature 527, 216-220 (2015) [Non-licensed document 2] Carne-Sanchez, A., Craig, GA, Larpent, P. et al. Self-assembly of metal-organic polyhedra into supramolecular polymers with intrinsic microporosity. Nat Commun 9, 2506 (2018) [Non-licensed document 3] Jigwei Hou, Adam F. Sapnik and Thomas D. Bennett, Metal-Organic framework gels and monoliths, Chem. Sci. 2020, 11, 310

Non-licensed Document 4

Non-licensed Document 5

[0014] Therefore, an object of the present invention is to provide a new type of physical gel that has both the physical properties of a gel and the guest adsorption properties of a porous material. [Means for solving the problem]

[0015] For example, aspects of the present invention are as follows. [1] A porous gel comprising: a metal-organic framework having intramolecular voids; and a size-exclusion solvent having a molecular size such that the voids cannot be occupied by the metal-organic framework; the metal-organic framework is configured to be capable of adsorbing at least one type of guest molecule in the voids; the metal-organic framework forms a plurality of particles, the plurality of particles being bonded to each other by physical cohesion to form a network structure; and the storage modulus E'(ω0) is greater than the loss modulus E''(ω0) at at least one angular frequency ω0 under ambient conditions. [2] The porous gel according to [1], wherein the size exclusion solvent has a boiling point of 200°C or higher at standard pressure. [3] The porous gel according to [1] or [2], wherein the size exclusion solvent is at least one selected from the group consisting of liquid polymers, ionic liquids, and crown ethers. [4] The CO2 adsorption capacity of the porous gel at 303K and saturated vapor pressure is 0.5 cm 3 / g or more. [5] The porous gel according to any one of [1] to [4], wherein the CO2 adsorption amount per unit mass of the porous gel at 303 K and saturated vapor pressure is at least twice the CO2 adsorption amount per unit mass of the size exclusion solvent at 303 K and saturated vapor pressure. [6] The porous gel according to any one of [1] to [5], wherein the content of the metal organic framework in the porous gel is within a range of 1% by mass to 50% by mass. [7] The porous gel according to any one of [1] to [6], which is configured so as to be convertible into a sol by destroying at least a part of the network structure. [8] A gas adsorption system comprising the porous gel according to any one of [1] to [7]. [9] A gas separation system comprising the porous gel according to any one of [1] to [7].

[10] A method for producing a porous gel, comprising: forming a precursor gel containing a metal-organic framework having voids in its molecules and a first solvent; and exchanging the first solvent in the precursor gel with a second solvent, wherein the first solvent has a molecular size large enough to occupy the voids, and the second solvent has a molecular size large enough not to occupy the voids.

[11] The method according to

[10] , further comprising an activation step of removing gas or liquid molecules present in the pores.

[12] The method according to

[10] or

[11] , wherein the second solvent has a boiling point of 200°C or higher at standard pressure.

[13] The method according to any one of

[10] to

[12] , wherein the second solvent is at least one selected from the group consisting of a liquid polymer, an ionic liquid, and a crown ether.

[14] The method according to any of

[10] to

[13] , wherein the step of exchanging the first solvent for the second solvent includes the steps of exchanging the first solvent for a third solvent and exchanging the third solvent for the second solvent.

[15] The method of

[14] , wherein the third solvent has a higher miscibility with the second solvent than the first solvent. Effect of the Invention

[0016] According to the present invention, a new type of physical gel is provided that has both the physical properties of a gel and the guest adsorption properties of a porous material. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a conceptual diagram showing a method for producing a porous gel according to one embodiment of the present invention. [Diagram 2] FIG. 2 shows the experimental results on the reversibility of the Al-BTC precursor gel. [Diagram 3] FIG. 3 shows the CO 2 gas adsorption isotherm at 303 K for the porous gel (Al-BTC / PDMS-OH) according to Example 1. [Figure 4] FIG. 4 shows the results of viscoelasticity measurement in the compression mode of the porous gel (Al-BTC / PDMS-OH) according to Example 1. [Diagram 5] FIG. 5 shows the experimental results regarding the reversibility of the porous gel (Al-BTC / PDMS-OH) according to Example 1. [Figure 6] FIG. 6 shows the experimental results regarding the reversibility of the Al-ADC precursor gel. [Figure 7] FIG. 7 shows the CO 2 gas adsorption isotherm at 303 K for the porous gel (Al-ADC / PDMS-OH) according to Example 2. [Figure 8] FIG. 8 shows the results of viscoelasticity measurement in the compression mode of the porous gel (Al-ADC / PDMS-OH) according to Example 2. [Figure 9]FIG. 9 shows the experimental results on the reversibility of the Fe-BTC precursor gel. [Figure 10] FIG. 10 shows the CO 2 gas adsorption isotherm at 303 K for the porous gel (Fe-BTC / PDMS-OH) according to Example 3. [Figure 11] FIG. 11 shows the results of viscoelasticity measurement in a compression mode of the porous gel (Fe-BTC / PDMS-OH) according to Example 3. [Figure 12] FIG. 12 shows the experimental results on the reversibility of the Ga-BTC precursor gel. [Figure 13] FIG. 13 shows the CO 2 gas adsorption isotherm at 303 K for the porous gel (Ga-BTC / PDMS-OH) according to Example 4. [Figure 14] FIG. 14 shows the results of viscoelasticity measurement in a compression mode of the porous gel (Ga-BTC / PDMS-OH) according to Example 4. [Figure 15] FIG. 15 shows the CO 2 gas adsorption isotherm at 303 K for the porous gel (In-BTC / PDMS-OH) according to Example 5. [Figure 16] FIG. 16 shows the results of viscoelasticity measurement in a compression mode of the porous gel (In-BTC / PDMS-OH) according to Example 5. [Figure 17] FIG. 17 shows a CO 2 gas adsorption isotherm at 303 K for the size exclusion solvent (PDMS-OH) according to Comparative Example 1. [Figure 18] FIG. 18 shows the TGA profiles of the porous gel (Al-BTC / PEG) according to Example 6, the corresponding aerogel (Al-BTC), and the corresponding size exclusion solvent (PEG). [Figure 19] FIG. 19 shows the results of viscoelasticity measurement in the compression mode of the porous gel (Al-BTC / PEG) according to Example 6. [Figure 20] FIG. 20 shows the TGA profiles of the porous gel (Al-ADC / PEG) according to Example 7, the corresponding aerogel (Al-ADC), and the corresponding size exclusion solvent (PEG). [Figure 21] FIG. 21 shows the CO 2 gas adsorption isotherm at 303 K for the porous gel (Al-ADC / PEG) according to Example 7. [Figure 22] FIG. 22 shows the results of viscoelasticity measurement in the compression mode of the porous gel (Al-ADC / PEG) according to Example 7. [Figure 23] FIG. 23 shows the experimental results regarding the reversibility of the porous gel (Al-ADC / PEG) according to Example 7. [Figure 24] FIG. 24 shows the TGA profiles of the porous gel (Fe-BTC / PEG) according to Example 8, the corresponding aerogel (Fe-BTC), and the corresponding size exclusion solvent (PEG). [Diagram 25] FIG. 25 shows the CO2 gas adsorption isotherm at 303 K for the porous gel (Fe-BTC / PEG) according to Example 8. [Figure 26] FIG. 26 shows the results of viscoelasticity measurement in the compression mode of the porous gel (Fe-BTC / PEG) according to Example 8. [Figure 27] FIG. 27 shows the experimental results regarding the reversibility of the porous gel (Fe-BTC / PEG) according to Example 8. [Figure 28] FIG. 28 shows the TGA profiles of the porous gel (Ga-BTC / PEG) according to Example 9, the corresponding aerogel (Ga-BTC), and the corresponding size exclusion solvent (PEG). [Figure 29] FIG. 29 shows the results of viscoelasticity measurement in a compression mode of the porous gel (Ga-BTC / PEG) according to Example 9. [Diagram 30] FIG. 30 shows the TGA profiles of the porous gel according to Example 10 (In-BTC / PEG), the corresponding aerogel (In-BTC), and the corresponding size exclusion solvent (PEG). [Diagram 31] FIG. 31 shows the CO 2 gas adsorption isotherm at 303 K for the porous gel (In-BTC / PEG) according to Example 10. [Diagram 32]FIG. 32 shows the results of viscoelasticity measurement in the compression mode of the porous gel (In-BTC / PEG) according to Example 10. [Diagram 33] FIG. 33 shows a CO 2 gas adsorption isotherm at 303 K for the size exclusion solvent (PEG) according to Comparative Example 2. [Diagram 34] FIG. 34 shows the TGA profiles of the porous gel (Al-BTC / [BMIM][BF4]) according to Example 11, the corresponding aerogel (Al-BTC), and the corresponding size exclusion solvent ([BMIM][BF4]). [Diagram 35] FIG. 35 shows the CO2 gas adsorption isotherm at 303 K for the porous gel (Al-BTC / [BMIM][BF4]) according to Example 11. [Diagram 36] FIG. 36 shows the results of viscoelasticity measurement in compression mode of the porous gel (Al-BTC / [BMIM][BF4]) according to Example 11. [Figure 37] FIG. 37 shows the TGA profiles of the porous gel (Al-ADC / [EMIM][BF4]) according to Example 12, the corresponding aerogel (Al-ADC), and the corresponding size exclusion solvent ([EMIM][BF4]). [Figure 38] FIG. 38 shows the CO2 gas adsorption isotherm at 303 K for the porous gel (Al-ADC / [EMIM][BF4]) according to Example 12. [Figure 39] FIG. 39 shows the TGA profiles of the porous gel (Fe-BTC / [EMIM][BF]) according to Example 13, the corresponding aerogel (Fe-BTC), and the corresponding size exclusion solvent ([EMIM][BF]). [Diagram 40] FIG. 40 shows the CO2 gas adsorption isotherm at 303 K for the porous gel (Fe-BTC / [EMIM][BF4]) according to Example 13. [Diagram 41] FIG. 41 shows the results of viscoelasticity measurement in compression mode of the porous gel (Fe-BTC / [EMIM][BF4]) according to Example 13. [Diagram 42]FIG. 42 shows the TGA profiles of the porous gel (Ga-BTC / [EMIM][BF4]) according to Example 14, the corresponding aerogel (Ga-BTC), and the corresponding size exclusion solvent ([EMIM][BF4]). [Diagram 43] FIG. 43 shows the CO2 gas adsorption isotherm at 303 K for the porous gel (Ga-BTC / [EMIM][BF4]) according to Example 14. [Diagram 44] FIG. 44 shows the results of viscoelasticity measurement in a compression mode of the porous gel (Ga-BTC / [EMIM][BF4]) according to Example 14. [Diagram 45] FIG. 45 shows the experimental results regarding the reversibility of the porous gel (Ga-BTC / [EMIM][BF4]) according to Example 14. [Figure 46] FIG. 46 shows the TGA profiles of the porous gel (In-BTC / [EMIM][BF4]) according to Example 15, the corresponding aerogel (In-BTC), and the corresponding size exclusion solvent ([EMIM][BF4]). [Figure 47] FIG. 47 shows the results of viscoelasticity measurement in a compression mode of the porous gel (In-BTC / [EMIM][BF4]) according to Example 15. [Figure 48] FIG. 48 shows a CO2 gas adsorption isotherm at 303 K for the size exclusion solvent ([BMIM][BF4]) according to Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, a porous gel according to one embodiment of the present invention and a method for producing the same will be described. In addition, a gas adsorption system and a gas separation system including the above-mentioned porous gel will also be described. In addition, when referring to drawings or chemical formulas, components that perform the same or similar functions are given the same reference symbols or symbols, and duplicated descriptions will be omitted.

[0019] A porous gel according to one embodiment of the present invention includes a metal-organic framework (MOF) having a void in a molecule, and a size-excluded solvent having a molecular size that is large enough not to occupy the void. The MOF is configured to be able to adsorb at least one type of guest molecule in the void. The MOF forms a plurality of particles, and these particles are bonded to each other by physical cohesive force to form a network structure. That is, the porous gel according to this embodiment includes the MOF as a gelator and the size-excluded solvent as a swelling agent. The network structure is typically a colloidal network structure. The term "particle" here means an aggregate composed of two or more molecules, and there is no limitation on the shape. Each of the plurality of particles may be, for example, a zero-dimensional shape such as a sphere, a one-dimensional shape such as a rod or fiber, or a two-dimensional shape such as a sheet. Each of the plurality of particles is typically a nanoparticle. Furthermore, the term "physical cohesion" as used herein means non-covalent intermolecular interactions that are not mediated by distinct chemical bonds such as covalent bonds, coordinate bonds, and ionic bonds.

[0020] As the above-mentioned MOF, for example, one capable of forming a precursor gel described below can be used. That is, as the above-mentioned MOF, one capable of forming a network structure by bonding a plurality of MOF particles to each other by physical cohesive force can be used. Such a precursor gel can be obtained, for example, by controlling the rate of nanoparticle formation and their aggregation in a system containing MOF or its raw material and a solvent (see, for example, Non-Patent Document 3). The MOF may be crystalline or amorphous.

[0021] There is no limit to the type of MOF that can be used. By appropriately combining the type and coordination number of metal ions and the type and topology of multidentate ligands, MOFs having a desired structure can be produced. MOFs may contain two or more metal elements and may contain two or more multidentate ligands. MOFs are typically synthesized by reacting a metal ion donor with a multidentate ligand.

[0022] Examples of the metal element constituting the metal ion donor include any element belonging to alkali metals (Group 1), alkaline earth metals (Group 2), and transition metals (Groups 3 to 12). The metal element is typically selected from the group consisting of magnesium, calcium, iron, aluminum, zinc, copper, nickel, cobalt, zirconium, gallium, indium, and chromium. The metal ion donor may contain a plurality of metal elements. Alternatively, a plurality of metal ion donors containing different metal elements may be used in combination.

[0023] As the metal ion donor, typically, a metal salt is used. The metal ion donor may be an organic salt or an inorganic salt. The metal ion donor is typically selected from the group consisting of hydroxides, carbonates, acetates, sulfates, nitrates, and chlorides. A plurality of metal ion donors each containing the same metal element may be used in combination. The metal ion donor may be in the form of a so-called secondary building unit (SBU). As such a secondary building unit, any one used in the synthesis of known MOFs may be selected.

[0024] The polydentate ligand is typically an organic polydentate ligand, and is selected from the group consisting of, for example, a carboxylate anion, an amine compound, a sulfonate anion, a phosphate anion, and a heterocyclic compound. The carboxylate anion may be, for example, a dicarboxylate or tricarboxylate anion. Specific examples include anions of citric acid, malic acid, terephthalic acid, isophthalic acid, trimesic acid, and derivatives thereof. The heterocyclic compound may be, for example, bipyridine, imidazole, adenine, and derivatives thereof. A plurality of polydentate ligands may be used.

[0025] Examples of MOFs capable of forming precursor gels are given below in Table 1. These are merely examples and do not preclude the use of other MOFs. [Table 1-1] [Table 1-2] [Table 1-3]

[0026] The list of references cited in Table 1 is as follows: A1:Bart Bueken et al. Gel-based morphological design of zirconium metal-organic frameworks. Chem. Sci., 2017, 8, 3939-3948 A2:Tian Tian et al. Mechanically and chemically robust ZIF-8 monoliths with high volumetric adsorption capacity. J. Mater. Chem. A, 2015, 3, 2999-3005 A3:Abhijeet K. Chaudhari et al. Multifunctional Supramolecular Hybrid Materials Constructed from Hierarchical Self-Ordering of In Situ Generated Metal-Organic Framework (MOF) Nanoparticles. Advanced Materials, Volume 27, Issue 30, August 12, 2015, 4438-4446 A4:Li, L., Xiang, S., Cao, S. et al. A synthetic route to ultralight hierarchically micro / mesoporous Al(III)-carboxylate metal-organic aerogels. Nat Commun 4, 1774 (2013)

[0027] As described above, the MOF constituting the porous gel according to the present embodiment has pores in its molecule and is configured to be able to adsorb at least one type of guest molecule in the pores. That is, this porous gel has permanent porosity and can also be used as an adsorbent for the guest molecules. The guest molecules may be gas molecules or liquid molecules.

[0028] When the guest molecule is a gas molecule, examples thereof include hydrogen, oxygen, nitrogen, carbon monoxide, carbon dioxide, nitrogen compounds such as nitrous oxide, nitric oxide, and ammonia, sulfur compounds such as hydrogen sulfide and sulfur dioxide, aliphatic hydrocarbons such as methane, ethane, propane, and acetylene, rare gases such as argon and xenon, and halogen compounds such as chlorine and hydrogen bromide. The gas molecule may be a water molecule constituting water vapor. The gas molecule may also be a vapor formed by vaporizing a liquid molecule described later.

[0029] When the guest molecule is a liquid molecule, examples thereof include aliphatic hydrocarbons such as n-hexane; aromatic hydrocarbons such as benzene, toluene, and dichlorobenzene; ethers such as diethyl ether, tetrahydrofuran (THF), and 1,4-dioxane; halogenated hydrocarbons such as chloroform and dichloromethane; esters such as ethyl acetate; ketones such as acetone; nitriles such as acetonitrile; amides such as N,N-dimethylformamide (DMF); sulfoxides such as dimethyl sulfoxide (DMSO); carboxylic acids such as formic acid and acetic acid; alcohols such as methanol, ethanol, n-propanol, i-propanol, and n-butanol; and water. The guest molecule may be a gas molecule in the form of vapor of these liquid molecules.

[0030] The porous gel according to the present embodiment is configured to adsorb, for example, carbon dioxide molecules. The CO adsorption amount of the porous gel according to the present embodiment at 303 K and saturated vapor pressure is, for example, 0.5 cm 3 / g or more, preferably 0.8 cm 3 / g or more, and more preferably 1.0 cm 3 / g or more. The CO2 adsorption amount per unit mass of the porous gel according to this embodiment at 303K and saturated vapor pressure is, for example, 2.0 times or more, preferably 2.5 times or more, and more preferably 3.0 times or more, compared to that of the size exclusion solvent alone. Here, the above CO2 adsorption amount is based on the value measured using BELSORP-max (Microtrack BEL Co., Ltd.) after activating the sample at 120°C for 12 hours.

[0031] As described above, the MOF constituting the porous gel according to the present embodiment forms a plurality of particles, and these particles are bonded to each other by physical cohesion to form a network structure. This porous gel is typically a physical gel that forms a colloidal network non-covalently, and a size exclusion solvent, which will be described later, is encapsulated inside the network structure.

[0032] Each of the plurality of particles is typically a nano-sized colloid particle having a diameter of 1 nm to 100 nm, that is, the porous gel is typically a colloid gel.

[0033] The colloidal gel can be prepared in a size of, for example, 100 nm to 10 cm or more. When the size of the colloidal gel is smaller than 1 μm, the gel is a nanogel or a gel nanoparticle.

[0034] As described above, the size-exclusion solvent constituting the porous gel according to this embodiment has a molecular size that is too large to occupy the pores of the MOF. By using such a size-exclusion solvent, it becomes possible to achieve both guest adsorption properties utilizing the pores of the MOF and physical properties as a gel in the porous gel. More specifically, this porous gel can maintain the viscoelasticity of a gel even after undergoing the above-mentioned activation process.

[0035] The size exclusion solvent preferably has a high boiling point and / or low volatility (or non-volatility). For example, the boiling point of the size exclusion solvent at standard pressure is 200° C. or higher. In such a case, the size exclusion solvent in the porous gel is less likely to evaporate, so that a more stable porous gel is obtained. In addition, the stability against the above-mentioned activation step is also higher.

[0036] As the size exclusion solvent, for example, at least one solvent selected from the group consisting of liquid polymers, ionic liquids, and crown ethers can be used. As the liquid polymer, for example, PEG (PEG-400; molecular weight: about 400, boiling point at 1013 hPa: 200° C. or higher, vapor pressure at 20° C.: less than 0.1 hPa), PDMS-OH (boiling point: 200° C. or higher, viscosity: about 65 cst), PDMS-PH, or a similar polymer can be used. As the ionic liquid, for example, [BMIM][BF4] (ignition point: about 288° C., vapor pressure: less than 0.000125 hPa), [EMIM][BF4] (boiling point at 1013 hPa: about 350° C.), [Bpy][NTf2], [N 8,8,8,1 [NTF2] or a similar ionic liquid can be used. As the crown ether, for example, 15-crown-5 (boiling point at 0.05 Torr: about 95° C., flash point: 113° C.) or 18-crown-6 (melting point: about 40° C., boiling point at 0.2 Torr: 116° C.) can be used. The size exclusion solvent may be selected from those outside these categories. The specific type of size exclusion solvent can be appropriately selected depending on the pore size of the MOF to be used, etc.

[0037] In the porous gel according to this embodiment, the storage modulus E'(ω0) is greater than the loss modulus E''(ω0) at at least one angular frequency ω0 under ambient conditions. That is, this porous gel has viscoelasticity specific to gels. Therefore, this porous gel has both guest adsorption properties utilizing the pores of the MOF and physical properties as a gel.

[0038] The measurement is performed as follows using an AR-G2 rheometer (manufactured by TA Instruments). First, a sample is placed on a glass slide with a thickness of about 1 mm. The glass slide is set in the above-mentioned device, and measurement is performed by frequency sweep in compression mode with 1% strain amplitude in the linear region (initial strain is fixed at 1.5%). The frequency sweep is performed in the range of 0.1 rad / s to 100 rad / s. Then, it is checked whether there is a frequency ω0 within this range where E'(ω0)>E''(ω0).

[0039] As described above, the porous gel according to this embodiment is a physical gel that utilizes the cohesive force between MOF particles. A physical gel is a reversible gel formed non-covalently, and can typically be resolubilized by an external stimulus. That is, the porous gel according to this embodiment can typically be converted into a sol by destroying at least a part of the above-mentioned network structure. Furthermore, this sol can typically be returned to a gel again. By utilizing such a reversible process, for example, the shape of a porous gel that has been formed once can be freely converted into a different shape by solization and regelation.

[0040] The external stimuli include, for example, changes in the concentration of MOF, the composition of the solvent, and pH. The external stimuli may be a mixing and dispersion promoting process such as sonication, and a mechanical stimuli such as a stirring process using a shaker. Here, it is preferable that the external stimuli do not include temperature changes such as heating. That is, it is preferable that the porous gel according to this embodiment is stable against the mild heating applied in the activation step.

[0041] In the porous gel according to this embodiment, the content of MOF in the gel is, for example, 1% by mass or more, preferably 2% by mass or more, and more preferably 4% by mass or more. The content of MOF in the gel is, for example, 50% by mass or less, preferably 40% by mass or less, and more preferably 30% by mass. Any combination of these upper and lower limits is possible. If this content is too small, the amount of adsorption of guest molecules may be insufficient. If this content is too large, it may be difficult to form a gel, or the viscoelasticity of the gel may be insufficient. The porous gel according to this embodiment may contain two or more types of MOFs and may contain two or more types of size exclusion solvents.

[0042] The content of MOF in the porous gel is determined as follows. Three samples, namely, the porous gel, the corresponding aerogel, and the corresponding size exclusion solvent, are prepared and subjected to thermogravimetric analysis (TGA) measurement. This measurement is performed by heating each sample from 30°C to 500°C at a rate of 10°C / min under a nitrogen atmosphere. Then, the amount of residue (mass%) at 500°C is measured for each sample.

[0043] Here, each symbol is R PG : Amount of porous gel residue R AG : Amount of aerogel residue R SES : Residual amount of size exclusion solvent c MOF : MOF content in the porous gel With this definition, the porous gel contains MOFs and size-exclusion solvent, while the aerogel contains only MOFs, and the following relationship holds:

number

[0044] Therefore, c MOF and its percentage notation C MOFis calculated by the following formula: In this way, the content C of MOF in the porous gel is MOF (% by mass) is calculated.

number

number

[0045] The porous gel can be produced, for example, as follows. That is, first, a precursor gel containing MOFs having pores in their molecules and a first solvent is formed. Next, in this precursor gel, the first solvent is exchanged for a second solvent. Here, the first solvent has a molecular size large enough to occupy the pores, and the second solvent has a molecular size large enough not to occupy the pores. That is, the second solvent is the same as the size-exclusion solvent described above.

[0046] Fig. 1 is a conceptual diagram showing a method for producing a porous gel according to one embodiment of the present invention. In the example shown in Fig. 1, a metal ion donor and a multidentate ligand are reacted to form a plurality of MOF particles. Next, these particles are bonded to each other by physical cohesion to form a network structure, thereby forming a precursor gel. After that, a solvent exchange process is performed to form the porous gel according to this embodiment. The above-mentioned porous gel may be produced by other methods.

[0047] The precursor gel may be, for example, the known MOF gel described above. In the precursor gel, a plurality of MOF particles are bonded to each other by physical cohesion to form a network structure, and the first solvent is encapsulated in the network structure. In the precursor gel, the pores of the MOF are typically occupied by the first solvent or gas molecules that were present in the system during the synthesis.

[0048] As the first solvent, for example, a solvent used in the preparation of the precursor gel can be used. Examples of the first solvent include those exemplified above as liquid molecules as guest molecules. As the first solvent, for example, amides such as N,N-dimethylformamide (DMF), sulfoxides such as dimethylsulfoxide (DMSO), ketones such as acetone, alcohols such as methanol, ethanol, n-propanol, i-propanol, and n-butanol, or water can be used. As the first solvent, a mixture of multiple solvents may be used.

[0049] As the second solvent, for example, the size exclusion solvent described above can be used. The solvent exchange from the first solvent to the second solvent is performed, for example, by immersion. By this solvent exchange, most of the first solvent is replaced with the second solvent. In this state, the pores of the MOF may be occupied by the first solvent or gas molecules that were present in the system during the synthesis. However, these pores are not occupied by the second solvent. As the second solvent, a mixture of multiple solvents may be used.

[0050] The method may further comprise, after the solvent exchange step, an activation step for removing gas or liquid molecules present in the pores. This activation step may comprise, for example, heating the porous gel at a temperature higher than the boiling point of the first solvent and lower than the boiling point of the second solvent, which renders the pores of the MOF unoccupied and makes the porous gel in a state more suitable for the adsorption of guest molecules, i.e. permanently porous.

[0051] The above-mentioned solvent exchange step may be carried out stepwise. That is, the step of exchanging the first solvent with the second solvent may include a step of exchanging the first solvent with a third solvent and a step of exchanging the third solvent with the second solvent. In this case, the third solvent typically has a molecular size large enough to occupy the pores. A mixture of multiple solvents may be used as the third solvent.

[0052] The third solvent preferably has a higher miscibility with the second solvent (co-solvent miscibility) than the first solvent. In this case, the solvent exchange from the third solvent to the second solvent is thermodynamically and / or kinetically more likely to occur than the solvent exchange from the first solvent to the second solvent. The miscibility between the first solvent and the third solvent can be experimentally determined. For example, this comparison can be performed by dropping the first and third solvents into the same amount of the second solvent and visually observing the degree of mixing of the two.

[0053] In the porous gel thus obtained, the MOF particles are bonded to each other by physical cohesion to form a network structure. That is, this porous gel is a physical gel capable of reversible sol-gel transition. Therefore, in the porous gel obtained by the above method, the gel can be reformed through a sol state. That is, the above manufacturing method may further include a step of converting the obtained porous gel into a sol and a step of returning the sol to a gel again. By utilizing such a reversible process, for example, the shape of a porous gel once formed can be freely converted into a different shape by solization and regelation.

[0054] As described above, the porous gel according to this embodiment is a new type of physical gel that has both the physical properties of a gel and the guest adsorption properties of a porous material. Such gels are advantageous in that they can be flexibly molded compared to conventional chemical gels. In addition, by using MOFs, which have been widely studied, the gels can be manufactured at low cost compared to, for example, the use of MOPs. In addition, by further functionalizing MOFs, it is possible to impart new properties to the porous gel.

[0055] The porous gel according to this embodiment can exhibit excellent guest adsorption properties because the pores of the MOF can be utilized. Therefore, such gels can be applied in fields such as gas adsorption or gas separation. For example, in gas adsorption systems and gas separation systems using existing porous materials, new gas adsorption systems and gas separation systems can be provided by replacing the porous material with a porous gel. Alternatively, new types of gas adsorption systems and gas separation systems can be provided by taking advantage of the physical properties of the gel and arranging it differently from conventional solid or liquid porous materials. EXAMPLES

[0056] The above porous gel will now be further described with reference to examples.

[0057] In the following examples, hydroxy-terminated poly(dimethylsiloxane) [PDMS-OH] and poly(dimethylsiloxane-co-methylphenylsiloxane) [PDMS-Ph] were purchased from Sigma-Aldrich and used as received. 1-Butyl-3-methylimidazolium tetrafluoroborate ([BMIM][BF4]), 1-ethyl-3-methylimidazolium tetrafluoroborate ([EMIM][BF4]), polyethylene glycol 400 (PEG), 1,3,5-benzenetricarboxylic acid (H3BTC), and 5-aminoisophthalic acid (H2ADC) were purchased from Tokyo Chemical Industry Co., Ltd. Al(NO3)3·9H2O, Fe(NO3)3·9H2O, Ga(NO3)3·nH2O, and In(NO3)3·nH2O were provided by Nacalai Tesque. Solvents were purchased from Wako Pure Chemicals, except for HPLC grade, which were purchased from Fisher Chemical Co.

[0058] Example 1: Al-BTC / PDMS-OH A porous gel containing Al-BTC [MIL-100(Al)] as the MOF and PDMS-OH as the size-exclusion solvent was synthesized as follows.

[0059] Synthesis of Al-BTC precursor gel 212 mg (1 mmol) of 1,3,5-benzenetricarboxylic acid and 375 mg (1 mmol) of Al(NO3)3·9H2O were each dissolved in 2.5 mL of ethanol. The two solutions were then mixed under stirring. The resulting solution was transferred into a sealed syringe and heated at 80 °C overnight. After gelation, a fresh gel was transferred to a vial for the next washing procedure. The gel was washed twice with ethanol and three times with acetone, replacing the solvent with fresh ones every day. At this stage, the obtained gel corresponds to the "precursor gel", ethanol corresponds to the "first solvent", and acetone corresponds to the "third solvent".

[0060] Reformation of Al-BTC precursor gel To confirm that the Al-BTC precursor gel before washing with acetone is a "physical gel," the following experiment was performed. First, ethanol was added to the obtained ethanol-containing Al-BTC precursor gel, and the gel was stirred with a shaker and ultrasonicated with an ultrasonic generator. The obtained sample was then heated at 80°C in a sealed container.

[0061] Figure 2 shows the experimental results on the reversibility of the Al-BTC precursor gel. As shown in the figure, the Al-BTC precursor gel could be returned to a sol state by the first step. Then, by the second step, the sol could be reformed as a gel with about twice the volume. From the above results, it was found that the Al-BTC precursor gel exhibits a reversible phase transition from gel to sol to gel by destruction and reformation of the network structure.

[0062] Synthesis of Al-BTC / PDMS-OH gel by solvent exchange The precursor gel in acetone obtained as above was immersed in PDMS-OH for 3 days, exchanging it with fresh PDMS-OH every day. As a result, most of the acetone in the gel was exchanged with PDMS-OH, and an Al-BTC / PDMS-OH gel was obtained. At this stage, the obtained gel corresponds to a "porous gel", Al-BTC corresponds to a "MOF", and PDMS-OH corresponds to a "size-exclusion solvent" or "second solvent".

[0063] Guest adsorption properties To confirm that the obtained samples had "porosity", CO2 adsorption measurements were performed. Specifically, the CO2 gas adsorption isotherm of the gel at 303 K was recorded using a BELSORP-max volumetric adsorption apparatus (Microtrack-Bell Corporation). Prior to the gas adsorption measurements, the samples were activated at 120 °C for 12 h.

[0064] Fig. 3 shows a CO2 gas adsorption isotherm at 303 K for the porous gel (Al-BTC / PDMS-OH) according to Example 1. In Fig. 3 and the adsorption measurement data shown below, the filled data points indicate the amount of adsorption when the pressure is increased, and the open data points indicate the amount of adsorption when the pressure is decreased.

[0065] As shown in Figure 3, the CO2 adsorption capacity of this gel at 303 K and saturated vapor pressure is 1.434 cm 3 This adsorption amount was 0.328 cm3 / g, which is the same as the adsorption amount for PDMS-OH alone (described later). 3 / g), which was about 4.37 times that of the porous gel of Example 1. This result indicates that pores of the MOF are present in the porous gel of Example 1.

[0066] Viscoelasticity Viscoelasticity measurements were performed to confirm that the obtained samples had the properties of a "gel". Rheological measurements of the gel were performed using a stress-controlled AR-G2 rheometer (TA Instruments). First, the gel sample after synthesis was carefully transferred to a clean glass slide (approximately 1 mm thick). The gel was then placed in the rheometer together with the glass slide for rheological testing. The gel was measured by frequency sweep in compression mode with 1% strain amplitude in the linear region (initial strain was fixed at 1.5%).

[0067] Fig. 4 shows the results of viscoelasticity measurement in a compression mode of the porous gel (Al-BTC / PDMS-OH) according to Example 1. In Fig. 4 and in the viscoelasticity measurement data shown below, the filled data points indicate the storage modulus E', and the open data points indicate the loss modulus E''.

[0068] As shown in FIG. 4, in this gel, E'(ω)>E''(ω) was established at all angular frequencies ω measured. This result indicates that the porous gel of Example 1 has physical properties as a gel.

[0069] As shown in FIG. 4, in the porous gel of Example 1, the change in both E'(ω) and E''(ω) due to the angular frequency was not large. Furthermore, E'(ω) was about one order of magnitude larger than E''(ω). In particular, the storage modulus E'(1) at 1 rad / s was 40.77 MPa.

[0070] Reformation of porous gel In order to confirm that the porous gel (Al-BTC / PDMS-OH) obtained as described above is a "physical gel," the following experiment was carried out. That is, first, a part of the obtained porous gel was placed in an ethanol solvent, and agitated with a shaker and ultrasonicated with an ultrasonic generator. Next, the obtained sample was transferred into a syringe. After that, the sample in the syringe was heated to 80°C to remove the ethanol.

[0071] FIG. 5 shows the experimental results regarding the reversibility of the porous gel (Al-BTC / PDMS-OH) according to Example 1. As shown in the figure, the Al-BTC / PDMS-OH gel could be returned to a sol state by the above-mentioned first and second steps. Then, the obtained sol could be reformed as a gel by the above-mentioned third step. From the above results, it was found that the Al-BTC / PDMS-OH gel exhibits a reversible phase transition from gel to sol to gel by destruction and reformation of the network structure.

[0072] This result suggests that reversible morphology control by solization and regelation is possible in the porous gel of Example 1. In this example, changes in the concentration of MOF and the composition of the solvent, as well as stirring with a shaker and ultrasonic treatment with an ultrasonic generator, were used as representative external stimuli, but other external stimuli can also be used.

[0073] Example 2 Al-ADC / PDMS-OH A porous gel containing Al-ADC(CAU-10-NH2) as the MOF and PDMS-OH as the size-exclusion solvent was synthesized as follows.

[0074] Synthesis of Al-ADC precursor gel 217 mg (1.2 mmol) of 5-aminoisophthalic acid and 450 mg (1.2 mmol) of Al(NO3)3·9H2O were each dissolved in 2 mL of ethanol. The two solutions were then mixed under stirring. The resulting solution was transferred into a sealed syringe and heated at 80 °C overnight. After gelation, a fresh gel was transferred into a vial for the next washing procedure. The gel was washed twice with ethanol and three times with acetone, replacing the solvent with fresh solvent every day.

[0075] Reformation of Al-ADC precursor gel To confirm that the Al-ADC precursor gel before washing with acetone was a "physical gel," an experiment similar to that described in Example 1 was carried out.

[0076] Figure 6 shows the experimental results on the reversibility of the Al-ADC precursor gel. As shown in the figure, the Al-ADC precursor gel was able to return to a sol state by the above-mentioned first step. Then, by the above-mentioned second step, the sol was able to reform into a gel with approximately twice the volume. From the above results, it was found that the Al-ADC precursor gel exhibits a reversible phase transition from gel to sol to gel by destruction and reformation of the network structure.

[0077] Synthesis of Al-ADC / PDMS-OH gel by solvent exchange The solvent was exchanged from acetone to PDMS-OH in the same manner as in Example 1. In this manner, an Al-ADC / PDMS-OH gel was obtained.

[0078] Guest adsorption properties CO2 adsorption measurements were carried out in the same manner as in Example 1.

[0079] 7 shows the CO2 gas adsorption isotherm at 303 K for the porous gel (Al-ADC / PDMS-OH) according to Example 2. As shown in FIG. 7, the CO2 adsorption amount of this gel at 303 K and saturated vapor pressure is 1.433 cm 3 This adsorption amount was 0.328 cm3 / g, which is the same as the adsorption amount for PDMS-OH alone (described later). 3 / g), which was about 4.37 times that of the porous gel of Example 2. This result indicates that pores of the MOF are present in the porous gel of Example 2.

[0080] Viscoelasticity The viscoelasticity was measured in the same manner as in Example 1.

[0081] Fig. 8 shows the results of viscoelasticity measurement in the compression mode of the porous gel (Al-ADC / PDMS-OH) according to Example 2. As shown in Fig. 8, in this gel, E'(ω)>E''(ω) holds in the region of ω<3 rad / s. This result indicates that the porous gel according to Example 2 has physical properties as a gel.

[0082] As shown in FIG. 8, in the porous gel of Example 2, the magnitudes of E'(ω) and E''(ω) were reversed depending on the angular frequency. In other words, this gel was found to exhibit thixotropy. In addition, the storage modulus E'(1) at 1 rad / s was 22.24 kPa.

[0083] Example 3: Fe-BTC / PDMS-OH A porous gel containing Fe-BTC [MIL-100(Fe)] as the MOF and PDMS-OH as the size-exclusion solvent was synthesized as follows.

[0084] Synthesis of Fe-BTC precursor gel 212 mg (1 mmol) of 1,3,5-benzenetricarboxylic acid and 404 mg (1 mmol) of Fe(NO3)3·9H2O were each dissolved in 5 mL of ethanol. The two solutions were then mixed under stirring. The resulting solution was transferred into a sealed syringe and left at room temperature for a few minutes. After gelation, a fresh gel was transferred into a vial for the next washing procedure. The gel was washed twice with ethanol and three times with acetone, replacing the solvent with fresh ones every day.

[0085] Reformation of the Fe-BTC precursor gel To confirm that the Fe-BTC precursor gel before washing with acetone was a "physical gel," an experiment was performed in the same manner as described in Example 1, except that the heating in the second step was performed unsealed and at 40°C instead of sealed and at 80°C.

[0086] Figure 9 shows the experimental results on the reversibility of the Fe-BTC precursor gel. As shown in the figure, the Fe-BTC precursor gel could be returned to a sol state by the first step described above. Then, the sol could be reformed as a gel by the second step described above. From the above results, it was found that the Fe-BTC precursor gel exhibits a reversible phase transition from gel to sol to gel by destruction and reformation of the network structure.

[0087] Synthesis of Fe-BTC / PDMS-OH gel by solvent exchange The solvent was exchanged from acetone to PDMS-OH in the same manner as in Example 1. In this manner, an Fe-BTC / PDMS-OH gel was obtained.

[0088] Guest adsorption properties CO2 adsorption measurements were carried out in the same manner as in Example 1.

[0089] 10 shows a CO2 gas adsorption isotherm at 303 K for the porous gel (Fe-BTC / PDMS-OH) according to Example 3. As shown in FIG. 10, the CO2 adsorption amount of this gel at 303 K and saturated vapor pressure is 1.505 cm 3 This adsorption amount was 0.328 cm3 / g, which is the same as the adsorption amount for PDMS-OH alone (described later). 3 / g), which was about 4.59 times that of the porous gel of Example 3. This result indicates that pores of the MOF are present in the porous gel of Example 3.

[0090] Viscoelasticity The viscoelasticity was measured in the same manner as in Example 1.

[0091] Fig. 11 shows the results of viscoelasticity measurement in the compression mode of the porous gel (Fe-BTC / PDMS-OH) according to Example 3. As shown in Fig. 11, in this gel, E'(ω)>E''(ω) holds in the region of ω<2 rad / s. This result indicates that the porous gel according to Example 3 has physical properties as a gel.

[0092] As shown in FIG. 11, in the porous gel of Example 3, the magnitudes of E'(ω) and E''(ω) were reversed depending on the angular frequency. In other words, this gel was found to exhibit thixotropy. In addition, the storage modulus E'(1) at 1 rad / s was 57.48 kPa.

[0093] Example 4 Ga-BTC / PDMS-OH A porous gel containing Ga-BTC [MIL-68(Ga)] as the MOF and PDMS-OH as the size-exclusion solvent was synthesized as follows.

[0094] Synthesis of Ga-BTC precursor gel 212 mg (1 mmol) of 1,3,5-benzenetricarboxylic acid and 256 mg (1 mmol) of Ga(NO3)3·nH2O were each dissolved in 5 mL of ethanol. The two solutions were then mixed under stirring. The resulting solution was transferred into a sealed syringe and heated at 40 °C overnight. After gelation, a fresh gel was transferred to a vial for the next washing procedure. The gel was washed twice with ethanol and three times with acetone, replacing the solvent with fresh solvent every day.

[0095] Reformation of Ga-BTC precursor gel To confirm that the Ga-BTC precursor gel before washing with acetone was a "physical gel," an experiment similar to that described in Example 1 was carried out.

[0096] Figure 12 shows the experimental results on the reversibility of the Ga-BTC precursor gel. As shown in the figure, the Ga-BTC precursor gel could be returned to a sol state by the first step. Then, by the second step, the sol could be reformed as a gel with about twice the volume. From the above results, it was found that the Ga-BTC precursor gel exhibits a reversible phase transition from gel to sol to gel by destruction and reformation of the network structure.

[0097] Synthesis of Ga-BTC / PDMS-OH gel by solvent exchange The solvent was exchanged from acetone to PDMS-OH in the same manner as in Example 1. In this manner, a Ga-BTC / PDMS-OH gel was obtained.

[0098] Guest adsorption properties CO2 adsorption measurements were carried out in the same manner as in Example 1.

[0099] 13 shows a CO2 gas adsorption isotherm at 303 K for the porous gel (Ga-BTC / PDMS-OH) according to Example 4. As shown in FIG. 13, the CO2 adsorption amount of this gel at 303 K and saturated vapor pressure is 1.400 cm 3 This adsorption amount was 0.328 cm3 / g, which is the same as the adsorption amount for PDMS-OH alone (described later). 3 / g), which was about 4.27 times that of the porous gel of Example 4. This result indicates that pores of the MOF are present in the porous gel of Example 4.

[0100] Viscoelasticity The viscoelasticity was measured in the same manner as in Example 1.

[0101] FIG. 14 shows the results of viscoelasticity measurement in the compression mode of the porous gel (Ga-BTC / PDMS-OH) according to Example 4. As shown in FIG. 14, in this gel, E'(ω)>E''(ω) was established at all angular frequencies ω measured. This result indicates that the porous gel according to Example 4 has physical properties as a gel.

[0102] As shown in FIG. 14, in the porous gel of Example 4, both E'(ω) and E''(ω) increased monotonically with respect to the angular frequency. Furthermore, E'(ω) was approximately one order of magnitude larger than E''(ω). In particular, the storage modulus E'(1) at 1 rad / s was 34.43 kPa.

[0103] Example 5: In-BTC / PDMS-OH A porous gel containing In-BTC [MIL-68(In)] as the MOF and PDMS-OH as the size-exclusion solvent was synthesized as follows.

[0104] Synthesis of In-BTC precursor gel 212 mg (1 mmol) of 1,3,5-benzenetricarboxylic acid and 301 mg (1 mmol) of In(NO3)3·nH2O were each dissolved in 5 mL of ethanol. The two solutions were then mixed under stirring. The resulting solution was transferred into a sealed syringe and heated at 40 °C overnight. After gelation, a fresh gel was transferred into a vial for the next washing procedure. The gel was washed twice with ethanol and three times with acetone, replacing the solvent with fresh solvent every day.

[0105] Synthesis of In-BTC / PDMS-OH gel by solvent exchange The solvent was exchanged from acetone to PDMS-OH in the same manner as in Example 1. In this manner, an In-BTC / PDMS-OH gel was obtained.

[0106] Guest adsorption properties CO2 adsorption measurements were carried out in the same manner as in Example 1.

[0107] 15 shows the CO2 gas adsorption isotherm at 303 K for the porous gel (In-BTC / PDMS-OH) according to Example 5. As shown in FIG. 15, the CO2 adsorption amount of this gel at 303 K and saturated vapor pressure is 1.721 cm 3 This adsorption amount was 0.328 cm3 / g, which is the same as the adsorption amount for PDMS-OH alone (described later). 3 / g), which was about 5.25 times that of the porous gel of Example 5. This result indicates that pores of the MOF are present in the porous gel of Example 5.

[0108] Viscoelasticity The viscoelasticity was measured in the same manner as in Example 1.

[0109] FIG. 16 shows the results of viscoelasticity measurement in the compression mode of the porous gel (In-BTC / PDMS-OH) according to Example 5. As shown in FIG. 16, in this gel, E'(ω)>E''(ω) was established at all angular frequencies ω measured. This result indicates that the porous gel according to Example 5 has physical properties as a gel.

[0110] As shown in FIG. 16, in the porous gel of Example 5, the change in both E'(ω) and E''(ω) due to the angular frequency was not large. Furthermore, E'(ω) was about one order of magnitude larger than E''(ω). In particular, the storage modulus E'(1) at 1 rad / s was 18.84 kPa.

[0111] (Comparative example 1; PDMS-OH) As a comparative example, the guest adsorption characteristics of PDMS-OH itself were evaluated. Specifically, CO2 adsorption measurements were performed in the same manner as in Example 1.

[0112] 17 shows the CO2 gas adsorption isotherm of the size-exclusion solvent (PDMS-OH) according to Comparative Example 1 at 303 K. As shown in FIG. 17, the CO2 adsorption amount of this liquid at 303 K and saturated vapor pressure is 0.328 cm 3 / g.

[0113] Since this PDMS-OH was a liquid, it was not possible to measure its viscoelasticity. The viscosity of PDMS-OH was about 65 cst.

[0114] Example 6 Al-BTC / PEG A porous gel containing Al-BTC as the MOF and PEG as the size-exclusion solvent was synthesized as follows: First, an Al-BTC precursor gel was synthesized in the same manner as in Example 1. Then, an Al-BTC / PEG gel was synthesized by solvent exchange in the same manner as in Example 1, except that PEG was used instead of PDMS-OH.

[0115] Determination of MOF content TGA measurements were performed to determine the content of Al-BTC in the Al-BTC / PEG gel. Specifically, measurements were performed using a Rigaku Thermo plus EVO2 under nitrogen atmosphere at temperatures ranging from room temperature to 500 °C with a heating rate of 10 °C / min. The measurements were performed for the porous gel (Al-BTC+PEG), aerogel (Al-BTC), and size exclusion solvent (PEG).

[0116] The aerogel was prepared by applying a supercritical CO2 drying process to the precursor gel in acetone obtained as described above. The drying process was carried out in a SCLEAD-2BD autoclave (KISCO) using supercritical CO2 at 14 MPa and 50°C.

[0117] FIG. 18 shows the TGA profiles of the porous gel (Al-BTC / PEG) according to Example 6, the corresponding aerogel (Al-BTC), and the corresponding size exclusion solvent (PEG). As shown in FIG. PG =1.68% by mass, R AG =65.33% by mass, R SES = 0 mass%. Therefore, the content of MOF in the porous gel, C MOF was calculated to be 2.6% by mass.

[0118] Viscoelasticity The viscoelasticity was measured in the same manner as in Example 1.

[0119] Fig. 19 shows the results of viscoelasticity measurement in compression mode of the porous gel (Al-BTC / PEG) according to Example 6. As shown in Fig. 19, in this gel, E'(ω)>E''(ω) was established at all angular frequencies ω measured. This result indicates that the porous gel according to Example 6 has physical properties as a gel.

[0120] As shown in FIG. 19, in the porous gel of Example 6, the change in both E'(ω) and E''(ω) due to the angular frequency was not large. Furthermore, E'(ω) was about one order of magnitude larger than E''(ω). In particular, the storage modulus E'(1) at 1 rad / s was 1.56 kPa.

[0121] Example 7 Al-ADC / PEG A porous gel containing Al-ADC as the MOF and PEG as the size-exclusion solvent was synthesized as follows: First, an Al-ADC precursor gel was synthesized in the same manner as in Example 2. Then, an Al-ADC / PEG gel was synthesized by solvent exchange in the same manner as in Example 2, except that PEG was used instead of PDMS-OH.

[0122] Determination of MOF content TGA measurements were performed to determine the content of Al-ADC in the Al-ADC / PEG gel. This measurement was performed for each of the porous gel (Al-ADC+PEG), aerogel (Al-ADC), and size exclusion solvent (PEG). The aerogel was prepared in the same manner as in Example 6.

[0123] FIG. 20 shows the TGA profiles of the porous gel (Al-ADC / PEG) according to Example 7, the corresponding aerogel (Al-ADC), and the corresponding size exclusion solvent (PEG). As shown in FIG. PG =6.68% by mass, R AG =76.04% by mass, R SES = 0 mass%. Therefore, the content of MOF in the porous gel, C MOF was calculated to be 11.0 mass%.

[0124] Guest adsorption properties CO2 adsorption measurements were carried out in the same manner as in Example 1.

[0125] Fig. 21 shows the CO2 gas adsorption isotherm at 303 K for the porous gel (Al-ADC / PEG) according to Example 7. As shown in Fig. 21, the CO2 adsorption amount of this gel at 303 K and saturated vapor pressure is 1.301 cm 3 This adsorption amount was 0.312 cm / g, which is the same as the adsorption amount for PEG alone (described later). 3 / g), which was about 4.17 times that of the porous gel of Example 7. This result indicates that pores of the MOF are present in the porous gel of Example 7.

[0126] Viscoelasticity The viscoelasticity was measured in the same manner as in Example 1.

[0127] Fig. 22 shows the results of viscoelasticity measurement in compression mode of the porous gel (Al-ADC / PEG) according to Example 7. As shown in Fig. 22, in this gel, E'(ω)>E''(ω) was established at all angular frequencies ω measured. This result indicates that the porous gel according to Example 7 has physical properties as a gel.

[0128] As shown in FIG. 22, in the porous gel of Example 7, the change in both E'(ω) and E''(ω) due to the angular frequency was not large. Furthermore, E'(ω) was about one order of magnitude larger than E''(ω). In particular, the storage modulus E'(1) at 1 rad / s was 45.17 kPa.

[0129] Reformation of porous gel In order to confirm that the porous gel (Al-ADC / PEG) obtained as described above is a "physical gel", an experiment similar to that described in Example 1 was carried out.

[0130] FIG. 23 shows the experimental results regarding the reversibility of the porous gel (Al-ADC / PEG) according to Example 7. As shown in the figure, the Al-ADC / PEG gel could be returned to a sol state by the above-mentioned first and second steps. Then, the obtained sol could be reformed as a gel by the above-mentioned third step. From the above results, it was confirmed that the Al-ADC / PEG gel shows a reversible phase transition from gel to sol to gel by the destruction and reformation of the network structure.

[0131] Example 8 Fe-BTC / PEG A porous gel containing Fe-BTC as the MOF and PEG as the size-exclusion solvent was synthesized as follows: First, an Fe-BTC precursor gel was synthesized in the same manner as in Example 3. Then, an Fe-BTC / PEG gel was synthesized by solvent exchange in the same manner as in Example 3, except that PEG was used instead of PDMS-OH.

[0132] Determination of MOF content TGA measurements were performed to determine the Fe-BTC content in the Fe-BTC / PEG gel. The measurements were performed on the porous gel (Fe-BTC+PEG), the aerogel (Fe-BTC), and the size exclusion solvent (PEG). The aerogel was prepared in the same manner as in Example 6.

[0133] FIG. 24 shows the TGA profiles of the porous gel (Fe-BTC / PEG) according to Example 8, the corresponding aerogel (Fe-BTC), and the corresponding size exclusion solvent (PEG). As shown in FIG. PG =6.50% by mass, R AG =42.14% by mass, R SES = 0 mass%. Therefore, the content of MOF in the porous gel, C MOF was calculated to be 15.2% by mass.

[0134] Guest adsorption properties CO2 adsorption measurements were carried out in the same manner as in Example 1.

[0135] Fig. 25 shows the CO2 gas adsorption isotherm at 303 K for the porous gel (Fe-BTC / PEG) according to Example 8. As shown in Fig. 25, the CO2 adsorption amount of this gel at 303 K and saturated vapor pressure is 1.193 cm 3 This adsorption amount was 0.312 cm / g, which is the same as the adsorption amount for PEG alone (described later). 3 / g), which was about 3.82 times that of the porous gel of Example 8. This result indicates that pores of the MOF are present in the porous gel of Example 8.

[0136] Viscoelasticity The viscoelasticity was measured in the same manner as in Example 1.

[0137] Fig. 26 shows the results of viscoelasticity measurement in compression mode of the porous gel (Fe-BTC / PEG) according to Example 8. As shown in Fig. 26, in this gel, E'(ω)>E''(ω) holds in the region of ω<about 10 rad / s and ω>about 60 rad / s. This result indicates that the porous gel according to Example 8 has physical properties as a gel.

[0138] As shown in FIG. 26, in the porous gel of Example 8, the magnitudes of E'(ω) and E''(ω) were reversed depending on the angular frequency. In other words, this gel was found to exhibit thixotropy. In addition, the storage modulus E'(1) at 1 rad / s was 15.69 kPa.

[0139] Reformation of porous gel In order to confirm that the porous gel (Fe-BTC / PEG) obtained as described above is a "physical gel", an experiment similar to that described in Example 1 was carried out.

[0140] FIG. 27 shows the experimental results regarding the reversibility of the porous gel (Fe-BTC / PEG) according to Example 8. As shown in the figure, the Fe-BTC / PEG gel could be returned to a sol state by the above-mentioned first and second steps. Then, the obtained sol could be reformed as a gel by the above-mentioned third step. From the above results, it was confirmed that the Fe-BTC / PEG gel shows a reversible phase transition from gel to sol to gel by the destruction and reformation of the network structure.

[0141] Example 9 Ga-BTC / PEG A porous gel containing Ga-BTC as the MOF and PEG as the size-exclusion solvent was synthesized as follows: First, a Ga-BTC precursor gel was synthesized in the same manner as in Example 4. Then, a Ga-BTC / PEG gel was synthesized by solvent exchange in the same manner as in Example 4, except that PEG was used instead of PDMS-OH.

[0142] Determination of MOF content TGA measurements were performed to determine the Ga-BTC content in the Ga-BTC / PEG gel. The measurements were performed on the porous gel (Ga-BTC+PEG), the aerogel (Ga-BTC), and the size exclusion solvent (PEG). The aerogel was prepared in the same manner as in Example 6.

[0143] FIG. 28 shows the TGA profiles of the porous gel (Ga-BTC / PEG) according to Example 9, the corresponding aerogel (Ga-BTC), and the corresponding size exclusion solvent (PEG). As shown in FIG. PG =2.39% by mass, R AG =45.57% by mass, R SES = 0 mass%. Therefore, the content of MOF in the porous gel, C MOF was calculated to be 5.3% by mass.

[0144] Viscoelasticity The viscoelasticity was measured in the same manner as in Example 1.

[0145] Fig. 29 shows the results of viscoelasticity measurement in compression mode of the porous gel (Ga-BTC / PEG) according to Example 9. As shown in Fig. 29, in this gel, E'(ω)>E''(ω) was established at all angular frequencies ω measured. This result indicates that the porous gel according to Example 9 has physical properties as a gel.

[0146] As shown in FIG. 29, in the porous gel of Example 9, the change in both E'(ω) and E''(ω) due to the angular frequency was not large. Furthermore, E'(ω) was about one order of magnitude larger than E''(ω). In particular, the storage modulus E'(1) at 1 rad / s was 21.52 kPa.

[0147] Example 10 In-BTC / PEG A porous gel containing In-BTC as the MOF and PEG as the size-exclusion solvent was synthesized as follows: First, an In-BTC precursor gel was synthesized in the same manner as in Example 5. Then, an In-BTC / PEG gel was synthesized by solvent exchange in the same manner as in Example 5, except that PEG was used instead of PDMS-OH.

[0148] Determination of MOF content TGA measurements were performed to determine the content of In-BTC in the In-BTC / PEG gel. This measurement was performed for each of the porous gel (In-BTC+PEG), aerogel (In-BTC), and size exclusion solvent (PEG). The aerogel was prepared in the same manner as in Example 6.

[0149] 30 shows the TGA profiles of the porous gel (In-BTC / PEG) according to Example 10, the corresponding aerogel (In-BTC), and the corresponding size exclusion solvent (PEG). PG =2.40% by mass, R AG =45.50% by mass, R SES= 0 mass%. Therefore, the content of MOF in the porous gel, C MOF was calculated to be 5.3% by mass.

[0150] Guest adsorption properties CO2 adsorption measurements were carried out in the same manner as in Example 1.

[0151] Fig. 31 shows the CO2 gas adsorption isotherm at 303 K for the porous gel (In-BTC / PEG) according to Example 10. As shown in Fig. 31, the CO2 adsorption amount of this gel at 303 K and saturated vapor pressure is 1.116 cm 3 This adsorption amount was 0.312 cm / g, which is the same as the adsorption amount for PEG alone (described later). 3 / g), which was about 3.58 times that of the porous gel of Example 10. This result indicates that pores of the MOF are present in the porous gel of Example 10.

[0152] Viscoelasticity The viscoelasticity was measured in the same manner as in Example 1.

[0153] Fig. 32 shows the results of viscoelasticity measurement in compression mode of the porous gel (In-BTC / PEG) according to Example 10. As shown in Fig. 32, in this gel, E'(ω)>E''(ω) was established at all angular frequencies ω measured. This result indicates that the porous gel according to Example 10 has physical properties as a gel.

[0154] As shown in FIG. 32, in the porous gel of Example 10, the change in both E'(ω) and E''(ω) due to the angular frequency was not large. Furthermore, E'(ω) was about one order of magnitude larger than E''(ω). In particular, the storage modulus E'(1) at 1 rad / s was 17.66 kPa.

[0155] (Comparative Example 2; PEG) As a comparative example, the guest adsorption characteristics of PEG itself were evaluated. Specifically, CO2 adsorption measurements were performed in the same manner as in Example 1.

[0156] Fig. 33 shows the CO2 gas adsorption isotherm at 303 K for the size exclusion solvent (PEG) according to Comparative Example 2. As shown in Fig. 33, the CO2 adsorption amount of this liquid at 303 K and saturated vapor pressure is 0.312 cm 3 / g.

[0157] Since this PEG was liquid, it was not possible to measure its viscoelasticity. The viscosity of the PEG was approximately 7.3 cst.

[0158] Example 11: Al-BTC / [BMIM][BF 4 ]) A porous gel containing Al-BTC as the MOF and [BMIM][BF4] as the size-exclusion solvent was synthesized as follows. That is, first, an Al-BTC precursor gel was synthesized in the same manner as in Example 1. Then, an Al-BTC / [BMIM][BF4] gel was synthesized by solvent exchange in the same manner as in Example 1, except that [BMIM][BF4] was used instead of PDMS-OH.

[0159] Determination of MOF content TGA measurements were performed to determine the content of Al-BTC in the Al-BTC / [BMIM][BF4] gel. The measurements were performed on the porous gel (Al-BTC+[BMIM][BF4]), the aerogel (Al-BTC), and the size-exclusion solvent ([BMIM][BF4]). The aerogel was prepared in the same manner as in Example 6.

[0160] FIG. 34 shows the TGA profiles of the porous gel (Al-BTC / [BMIM][BF4]) according to Example 11, the corresponding aerogel (Al-BTC), and the corresponding size exclusion solvent ([BMIM][BF4]). As shown in FIG. PG =13.70% by mass, R AG =65.33% by mass, R SES = 11.54 mass%. Therefore, the content of MOF in the porous gel, C MOF was calculated to be 4.0% by mass.

[0161] Guest adsorption properties CO2 adsorption measurements were carried out in the same manner as in Example 1.

[0162] Fig. 35 shows the CO2 gas adsorption isotherm of the porous gel (Al-BTC / [BMIM][BF4]) according to Example 11 at 303 K. As shown in Fig. 35, the CO2 adsorption amount of this gel at 303 K and saturated vapor pressure is 0.822 cm 3 This adsorption amount was 0.316 cm3 / g, which is the same as the adsorption amount for [BMIM][BF4] alone (described later). 3 / g), which is about 2.60 times that of the porous gel of Example 11. This result indicates that pores of the MOF are present in the porous gel of Example 11.

[0163] Viscoelasticity The viscoelasticity was measured in the same manner as in Example 1.

[0164] Fig. 36 shows the results of viscoelasticity measurement in compression mode of the porous gel (Al-BTC / [BMIM][BF4]) according to Example 11. As shown in Fig. 36, in this gel, E'(ω)>E''(ω) was established at all angular frequencies ω measured. This result indicates that the porous gel according to Example 11 has physical properties as a gel.

[0165] As shown in FIG. 36, in the porous gel of Example 11, the change in both E'(ω) and E''(ω) due to the angular frequency was not large. Furthermore, E'(ω) was about one order of magnitude larger than E''(ω). In particular, the storage modulus E'(1) at 1 rad / s was 43.40 kPa.

[0166] Example 12: Al-ADC / [EMIM][BF 4 ]) A porous gel containing Al-ADC as the MOF and [EMIM][BF4] as the size-exclusion solvent was synthesized as follows. That is, first, an Al-BTC precursor gel was synthesized in the same manner as in Example 1. Then, an Al-ADC / [EMIM][BF4] gel was synthesized by solvent exchange in the same manner as in Example 2, except that [EMIM][BF4] was used instead of PDMS-OH.

[0167] Determination of MOF content TGA measurements were performed to determine the content of Al-ADC in the Al-ADC / [EMIM][BF4] gel. This measurement was performed for each of the porous gel (Al-ADC+[EMIM][BF4]), the aerogel (Al-ADC), and the size exclusion solvent ([EMIM][BF4]). The aerogel was prepared in the same manner as in Example 7.

[0168] FIG. 37 shows the TGA profiles of the porous gel (Al-ADC / [EMIM][BF4]) according to Example 12, the corresponding aerogel (Al-ADC), and the corresponding size exclusion solvent ([EMIM][BF4]). As shown in FIG. PG =19.05% by mass, R AG =76.04% by mass, R SES = 17.01 mass%. Therefore, the content of MOF in the porous gel, C MOF was calculated to be 4.7% by mass.

[0169] Guest adsorption properties CO2 adsorption measurements were carried out in the same manner as in Example 1.

[0170] Fig. 38 shows the CO2 gas adsorption isotherm at 303 K for the porous gel (Al-ADC / [EMIM][BF4]) according to Example 12. As shown in Fig. 38, the CO2 adsorption amount of this gel at 303 K and saturated vapor pressure is 1.155 cm 3 / g. This result indicates that the porous gel of Example 11 has pores of MOF.

[0171] Example 13: Fe-BTC / [EMIM][BF 4 ]) A porous gel containing Fe-BTC as the MOF and [EMIM][BF4] as the size exclusion solvent was synthesized as follows. That is, first, an Fe-BTC precursor gel was synthesized in the same manner as in Example 3. Then, an Fe-BTC / [EMIM][BF4] gel was synthesized by solvent exchange in the same manner as in Example 3, except that [EMIM][BF4] was used instead of PDMS-OH.

[0172] Determination of MOF content TGA measurements were performed to determine the Fe-BTC content in the Fe-BTC / [EMIM][BF4] gel. The measurements were performed on the porous gel (Fe-BTC+[EMIM][BF4]), the aerogel (Fe-BTC), and the size exclusion solvent ([EMIM][BF4]). The aerogel was prepared as in Example 8.

[0173] FIG. 39 shows the TGA profiles of the porous gel (Fe-BTC / [EMIM][BF4]) according to Example 13, the corresponding aerogel (Fe-BTC), and the corresponding size exclusion solvent ([EMIM][BF4]). As shown in FIG. PG =18.80% by mass, R AG =42.14% by mass, R SES = 17.01 mass%. Therefore, the content of MOF in the porous gel, C MOF was calculated to be 7.1% by mass.

[0174] Guest adsorption properties CO2 adsorption measurements were carried out in the same manner as in Example 1.

[0175] Fig. 40 shows the CO2 gas adsorption isotherm of the porous gel (Fe-BTC / [EMIM][BF4]) according to Example 13 at 303 K. As shown in Fig. 40, the CO2 adsorption amount of this gel at 303 K and saturated vapor pressure is 1.378 cm 3 / g. This result indicates that the porous gel of Example 13 has pores in the MOF.

[0176] Viscoelasticity The viscoelasticity was measured in the same manner as in Example 1.

[0177] Fig. 41 shows the results of viscoelasticity measurement in compression mode of the porous gel (Fe-BTC / [EMIM][BF4]) according to Example 13. As shown in Fig. 41, in this gel, E'(ω)>E''(ω) was established at all angular frequencies ω measured. This result indicates that the porous gel according to Example 13 has physical properties as a gel.

[0178] As shown in Fig. 41, the porous gel of Example 13 had a particularly high dependency on the angular frequency of E''(ω). The storage modulus E'(1) at 1 rad / s was 25.77 kPa.

[0179] Example 14: Ga-BTC / [EMIM][BF 4 ]) A porous gel containing Ga-BTC as the MOF and [EMIM][BF4] as the size exclusion solvent was synthesized as follows. That is, first, a Ga-BTC precursor gel was synthesized in the same manner as in Example 4. Then, a Ga-BTC / [EMIM][BF4] gel was synthesized by solvent exchange in the same manner as in Example 4, except that [EMIM][BF4] was used instead of PDMS-OH.

[0180] Determination of MOF content TGA measurements were performed to determine the Ga-BTC content in the Ga-BTC / [EMIM][BF4] gel. The measurements were performed on the porous gel (Ga-BTC+[EMIM][BF4]), the aerogel (Ga-BTC), and the size exclusion solvent ([EMIM][BF4]). The aerogel was prepared in the same manner as in Example 9.

[0181] FIG. 42 shows the TGA profiles of the porous gel (Ga-BTC / [EMIM][BF4]) according to Example 14, the corresponding aerogel (Ga-BTC), and the corresponding size exclusion solvent ([EMIM][BF4]). As shown in FIG. PG =18.76% by mass, R AG =45.57% by mass, R SES = 17.01% by mass. Therefore, the MOF content in the porous gel, C MOF was calculated to be 6.1% by mass.

[0182] Guest adsorption properties CO2 adsorption measurements were carried out in the same manner as in Example 1.

[0183] Fig. 43 shows the CO2 gas adsorption isotherm of the porous gel (Ga-BTC / [EMIM][BF4]) according to Example 14 at 303 K. As shown in Fig. 43, the CO2 adsorption amount of this gel at 303 K and saturated vapor pressure is 1.383 cm 3 / g. This result indicates that pores of the MOF are present in the porous gel of Example 14.

[0184] Viscoelasticity The viscoelasticity was measured in the same manner as in Example 1.

[0185] Fig. 44 shows the results of viscoelasticity measurement in compression mode of the porous gel (Ga-BTC / [EMIM][BF4]) according to Example 14. As shown in Fig. 44, in this gel, E'(ω)>E''(ω) was established at all angular frequencies ω measured. This result indicates that the porous gel according to Example 14 has physical properties as a gel.

[0186] As shown in FIG. 44, in the porous gel of Example 14, the change in both E'(ω) and E''(ω) due to the angular frequency was not large. Furthermore, E'(ω) was about one order of magnitude larger than E''(ω). In particular, the storage modulus E'(1) at 1 rad / s was 39.03 kPa.

[0187] Reformation of porous gel In order to confirm that the porous gel (Ga-BTC / [EMIM][BF4]) obtained in the above manner was a "physical gel," an experiment was carried out in the same manner as described in Example 1, except that acetone was used instead of ethanol.

[0188] FIG. 45 shows the experimental results on the reversibility of the porous gel (Ga-BTC / [EMIM][BF4]) according to Example 14. As shown in the figure, the Ga-BTC / [EMIM][BF4] gel could be returned to a sol state by the above-mentioned first and second steps. Then, the obtained sol could be reformed as a gel by the above-mentioned third step. From the above results, it was confirmed that the Ga-BTC / [EMIM][BF4] gel shows a reversible phase transition from gel to sol to gel by destruction and reformation of the network structure.

[0189] Example 15: In-BTC / [EMIM][BF 4 ]) A porous gel containing In-BTC as the MOF and [EMIM][BF4] as the size exclusion solvent was synthesized as follows. That is, first, an In-BTC precursor gel was synthesized in the same manner as in Example 5. Then, an In-BTC / [EMIM][BF4] gel was synthesized by solvent exchange in the same manner as in Example 5, except that [EMIM][BF4] was used instead of PDMS-OH.

[0190] Determination of MOF content TGA measurements were performed to determine the content of In-BTC in the In-BTC / [EMIM][BF4] gel. This measurement was performed for each of the porous gel (In-BTC+[EMIM][BF4]), the aerogel (In-BTC), and the size exclusion solvent ([EMIM][BF4]). The aerogel was prepared as in Example 10.

[0191] FIG. 46 shows the TGA profiles of the porous gel (In-BTC / [EMIM][BF4]) according to Example 15, the corresponding aerogel (In-BTC), and the corresponding size exclusion solvent ([EMIM][BF4]). As shown in FIG. PG =23.63% by mass, R AG =45.50% by mass, R SES = 17.01% by mass. Therefore, the MOF content in the porous gel, C MOF was calculated to be 23.2% by mass.

[0192] Viscoelasticity The viscoelasticity was measured in the same manner as in Example 1.

[0193] Fig. 47 shows the results of viscoelasticity measurement in compression mode of the porous gel (In-BTC / [EMIM][BF4]) according to Example 15. As shown in Fig. 47, in this gel, E'(ω)>E''(ω) was established at all angular frequencies ω measured. This result indicates that the porous gel according to Example 15 has physical properties as a gel.

[0194] As shown in FIG. 47, in the porous gel of Example 15, the change in both E'(ω) and E''(ω) due to the angular frequency was not large. Furthermore, E'(ω) was about one order of magnitude larger than E''(ω). In particular, the storage modulus E'(1) at 1 rad / s was 19.86 kPa.

[0195] (Comparative example 3; [BMIM][BF 4 ]) As a comparative example, the guest adsorption characteristics of [BMIM][BF4] itself were evaluated. Specifically, CO2 adsorption measurements were performed in the same manner as in Example 1.

[0196] Fig. 48 shows the CO2 gas adsorption isotherm at 303 K for the size exclusion solvent ([BMIM][BF4]) according to Comparative Example 3. As shown in Fig. 48, the CO2 adsorption amount of this liquid at 303 K and saturated vapor pressure is 0.316 cm 3 / g.

[0197] In addition, this [BMIM][BF4] was liquid, and viscoelasticity measurements could not be performed. The viscosity of [BMIM][BF4] was approximately 43 mPa·s.

[0198] The above results are summarized in Table 2. [Table 2]

[0199] As shown in Table 2, for a wide variety of combinations of MOFs and size-exclusion solvents, porous gels were obtained that had both the guest adsorption properties of a porous material and the viscoelasticity of a gel. It was also confirmed that reversible gel reformation was possible for many of these porous gels.

Claims

1. A metal organic framework having a vacancy in its molecule; a size exclusion solvent having a molecular size that is too large to occupy the pores; Including, the metal organic framework is configured to be capable of adsorbing at least one type of guest molecule in the pores; the metal organic framework forms a plurality of particles, the plurality of particles being bonded to each other by physical cohesive forces to form a network structure, Under ambient conditions, at least one angular frequency ω 0 In the storage modulus E' (ω 0 ) is the loss modulus E''(ω 0 ) larger, porous gels.

2. The porous gel according to claim 1 , wherein the size exclusion solvent has a boiling point of 200° C. or higher at standard pressure.

3. 3. The porous gel according to claim 1, wherein the size exclusion solvent is at least one selected from the group consisting of liquid polymers, ionic liquids, and crown ethers.

4. CO at 303K and saturated vapor pressure of the porous gel 2 The adsorption amount is 0.5 cm 3 The porous gel according to claim 1 or 2, wherein the molecular weight is 1 / g or more.

5. CO per unit mass of the porous gel at 303 K and saturated vapor pressure 2 The amount of adsorption is expressed as the amount of CO per unit mass of the size-exclusion solvent at 303 K and saturated vapor pressure. 2 The porous gel according to claim 1 or 2, which has an adsorption capacity of at least twice the adsorption capacity.

6. The porous gel according to claim 1 or 2, wherein a content of the metal organic framework in the porous gel is in a range of 1 mass % to 50 mass %.

7. 3. The porous gel according to claim 1 or 2, which is configured so that it can be converted into a sol by destroying at least a part of the network structure.

8. A gas adsorption system comprising the porous gel according to claim 1 or 2.

9. A gas separation system comprising the porous gel according to claim 1 or 2.

10. forming a precursor gel including a metal organic framework having intramolecular voids and a first solvent; exchanging the first solvent for a second solvent in the precursor gel; Including, the first solvent has a molecular size large enough to occupy the pores, The second solvent has a molecular size that is not large enough to occupy the pores. A method for producing a porous gel.

11. The method of claim 10 further comprising an activation step to remove gas or liquid molecules present in the pores.

12. 12. The method according to claim 10 or 11, wherein the second solvent has a boiling point at standard pressure of 200°C or higher.

13. 12. The method of claim 10 or 11, wherein the second solvent is at least one selected from the group consisting of liquid polymers, ionic liquids, and crown ethers.

14. 12. The method of claim 10 or 11, wherein exchanging the first solvent into the second solvent comprises exchanging the first solvent into a third solvent and exchanging the third solvent into the second solvent.

15. 15. The method of claim 14, wherein the third solvent is more miscible with the second solvent as compared to the first solvent.

Citation Information

Patent Citations

  • Porous liquids

    WO2018206977A1

  • Organic cage microparticle dispersions for gas absorption

    WO2020053589A1

Cited By

  • Aerogel reinforced ship antifouling paint and preparation method thereof

    CN120682678A