Protective sheet and electronic component device manufacturing method

A protective sheet with a water-soluble polymer and hydrophilic polyester layers ensures effective surface protection during semiconductor dicing and easy removal with high-temperature water, addressing the limitations of existing protective sheets.

JP2024135137APending Publication Date: 2024-10-04NITTO DENKO CORP

Patent Information

Application Number
JP2023045674
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing protective sheets used in the dicing process of semiconductor wafers fail to effectively protect the surface from cooling water during cutting, leading to potential removal or failure of the protective sheet, and are difficult to remove after use due to low water solubility.

Method used

A protective sheet comprising a first protective layer with a water-soluble polymer compound and a second protective layer with a hydrophilic polyester compound, designed to withstand cooling water during dicing and be easily removable with a high-temperature water-containing liquid.

Benefits of technology

The protective sheet maintains surface protection during dicing with cooling water and can be efficiently removed using a high-temperature water-containing liquid, reducing foreign matter adherence and facilitating the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135137000001_ABST
    Figure 2024135137000001_ABST
Patent Text Reader

Abstract

To provide a protective sheet and the like that can continue to protect a surface to be protected even after being divided by a dicing step using cooling water, and that is removed by a relatively hot water-containing liquid after protecting the surface to be protected.SOLUTION: A protective sheet for protecting a surface to be protected of an electronic component includes: a first protective layer that is bonded to the surface to be protected; and a second protective layer that overlaps one surface of the first protective layer. The first protective layer contains a water-soluble polymer compound. The second protective layer contains a hydrophilic polyester compound.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a protective sheet to be attached to a surface of an electronic component to be protected, for example. The present invention also relates to a method for manufacturing an electronic component device using the protective sheet during a manufacturing process. [Background technology]

[0002] Conventionally, in the manufacture of electronic component devices, protective sheets are known that are used to protect, for example, at least a part of the surface of an object to be protected (i.e., the surface to be protected). The object to be protected with this type of protective sheet is, for example, a semiconductor wafer. This type of protective sheet is used by being attached to the surface to be protected during the manufacturing process of the electronic component device.

[0003] An example of an electronic component device is a semiconductor device. In general, a method for manufacturing a semiconductor device includes a front-end process in which a circuit surface is formed on one side of a disk-shaped bare wafer using highly integrated electronic circuits, and a back-end process in which semiconductor chips are cut out from the semiconductor wafer on which the circuit surface is formed and assembled. In the back-end process, a dicing tape having a base sheet and an adhesive sheet, and a die-bonding sheet laminated on the dicing tape and bonded to the semiconductor wafer are used, and in addition, for example, the above-mentioned protective sheet is used.

[0004] For details, the post-processing is a backgrinding process in which a backgrind tape is superimposed on a circuit surface of a disk-shaped semiconductor wafer, and in a state in which the semiconductor wafer and the backgrind tape are laminated, a surface of the semiconductor wafer on which the circuit surface is not formed is ground until the semiconductor wafer reaches a predetermined thickness; a mounting process in which the ground surface of the semiconductor wafer (the surface on which the circuit surface is not formed) is superimposed on a die bond sheet on a dicing tape, and the semiconductor wafer is fixed to the dicing tape via the die bond sheet; a dicing process for obtaining a large number of semiconductor chips (dies) by dicing the semiconductor wafer and the die bond sheet; an expanding step of, as necessary, stretching the dicing tape in the radial direction of the semiconductor wafer to widen the gap between adjacent semiconductor chips (dies); a pick-up step of peeling the dicing tape from the small piece of die bond sheet and taking out the semiconductor chip with the small piece of die bond sheet attached thereto; and a die bonding process of bonding the semiconductor chip to an adherend via the small piece of die bond sheet attached to the removed semiconductor chip. A semiconductor device is manufactured through these steps, for example.

[0005] As the above-mentioned protective sheet, for example, there is known one which is used as a temporary fixing sheet for temporarily fixing a semiconductor wafer in the above-mentioned subsequent process such as a back-grinding process or a dicing process, and is then removed with water (for example, Patent Document 1). The protective sheet described in Patent Document 1 is attached to a surface to be protected and is also used for masking purposes to prevent deposition material from adhering to the surface to be protected, such as a semiconductor wafer, during a coating formation process by deposition or the like.

[0006] The protective sheet described in Patent Document 1 has a resin composition containing an oxyalkylene group-containing polyvinyl alcohol resin having a degree of saponification of 55 mol% or less. The resin composition of the protective sheet described in Patent Document 1 is water-soluble, and therefore can be easily removed with water after protecting the surface to be protected, such as a semiconductor wafer. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2021-161735 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, the protective sheet described in Patent Document 1 is used to protect the surface (surface to be protected) of a semiconductor wafer or the like, and when the semiconductor wafer or the like is cut by a dicing blade in the dicing process, there is a risk that the surface to be protected cannot be protected during the dicing process. In more detail, if cooling water is used during the dicing process to suppress the temperature rise accompanying the cutting of the semiconductor wafer or the like, the protective sheet may dissolve and be removed from the surface to be protected during the cutting of the semiconductor wafer or the like. In other words, there is a risk that the protective sheet will not be able to protect the surface to be protected during the dicing process using a dicing blade and cooling water.

[0009] In response to this, it is possible to reduce the water solubility of the protective sheet so that the protective sheet is not removed by the cooling water during the dicing process. However, simply reducing the water solubility of the protective sheet makes it difficult to remove the protective sheet with water after protecting the surface to be protected with the protective sheet.

[0010] To prevent such problems, there is a demand for a protective sheet that can continue to protect the surface to be protected even when cut into small pieces by a dicing process using cooling water, and that can be removed by a water-containing liquid after protecting the surface to be protected.

[0011] However, it cannot be said that sufficient research has been conducted on a protective sheet that can continue to protect the surface to be protected even when divided by a dicing process using cooling water, and that can be removed by a water-containing liquid after protecting the surface to be protected.

[0012] Therefore, the present invention focuses on the use of a relatively high-temperature water-containing liquid in removing the protective sheet. An object of the present invention is to provide a protective sheet that can continue to protect the surface to be protected even when it is divided by a dicing process using cooling water, and that can be removed by the relatively high-temperature water-containing liquid after protecting the surface to be protected. Another object of the present invention is to provide a method for manufacturing an electronic component device, which can protect the surface to be protected even if the protective sheet protecting the surface to be protected is divided by a dicing process using cooling water, and which can remove the protective sheet after protecting the surface to be protected with a relatively high-temperature water-containing liquid. [Means for solving the problem]

[0013] In order to solve the above problems, the protective sheet of the present invention comprises: A protective sheet for protecting a surface to be protected of an electronic component, A first protective layer is attached to the surface to be protected, and a second protective layer is overlapped on one side of the first protective layer, the first protective layer contains a water-soluble polymer compound, The second protective layer includes a hydrophilic polyester compound.

[0014] The method for manufacturing an electronic component device according to the present invention includes the steps of: A step of attaching a protective sheet to a surface of an electronic component to be protected; cutting the electronic components and the protective sheet together into a plurality of small pieces while bringing cooling water of 30° C. or less into contact with the protective sheet; and removing the piece of protective sheet from the surface to be protected of the piece of electronic component, the protective sheet has a first protective layer attached to the surface to be protected and a second protective layer overlapping one side of the first protective layer, the first protective layer contains a water-soluble polymer compound, and the second protective layer contains a hydrophilic polyester compound; The removing step includes removing the protective sheet pieces by dissolving at least a portion of the protective sheet pieces in a water-containing liquid at 40° C. or higher. Effect of the Invention

[0015] The protective sheet of the present invention can continue to protect the surface to be protected even when it is divided by a dicing process using cooling water, and after protecting the surface to be protected, it is removed by a relatively high-temperature water-containing liquid. In the manufacturing method for electronic component devices according to the present invention, the above-mentioned protective sheet is used, so that the protective sheet protecting the surface to be protected of the electronic component can protect the surface to be protected even when it is divided by a dicing process using cooling water, and the protective sheet after protecting the surface to be protected can be removed by a relatively high-temperature water-containing liquid. [Brief description of the drawings]

[0016] [Figure 1A] 1 is a schematic cross-sectional view of a first example of a protective sheet according to this embodiment cut in the thickness direction. [Figure 1B] FIG. 2 is a schematic cross-sectional view showing a state immediately before use of a protection sheet according to a first example of the present embodiment. [Figure 1C] 1 is a schematic cross-sectional view showing a state in which a protective sheet according to a first example of the present embodiment is attached to a surface to be protected of an electronic component. [Figure 2A] FIG. 4 is a schematic cross-sectional view of a second example of a protective sheet according to the present embodiment, cut in the thickness direction. [Figure 2B] FIG. 4 is a schematic cross-sectional view showing a state immediately before use of a protection sheet according to a second example of the present embodiment. [Figure 2C] 5 is a schematic cross-sectional view showing a state in which a protective sheet according to a second example of the present embodiment is attached to a surface to be protected of an electronic component. [Figure 3A] 5A to 5C are schematic diagrams illustrating a mounting process in the example of a method for manufacturing an electronic component device. [Figure 3B] 5A to 5C are schematic diagrams illustrating a mounting process in the example of a method for manufacturing an electronic component device. [Figure 3C] 5A to 5C are schematic diagrams illustrating a mounting process in the example of a method for manufacturing an electronic component device. [Figure 4] 5A to 5C are schematic diagrams illustrating a dicing process in the example of a method for manufacturing an electronic component device. [Diagram 5] 5A to 5C are schematic diagrams illustrating a state during a removal step in the example of a method for manufacturing an electronic component device. [Figure 6] 5A to 5C are schematic diagrams illustrating a pickup process in the example of a method for manufacturing an electronic component device. [Figure 7]FIG. 13 is a schematic diagram showing a state after a die bonding process in the example of a method for manufacturing an electronic component device. [Figure 8] 5A and 5B are schematic diagrams illustrating a state after a wire bonding step and a sealing step in the example of a method for manufacturing an electronic component device. [Figure 9A] 11A to 11C are schematic diagrams illustrating a back grinding process in another example of a method for manufacturing an electronic component device. [Figure 9B] 11A to 11C are schematic diagrams illustrating a back grinding process in another example of a method for manufacturing an electronic component device. [Figure 9C] 13 is a schematic diagram showing a state after a back grinding process in another example of a method for manufacturing an electronic component device. FIG. [Figure 10A] 11A to 11C are schematic diagrams illustrating a mounting process in another example of a method for manufacturing an electronic component device. [Figure 10B] 11A to 11C are schematic diagrams illustrating a mounting process in another example of a method for manufacturing an electronic component device. [Figure 11] 1 is a schematic cross-sectional view of a dicing die bond film used as a manufacturing auxiliary tool in a manufacturing method for an electronic component device, cut in the thickness direction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, one embodiment of a protective sheet according to the present invention will be described with reference to the drawings. It should be noted that the figures in the drawings are schematic diagrams and the aspect ratios are not necessarily the same as those of the actual products.

[0018] 1A, the protective sheet 1 of the present embodiment is a protective sheet 1 for protecting a surface of an electronic component to be protected, and includes a first protective layer 11 that is attached to the surface to be protected, and a second protective layer 12 that overlaps one side of the first protective layer 11. The first protective layer 11 contains a water-soluble polymer compound, and the second protective layer 12 contains a hydrophilic polyester compound.

[0019] As shown in Fig. 1A, the protective sheet 1 of this embodiment may further include a first release liner 15 and a second release liner 17 overlapping the second protective layer 12. The first release liner 15 overlaps the surface of the first protective layer 11 that is to be bonded to the surface to be protected (hereinafter also referred to as the attachment surface). As shown in Fig. 1B, the first release liner 15 is peeled off from the attachment surface of the first protective layer 11 before use. For example, as shown in Fig. 1C, after the first protective layer 11 is attached to the surface to be protected of an adherend (such as substrate G), the second release liner 17 is peeled off from one side of the second protective layer 12.

[0020] The protective sheet 1 of this embodiment is used, for example, during the process of manufacturing an electronic component device. Specifically, the protective sheet 1 of this embodiment is used for the purpose of temporarily protecting the surface to be protected (surface to be protected) of the adherend, which is an electronic component. More specifically, the protective sheet 1 of this embodiment is used, for example, by being attached to the surface to be protected (surface to be protected) of the electronic component. Examples of the electronic component include a semiconductor wafer, a semiconductor chip, a substrate such as a wired circuit board, a connected wired circuit board formed by connecting a plurality of wired circuit boards, and a pseudo wafer.

[0021] The above-mentioned semiconductor chip usually has a semiconductor chip body and an electrode part disposed on one or both sides of the semiconductor chip body and electrically connected to an electrode part of another member. Examples of the other member include a wiring circuit board or another semiconductor chip. The semiconductor chip has, for example, at least one surface formed with a circuit surface on which a circuit is formed. Specifically, the semiconductor chip may be a TSV (Through Silicon Via) type semiconductor chip having paired electrode parts arranged on both sides of the semiconductor chip body, and a conductive part penetrating the semiconductor chip body in the thickness direction so as to electrically connect one of the electrode parts to the other. In the TSV type semiconductor chip, a circuit surface may be formed on only one side, or a circuit surface may be formed on each of both sides. The circuit of the semiconductor chip may include a sensor element (e.g., a light receiving element or a vibration element) as an element. This type of semiconductor chip is, for example, a sensor chip. Examples of the sensor chip include a CMOS (Complementary Metal-Oxide Semiconductor) chip and a MEMS (Micro Electro Systems) chip.

[0022] The pseudo wafer includes, for example, a support substrate and a package body in which a plurality of semiconductor chips arranged on the support substrate are collectively sealed with resin. The pseudo wafer may be the package body removed from the support substrate. A rewiring layer may be formed on at least a portion of the surface of the pseudo wafer. The protective sheet 1 may be used to cover the rewiring layer. The divided bodies obtained by dividing the pseudo wafer into units each including at least one semiconductor chip may be electronic components.

[0023] As described above, there are various types of electronic components having a surface to be protected. For example, the electronic components that are adherends include substrates G made of various materials. Examples of the materials of the substrate G that are adherends include glass, silicon, stainless steel (SUS), plastic, and ceramic.

[0024] The first protective layer 11 has an adhesive property that enables it to adhere closely to the surface to be protected of the adherend, that is, the substrate G. By overlapping the first protective layer 11 of the protective sheet 1 on the surface to be protected of the adherend, that is, the substrate G, it is possible to prevent foreign matter from adhering to the surface to be protected until the first protective layer 11 overlapping the surface to be protected is removed. The protective sheet 1 is used in a process for manufacturing an electronic component device such as a semiconductor device. During this process, the protective sheet 1 may come into contact with cooling water or the like. Under such circumstances, at least a portion of the first protective layer 11 containing a water-soluble polymer compound may dissolve. In contrast, in the protective sheet 1 of the present embodiment, the first protective layer 11 contains a water-soluble polymer compound, and the second protective layer 12 contains a hydrophilic polyester compound. The hydrophilicity of the hydrophilic polyester compound with respect to relatively low temperature water is lower than that of the water-soluble polymer compound. Therefore, by using the first protective layer 11 attached to the surface to be protected and the second protective layer 12 arranged so as to be in contact with cooling water, even if the protective sheet 1 comes into contact with cooling water while protecting the surface to be protected, it is possible to prevent the protective sheet 1 from being removed by the cooling water. Moreover, after protective sheet 1 has been used, for example, to temporarily protect a surface to be protected as described above, it is removed by a relatively hot water-containing liquid. The method of using protective sheet 1, in which protective sheet 1 is attached to substrate G as an adherend, will be described in detail later.

[0025] [1st protective layer] The first protective layer 11 contains a water-soluble polymer compound. The water-soluble polymer compound has a hydrophilic group in the molecule in an amount sufficient to exhibit water solubility. The first protective layer 11 preferably contains 90% by mass or more of the water-soluble polymer compound, more preferably 95% by mass or more, and even more preferably 99% by mass or more. This makes the first protective layer 11 more easily removable by a water-containing liquid at a relatively high temperature.

[0026] The water-soluble polymer has such water solubility that when a thin film (thickness 50 μm or less) of the water-soluble polymer is immersed in water at 40° C., the entirety of the film is dissolved.

[0027] The first protective layer 11 has a predetermined level of hydrophilicity or more. When the first protective layer 11 has a predetermined level of hydrophilicity or more, usually, at least a part of the first protective layer 11 is dissolved in a relatively high-temperature water-containing liquid. Since the first protective layer 11 has a predetermined level of hydrophilicity or more, at least a part of the first protective layer 11 is dissolved when it comes into contact with a relatively high-temperature water-containing liquid, and is removed from the surface to be protected of the electronic component that is the adherend.

[0028] The contact angle of water on the surface of the first protective layer 11 can be an index of the hydrophilicity of the first protective layer 11. The contact angle of water on the surface of the first protective layer 11 is preferably 25° or more and 45° or less. When the contact angle is 25° or more, the adhesion of the first protective layer 11 to the adherend can be further improved. On the other hand, when the contact angle is 45° or less, the solubility of the first protective layer 11 in water is further increased.

[0029] The contact angle can be increased by using a water-soluble polymer compound having a higher ratio of hydrophilic groups (e.g., -OH groups, polyoxyethylene groups) in the molecule, whereas the contact angle can be decreased by using a water-soluble polymer compound having a lower ratio of hydrophilic groups (e.g., -OH groups, polyoxyethylene groups) in the molecule.

[0030] The contact angle is measured as follows. Specifically, the contact angle of water on one surface of the first protective layer 11 (the surface to be attached to the surface to be protected) is measured using a general contact angle meter. More specifically, in accordance with JIS R3257, the contact angle with 1.5 μL of water is measured at 25° C. using a fully automatic contact angle measuring device (for example, product name: DM-500 manufactured by Kyowa Interface Science Co., Ltd.). The average value of five measurements is used.

[0031] The physical property of the first protective layer 11 is indicated, for example, by a shear adhesive strength. The shear adhesive strength of the first protective layer 11 is preferably greater than 0.10 MPa, and more preferably equal to or greater than 0.20 MPa. When the shear adhesive strength of the first protective layer 11 is greater than 0.10 MPa, the adhesion to the adherend is enhanced, and the surface to be protected can be protected more sufficiently. That is, peeling of the first protective layer 11 from the surface to be protected in the dicing step (described in detail later) can be more sufficiently suppressed. The shear adhesive strength of the first protective layer 11 may be equal to or less than 2.00 MPa.

[0032] The shear adhesive strength can be increased by using a water-soluble polymer compound having a smaller molecular weight or a lower glass transition point, while the shear adhesive strength can be decreased by using a water-soluble polymer compound having a larger molecular weight or a higher glass transition point.

[0033] The shear adhesive strength is measured by a die shear strength test as follows. Specifically, first, a double-sided tape is attached to one side of a SUS plate at room temperature using a hand roller to prepare a support for testing. Next, each first protective layer for testing is attached to the exposed surface (upper surface) of the double-sided tape using a hand roller at room temperature. Then, a silicon chip (a square with a side length of 5 mm and a thickness of 500 μm) is attached to the exposed surface (upper surface) of each first protective layer at a speed of 10 mm / sec using a laminator at 80°C. A force (shear force) is applied to the upper portion of the silicon chip in one direction among the surface directions of each first protective layer. At this time, a shear force is applied to a portion of the silicon chip from the upper surface to 50 μm downward at a speed of 500 μm / sec at 25°C. Then, the force when the silicon chip is peeled off from the upper surface of each first protective layer is measured.

[0034] In this embodiment, the hydrophilic group of the water-soluble polymer compound contained in the first protective layer 11 may be, for example, at least one type selected from the group consisting of a hydroxy group, a carboxy group, a pyrrolidone group, and a polyoxyethylene group (polyoxyethylene structure).

[0035] The water-soluble polymeric compound is preferably at least one of polyvinyl alcohol obtained by hydrolyzing a portion of the ester bonds in a vinyl acetate polymer, a water-soluble polymeric compound having at least a polyethylene oxide structure in the molecule, and polyvinyl acetal obtained by reacting polyvinyl alcohol with an aldehyde.

[0036] The water-soluble polymer compound preferably has at least one of a hydroxy group and a polyoxyethylene structure as a hydrophilic group in the molecule. By having a hydroxy group or a polyoxyethylene structure as a hydrophilic group in the molecule, the first protective layer 11 can be more sufficiently adhered to the surface of the substrate G (electronic component) to be protected.

[0037] For example, the first protective layer 11 may contain polyvinyl alcohol having many hydroxyl groups in the molecule as the water-soluble polymer compound.

[0038] When the water-soluble polymer compound is polyvinyl alcohol (PVA), the degree of saponification (mol %) of the polyvinyl alcohol may be 70 or more and 100 or less. The degree of saponification (mol %) of polyvinyl alcohol is preferably 80 or more, and more preferably 90 or more. As the degree of saponification of polyvinyl alcohol increases, the first protective layer 11 has higher hydrophilicity. Therefore, the first protective layer 11 can be more easily removed by a water-containing liquid at a relatively high temperature. On the other hand, in terms of further improving the adhesive strength to the adherend, the saponification degree of polyvinyl alcohol is preferably 98 or less, and more preferably 95 or less.

[0039] <Method and conditions for measuring saponification degree> The above saponification degree was measured by proton magnetic resonance spectroscopy under the following analytical conditions ( 1 H MNR). When the first protective layer 11 contains a component other than PVA, the measurement is carried out after performing a separation and extraction process of the PVA by methanol extraction or the like in order to avoid overlapping of peaks in the measurement chart. Analyzer: FT-NMR (For example, "AVANCEIII-400" manufactured by Bruker Biospin) Observation frequency: 400MHz ( 1 H) Measurement solvent: deuterium oxide or deuterated dimethyl sulfoxide (DMSO) Measurement temperature: 80℃ Chemical shift standard: External standard TSP-d4 (0.00ppm) (when measuring heavy water) : Measurement solvent (2.50 ppm) (when measuring deuterated DMSO)

[0040] The average degree of polymerization of the polyvinyl alcohol is preferably at least 100, and more preferably at least 200. The average degree of polymerization is preferably at most 1000, and more preferably at most 800. When the average polymerization degree of polyvinyl alcohol is 100 or more, it becomes easier to form the first protective layer 11. On the other hand, when the average polymerization degree of polyvinyl alcohol is 1000 or less, the hydrophilicity of polyvinyl alcohol is increased, and the first protective layer 11 becomes more easily soluble in a water-containing liquid at a relatively high temperature.

[0041] The average degree of polymerization is determined by the following measurement method and measurement conditions. <Method and conditions for measuring average degree of polymerization> ·Analytical equipment: Gel permeation chromatography analytical equipment (For example, Agilent's instrument name "1260Infinity") Column: TSKgel G6000PWXL and TSKgel G3000PWXL (Tosoh Corporation, serial connection) Column temperature: 40℃ Eluent: 0.2M aqueous sodium nitrate solution ·Flow rate: 0.8mL / min ·Injection volume: 100μL Detector: Differential Refractometer (RI) Standard samples: PEG standard sample and PVA standard sample The mass average molecular weight Mw of the sample (PVA) and the PVA standard sample with a known average degree of polymerization are calculated by GPC measurement using a PEG standard sample. A calibration curve is created from the average degree of polymerization of the PVA standard sample and the calculated mass average molecular weight Mw of the PVA standard sample. Using this calibration curve, the average degree of polymerization of the sample (PVA) is calculated from the mass average molecular weight Mw of the sample (PVA).

[0042] In this embodiment, the first protective layer 11 may contain, for example, polyethylene oxide (PEO) (e.g., molecular weight of 50,000 or more) having only a polyoxyethylene structure in the molecule as the water-soluble polymer compound. On the other hand, the first protective layer 11 may contain, as the water-soluble polymer compound, a polyalkylene oxide copolymer (e.g., molecular weight of 50,000 or more) having a polyoxyethylene structure and a polyoxypropylene structure in the molecule. The polyalkylene oxide copolymer may be a block copolymer having a block of a polyoxyethylene structure and a block of a polyoxypropylene structure in the molecule, or may be a random copolymer of ethylene oxide and propylene oxide.

[0043] When the water-soluble polymer compound has a polyoxypropylene structure in the molecule in addition to a polyoxyethylene structure, the adhesion of the first protective layer 11 to an adherend is further improved.

[0044] The mass average molecular weight Mw of the water-soluble polymer compound having a polyoxyethylene structure in the molecule is preferably 1,000,000 (1 million) or less. By having a mass average molecular weight Mw of 1,000,000 or less, the water-soluble polymer compound can have a sufficiently low softening point. This can improve the adhesion of the first protective layer 11 to the adherend at low temperatures. In addition, the first protective layer 11 can be efficiently removed from the surface of the adherend to be protected in a shorter time by a relatively high-temperature water-containing liquid. The mass average molecular weight Mw may be, for example, 50,000 or more.

[0045] The first protective layer 11 of the present embodiment may further contain, in addition to the above-mentioned blended components, for example, a surfactant or a plasticizer.

[0046] The thickness of the first protective layer 11 is not particularly limited, but is, for example, 1 μm or more and 100 μm or less. Such a thickness may be 3 μm or more, or 5 μm or more. Moreover, such a thickness may be 40 μm or less, or 30 μm or less. Note that, when the first protective layer 11 is a laminate, the above thickness is the total thickness of the laminate.

[0047] [Second protective layer of protective sheet] As described above, the second protective layer 12 contains a hydrophilic polyester compound. The second protective layer 12 may be formed only of the hydrophilic polyester compound, or may contain a component other than the hydrophilic polyester compound. The second protective layer 12 is, for example, a film formed of the hydrophilic polyester compound.

[0048] Second protective layer 12 preferably contains 95% by mass or more, and more preferably 98% by mass or more, of a hydrophilic polyester compound, which allows second protective layer 12 to more reliably maintain the laminated state with first protective layer 11 even when in contact with the coolant used in the dicing step (described in detail later), and therefore allows first protective layer 11 to be more sufficiently prevented from dissolving in the coolant.

[0049] The degree of hydrophilicity of the second protective layer 12 can be indicated, for example, by the contact angle of water on the surface of the second protective layer 12. The contact angle of water on the surface of the second protective layer 12 is preferably 60° or more and 80° or less. When the contact angle is 60° or more, the solubility of the second protective layer 12 in cooling water of, for example, less than 30° C. becomes lower. On the other hand, when the contact angle is 80° or less, the second protective layer 12 becomes more soluble in a water-containing liquid at a relatively high temperature. The details of the method for measuring the contact angle are as described above.

[0050] The contact angle can be increased by using a hydrophilic polyester compound having a smaller acid value, for example, whereas the contact angle can be decreased by using a hydrophilic polyester compound having a larger acid value.

[0051] The hydrophilic polyester compound contained in the second protective layer 12 is an esterification reaction product of at least a polycarboxylic acid and a polyol. Therefore, the hydrophilic polyester compound has a polycarboxylic acid residue and a polyol residue in the molecule. An example of the polycarboxylic acid is terephthalic acid.

[0052] The hydrophilic polyester compound has a carboxy group or a sulfonic acid group in the molecule. The carboxy group or the sulfonic acid group may be in the form of a salt. Since the hydrophilic polyester compound has the above-mentioned hydrophilic group in the molecule, it can be dissolved in a water-containing liquid at a relatively high temperature.

[0053] The hydrophilic polyester compound preferably has the following physical properties: Specifically, when a mixture of hydrophilic polyester compound powder and 50°C water in a mass ratio of 1:5 is prepared and irradiated with ultrasound for 10 minutes, all of the hydrophilic polyester compound dissolves in water.

[0054] The weight average molecular weight Mw of the hydrophilic polyester compound is preferably 25,000 (25,000) or less, and more preferably 20,000 (20,000) or less, which makes it easier to form the second protective layer 12. The weight average molecular weight Mw of the hydrophilic polyester compound is preferably 10,000 (10,000) or more. This makes the second protective layer 12 less likely to dissolve when it comes into contact with cooling water (e.g., 30°C or less), while the second protective layer 12 can be relatively easily removed from the surface to be protected when it comes into contact with relatively high-temperature water (e.g., hot water of 40°C or more). Since the mass average molecular weight Mw of the hydrophilic polyester compound is within the above range, the second protective layer 12 can maintain protection of the surface to be protected even when it is cut by a dicing blade or the like while coming into contact with cooling water at a relatively low temperature, for example, 30° C. or lower (for example, during a blade dicing process, which will be described in detail later). On the other hand, the second protective layer 12 can be dissolved and removed relatively easily when it comes into contact with a water-containing liquid at, for example, 40° C. or higher (for example, during a removal step, which will be described in detail later).

[0055] The acid value of the hydrophilic polyester compound is preferably less than 5 mgKOH / g. A smaller acid value of the hydrophilic polyester compound further suppresses dissolution of the second protective layer 12 when it comes into contact with relatively low-temperature cooling water. The acid value is determined by the neutralization titration method specified in JIS K 0070-1992.

[0056] The thickness of the second protective layer 12 is not particularly limited, but is, for example, 1 μm or more and 100 μm or less. Such a thickness may be 3 μm or more, or 5 μm or more. Also, such a thickness may be 40 μm or less. Note that, when the second protective layer 12 is a laminate, the above thickness is the total thickness of the laminate.

[0057] [First release liner and second release liner] As described above, before use, protective sheet 1 of this embodiment may include a first release liner 15 that covers one side of first protective layer 11 (the side of first protective layer 11 that is not overlapped with second protective layer 12). First release liner 15 is used to protect first protective layer 11, and is peeled off from the above-mentioned one side of first protective layer 11, for example, immediately before first protective layer 11 is attached to an adherend (such as a substrate G as an electronic component). Furthermore, the protective sheet 1 of the present embodiment may include a second release liner 17 covering one side of the second protective layer 12 (the side of the second protective layer 12 that does not overlap with the first protective layer 11) as described above. The second release liner 17 is used to protect the second protective layer 12, and is peeled off from the above-mentioned one side of the second protective layer 12, for example, after the first protective layer 11 and the second protective layer 12 are attached to an adherend (such as a substrate G).

[0058] Each of the above release liners may be a plastic film or paper, etc., the surface of which has been treated with a release agent such as a silicone-based release agent, a long-chain alkyl-based release agent, a fluorine-based release agent, or molybdenum sulfide.

[0059] The protective sheet 1 of this embodiment may be a first example as shown in Figure 1A. The protective sheet 1 of the first example includes both a first release liner 15 and a second release liner 17. The protective sheet of the first example can be produced by a general method, for example, as follows.

[0060] To prepare the first protective layer 11, first, a water-soluble polymer compound is dissolved in a solvent containing water. Heating may be used during dissolution. As the solvent, an organic solvent other than water may be used. As the organic solvent, an aqueous organic solvent that dissolves in water at any ratio is preferable. Examples of such aqueous organic solvents include methanol, ethanol, and isopropyl alcohol. Next, the polymer solution prepared as described above is applied (coated) onto the first release liner 15. After application, the solution is heated to a temperature at which the solvent volatilizes, thereby forming the first protective layer 11 overlapping the first release liner 15.

[0061] On the other hand, in order to prepare the second protective layer 12, the hydrophilic polyester compound is dissolved in a solvent containing water or an organic solvent. Heating may be performed during dissolution. The organic solvent is preferably water or a polar organic solvent. Examples of such polar organic solvents include methanol, ethanol, and isopropyl alcohol. Next, the solution of the hydrophilic polyester compound prepared as described above is applied (coated) onto the second release liner 17. After application, the solution is heated to a temperature at which the solvent volatilizes, thereby forming the second protective layer 12 overlapping the second release liner 17.

[0062] Then, the first protective layer 11 overlapped on the first release liner 15 and the second protective layer 12 overlapped on the second release liner 17 are overlapped and pressure is applied. In other words, the first protective layer 11 and the second protective layer 12 are sandwiched between the first release liner 15 and the second release liner 17, thereby laminating the first protective layer 11 and the second protective layer 12, and then pressure is applied. Although protective sheet 1 can be produced in this manner, the method for producing the protective sheet is not limited to the above-mentioned exemplary method.

[0063] The protective sheet 1 is used, for example, as an auxiliary tool for manufacturing an electronic component device. The protective sheet 1 is used, for example, temporarily during the process of manufacturing the electronic component device. Therefore, the manufactured electronic component device may not include the protective sheet 1.

[0064] The electronic component device is a device that includes at least one of the various electronic components described above. Examples of the electronic component device include a semiconductor device such as a semiconductor integrated circuit including a semiconductor chip, a device including a system LSI having a complementary MOS (CMOS), or a device including a device (MEMS Micro Electro Mechanical Systems) in which mechanical elements, sensors, actuators, or electronic circuits are integrated on a single silicon substrate, glass substrate, or organic material substrate by microfabrication technology. The electronic component device to be manufactured may be a device including a wiring circuit board.

[0065] In the above embodiment, a protective sheet (a first example of this embodiment) that may have a first release liner 15 and a second release liner 17 is described in detail, but the protective sheet of this embodiment may also be a protective sheet as described below (a second example of this embodiment).

[0066] A second example of the protective sheet of this embodiment may include an adhesive tape 13 (e.g., a backgrind tape) instead of the second release liner 17 of the protective sheet of the first example, as shown in Fig. 2A. The protective sheet of the second example is used after the first release liner 15 is removed, as in the first example (see Fig. 2B). Then, for example, as shown in Fig. 2C, after the first protective layer 11 is attached to the surface to be protected of the substrate G, the adhesive tape 13 is peeled off from one side of the second protective layer 12.

[0067] The adhesive tape 13 has a base layer 13a and an adhesive layer 13b overlapping the base layer 13a. In this embodiment, the adhesive layer 13b is formed of a pressure-sensitive adhesive, so that the adhesive tape 13 can be used as a pressure-sensitive adhesive tape.

[0068] (Adhesive tape base layer) The base layer 13a is made of, for example, a resin. Examples of such resins include polyester resins such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), and polybutylene naphthalate (PBN), polyolefin resins such as ethylene-vinyl acetate copolymer, ethylene-methyl methacrylate copolymer, polyethylene, polypropylene, and ethylene-propylene copolymer, polyvinyl alcohol, polyvinylidene chloride, polyvinyl chloride, vinyl chloride-vinyl acetate copolymer, polyvinyl acetate, polyamide, polyimide, cellulose, fluorine resin, polyether, and polystyrene resins such as polystyrene, polycarbonate, and polyethersulfone. Preferably, polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, or polybutylene naphthalate may be used.

[0069] The base layer 13a may further contain additives such as an antioxidant, an ultraviolet absorbing agent, or a light stabilizer.

[0070] The thickness of the base layer 13a may be, for example, 10 μm or more and 200 μm or less. The tensile modulus of elasticity of the base layer 13a may be, for example, 50 MPa or more and 6000 MPa or less.

[0071] (Adhesive layer of adhesive tape) The adhesive layer 13b of the adhesive tape 13 contains, for example, an acrylic resin, an isocyanate compound, and a polymerization initiator (such as a photopolymerization initiator).

[0072] The acrylic resin has, for example, at least an alkyl (meth)acrylate structural unit, a hydroxyl group-containing (meth)acrylate structural unit, and a polymerizable group-containing (meth)acrylate structural unit in the molecule. The structural units are units that constitute the main chain of the acrylic resin.

[0073] The constituent unit of the alkyl (meth)acrylate is derived from an alkyl (meth)acrylate monomer. In other words, the molecular structure after the alkyl (meth)acrylate monomer is polymerized is the constituent unit of the alkyl (meth)acrylate. The term "alkyl" refers to a hydrocarbon moiety that is ester-bonded to (meth)acrylic acid. The number of carbon atoms in the alkyl moiety may be 6 or more and 12 or less.

[0074] Examples of the constituent units of alkyl(meth)acrylate include methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, isopropyl(meth)acrylate, n-butyl(meth)acrylate, isobutyl(meth)acrylate, s-butyl(meth)acrylate, pentyl(meth)acrylate, isopentyl(meth)acrylate, hexyl(meth)acrylate, heptyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, octyl(meth)acrylate, isooctyl(meth)acrylate, and isooctyl(meth)acrylate. Examples of structural units include acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate.

[0075] The acrylic resin has a hydroxyl group-containing (meth)acrylate structural unit, and the hydroxyl group of such a structural unit easily reacts with an isocyanate group. By allowing the acrylic resin having a hydroxyl group-containing (meth)acrylate structural unit and the isocyanate compound to coexist in the adhesive layer 13b, the adhesive layer 13b can be appropriately cured. Therefore, the acrylic resin can be sufficiently gelled. Therefore, the adhesive layer 13b can exhibit adhesive performance while maintaining its shape.

[0076] The structural unit of the hydroxyl group-containing (meth)acrylate is preferably a structural unit of a hydroxyl group-containing C2-C4 alkyl (meth)acrylate. The term "C2-C4 alkyl" refers to the hydrocarbon moiety ester-bonded to the (meth)acrylic acid and the number of carbon atoms. In other words, the hydroxyl group-containing C2-C4 alkyl (meth)acrylate monomer refers to a monomer in which (meth)acrylic acid is ester-bonded to an alcohol (usually a dihydric alcohol) having 2 to 4 carbon atoms. The hydrocarbon moiety of the C2-C4 alkyl is usually a saturated hydrocarbon.

[0077] Examples of the structural unit of the hydroxyl group-containing C2 to C4 alkyl(meth)acrylate include structural units of hydroxyethyl(meth)acrylate, hydroxypropyl(meth)acrylate, hydroxy n-butyl(meth)acrylate, and hydroxy iso-butyl(meth)acrylate.

[0078] The acrylic resin contains a structural unit of a polymerizable group-containing (meth)acrylate having a polymerizable unsaturated double bond in the side chain. Since the acrylic resin contains a structural unit of a polymerizable group-containing (meth)acrylate, the photopolymerization initiator generates radicals when irradiated with active energy rays such as ultraviolet rays, and the acrylic resin can be crosslinked by the action of the radicals. This allows the adhesive strength of the adhesive layer 13b before irradiation to be reduced by irradiation. The active energy rays include ultraviolet rays, radioactive rays, and electron beams.

[0079] Specifically, the structural unit of the polymerizable group-containing (meth)acrylate may have a molecular structure in which an isocyanate group of an isocyanate group-containing (meth)acrylate monomer is bonded via urethane to a hydroxyl group in the structural unit of the above-mentioned hydroxyl group-containing (meth)acrylate.

[0080] The structural unit of the polymerizable group-containing (meth)acrylate having a polymerizable group can be prepared after the polymerization reaction of synthesizing the acrylic resin. For example, after the copolymerization of an alkyl (meth)acrylate monomer and a hydroxyl group-containing (meth)acrylate monomer, the hydroxyl group in a part of the structural unit of the hydroxyl group-containing (meth)acrylate and the isocyanate group of the isocyanate group-containing polymerizable monomer are reacted with each other to form a urethane reaction, thereby obtaining the structural unit of the polymerizable group-containing (meth)acrylate.

[0081] The isocyanate group-containing (meth)acrylate monomer preferably has one isocyanate group and one (meth)acryloyl group in the molecule, such as 2-isocyanatoethyl (meth)acrylate.

[0082] The adhesive layer 13b may further contain an isocyanate compound, part of which may be in a state after reaction such as urethane reaction. The isocyanate compound has a plurality of isocyanate groups in the molecule, which allows the crosslinking reaction between the acrylic resins in the adhesive layer 13b to proceed.

[0083] Examples of the isocyanate compound include diisocyanates such as aliphatic diisocyanates, alicyclic diisocyanates, and aromatic aliphatic diisocyanates. Examples of the isocyanate compound include polymerized polyisocyanates such as dimers and trimers of diisocyanates, and polymethylene polyphenylene polyisocyanates. The above isocyanate compounds can be used alone or in combination of two or more.

[0084] The polymerization initiator contained in the adhesive layer 13b is a compound that can initiate a polymerization reaction by the applied heat or light energy. By containing the polymerization initiator in the adhesive layer 13b, when heat energy or light energy is applied to the adhesive layer 13b, a crosslinking reaction between the acrylic resins can be promoted, and the adhesive layer 13b can be hardened. This reduces the adhesive strength of the adhesive layer 13b, and after the backgrinding process (described in detail later), the second protective layer 12 and the hardened adhesive layer 13b can be easily peeled off from each other. As the polymerization initiator, for example, a commercially available general photopolymerization initiator or thermal polymerization initiator is used.

[0085] The adhesive layer 13b may further contain an additive, such as an antioxidant, an ultraviolet absorbing agent, or a surfactant.

[0086] The thickness of the adhesive layer 13b may be, for example, not less than 5 μm and not more than 150 μm.

[0087] The second example protective sheet 1 can be produced, for example, by removing the second release liner 17 of the first example produced as described above, and then attaching the adhesive layer 13b of the adhesive tape 13 to the second protective layer 12 in place of the second release liner 17. A commercially available product can be used as the adhesive tape 13. The adhesive tape 13 may be, for example, a commercially available backgrind tape.

[0088] <How to use protective sheets when manufacturing electronic component devices> Next, a method of using the protective sheet 1 of this embodiment will be described. Specifically, a method of manufacturing an electronic component device will be described. In other words, a specific example of a method of using the protective sheet 1 used to manufacture such an electronic component device will be described.

[0089] The method for manufacturing an electronic component device according to the present embodiment includes the steps of: A process of attaching a protective sheet to a surface of an electronic component to be protected (protection process); a step of cutting the electronic component and the protective sheet together into a plurality of small pieces while bringing cooling water of 30° C. or less into contact with the protective sheet (dicing step); and a step of removing the small piece of the protective sheet from the surface to be protected of the small piece of the electronic component (a removing step), The protective sheet has a first protective layer 11 that is attached to the surface to be protected, and a second protective layer 12 that overlaps one side of the first protective layer 11, the first protective layer 11 contains a water-soluble polymer compound, and the second protective layer 12 contains a hydrophilic polyester compound; The removing step includes removing the protective sheet pieces by dissolving at least a portion of the protective sheet pieces in a water-containing liquid at 40° C. or higher.

[0090] In the manufacturing method of an electronic component device of the present embodiment, the electronic component device is manufactured using the above-mentioned protective sheet 1. The surface to be protected by the above-mentioned protective sheet 1 is, for example, at least a part of the surface of an electronic component (e.g., a substrate) constituting the electronic component device. Examples of electronic component devices manufactured using the above-mentioned protective sheet 1 include the devices described above.

[0091] In the manufacturing method of the electronic component device of this embodiment, a dicing die bond film 50 can further be used as a manufacturing auxiliary tool. As shown in Fig. 11, the dicing die bond film 50 includes a dicing tape 20 and a die bond sheet 30 laminated on the dicing tape 20. The dicing tape 20 has a support layer 21 and an adhesive layer 22 overlapping the support layer 21. As the dicing die bond film 50, a commercially available product can be used.

[0092] In the manufacturing method for electronic component devices using the above-mentioned protective sheet 1, a surface to be protected, which is, for example, one surface of a substrate G, is protected by the protective sheet 1. The surface to be protected of the substrate G may be, for example, a circuit surface on which a circuit is formed, or a non-circuit surface on which no circuit is formed.

[0093] There is no particular limitation on the material of the substrate G as long as it is plate-shaped. Examples of the substrate G include a semiconductor wafer, a sensor wafer such as a CMOS or MEMS, a pseudo wafer, and a wiring circuit board.

[0094] The method for manufacturing an electronic component device according to this embodiment will be described in detail below, taking as an example a method for manufacturing a semiconductor device as an electronic component device.

[0095] In a manufacturing method of a semiconductor device (electronic component device), for example, a semiconductor chip X is cut out from a semiconductor wafer W on which a circuit surface is formed, and a semiconductor device is assembled having the cut out semiconductor chip X. In the manufacturing method of a semiconductor device described below, at least a protective sheet 1 and a dicing die bond film 50 are used to manufacture the semiconductor device.

[0096] In general, a method for manufacturing a semiconductor device includes a front-end process of forming a circuit surface on one side of a bare wafer using highly integrated electronic circuits, and a back-end process of cutting out semiconductor chips X from the semiconductor wafer W on which the circuit surface has been formed and assembling them.

[0097] In a post-process, for example, a wafer (semiconductor wafer W) serving as a substrate on which a circuit surface is formed is diced into small semiconductor chips X (dies), and then the diced semiconductor chips X are bonded to an adherend, thereby assembling a semiconductor integrated circuit (semiconductor device).

[0098] The semiconductor wafer W is configured to obtain a plurality of semiconductor chips X. More specifically, the semiconductor wafer W is configured to be divided into small pieces at intervals in a plurality of directions along the surface (for example, directions along the surface that are perpendicular to each other), so that a plurality of semiconductor chips X can be fabricated. The semiconductor wafer W has, on one surface, a circuit surface on which at least one type of circuit components is arranged.

[0099] In recent years, with the further advancement of integration technology in the semiconductor industry, there is a demand for thinner semiconductor chips (e.g., thicknesses of 20 μm to 50 μm). When viewed from one side in the thickness direction, the shape of the semiconductor chip is, for example, rectangular, with the length of one side being a predetermined length of, for example, 5 mm to 20 mm.

[0100] A first and second specific example of the method for manufacturing a semiconductor device will be described below. In the first example, a protective sheet 1 shown in Fig. 1A is used, and in the second example, a protective sheet 1 shown in Fig. 2A is used. In addition, the drawings showing the manufacturing method of the first example are marked with "I." Similarly, the drawings showing the manufacturing method of the second example are marked with "II."

[0101] "First Example of a Manufacturing Method for a Semiconductor Device" The first example of the method for manufacturing a semiconductor device includes an assembly process in which a semiconductor wafer W (substrate) on which a circuit surface is formed is diced to produce semiconductor chips X, and a semiconductor device having such semiconductor chips X is assembled. The assembly process includes a protection process of protecting at least one of the circuit surfaces (surface to be protected) of the semiconductor wafer W, the circuit surface on which the circuit components are arranged, by overlaying a protective sheet 1 for protecting the circuit surface. a mounting process in which a semiconductor wafer W having a circuit surface formed on one side is attached to a dicing die bond film 50 (a die bond sheet 30 overlapping a dicing tape 20) to fix the semiconductor wafer W to the dicing die bond film 50; a dicing process for dividing and dividing the laminate of the semiconductor wafer W, the protective sheet 1, and the die bond sheet 30 into small pieces to produce a plurality of small laminates in which the semiconductor chips X obtained by dividing the semiconductor wafer W, the small pieces of the protective sheet, and the small pieces 30' of the die bond sheet are overlapped with each other; an expanding step of expanding the intervals between adjacent semiconductor chips X, which is performed as necessary; a removing step of removing each of the small pieces of the protective layer overlying the circuit surface of the semiconductor chip X by contacting the small pieces of the protective layer with a relatively high-temperature water-containing liquid; a pick-up process of peeling the dicing tape 20 and the die-bonding sheet piece 30' to take out the semiconductor chip X with the die-bonding sheet piece 30' attached; and a die bonding step of bonding the extracted semiconductor chip X to an adherend via the small piece 30' of the die bond sheet.

[0102] In the protection step, the first protective layer 11 of the protective sheet 1 is superimposed on the circuit surface of the semiconductor wafer W. By superimposing the protective sheet 1 on the circuit surface of the semiconductor wafer W, the circuit surface can be protected by the protective sheet 1 until the protective sheet 1 is removed. Therefore, it is possible to prevent foreign matter and the like from adhering to the circuit surface of the semiconductor wafer W covered with the protective sheet 1.

[0103] In the mounting step, first, a dicing ring R may be attached to the adhesive layer 22 of the dicing tape 20, and then the dicing ring R may be fixed to a holder H of an expanding device. Then, as shown in FIG. 3A, the semiconductor wafer W, the protective sheet 1, and the second release liner 17 are attached to the die bond sheet 30 overlapping the dicing tape 20 at once. For example, the semiconductor wafer W is fixed to the die bond sheet 30 in this manner. Then, the protective sheet 1 is pressed against the semiconductor wafer W via the second release liner 17, thereby pressure-sensitively adhering the protective sheet 1 to the circuit surface.

[0104] In addition, the mounting process may be performed after the protective sheet 1 is superimposed on the circuit surface of the semiconductor wafer W and a protective process is performed, or the semiconductor wafer W with the exposed circuit surface is fixed to a die bond sheet 30 and a mounting process is performed, and then the protective process is performed.

[0105] When second release liner 17 is used as described above, second release liner 17 is removed by peeling it off from protective sheet 1, as shown in Figures 3B and 3C.

[0106] In the dicing step, a blade dicing process is performed. In the blade dicing process, the die bond sheet 30, the semiconductor wafer W, and the protective sheet 1 are divided into small pieces by a dicing blade T or the like, and the semiconductor wafer W is divided into small pieces to produce semiconductor chips X (dies).

[0107] In the dicing process, the temperature of the semiconductor wafer W etc. rises due to frictional heat etc. as the relatively hard semiconductor wafer W is cut using the dicing blade T. In order to suppress an excessive temperature rise, cooling water is brought into contact with the protective sheet 1 during the blade dicing process. Specifically, the laminate of the die bond sheet 30, the semiconductor wafer W, and the protective sheet 1 is cut by the dicing blade T while the cooling water is being applied to the second protective layer 12 of the protective sheet 1.

[0108] More specifically, in the dicing process, the protective sheet 1 and the semiconductor wafer W are cut together with the die bond sheet 30 to a predetermined size to form a semiconductor chip X with a small piece 30' of the die bond sheet. At this time, a small piece of the protective sheet is also formed. That is, a laminate of the small pieces 11' of the first protective layer and the small pieces 12' of the second protective layer is also formed. The blade dicing process is performed in a conventional manner using, for example, a dicing blade T. In the blade dicing process, for example, a cutting method called full cut, in which the cut is made up to the die bond sheet 30, can be adopted. The dicing device used in the blade dicing process is not particularly limited, and a conventionally known device can be used. In blade dicing, foreign matter such as debris may be generated when cutting the semiconductor wafer W. At this time, since the surface to be protected of the semiconductor wafer W is protected by the protective sheet 1, it is possible to prevent the foreign matter from adhering to the surface to be protected.

[0109] The temperature of the cooling water used in the dicing step is 30° C. or less, and preferably 25° C. or less. The temperature of the cooling water may be 0° C. or more, 5° C. or more, or 10° C. or more.

[0110] The cooling water is not particularly limited as long as it is a liquid containing water. In terms of simplifying the disposal of the cooling water after use, the cooling water preferably contains 90% by mass or more of water, more preferably contains 95% by mass or more of water, even more preferably contains 98% by mass or more of water, and is most preferably water.

[0111] Even if the protective sheet comes into contact with the cooling water in the dicing process, the protective sheet is arranged so that the second protective layer 12 comes into contact with the cooling water, so that the contact between the first protective layer 11 of the protective sheet and the cooling water is suppressed. Therefore, dissolution of the first protective layer 11 in the cooling water is suppressed. Therefore, even if the protective sheet comes into contact with the cooling water, the surface to be protected (circuit surface) of the semiconductor wafer W can remain protected by the protective sheet.

[0112] In the expanding process, which is performed as necessary, the interval between adjacent semiconductor chips (dies) X produced by dividing the semiconductor wafer W is expanded. In detail, a dicing ring R is attached to the adhesive layer 22 of the dicing tape 20, and then fixed to a holder H of the expanding device. A push-up member U provided in the expanding device is pushed up from the lower side of the dicing die bond film 50, thereby stretching the dicing die bond film 50 so as to expand it in the surface direction. The above-mentioned interval is expanded by stretching.

[0113] In the removal step, as shown in Fig. 5, for example, a water-containing liquid at 40°C or higher is brought into contact with the protective sheet pieces (a laminate of the first protective layer pieces 11' and the second protective layer pieces 12') to dissolve at least a portion of each protective sheet piece in the relatively hot water-containing liquid. This makes it possible to remove all of the protective sheet pieces overlapping the surface to be protected of the semiconductor chip X. In other words, it is possible to remove both the first protective layer pieces 11' and the second protective layer pieces 12' from the surface (surface to be protected) of the semiconductor chip X. By carrying out the removing step in this manner, all of the multiple small pieces of the protective sheet can be removed relatively easily. Also, the number of foreign matters attached to the semiconductor chip surface can be relatively easily reduced by the water-containing liquid. Also, the surface (surface to be protected) of each semiconductor chip X can be washed with a relatively high-temperature water-containing liquid.

[0114] The temperature of the water-containing liquid that is brought into contact with the protective sheet pieces is preferably 50° C. or higher, and more preferably 60° C. or higher, in order to remove the protective sheet pieces in a shorter time. The temperature of the water-containing liquid may be 100° C. or lower.

[0115] In the removal step, the semiconductor chip X with the protective sheet pieces (11', 12') attached thereto may be immersed in a stirred liquid containing relatively high temperature water, or liquid sprayed from a nozzle or the like may be brought into contact with the protective sheet pieces.

[0116] In the removal step, the multiple small pieces of the protective sheet may be removed by dissolving all of the components of the protective sheet 1 in the liquid. On the other hand, the multiple small pieces of the protective sheet may be removed by dissolving a portion of the components of the protective sheet in the liquid, causing each small piece to lose adhesion to the semiconductor chip X and become detached from the semiconductor chip X.

[0117] For example, in the removal step, a relatively high-temperature water-containing liquid is sprayed toward the semiconductor chips X attached to the small pieces 30' of the die bond sheet while rotating a disk-shaped stage supporting the dicing tape 20 from below in the circumferential direction. This makes it possible to efficiently remove the multiple small pieces of the protective sheet overlapping the semiconductor chips X.

[0118] The water-containing liquid is not particularly limited as long as it is a liquid substance containing water. Such a liquid may contain water in an amount of 90% by mass or more, 95% by mass or more, or 98% by mass or more. The water-containing liquid may be water. The liquid may contain a component that dissolves in water in addition to water. Examples of such components include water-soluble organic solvents. Examples of such water-soluble organic solvents include monohydric alcohols having 4 or less carbon atoms, such as methanol, ethanol, propanols such as isopropyl alcohol, and butanols such as t-butanol.

[0119] When performing the pick-up process, it is necessary that the small piece 30' of the die bond sheet attached to the semiconductor chip X can be easily peeled off from the adhesive layer 22 of the dicing tape 20. The above-mentioned dicing tape 20 is designed to be able to exhibit such a performance well. For example, the dicing tape 20 is configured so that the adhesive layer 22 is cured and the adhesive strength of the adhesive layer 22 is reduced by irradiation with active energy rays (e.g., ultraviolet rays). Since the adhesive layer 22 is cured after irradiation, the adhesive strength of the adhesive layer 22 can be reduced, and therefore the semiconductor chip X and the small piece 30' of the die bond sheet can be relatively easily peeled off from the adhesive layer 22 after irradiation. Dicing tapes 20 configured in this way are commercially available.

[0120] In the pick-up process, as shown in Fig. 6, the piece 30' of the die bond sheet attached to the semiconductor chip X is peeled off from the adhesive layer 22 of the dicing tape 20. More specifically, the pin member P is raised to push up the semiconductor chip X to be picked up through the dicing tape 20. The pushed-up semiconductor chip X and the piece 30' of the die bond sheet are held by a suction jig J. In this way, the semiconductor chip (die) is taken out with the piece 30' of the die bond sheet attached.

[0121] In the die bonding process, the semiconductor chip X with the die bond sheet piece 30' attached thereto is bonded to an adherend Z. In other words, the semiconductor chip X is bonded to an adherend such as a substrate or a semiconductor chip X via the die bond sheet piece 30'. In the die bonding process, as shown in FIG. 7, a plurality of semiconductor chips X with the die bond sheet piece 30' attached thereto may be stacked. The adherend Z may be, for example, an interposer, a wiring circuit board, or a small piece of a substrate (when small pieces of a substrate are stacked and laminated).

[0122] The manufacturing method of the semiconductor device of this embodiment may further include a curing process for hardening the die bond sheet 30 adhered to the adherend, a wire bonding process for electrically connecting the electrodes of the electronic circuit in the semiconductor chip (die) to the adherend via wires, and a sealing process for sealing the semiconductor chip (die) and wires on the adherend with a thermosetting resin.

[0123] In the curing step after the die bonding step, in order to promote the hardening of the die bonding sheet 30, a heat treatment may be performed at a temperature of, for example, 100° C. or higher and 180° C. or lower.

[0124] In the wire bonding step following the curing step, the semiconductor chip X (die) and the adherend Z may be connected with a wire L while being heated.

[0125] In the sealing process after the wire bonding process, the semiconductor chip X (die) and the small piece 30' of the die bond sheet are sealed (covered) with a thermosetting resin M such as epoxy resin, as shown in Fig. 8. At this time, in order to promote the curing reaction of the thermosetting resin M, a heat treatment may be performed at a temperature of 100°C or higher and 180°C or lower.

[0126] Next, a method for manufacturing a semiconductor device according to a second example will be described. The manufacturing method according to the second example is similar to the manufacturing method according to the first example, but differs from the manufacturing method according to the first example in that a protective sheet 1 having an adhesive tape 13 (see FIG. 2A) is used. Specifically, the manufacturing method according to the second example differs from the manufacturing method according to the first example in that a back grinding process is performed using the protective sheet 1 having the adhesive tape 13 between the protection process and the mounting process.

[0127] "Second Example of a Method for Manufacturing a Semiconductor Device" The second example manufacturing method for a semiconductor device includes at least a protection step of overlapping a protective sheet 1 having an adhesive tape 13, such as a back-grinding tape, on the surface of a semiconductor wafer W to be protected, a back-grinding step of grinding the semiconductor wafer W with the protective sheet 1 attached thereto to reduce its thickness, a mounting step of attaching one side (e.g., the side opposite the circuit side) of the thinned semiconductor wafer W to a die bond sheet 30 to fix the semiconductor wafer to the dicing tape 20, a dicing step similar to the above, an expanding step similar to the above which is performed if necessary, a removing step similar to the above, a pick-up step similar to the above, and a die bond step similar to the above.

[0128] In the backgrinding process, as shown in Figures 9A and 9B, a grinding process is performed on the semiconductor wafer W with an adhesive tape 13 (e.g., a backgrinding tape) attached thereto, and the thickness of the semiconductor wafer W is reduced to the thickness of the chip (die) that will be produced in the subsequent dicing process (see Figure 9C).

[0129] The protective sheet 1 used in the backgrinding process has an adhesive layer 13b, and the adhesive layer 13b can strongly adhere to the second protective layer 12. Therefore, as shown in Fig. 9B, even if a relatively strong force is applied through the semiconductor wafer W during the backgrinding process, peeling between the adhesive layer 13b of the protective sheet 1 and the adjacent layer is suppressed. Therefore, the backgrinding process can be stably performed.

[0130] In the mounting step, the semiconductor wafer W is fixed to the dicing tape 20 in the same manner as in the manufacturing method of the first example described above (see FIG. 10A). Next, the adhesive tape 13 (for example, a backgrind tape) is peeled off from the semiconductor wafer W (see FIG. 10B). When peeling the adhesive tape 13 (for example, a backgrind tape) from the semiconductor wafer W, the peeling can be easily performed by hardening the adhesive layer 13b as described above.

[0131] The subsequent steps can be carried out in the same manner as in the manufacturing method of the first example described above.

[0132] The manufacturing method of the protective sheet and electronic component device of this embodiment is as exemplified above, but the present invention is not limited to the manufacturing method of the protective sheet and electronic component device exemplified above. In other words, various configurations used in general protective sheets and methods for manufacturing electronic component devices can be adopted as long as they do not impair the effects of the present invention.

[0133] The matters disclosed in this specification include the following. (1) A protective sheet for protecting a surface to be protected of an electronic component, A first protective layer is attached to the surface to be protected, and a second protective layer is overlapped on one side of the first protective layer, the first protective layer contains a water-soluble polymer compound, The second protective layer comprises a hydrophilic polyester compound. (2) The protective sheet according to (1) above, wherein the first protective layer contains at least one of polyvinyl alcohol and polyethylene oxide as the water-soluble polymer compound. (3) The protective sheet according to (1) or (2) above, wherein the contact angle of water on the surface of the first protective layer is 25° or more and 45° or less, and the contact angle of water on the surface of the second protective layer is 60° or more and 80° or less. (4) Further provided is an adhesive tape having a base layer and an adhesive layer overlapping one surface of the base layer, The protective sheet according to any one of (1) to (3) above, wherein the adhesive layer of the adhesive tape is disposed so as to overlap the second protective layer. (5) The shear adhesion strength of the first protective layer to the silicon wafer is 25 mm 2 The protective sheet according to any one of (1) to (4) above, having an adhesive area of ​​0.20 MPa or more at 25°C. (6) A step of attaching a protective sheet to a surface of an electronic component to be protected; cutting the electronic components and the protective sheet together into a plurality of small pieces while bringing cooling water of 30° C. or less into contact with the protective sheet; and removing the piece of protective sheet from the surface to be protected of the piece of electronic component, the protective sheet has a first protective layer attached to the surface to be protected and a second protective layer overlapping one side of the first protective layer, the first protective layer contains a water-soluble polymer compound, and the second protective layer contains a hydrophilic polyester compound; A method for manufacturing an electronic component device, wherein the removing step includes removing the protective sheet fragments by dissolving at least a portion of the protective sheet fragments in a water-containing liquid at 40°C or higher. EXAMPLES

[0134] The present invention will now be described in more detail with reference to experimental examples, but the present invention is not limited thereto.

[0135] The protective sheets shown in Table 1 were produced using the following raw materials.

[0136] <Raw material for the first protective layer> (Water-soluble polymer compound) [A-1] Polyvinyl alcohol (PVA) Product name: "JMR-3M" manufactured by Japan Vinyl Acetate & Poval Co., Ltd. (Saponification degree: 60, polymerization degree: 100) [A-2] Polyvinyl alcohol (PVA) Product name: "JMR-3H" manufactured by Japan Vinyl Acetate & Poval Co., Ltd. (Saponification degree: 80, polymerization degree: 100) [A-3] Polyvinyl alcohol (PVA) Product name: "JMR-10L" manufactured by Japan Vinyl Acetate & Poval Co., Ltd. (Saponification degree: 35, polymerization degree: 250)

[0137] <Raw material for the second protective layer> (hydrophilic polyester compound) [B-1] -SO 3 Hydrophilic polyester compound containing sodium in the molecule Product name: Pluscoat Z-221, manufactured by GOO Chemical Industry Co., Ltd. (Glass transition point Tg: 47°C, softening point: 135-140°C, acid value: less than 5mgKOH / g) [B-2] -SO 3 Hydrophilic polyester compound containing sodium in the molecule Product name: Pluscoat Z-446, manufactured by GOO Chemical Industry Co., Ltd. (-SO in the molecule 3 (Na is less than B-1 above) (Glass transition point Tg: 47°C, softening point: 115-125°C, acid value: less than 5mgKOH / g)

[0138] <First release liner and second release liner> (First release liner) PET film with release-treated surface Mitsubishi Chemical Corporation product name: "Diafoil MRA50" thickness 50μm (Second release liner) PET film with release-treated surface Mitsubishi Chemical Corporation product name: "Diafoil MRA50" (thickness 25μm)

[0139] The configuration of the protective sheet in each of the examples and comparative examples is shown in Table 1.

[0140] (Examples 1 to 3) Each water-soluble polymer compound was dispersed in water, and the mixture was heated to 90°C and stirred to prepare an aqueous solution of each water-soluble polymer compound. Next, the aqueous solution was applied to one side (release-treated side) of each first release liner using an applicator. A first protective layer was formed on the first release liner by drying at 110°C for 2 minutes. In this manner, a first protective layer (10 μm thick) having the configuration shown in Table 1 was produced. On the other hand, each hydrophilic polyester compound was dispersed in water, heated to 90°C, and stirred to prepare a solution of each hydrophilic polyester compound. Next, the above solution was applied to one side (release-treated side) of each second release liner using an applicator. A second protective layer was formed on the second release liner by drying at 110°C for 2 minutes. In this way, a second protective layer having the configuration shown in Table 1 was produced. Next, the laminate of the first protective layer and the first release liner and the laminate of the second protective layer and the second release liner were laminated together at a temperature of 70° C. and a speed of 10 mm / sec. When laminated, the first protective layer and the second protective layer were arranged so as to be in direct contact with each other, and these protective layers were sandwiched between the first release liner and the second release liner. (Comparative Examples 1 to 3) The second protective layer was formed in the same manner as the first protective layer in Example 1, and each protective sheet having the configuration shown in Table 1 was produced.

[0141] [Table 1]

[0142] [Measurement of physical properties (contact angle of water) of the first and second protective layers] The contact angle of water was measured by the above-mentioned measuring method, and the measurement results were as follows. Contact angle of water on the surface of the first protective layer formed only from [A-1] (25°C) 40.8° Contact angle of water on the surface of the first protective layer formed only from [A-3] (25°C) 79.5° Contact angle of water on the surface of the second protective layer formed only from [B-1] (25°C) 68.4° Contact angle of water on the surface of the second protective layer formed only from [B-2] (25°C) 74.7° Contact angle of water on the surface of the second protective layer formed only from [A-2] (25°C) 40.6°

[0143] [Measurement of physical properties (shear adhesive strength) of the first and second protective layers] The shear adhesive strength of each of the first protective layer and the second protective layer was measured according to the above-mentioned measuring method, and the measurement results were as follows. Shear adhesive strength of the first protective layer formed only from [A-1] above (25°C) 0.46MPa Shear adhesive strength of the first protective layer formed only from [A-3] above (25°C) 1.21MPa Shear adhesive strength of the second protective layer formed only from [B-1] above (25°C) 0.06MPa Shear adhesive strength of the second protective layer formed only from [B-2] above (25°C) 0.05MPa Shear adhesive strength of the second protective layer formed only from [A-2] above (25°C) 0.08MPa

[0144] <Dicing ability> After attaching each of the above protective sheets to the surface of a bare silicon wafer, blade dicing was performed under the following conditions: The first protective layer of the protective sheet was attached to the bare wafer, and the blade dicing was performed with one side of the second protective layer exposed. Wafer thickness: 200μm Single Cut Blade: ZH05 SD-3000-N1-70 CC Dicing speed: 50mm / sec Rotational speed: 45,000 rpm Water amount: 0.5L / min Cooling water temperature: 23℃ For each small piece of the protective sheet divided after the blade dicing process, the length of peeling from the edge (the length from the edge of the turned-over portion) was observed. In other words, the degree of exposure of the wafer was observed. Then, evaluation was made according to the following criteria. 500μm or less: Good (○) 500μm or more and 1mm or less: Fairly good (△) 1mm or more: Defective (×) <Hot water removal performance> After the above blade dicing process, a washing process was carried out using 50° C. warm water (running water) for 60 seconds to remove a number of small pieces of the protective sheet. Thereafter, the remaining glue on the chip was checked. If glue remains: Poor (×) If only a small piece of protective sheet remains: Fairly good (△) If no small pieces of protective sheet remain: Good (〇) The results are shown in Table 1.

[0145] As can be seen from the above results, the protective sheet of the example was not removed even when cut while in contact with 23°C cooling water, but was easily removed with 50°C hot water. In contrast, in Comparative Example 1, the protective sheet cut while in contact with cooling water peeled off from the surface to be protected due to weak adhesion to the surface to be protected. In Comparative Example 2, the protective sheet cut while in contact with cooling water peeled off from the surface to be protected as it dissolved in the cooling water. In Comparative Example 3, the protective sheet was not sufficiently removed even when in contact with 50°C hot water.

[0146] The protective sheet of the embodiment includes a first protective layer containing a water-soluble polymer compound and a second protective layer containing a hydrophilic polyester compound. By using the protective sheet of such an embodiment in the manufacture of electronic component devices, the electronic component devices can be manufactured efficiently. For example, the protective sheet as in the embodiment is used to protect the circuit surface on which electronic circuits are formed in a semiconductor wafer, and can adequately maintain protection of the surface to be protected even when cut while in contact with cooling water during dicing, and furthermore, after protection, is removed by a relatively high-temperature water-containing liquid. Thus, by using the protective sheet as in the embodiment, electronic component devices can be efficiently manufactured. [Industrial Applicability]

[0147] The protective sheet of the present invention is suitably used, for example, as an auxiliary tool when manufacturing electronic component devices such as semiconductor devices. The method for manufacturing an electronic component device of the present invention is preferably used when manufacturing an electronic component device such as a semiconductor device. [Explanation of symbols]

[0148] 1: Protective sheet, 11: 1st protective layer, 12: 2nd protective layer, 13: adhesive tape; 13a: base layer; 13b: adhesive layer; 15: first release liner, 17: second release liner, 20: dicing tape; 21: support layer; 22: adhesive layer; 30: Die bond sheet, 50: Dicing die bond film.

Claims

1. A protective sheet for protecting a surface to be protected of an electronic component, A first protective layer is attached to the surface to be protected, and a second protective layer is overlapped on one surface of the first protective layer, the first protective layer contains a water-soluble polymer compound, A protective sheet, wherein the second protective layer comprises a hydrophilic polyester compound.

2. The protective sheet according to claim 1 , wherein the first protective layer contains at least one of polyvinyl alcohol and polyethylene oxide as the water-soluble polymer compound.

3. 3. The protective sheet according to claim 1, wherein the surface of the first protective layer has a contact angle with water of 25° or more and 45° or less, and the surface of the second protective layer has a contact angle with water of 60° or more and 80° or less.

4. Further provided is an adhesive tape having a base layer and an adhesive layer overlapping one surface of the base layer, The protective sheet according to claim 1 , wherein the adhesive tape is disposed so that the adhesive layer overlaps the second protective layer.

5. A step of attaching a protective sheet to a surface of an electronic component to be protected; cutting the electronic components and the protective sheet into a plurality of small pieces while bringing cooling water of 30° C. or less into contact with the protective sheet; and removing the piece of protective sheet from the surface to be protected of the piece of electronic component, the protective sheet has a first protective layer attached to the surface to be protected and a second protective layer overlapping one side of the first protective layer, the first protective layer contains a water-soluble polymer compound, and the second protective layer contains a hydrophilic polyester compound; The method for manufacturing an electronic component device, wherein the removing step includes removing the protective sheet fragments by dissolving at least a portion of the protective sheet fragments in a water-containing liquid at 40° C. or higher.

Citation Information

Patent Citations

  • Tentatively fixing sheet, processing method, coated film formation method, and method for manufacturing electronic component

    JP2021161735A

Cited By

  • Method for producing molded body

    WO2026100605A1

  • Wafer protective film forming method and wafer grinding device

    WO2026141438A1