Nonaqueous electrolyte secondary battery

A non-aqueous electrolyte secondary battery with lithium nickel cobalt manganese composite oxide and a specific electrolyte composition addresses cobalt depletion by enhancing output characteristics through a hollow particle structure and electrolyte additives.

JP2024135222AActive Publication Date: 2024-10-04PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2023045802
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

The increasing demand for non-aqueous electrolyte secondary batteries in electric vehicles poses a risk of cobalt depletion, and ternary active materials with reduced cobalt content suffer from insufficient output characteristics.

Method used

A non-aqueous electrolyte secondary battery design using lithium nickel cobalt manganese composite oxide with a specific molar ratio of Ni and Co, in the form of hollow particles with a through hole, combined with a non-aqueous electrolyte containing a carboxylic acid ester and lithium bis(oxalato)borate, enhances the battery's output characteristics.

Benefits of technology

The battery achieves excellent output characteristics despite using a ternary active material with a low cobalt content, addressing resource depletion concerns and improving discharge efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135222000001_ABST
    Figure 2024135222000001_ABST
Patent Text Reader

Abstract

To provide a nonaqueous electrolyte secondary battery having excellent output characteristics while using a ternary active material with low cobalt content.SOLUTION: A nonaqueous electrolyte secondary battery disclosed herein includes a positive electrode, a negative electrode and a nonaqueous electrolyte. The positive electrode has a positive electrode active material layer including a positive electrode active material. The positive electrode active material is a lithium-nickel-cobalt-manganese composite oxide. In the composite oxide, a molar ratio of Ni to an all metal elements other than Li is 40-60 mol%, and a molar ratio of Co is 15-25 mol%. The composite oxide is hollow particles each including a shell part, a hollow part formed inside the shell part, and a through hole penetrating through the shell part. The BET specific surface area of the composite oxide is 3.0 m2 / g or more. The nonaqueous electrolyte contains a nonaqueous solvent, an electrolyte salt, and lithium bis(oxalate)borate. The nonaqueous solvent contains a carboxylic acid ester with a carbon number of 4 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a non-aqueous electrolyte secondary battery. [Background technology]

[0002] In recent years, from the perspective of decarbonization, the demand for electric vehicles (BEVs), hybrid vehicles (HEVs), plug-in hybrid vehicles (PHEVs), etc. is rapidly increasing. As a result, the demand for nonaqueous electrolyte secondary batteries, which serve as the driving power sources for these vehicles, is also rapidly increasing.

[0003] Lithium nickel cobalt manganese composite oxides, also known as ternary active materials, are known as typical positive electrode active materials used in nonaqueous electrolyte secondary batteries (see, for example, Patent Documents 1 to 4). As ternary active materials, those containing approximately equimolar amounts of Ni, Co, and Mn (i.e., a molar ratio of approximately 1:1:1) are often used in practice. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2022-09722 [Patent Document 2] JP 2020-95842 A [Patent Document 3] Special Publication No. 2018-530122 [Patent Document 4] International Publication No. 2021 / 186949 Summary of the Invention [Problem to be solved by the invention]

[0005] If the demand for BEVs continues to expand for decarbonization, there is concern that the resources used in non-aqueous electrolyte secondary batteries will be depleted in the future. One of the resources that is feared to be depleted is cobalt (Co). One possible solution to this problem is to reduce the cobalt content of ternary active materials. However, on the other hand, there is a demand for even higher output from non-aqueous electrolyte secondary batteries, and ternary active materials with a low cobalt content have the problem of insufficient output characteristics.

[0006] SUMMARY OF THE PRESENT EMBODIMENTS The present invention has an object to provide a non-aqueous electrolyte secondary battery that has excellent output characteristics while using a ternary active material with a low cobalt content. [Means for solving the problem]

[0007] The non-aqueous electrolyte secondary battery disclosed herein contains a positive electrode, a negative electrode, and a non-aqueous electrolyte. The positive electrode has a positive electrode active material layer containing a positive electrode active material. The positive electrode active material is a lithium nickel cobalt manganese based composite oxide. In the lithium nickel cobalt manganese based composite oxide, the molar ratio of Ni to all metal elements other than Li is 40 mol % to 60 mol %, and the molar ratio of Co is 15 mol % to 25 mol %. The lithium nickel cobalt manganese based composite oxide is in the form of hollow particles having a shell portion, a hollow portion formed inside the shell portion, and through holes penetrating the shell portion. The BET specific surface area of ​​the lithium nickel cobalt manganese based composite oxide is 3.0 m 2 / g or more. The non-aqueous electrolyte contains a non-aqueous solvent, an electrolyte salt, and lithium bis(oxalato)borate. The non-aqueous solvent contains a carboxylic acid ester having 4 or less carbon atoms.

[0008] According to this configuration, it is possible to provide a nonaqueous electrolyte secondary battery that has excellent output characteristics even when using a ternary active material with a low cobalt content. [Brief description of the drawings]

[0009] [Figure 1]1 is a cross-sectional view showing a schematic internal structure of a lithium-ion secondary battery according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic exploded view showing the configuration of a wound electrode body of a lithium ion secondary battery according to one embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic cross-sectional view of an example of a hollow particle of a positive electrode active material used in a lithium ion secondary battery according to one embodiment of the present invention. [Figure 4] FIG. 2 is a schematic cross-sectional view of another example of a hollow particle of a positive electrode active material used in a lithium ion secondary battery according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Matters not mentioned in this specification but necessary for carrying out the present invention can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The present invention can be carried out based on the contents disclosed in this specification and the technical common sense in the relevant field. In addition, in the following drawings, members and parts having the same function are described with the same reference numerals. Furthermore, the dimensional relationships (length, width, thickness, etc.) in each drawing do not reflect the actual dimensional relationships. In addition, the numerical range expressed as "A to B" in this specification includes A and B.

[0011] In this specification, the term "secondary battery" refers to an electricity storage device that can be repeatedly charged and discharged. In addition, in this specification, the term "lithium ion secondary battery" refers to a secondary battery that uses lithium ions as a charge carrier and realizes charging and discharging by the transfer of charge associated with the lithium ions between the positive and negative electrodes.

[0012] Hereinafter, the present invention will be described in detail using as an example a flat rectangular lithium ion secondary battery having a flat wound electrode body and a flat battery case, but it is not intended that the present invention be limited to the embodiment described therein.

[0013] The lithium ion secondary battery 100 shown in FIG. 1 is a sealed battery constructed by housing a flat wound electrode body 20 and a nonaqueous electrolyte 80 in a flat rectangular battery case (i.e., an outer container) 30. The battery case 30 is provided with a positive electrode terminal 42 and a negative electrode terminal 44 for external connection, and a thin-walled safety valve 36 that is set to release the internal pressure when the internal pressure of the battery case 30 rises to a predetermined level or higher. The battery case 30 is also provided with an injection port (not shown) for injecting the nonaqueous electrolyte 80. The positive electrode terminal 42 is electrically connected to the positive electrode current collector plate 42a. The negative electrode terminal 44 is electrically connected to the negative electrode current collector plate 44a. The material of the battery case 30 is, for example, a lightweight metal material with good thermal conductivity, such as aluminum. Note that FIG. 1 does not accurately represent the amount of the nonaqueous electrolyte 80.

[0014] 1 and 2, the wound electrode body 20 has a configuration in which a positive electrode sheet 50 and a negative electrode sheet 60 are overlapped with two long separator sheets 70 interposed therebetween and wound in the longitudinal direction. The positive electrode sheet 50 has a configuration in which a positive electrode active material layer 54 is formed along the longitudinal direction on one or both sides (both sides here) of a long positive electrode current collector 52. The negative electrode sheet 60 has a configuration in which a negative electrode active material layer 64 is formed along the longitudinal direction on one or both sides (both sides here) of a long negative electrode current collector 62. The positive electrode active material layer-free portion 52a (i.e., a portion where the positive electrode active material layer 54 is not formed and the positive electrode current collector 52 is exposed) and the negative electrode active material layer-free portion 62a (i.e., a portion where the negative electrode active material layer 64 is not formed and the negative electrode current collector 62 is exposed) are formed so as to protrude outward from both ends in the winding axis direction (i.e., the sheet width direction perpendicular to the longitudinal direction) of the wound electrode body 20. The positive electrode active material layer-free portion 52a and the negative electrode active material layer-free portion 62a are joined to the positive electrode current collector 42a and the negative electrode current collector 44a, respectively.

[0015] The positive electrode current collector 52 constituting the positive electrode sheet 50 may be a known positive electrode current collector used in lithium ion secondary batteries, and examples thereof include a sheet or foil made of a metal having good electrical conductivity (e.g., aluminum, nickel, titanium, stainless steel, etc.). The positive electrode current collector 52 is preferably aluminum foil.

[0016] The dimensions of the positive electrode current collector 52 are not particularly limited and may be appropriately determined depending on the battery design. When an aluminum foil is used as the positive electrode current collector 52, the thickness is not particularly limited, but is, for example, 5 μm or more and 35 μm or less, and preferably 7 μm or more and 20 μm or less.

[0017] The positive electrode active material layer 54 contains a positive electrode active material. In this embodiment, at least a lithium nickel cobalt manganese based composite oxide is used as the positive electrode active material.

[0018] In this specification, the term "lithium nickel cobalt manganese composite oxide" includes oxides containing Li, Ni, Co, Mn, and O as constituent elements, as well as oxides containing one or more additional elements other than these. Examples of such additional elements include transition metal elements and typical metal elements such as Mg, Ca, Al, Ti, V, Cr, Y, Zr, Nb, Mo, Hf, Ta, W, Na, Fe, Zn, and Sn. The additional element may also be a metalloid element such as B, C, Si, or P, or a nonmetal element such as S, F, Cl, Br, or I.

[0019] In the lithium nickel cobalt manganese based composite oxides that are often used in practice, the molar ratio of Co to all metal elements other than Li is about 30 mol% to 33.3 mol%. In contrast, the lithium nickel cobalt manganese based composite oxides used in this embodiment have a small Co content ratio, and therefore, in the lithium nickel cobalt manganese based composite oxide, the molar ratio of Co to all metal elements other than Li is 15 mol% to 25 mol%. In addition, the molar ratio of Ni to all metal elements other than Li is 40 mol% to 60 mol%. In this embodiment, as the lithium nickel cobalt manganese based composite oxide, one that satisfies the molar ratio of Ni and the molar ratio of Co may be used alone, or two or more types that satisfy the molar ratio of Ni and the molar ratio of Co may be used in combination. The molar ratio of Co is preferably 15 mol% to 22 mol%, more preferably 15 mol% to 20 mol%.

[0020] Specifically, the lithium nickel cobalt manganese based composite oxide has a composition represented by the following formula (I), for example. Li 1+x Ni y Co z Mn (1-y-z) M α O 2-β Q β (I)

[0021] In formula (I), x, y, z, α, and β satisfy the following conditions: -0.05≦x≦0.3, 0.4≦y≦0.6, 0.15≦z≦0.25, 0≦α≦0.1, and 0≦β≦0.5. M is at least one element selected from the group consisting of Zr, Mo, W, Mg, Ca, Na, Fe, Cr, Zn, Sn, B, and Al. Q is at least one element selected from the group consisting of F, Cl, and Br.

[0022] x preferably satisfies 0≦x≦0.3, and more preferably satisfies 0≦x≦0.20. y preferably satisfies 0.45≦y≦0.6. z preferably satisfies 0.15≦z≦0.22, and more preferably satisfies 0.15≦z≦0.20. α preferably satisfies 0≦α≦0.05, and more preferably 0≦α≦0.03. β preferably satisfies 0≦β≦0.1, and more preferably is 0.

[0023] Regarding the particle shape of the positive electrode active material used in this embodiment, the lithium nickel cobalt manganese composite oxide is a hollow particle, and the hollow particle has a shell, a hollow portion formed inside the shell, and a through hole penetrating the shell. The number of hollow portions is not particularly limited, and may be one, or may be two or more, and is preferably one. The number of through holes is not particularly limited, and may be one, or may be two or more.

[0024] Examples of hollow particles are shown in Fig. 3 and Fig. 4. Fig. 3 and Fig. 4 are schematic cross-sectional views of an example of a hollow particle of a positive electrode active material. In the example shown in Fig. 3, a hollow particle 10A has one hollow portion 14A, and in the hollow particle 10A, primary particles 12A made of a lithium nickel manganese cobalt composite oxide are connected in an annular shape to form a shell portion 16A. In the illustrated example, the primary particles 12A form a single layer, but a plurality of primary particles 12A may be stacked in the thickness direction of the shell portion 16A to form a multi-layer. The shell portion 16A surrounds the hollow portion 14A. A through hole 14Aa is formed in the shell portion 16A, and the opening width h of the through hole 14Aa has a dimension that allows the nonaqueous electrolyte 80 to penetrate.

[0025] In the example shown in Fig. 4, the primary particles 12B are loosely aggregated compared to normal, and therefore the hollow particle 10B has a plurality of relatively large hollow portions 14B. In Fig. 4, some of the primary particles 12B are present apart from each other, but this is because the figure is a cross-sectional view, and in reality, the primary particles 12B are in contact with other primary particles (not shown) in portions outside the figure. In the hollow particle 10B, the aggregated primary particles 12B form a shell portion 16B surrounding the hollow portion 14B. A through hole 14Ba is formed in the shell portion 16B, and the opening width h of the through hole 14Ba has a dimension that allows the nonaqueous electrolyte 80 to penetrate therein.

[0026] The BET specific surface area of ​​the lithium nickel cobalt manganese composite oxide is 3.0 m 2 / g or more. Such a high BET specific surface area can be achieved by forming the lithium nickel cobalt manganese composite oxide into hollow particles and increasing the internal surface area of ​​the particles. The BET specific surface area is preferably 3.1 m 2 / g or more. There is no particular upper limit to the BET specific surface area, and it is determined by technical limitations. The BET specific surface area is, for example, 4.0 m 2 / g or less, 3.8m 2 / g or less, 3.6m 2 / g or less, or 3.4m 2 The BET specific surface area is preferably 3.0 m 2 / g~3.6m 2 / g, more preferably 3.1m 2 / g~3.4m 2 / g. The BET specific surface area can be measured by a known method using nitrogen (N2) gas as an adsorbate. Specifically, for example, the BET specific surface area can be determined by performing a measurement based on the BET method using nitrogen (N2) gas and a commercially available specific surface area measuring device.

[0027] By combining such a lithium nickel cobalt manganese based composite oxide with a non-aqueous electrolyte solution 80 containing a carboxylate having 4 or less carbon atoms and lithium bis(oxalato)borate, the lithium ion secondary battery 100 has excellent output characteristics despite using a ternary active material with a low cobalt content. This is for the following reason. The specific contents of the non-aqueous electrolyte solution 80 will be described in detail later.

[0028] Lithium nickel cobalt manganese composite oxide is 3.0m 2 The hollow particle structure has a specific surface area increased to a range of 1 / g or more, which increases the surface area available for battery reactions. In particular, the viscosity of the nonaqueous electrolyte 80 is reduced by the carboxylic acid ester having 4 or less carbon atoms, and the hollow particles have through holes in their shells, which allows the nonaqueous electrolyte 80 to easily enter the hollows of the hollow particles, thereby allowing the battery reaction to occur efficiently even on the inner surfaces of the particles. This allows the lithium ion secondary battery 100 to have a low resistance during discharge (i.e., a high output).

[0029] However, since the carboxylate ester is easily decomposed, and the specific surface area of ​​the lithium nickel cobalt manganese composite oxide is very large, the decomposition reaction of the carboxylate ester occurs more easily. Therefore, the resistance reducing effect (output improving effect) by the carboxylate ester cannot be fully exhibited. Therefore, in this embodiment, the non-aqueous electrolyte 80 contains lithium bis(oxalato)borate (LiBOB) as a film forming agent. This LiBOB forms a coating not only on the negative electrode 60 but also on the surface of the positive electrode 50 (particularly the positive electrode active material), suppresses the oxidative decomposition of the carboxylate ester, and significantly exhibits the resistance reducing effect (i.e., the output improving effect). In this way, the special particle shape and BET specific surface area of ​​the lithium nickel cobalt manganese composite oxide, the carboxylate ester with 4 or less carbon atoms of the non-aqueous solvent, and the LiBOB as the film forming agent work together to significantly improve the output characteristics of the lithium ion secondary battery 100.

[0030] The porosity of hollow particles is not particularly limited, but is preferably 20% to 50%. The porosity of hollow particles can be determined as follows. A cross-sectional electron microscope image of a hollow particle is obtained, and the ratio of the total area of ​​the void parts to the area of ​​the entire particle (the sum of the area occupied by the particle and the total area of ​​the void parts) is calculated as a percentage. This value is calculated for 100 or more hollow particles, and the average value is taken as the porosity of the hollow particle.

[0031] The DBP oil absorption of the hollow particles is not particularly limited, but is preferably 35 mL / 100 g to 50 mL / 100 g. The DBP absorption can be measured using dibutyl phthalate (DBP) as a reagent liquid in accordance with the method described in JIS K6217-4:2008, and can be calculated as the average value of three measurement results.

[0032] The average particle size (median size: D50) of the lithium nickel cobalt manganese composite oxide is not particularly limited, but is, for example, 0.05 μm or more and 25 μm or less, preferably 1 μm or more and 20 μm or less, and more preferably 2 μm or more and 15 μm or less. The average particle size (D50) of the positive electrode active material can be determined, for example, by a laser diffraction scattering method.

[0033] Various methods for producing hollow particulate lithium nickel cobalt manganese based composite oxides are known, and the hollow particulate lithium nickel cobalt manganese based composite oxide used in this embodiment can be produced according to a known method.

[0034] The positive electrode active material may contain a positive electrode active material other than the lithium nickel manganese cobalt-based composite oxide within a range that does not impair the effects of the present invention (for example, less than 10 mass % relative to the total mass of the positive electrode active material, preferably 5 mass % or less). The positive electrode active material may be composed only of the lithium nickel manganese cobalt-based composite oxide.

[0035] The content of the positive electrode active material in the positive electrode active material layer 54 (i.e., the content of the positive electrode active material relative to the total mass of the positive electrode active material layer 54) is not particularly limited, but is, for example, 80 mass% or more, preferably 87 mass% or more, more preferably 90 mass% or more, even more preferably 95 mass% or more, and most preferably 97 mass% or more.

[0036] The positive electrode active material layer 54 may contain components (that is, optional components) other than the positive electrode active material. Examples of the optional components include a conductive material and a binder.

[0037] As the conductive material, for example, carbon materials such as carbon black (e.g., acetylene black), carbon nanotubes (CNT), graphite, etc. can be used, and among them, CNT is preferable. Since CNT has high conductivity, it can further improve the output characteristics of the lithium ion secondary battery 100. In addition, CNT has a hollow structure, and since a carboxylic acid ester having 4 or less carbon atoms can enter this hollow structure, the wettability between the positive electrode active material layer 54 and the nonaqueous electrolyte 80 is improved, and the output characteristics of the lithium ion secondary battery 100 can be further improved. When the positive electrode active material layer 54 contains CNT, the positive electrode active material layer 54 may further contain a dispersant for CNT (e.g., a surfactant-type dispersant, a polymer-type dispersant, an inorganic-type dispersant, etc.).

[0038] The content of the conductive material in the positive electrode active material layer 54 is not particularly limited, but is preferably from 0.1 mass % to 15 mass %, and more preferably from 0.5 mass % to 13 mass %.

[0039] The binder may be, for example, polyvinylidene fluoride (PVdF), etc. The content of the binder in the positive electrode active material layer 54 is not particularly limited, but is preferably from 1 mass % to 15 mass %, and more preferably from 1.5 mass % to 10 mass %.

[0040] The thickness of the positive electrode active material layer 54 is not particularly limited, but is, for example, from 10 μm to 300 μm, and preferably from 20 μm to 200 μm.

[0041] The weight of the positive electrode active material layer 54 is not particularly limited, but is preferably 4 mg / cm 2 More preferably, it is 8 mg / cm or more. 2 More preferably, it is 10 mg / cm or more. 2 More preferably, it is 20 mg / cm or more. 2 The weight per unit area of ​​the positive electrode active material layer 54 is 50 mg / cm 2 or less than 40 mg / cm 2 It may be the following:

[0042] The positive electrode sheet 50 may contain an insulating layer (not shown) at the boundary between the positive electrode active material layer non-forming portion 52a and the positive electrode active material layer 54. The insulating layer contains, for example, ceramic particles.

[0043] The negative electrode current collector 62 constituting the negative electrode sheet 60 may be a known negative electrode current collector used in lithium ion secondary batteries, and examples thereof include a sheet or foil made of a metal having good electrical conductivity (e.g., copper, nickel, titanium, stainless steel, etc.). Copper foil is preferable as the negative electrode current collector 62.

[0044] The dimensions of the negative electrode current collector 62 are not particularly limited and may be appropriately determined depending on the battery design. When a copper foil is used as the negative electrode current collector 62, the thickness is not particularly limited, but is, for example, 5 μm or more and 35 μm or less, and preferably 6 μm or more and 20 μm or less.

[0045] The negative electrode active material layer 64 contains a negative electrode active material. As the negative electrode active material, for example, a carbon material such as graphite, hard carbon, soft carbon, etc. The graphite may be natural graphite or artificial graphite, or may be amorphous carbon-coated graphite in which graphite is coated with an amorphous carbon material.

[0046] The average particle diameter (median diameter: D50) of the negative electrode active material is not particularly limited, but is, for example, 0.1 μm to 50 μm, preferably 1 μm to 25 μm, and more preferably 5 μm to 20 μm. The average particle diameter (D50) of the negative electrode active material can be determined, for example, by a laser diffraction scattering method.

[0047] The negative electrode active material layer 64 may contain components other than the active material, such as a binder, a thickener, etc. As the binder, for example, styrene butadiene rubber (SBR), polyvinylidene fluoride (PVdF), etc. may be used. As the thickener, for example, carboxymethyl cellulose (CMC), etc. may be used.

[0048] The content of the negative electrode active material in the negative electrode active material layer 64 is preferably 90% by mass or more, and more preferably 95% by mass or more and 99% by mass or less. The content of the binder in the negative electrode active material layer 64 is preferably 0.1% by mass or more and 8% by mass or less, and more preferably 0.5% by mass or more and 3% by mass or less. The content of the thickener in the negative electrode active material layer 64 is preferably 0.3% by mass or more and 3% by mass or less, and more preferably 0.5% by mass or more and 2% by mass or less.

[0049] The thickness of the negative electrode active material layer 64 is not particularly limited, but is, for example, not less than 10 μm and not more than 400 μm, and preferably not less than 20 μm and not more than 300 μm.

[0050] The separator 70 may be a porous sheet (film) made of a resin such as polyethylene (PE), polypropylene (PP), polyester, cellulose, or polyamide. Such a porous sheet may have a single-layer structure or a laminated structure of two or more layers (for example, a three-layer structure in which a PP layer is laminated on both sides of a PE layer). A heat-resistant layer (HRL) containing ceramic particles or the like may be provided on the surface of the separator 70.

[0051] The thickness of the separator 70 is not particularly limited, but is, for example, 5 μm to 50 μm, and preferably 10 μm to 30 μm. The air permeability of the separator 70 obtained by the Gurley test method is not particularly limited, but is preferably 350 sec / 100 cc or less.

[0052] In this embodiment, the non-aqueous electrolyte solution 80 contains a non-aqueous solvent, an electrolyte salt, and lithium bis(oxalato)borate. The non-aqueous solvent contains a carboxylic acid ester having 4 or less carbon atoms.

[0053] As described above, the carboxylate having 4 or less carbon atoms acts to reduce the viscosity of the nonaqueous electrolyte solution 80. Examples of the carboxylate having 4 or less carbon atoms include methyl acetate, ethyl acetate, and propyl acetate, and among these, methyl acetate is preferable.

[0054] If the content of the carboxylate in the non-aqueous solvent is too low, the output improvement effect may be small. Therefore, the volume ratio of the carboxylate in the non-aqueous solvent is preferably 1 volume % or more, more preferably 3 volume % or more, even more preferably 10 volume % or more, and particularly preferably 15 volume % or more. On the other hand, if the content of the carboxylate in the non-aqueous solvent is too high, the decomposition of the carboxylate may easily occur. Therefore, the volume ratio of the carboxylate in the non-aqueous solvent is 50 volume % or less, preferably 40 volume % or less, and more preferably 30 volume % or less.

[0055] The non-aqueous solvent includes an organic solvent other than the carboxylate ester. Examples of the organic solvent include carbonates, ethers, nitriles, sulfones, lactones, etc., and among them, carbonates are preferred. Examples of carbonates include ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), monofluoroethylene carbonate (MFEC), difluoroethylene carbonate (DFEC), monofluoromethyl difluoromethyl carbonate (F-DMC), trifluorodimethyl carbonate (TFDMC), etc. Such organic solvents can be used alone or in appropriate combination of two or more. The non-aqueous solvent may contain only carbonates and carboxylate esters.

[0056] The non-aqueous electrolyte solution 80 may contain an electrolyte salt (in other words, a supporting salt). As the electrolyte salt, for example, a lithium salt such as LiPF6, LiBF4, or lithium bis(fluorosulfonyl)imide (LiFSI) (preferably LiPF6) can be suitably used. The concentration of the electrolyte salt in the non-aqueous electrolyte solution 80 is preferably 0.7 mol / L or more and 1.3 mol / L or less.

[0057] The nonaqueous electrolyte 80 contains lithium bis(oxalato)borate (LiBOB). As described above, LiBOB forms a coating on the surface of the positive electrode active material, thereby suppressing the decomposition of the carboxylate, which contributes to lowering the resistance (i.e., improving the output) of the lithium ion secondary battery 100. If the concentration of LiBOB in the nonaqueous electrolyte 80 is too low, the output improvement effect may be reduced. Therefore, the concentration of LiBOB in the nonaqueous electrolyte 80 is preferably 0.15 mass% or more, more preferably 0.20 mass% or more, and even more preferably 0.30 mass% or more. On the other hand, if the concentration of LiBOB in the nonaqueous electrolyte 80 is too high, an excessive coating is formed, and the output improvement effect is reduced. Therefore, the concentration of LiBOB in the nonaqueous electrolyte 80 is preferably 0.80 mass% or less, more preferably 0.70 mass% or less, and even more preferably 0.60 mass% or less.

[0058] In addition, the nonaqueous electrolyte 80 may contain various additives, such as components other than the above-mentioned components, for example, gas generating agents such as biphenyl (BP) and cyclohexylbenzene (CHB), thickeners, etc., as long as the effects of the present invention are not significantly impaired.

[0059] The lithium ion secondary battery 100 has excellent output characteristics even though it uses a ternary active material with a low cobalt content. Since the lithium ion secondary battery 100 uses a ternary active material with a low cobalt content, it can significantly alleviate the problem of cobalt resource depletion associated with decarbonization.

[0060] The lithium ion secondary battery 100 can be used for various applications. Suitable applications include a driving power source mounted on vehicles such as electric vehicles (BEVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs). The lithium ion secondary battery 100 can also be used as a storage battery for small power storage devices and the like. Since the lithium ion secondary battery 100 has excellent output characteristics, a particularly suitable application of the lithium ion secondary battery 100 is as a driving power source mounted on vehicles such as electric vehicles (BEVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs) (particularly, a driving power source for HEVs). The lithium ion secondary battery 100 can also be used in the form of a battery pack in which a plurality of lithium ion secondary batteries 100 are typically connected in series and / or in parallel.

[0061] The above describes, as an example, a rectangular lithium ion secondary battery 100 equipped with a flat wound electrode assembly 20. However, the lithium ion secondary battery can also be configured as a lithium ion secondary battery equipped with a laminated electrode assembly (i.e., an electrode assembly in which multiple positive electrodes and multiple negative electrodes are alternately laminated). The lithium ion secondary battery can also be configured as a cylindrical lithium ion secondary battery, a laminated case type lithium ion secondary battery, etc.

[0062] The secondary battery according to this embodiment can be constructed as a non-aqueous electrolyte secondary battery other than a lithium ion secondary battery in accordance with a known method.

[0063] Examples of the present invention will be described in detail below, but it is not intended that the present invention be limited to those shown in these examples.

[0064] [Examples 1 to 12 and Comparative Examples 1 to 6] The positive electrode active material is LiNi with the BET specific surface area shown in Table 1. 0.5 Co 0.2 Mn 0.3O2 was prepared. The BET specific surface area was determined using a commercially available specific surface area measuring device with nitrogen (N2) gas as an adsorbate. The positive electrode active material of each example and each comparative example was a hollow particle having a shell portion, a hollow portion formed inside the shell portion, and a through hole penetrating the shell portion.

[0065] The positive electrode active material, a carbon nanotube (CNT) dispersion as a conductive material, and PVdF as a binder were kneaded in N-methyl-2-pyrrolidone at a solid mass ratio of active material:CNT:PVdF=97.5:1.5:1.0 to prepare a positive electrode slurry. The positive electrode slurry was applied onto an aluminum foil as a positive electrode current collector and dried to obtain a positive electrode sheet.

[0066] A negative electrode slurry was prepared by mixing natural graphite (C) as a negative electrode active material, styrene butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener in a mass ratio of C:SBR:CMC=98:1:1 in pure water. This negative electrode slurry was applied onto copper foil and dried to obtain a negative electrode sheet.

[0067] A porous polyolefin sheet was prepared as a separator. The positive electrode sheet and the negative electrode sheet were stacked together with the separator sandwiched between them to prepare an electrode assembly. In this electrode assembly, the electrode facing area was approximately 20 cm2. 2 It was.

[0068] A mixed solvent containing ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and a carboxylic acid ester shown in Table 1 in a volume ratio (volume %) of 30:30-x:40:x was prepared. The value of x was set to the value shown in Table 1. In this mixed solvent, LiPF6 as a supporting salt was dissolved at a concentration of 1.1 mol / L, and lithium bis(oxalate)borate was also dissolved at the concentration shown in Table 1. In this way, a nonaqueous electrolyte was obtained.

[0069] Terminals were attached to the electrode body, and the electrode body was housed in a laminate case together with a non-aqueous electrolyte. The laminate case was then sealed to obtain a lithium-ion secondary battery for evaluation with a capacity of about 20 mAh. The lithium-ion secondary battery for evaluation was initially charged at a current value of 1 / 3 C, and then activated by aging at 60°C for 24 hours.

[0070] <Output evaluation - Output resistance measurement> Each activated evaluation lithium ion secondary battery was adjusted to SOC (State of charge) 50% in a thermostatic bath at 25°C. Next, each evaluation lithium ion secondary battery was discharged at a current value of 5C to 45C for 10 seconds in a thermostatic bath at 25°C, and the battery voltage after discharging at each current value was measured. Each current value and each battery voltage were plotted to obtain IV characteristics during discharge, and the IV resistance (Ω) during discharge was obtained as output resistance from the slope of the obtained straight line. When the output resistance of the evaluation lithium ion secondary battery of Comparative Example 1 was set to "1.00", the ratio of the output resistance of the other evaluation lithium ion secondary batteries to the evaluation lithium ion secondary battery of Comparative Example 1 was obtained. The results are shown in Table 1.

[0071] [Table 1]

[0072] As shown in the results in Table 1, in the lithium nickel cobalt manganese based composite oxide, the molar ratio of Ni to all metal elements other than Li is 40 mol % to 60 mol %, and the molar ratio of Co is 15 mol % to 25 mol %, the lithium nickel cobalt manganese based composite oxide is in the form of hollow particles having a shell portion, a hollow portion, and through holes penetrating the shell portion, and the BET specific surface area of ​​the lithium nickel cobalt manganese based composite oxide is 3.0 m 2 / g or more, and the output resistance is significantly small when the nonaqueous electrolyte contains a carboxylate having 4 or less carbon atoms and lithium bis(oxalato)borate. Therefore, the nonaqueous electrolyte secondary battery disclosed herein has excellent output characteristics even when using a ternary active material with a low cobalt content.

[0073] Although the specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above.

[0074] That is, the nonaqueous electrolyte secondary battery disclosed herein has the following features [1] to [7]. [1] A positive electrode, A negative electrode; A non-aqueous electrolyte; A non-aqueous electrolyte secondary battery comprising: The positive electrode has a positive electrode active material layer containing a positive electrode active material, The positive electrode active material is a lithium nickel cobalt manganese based composite oxide, In the lithium nickel cobalt manganese based composite oxide, the molar ratio of Ni to all metal elements other than Li is 40 mol% to 60 mol%, and the molar ratio of Co is 15 mol% to 25 mol%, The lithium nickel cobalt manganese based composite oxide is in the form of hollow particles having a shell portion, a hollow portion formed inside the shell portion, and a through hole penetrating the shell portion, The BET specific surface area of ​​the lithium nickel cobalt manganese composite oxide is 3.0 m 2 / g or more, the non-aqueous electrolyte solution contains a non-aqueous solvent, an electrolyte salt, and lithium bis(oxalato)borate; The non-aqueous solvent contains a carboxylic acid ester having 4 or less carbon atoms. Nonaqueous electrolyte secondary battery. [2] The nonaqueous electrolyte secondary battery according to item [1], wherein the concentration of lithium bis(oxalato)borate in the nonaqueous electrolyte is 0.20% by mass to 0.80% by mass. [3] The nonaqueous electrolyte secondary battery according to item [1] or [2], wherein a volume ratio of the carboxylic acid ester in the nonaqueous solvent is 1 volume % to 50 volume %. [4] The nonaqueous electrolyte secondary battery according to item [1] or [2], wherein a volume ratio of the carboxylic acid ester in the nonaqueous solvent is 15 volume % to 30 volume %. [5] The nonaqueous electrolyte secondary battery according to any one of items [1] to [4], wherein the carboxylate ester is methyl acetate. [6] The BET specific surface area of ​​the lithium nickel cobalt manganese composite oxide is 3.0 m 2 / g~3.6m 2 / g. [7] The nonaqueous electrolyte secondary battery according to any one of items [1] to [6], which is used as a power source for driving a vehicle. [Explanation of symbols]

[0075] 10A,10B hollow particles 12A,12B Primary particles 14A,14B Hollow part 14Aa,14Ba through hole 16A,16B shell part 20 Wound electrode body 30 Battery case 36 Safety valve 42 Positive terminal 42a Positive current collector 44 Negative terminal 44a Negative current collector plate 50 Positive electrode sheet (positive electrode) 52 Positive electrode current collector 52a Portion where positive electrode active material layer is not formed 54 Cathode active material layer 60 Negative electrode sheet (negative electrode) 62 Negative electrode current collector 62a Part where negative electrode active material layer is not formed 64 Negative electrode active material layer 70 Separator sheet (separator) 80 Nonaqueous electrolyte 100 Lithium-ion secondary battery

Claims

1. A positive electrode and A negative electrode; A non-aqueous electrolyte; A non-aqueous electrolyte secondary battery comprising: The positive electrode has a positive electrode active material layer containing a positive electrode active material, The positive electrode active material is a lithium nickel cobalt manganese based composite oxide, In the lithium nickel cobalt manganese based composite oxide, the molar ratio of Ni to all metal elements other than Li is 40 mol% to 60 mol%, and the molar ratio of Co is 15 mol% to 25 mol%, The lithium nickel cobalt manganese based composite oxide is in the form of hollow particles having a shell portion, a hollow portion formed inside the shell portion, and a through hole penetrating the shell portion, The BET specific surface area of ​​the lithium nickel cobalt manganese composite oxide is 3.0 m 2 / g or more, the non-aqueous electrolyte solution contains a non-aqueous solvent, an electrolyte salt, and lithium bis(oxalato)borate; The non-aqueous solvent contains a carboxylic acid ester having 4 or less carbon atoms. Nonaqueous electrolyte secondary battery.

2. 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the concentration of lithium bis(oxalato)borate in the nonaqueous electrolyte is 0.20% by mass to 0.80% by mass.

3. 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein a volume ratio of the carboxylic acid ester in the nonaqueous solvent is 1 volume % to 50 volume %.

4. 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein a volume ratio of the carboxylic acid ester in the nonaqueous solvent is 15% by volume to 30% by volume.

5. 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the carboxylic acid ester is methyl acetate.

6. The BET specific surface area of ​​the lithium nickel cobalt manganese composite oxide is 3.0 m 2 / g to 3.6 m 2 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the capacitance is 1 / g.

7. 2. The nonaqueous electrolyte secondary battery according to claim 1, which is used as a power source for driving a vehicle.

Citation Information

Patent Citations

  • Lithium composite metal oxide and method for producing the same

    JP2012079688A

  • Lithium complex metal oxide and nonaqueous electrolytic secondary battery

    JP2012109191A

  • Electrolyte solution for rechargeable batteries

    JP2017528885A

  • Nickel, manganese, cobalt-containing composite hydroxide and manufacturing method thereof, positive electrode active material for lithium ion secondary battery and manufacturing method thereof, and lithium ion secondary battery

    JP2020119784A

  • Nickel, manganese, cobalt-containing composite hydroxide and manufacturing method thereof, positive electrode active material for lithium ion secondary battery and manufacturing method thereof, and lithium ion secondary battery

    JP2020119785A