Alkali-free glass and glass plate

The specified alkali-free glass composition addresses dielectric loss and chemical resistance issues, enabling effective transmission of high-frequency signals by maintaining surface integrity and reducing conductor loss.

JP2024138014AActive Publication Date: 2024-10-07AGC INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024114255
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-11-27
Filing Date
2024-07-17
Publication Date
2024-10-07
Estimated Expiration
2040-04-07

AI Technical Summary

Technical Problem

Conventional alkali-free glass substrates face limitations in reducing dielectric loss beyond 30 GHz and have poor chemical resistance, leading to surface melting and conductor loss during acid cleaning, which affects the quality and strength of high-frequency signals.

Method used

A specific composition of alkali-free glass with SiO2 57-70%, Al2O3 5-15%, B2O3 15-24%, and controlled ratios of [Al2O3]/[B2O3] and [MgO]+[CaO]+[SrO]+[BaO] within certain ranges, along with minimal alkali metal oxides, to achieve low dielectric loss and acid resistance.

Benefits of technology

The glass exhibits a dielectric loss tangent of 0.006 or less at 35 GHz, maintains surface smoothness during acid cleaning, and reduces conductor loss, ensuring high-frequency signal quality and strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138014000013
    Figure 2024138014000013
  • Figure 2024138014000001
    Figure 2024138014000001
  • Figure 2024138014000002
    Figure 2024138014000002
Patent Text Reader

Abstract

To provide an alkali-free glass which combines a low dielectric dissipation factor in the high-frequency range with acid resistance.SOLUTION: An alkali-free glass includes, as represented by mole percentage based on oxides, SiO2 of 57-70%, Al2O3 of 5-15%, B2O3 of 15-24%, MgO of 0.2-10%, CaO of 0.1-7%, SrO of 0.1-2.5%, BaO of 0-10%, and ZnO of 0-0.1%. The value of formula (A) represented by [Al2O3] / [B2O3] is more than 0.35 and 1.4 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an alkali-free glass. It also relates to a glass plate, a glass substrate for a high-frequency device, a panel-type antenna, a window glass, a window glass for a vehicle, and a cover glass for a touch panel, each of which contains the alkali-free glass. [Background technology]

[0002] Electronic devices include communication devices such as mobile phones, smartphones, personal digital assistants, and Wi-Fi devices, as well as surface acoustic wave (SAW) devices, radar components, and antenna components. In these electronic devices, signal frequencies are becoming higher in order to increase communication capacity and speed. Insulating substrates such as resin substrates, ceramic substrates, and glass substrates are generally used for circuit boards used in electronic devices for high-frequency applications. Insulating substrates used in high-frequency devices are required to reduce transmission losses due to dielectric loss, conductor loss, and the like in order to ensure characteristics such as the quality and strength of high-frequency signals.

[0003] Of these insulating substrates, resin substrates have low rigidity due to their characteristics. Therefore, resin substrates are difficult to use when rigidity (strength) is required for semiconductor package products. Ceramic substrates have the drawback that it is difficult to improve the smoothness of their surface, which tends to increase conductor loss due to the conductor formed on the substrate surface. On the other hand, glass substrates have the characteristics of being highly rigid, making it easy to make packages smaller and thinner, having excellent surface smoothness, and being easy to enlarge as a substrate itself.

[0004] However, while conventional alkali-free glass substrates are effective in reducing dielectric loss and the transmission loss resulting therefrom up to about 20 GHz, there is a limit to the reduction of dielectric loss beyond that, for example, in the region exceeding 30 GHz. Therefore, in circuit boards using conventional alkali-free glass substrates, it becomes difficult to maintain characteristics such as the quality and strength of high-frequency signals exceeding 30 GHz. On the other hand, while quartz glass substrates can maintain low dielectric loss even in the region exceeding 30 GHz, their thermal expansion coefficient is too small, so that the difference in thermal expansion coefficient between them and other components becomes too large when constructing electronic devices. This is a factor that reduces the practicality of electronic devices.

[0005] Patent Document 1 discloses a glass substrate for a high frequency device having a dielectric loss tangent of 0.0007 or less at 35 GHz. It is said that the glass substrate for a high frequency device described in Patent Document 1 can have a dielectric loss tangent of 0.0007 or less by satisfying predetermined conditions for the amounts and ratios of Al2O3 and B2O3. Therefore, it is believed that in order to reduce dielectric loss in the high frequency range exceeding 30 GHz, the B2O3 content should be increased. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2018 / 051793 Summary of the Invention [Problem to be solved by the invention]

[0007] However, increasing the B2O3 content reduces the chemical resistance of the glass. In the manufacturing process of circuit boards for liquid crystal antennas, high-frequency devices, etc., chemical cleaning is performed as a pretreatment for forming a wiring layer on a glass substrate. If the chemical resistance of the glass is low, for example, during acid cleaning, the substrate surface may dissolve and the smoothness of the substrate surface may be impaired, which may reduce the adhesion of the film formed on the substrate surface. There is also a risk that eluted material may adhere to the substrate surface. This may increase the conductor loss caused by the conductor formed on the substrate surface.

[0008] An object of the present invention is to provide an alkali-free glass which has both a low dielectric tangent in the high frequency range and acid resistance. [Means for solving the problem]

[0009] As a result of intensive research, the present inventors have found that the above object can be achieved by adopting the following configuration. [1] An alkali-free glass containing, in mole percentages based on oxides, 57-70% SiO2, 5-15% Al2O3, 15-24% B2O3, 0.2-10% MgO, 0.1-7% CaO, 0.1-2.5% SrO, 0-10% BaO, and 0-0.1% ZnO, in which the formula (A) is [Al2O3] / [B2O3], and the value of said formula (A) is greater than 0.35 and less than or equal to 1.4. [2] An alkali-free glass containing, in mole percentages based on oxides, 57-70% SiO2, 5-15% Al2O3, 15-24% B2O3, 0.1-10% MgO, 0.1-10% CaO, 0.1-10% SrO, 0.1-10% BaO, and 0-0.1% ZnO, wherein the formula (A) is [Al2O3] / [B2O3], and the value of said formula (A) is greater than 0.35 and less than or equal to 1.4. [3] The alkali-free glass according to [1] or [2], wherein formula (B) is [MgO] + [CaO] + [SrO] + [BaO], and the value of formula (B) is 7% or more and 16% or less. [4] The alkali-free glass according to any one of the above [1] to [3], wherein the value of the formula (B) is 8% or more and 16% or less. [5] The alkali-free glass according to any one of the items [1] to [4], wherein formula (C) is [Al2O3]-([MgO]+[CaO]+[SrO]+[BaO]), and the value of formula (C) is greater than -3% and less than 2%. [6] The alkali-free glass according to any one of the above [1] to [5], wherein the value of the above formula (A) is 0.49 or more. [7] The alkali-free glass according to any one of the items [1] to [5], wherein formula (D) is [SrO] / ([MgO]+[CaO]+[SrO]+[BaO]), and the value of formula (D) is 0.64 or more. [8] The alkali-free glass according to any one of [1] to [7] above, containing 1 mol % or less of Fe calculated as Fe2O3. [9] The β-OH value of glass is 0.05 mm. -1 Above 1.0mm -1 The alkali-free glass according to any one of the above [1] to [8], which is:

[10] The alkali-free glass according to any one of the above [1] to [9], wherein the total content represented by [Li2O] + [Na2O] + [K2O] is 0 to 0.2 mol %.

[11] The alkali-free glass according to any one of the above [1] to

[10] , containing 1 mol % or less in total of at least one selected from the group consisting of SnO2, Cl and SO3.

[12] The alkali-free glass according to any one of [1] to

[11] above, containing 1 mol % or less in total of at least one selected from the group consisting of Sc2O3, TiO2, ZnO2, Ga2O3, GeO2, Y2O3, ZrO2, Nb2O5, In2O3, TeO2, HfO2, Ta2O5, WO3, Bi2O3, La2O3, Gd2O3, Yb2O3, and Lu2O3.

[13] The alkali-free glass according to any one of the above [1] to

[12] , which contains 1 mol % or less of F.

[14] The alkali-free glass according to any one of the above [1] to

[13] , which has a dielectric tangent at 35 GHz of 0.006 or less.

[15] The alkali-free glass according to any one of the above [1] to

[14] , which has a resistivity of 400 Ω·cm or less at 1500° C.

[16] The alkali-free glass according to any one of the above [1] to

[15] , which has a resistivity of 300 Ω·cm or less at 1500° C.

[17] The alkali-free glass according to any one of the above [1] to

[16] , having a Young's modulus of 58 GPa or more.

[18] Density is 2.58 g / cm 3 The average thermal expansion coefficient at 50 to 350°C is 30×10 -7 / ℃~40×10 -7 The alkali-free glass according to any one of the above [1] to

[17] , wherein the temperature is 0.1 to 1.5° C.

[19] Glass viscosity is 10 2 The temperature T2 at which the glass viscosity becomes dPa·s is 1500 to 1700°C, and the glass viscosity is 10 4 The alkali-free glass according to any one of the above [1] to

[18] , having a temperature T4 at which the glass has a viscosity of dPa·s of 1290° C. or lower.

[20] The alkali-free glass according to any one of the above [1] to

[19] , which has a glass transition temperature of 700° C. or lower or a strain point of 700° C. or lower.

[21] The alkali-free glass according to any one of the above [1] to

[20] , having a surface devitrification temperature of 1,300° C. or lower.

[22] When immersed in an aqueous solution containing 6% by weight of HNO3 and 5% by weight of H2SO4 at 45°C for 170 seconds, the amount of glass components dissolved per unit surface area was 0.025 mg / cm 2 The alkali-free glass according to any one of the above [1] to

[21] , which is:

[23] A glass plate comprising the alkali-free glass according to any one of [1] to

[22] above, the glass plate having main surfaces and end faces, wherein at least one of the main surfaces has an arithmetic mean roughness Ra of 1.5 nm or less.

[24] The glass plate according to

[23] above, having at least one side measuring 900 mm or more and a thickness of 0.7 mm or less.

[25] The glass plate according to

[22] or

[23] above, which is produced by a float process or a fusion process.

[26] A glass substrate for a high-frequency device, comprising the alkali-free glass according to any one of [1] to

[22] above.

[27] A panel-type antenna comprising the alkali-free glass according to any one of [1] to

[22] above.

[28] A window glass comprising the alkali-free glass according to any one of the above [1] to

[22] .

[29] A window glass for a vehicle comprising the alkali-free glass according to any one of the above [1] to

[22] .

[30] A cover glass for a touch panel, comprising the alkali-free glass according to any one of [1] to

[22] above. Effect of the Invention

[0010] The alkali-free glass of the present invention can reduce the dielectric loss of high-frequency signals. Therefore, it is suitable for use as a glass substrate for high-frequency devices. Circuit boards using such glass substrates can reduce the transmission loss of high-frequency signals, and can provide practical high-frequency devices such as electronic devices. The alkali-free glass of the present invention has excellent acid resistance. Therefore, when a glass substrate is acid-washed in the manufacturing process of a circuit substrate for a liquid crystal antenna, a high-frequency device, or the like, there is no risk of the substrate surface being dissolved, the smoothness of the substrate surface being deteriorated, or eluted material being attached to the substrate surface. Therefore, it is possible to prevent the adhesion of a film formed on the substrate surface from being reduced. In addition, it is possible to prevent the conductor loss from being increased. The alkali-free glass of the present invention can reduce transmission loss of radio waves in the high frequency band and is less susceptible to damage and destruction, and is therefore suitable for glass products that transmit and receive radio waves in the high frequency band. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the configuration of a circuit board for a high-frequency device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described. In the following description, a numerical range indicated using "to" indicates a range including the numerical values ​​before and after "to" as the minimum and maximum values, respectively. The content of each component in the alkali-free glass or glass sheet indicates a mole percentage (mol%) based on the oxide, unless otherwise specified. In addition, the description of [metal oxide] in formulas (A) to (D), such as [MgO], indicates the mole % of a metal oxide component, such as magnesium oxide. In this specification, the term "high frequency" refers to 10 GHz or higher, preferably higher than 30 GHz, and more preferably 35 GHz or higher.

[0013] The alkali-free glass according to this embodiment (hereinafter, sometimes simply referred to as "glass") will be described below.

[0014] If the content of SiO2 as a network former is 57 mol% (hereinafter simply referred to as %) or more, the glass forming ability and weather resistance can be improved, and devitrification can be suppressed. The content of SiO2 is preferably 58% or more, more preferably 60% or more, and even more preferably 61% or more. Also, if the content of SiO2 is 70% or less, the melting property of the glass can be improved. The content of SiO2 is preferably 68% or less, more preferably 66% or less, even more preferably 65% ​​or less, particularly preferably 64% or less, and most preferably 63% or less.

[0015] Al2O3 is a component that is effective in improving weather resistance, improving Young's modulus, suppressing phase separation of glass, and decreasing the thermal expansion coefficient. If the content of Al2O3 is 5% or more, the effect of including Al2O3 can be sufficiently obtained. The content of Al2O3 is preferably 6% or more, more preferably 7% or more, and even more preferably 8% or more. Also, if the content of Al2O3 is 15% or less, the melting property of glass is good. The content of Al2O3 is preferably 14% or less, more preferably 13% or less, and even more preferably 12% or less.

[0016] If the B2O3 content is 24% or less, the chemical resistance can be improved. The B2O3 content is preferably 23% or less, more preferably 22% or less, even more preferably 21% or less, still more preferably 20% or less, particularly preferably 19% or less, and most preferably 18% or less. If the B2O3 content is 15% or more, the solubility is improved. Also, the dielectric tangent in the high frequency range can be reduced. The B2O3 content is preferably 16% or more, more preferably 17% or more, and even more preferably 17.5% or more.

[0017] MgO is a component that increases the Young's modulus without increasing the specific gravity. In other words, MgO is a component that increases the specific elastic modulus, which can reduce the problem of deflection and improve the fracture toughness value to increase the glass strength. MgO is also a component that improves solubility. If the content of MgO is 0.1% or more, the effect of containing MgO can be obtained and the thermal expansion coefficient can be prevented from becoming too low. The content of MgO is preferably 0.2% or more, more preferably 1% or more, and even more preferably 2% or more. If the content of MgO is 10% or less, the increase in the devitrification temperature can be suppressed. The content of MgO is preferably 9% or less, more preferably 8% or less, even more preferably 7% or less, even more preferably 6% or less, especially preferably 5% or less, particularly preferably 4% or less, and most preferably 3% or less.

[0018] CaO is the component that increases the specific elastic modulus next to MgO among alkaline earth metals and does not excessively lower the strain point, and improves solubility like MgO. Furthermore, it is a component that is less likely to increase the devitrification temperature than MgO. If the CaO content is 0.1% or more, the effect of containing CaO can be fully obtained. The CaO content is preferably 0.2% or more, more preferably 0.5% or more, even more preferably 1% or more, and particularly preferably 2% or more. Also, if the CaO content is 10% or less, the average thermal expansion coefficient does not become too high, and the increase in the devitrification temperature is suppressed to prevent devitrification during glass production. The CaO content is preferably 8% or less, more preferably 7% or less, even more preferably 6% or less, even more preferably 5% or less, especially preferably 4% or less, and particularly preferably 3% or less.

[0019] SrO is a component that does not increase the devitrification temperature of glass and improves the melting point. If the content of SrO is 0.1% or more, the effect of including SrO can be sufficiently obtained. The content of SrO is preferably 0.2% or more, more preferably 0.5% or more, even more preferably 1% or more, and particularly preferably 2% or more. If the content of SrO is 10% or less, the specific gravity is not too high, and the average thermal expansion coefficient is prevented from becoming too high. The content of SrO is preferably 9% or less, more preferably 8% or less, even more preferably 7% or less, even more preferably 6% or less, especially preferably 5% or less, even more preferably 4% or less, particularly preferably 3% or less, and most preferably 2.5% or less.

[0020] BaO is not an essential component, but it is a component that does not increase the devitrification temperature of glass and improves the solubility. When BaO is contained, its content of 0.1% or more is preferable because the above-mentioned effect of containing BaO can be sufficiently obtained. The content of BaO is more preferably 0.2% or more, even more preferably 1% or more, and particularly preferably 2% or more. However, if BaO is contained in a large amount, the specific gravity increases, the Young's modulus decreases, the relative dielectric constant increases, and the average thermal expansion coefficient tends to become too large. Therefore, the content of BaO is preferably 10% or less, more preferably 8% or less, even more preferably 5% or less, and even more preferably 3% or less.

[0021] ZnO is not an essential component, but it is a component that improves chemical resistance. However, if a large amount of ZnO is contained, phase separation is likely to occur and the devitrification temperature may become high. Therefore, the content of ZnO is 0.1% or less. The content of ZnO is preferably 0.05% or less, more preferably 0.03% or less, even more preferably 0.01% or less, and particularly preferably substantially not contained. In the present invention, substantially not containing ZnO means, for example, less than 0.01%.

[0022] In the alkali-free glass according to the present embodiment, when formula (A) is the ratio of the content represented by [Al2O3] / [B2O3], the value of formula (A) is more than 0.35 and 1.4 or less. If the value represented by formula (A) is within the above range, the dielectric loss in a high frequency region exceeding 30 GHz can be reduced, and the acid resistance of the glass is improved. In addition, phase separation is suppressed, resulting in a glass with excellent uniformity. If the value represented by formula (A) is 0.35 or less, the acid resistance of the glass deteriorates. In addition, it becomes difficult to obtain a glass with excellent uniformity due to phase separation. If the value represented by formula (A) is more than 1.4, the dielectric loss in a high frequency region exceeding 30 GHz cannot be reduced. The value represented by formula (A) is preferably 1.2 or less, more preferably 1.0 or less, and even more preferably 0.8 or less. The value represented by formula (A) is preferably 0.40 or more, more preferably 0.45 or more, and even more preferably 0.49 or more. Moreover, when the value represented by formula (A) is 0.49 or more, the Young's modulus is improved, for example, the Young's modulus is 64 GPa or more, which is more preferable. The value represented by formula (A) is more preferably 0.52 or more, even more preferably 0.56 or more, particularly preferably 0.59 or more, and most preferably 0.61 or more.

[0023] In the alkali-free glass according to the present embodiment, when formula (B) is the total content represented by [MgO]+[CaO]+[SrO]+[BaO], the value represented by formula (B) is preferably 7% or more and 16% or less. If the value represented by formula (B) is within the above range, the resistance value in the melting temperature range, for example, the resistance value at 1500°C, is low, and the acid resistance of the glass is improved. The alkali-free glass according to the present embodiment, which has a low resistance value in the melting temperature range, can improve the productivity and quality of the alkali-free glass by applying electric melting when melting the glass raw materials. Specifically, when the value represented by formula (B) is 7% or more, the resistance value in the melting temperature range can be reduced. When the value represented by formula (B) is 16% or less, the acid resistance of the glass can be improved. In addition, the dielectric loss in the high frequency range exceeding 30 GHz can be suitably reduced. The value represented by formula (B) is more preferably 14% or less, even more preferably 13% or less, even more preferably 12% or less, particularly preferably 11% or less, and most preferably 10.5% or less. The value represented by formula (B) is more preferably 8% or more, further preferably 8.5% or more, and even further preferably 9% or more.

[0024] In the alkali-free glass according to this embodiment, when the content of formula (C) is represented by [Al2O3]-([MgO]+[CaO]+[SrO]+[BaO]), the value represented by formula (C) is preferably more than -3% and less than 2%. If the value represented by formula (C) is within the above range, devitrification of the glass can be suppressed and the acid resistance of the glass can be improved. Specifically, if the value represented by formula (C) is more than -3%, the acid resistance of the glass can be improved. If the value represented by formula (C) is less than 2%, the glass is less likely to devitrify. The value represented by formula (C) is more preferably 1.5% or less, even more preferably 1.0% or less, and particularly preferably 0.5% or less. The value represented by formula (C) is more preferably -2% or more, even more preferably -1% or more, and particularly preferably -0.5% or more.

[0025] In the alkali-free glass according to this embodiment, when formula (D) is the ratio of contents represented by [SrO] / ([MgO]+[CaO]+[SrO]+[BaO]), the value of formula (D) is preferably 0.64 or more. If the value represented by formula (D) is within the above range, the surface devitrification temperature is lowered, for example, the surface devitrification temperature is 1219°C or less, and the productivity of the glass is improved. The value of formula (D) is more preferably 0.7 or more, further preferably 0.75 or more, and particularly preferably 0.8 or more. In addition, the upper limit is not particularly limited, but for example, 0.95 or less is preferable.

[0026] The alkali-free glass according to this embodiment may contain Fe in order to reduce the resistance in the melting temperature range, for example, the resistance at 1500° C. However, from the viewpoint of suppressing a decrease in the transmittance in the visible range, the Fe content is preferably 1 mol % or less, more preferably 0.5 mol % or less, and even more preferably 0.1 mol % or less, calculated as Fe2O3.

[0027] The alkali-free glass according to this embodiment has a β-OH value (mm -1 ) is 0.05 mm -1 Above 1.0mm -1 The following is preferred: The β-OH value is an index of the water content in glass. The absorbance of a glass sample is measured for light with wavelengths of 2.75 to 2.95 μm, and the maximum absorbance value β max The β-OH value is calculated by dividing the resistance value by the thickness (mm) of the sample. If the β-OH value is within the above range, the resistance value in the temperature range for melting the glass raw material, for example, in the vicinity of 1500°C, is low, which is suitable for melting the glass by electrical heating, and there are few bubble defects in the glass. Specifically, if the β-OH value is 0.05 mm -1 If the β-OH value is 1.0 mm or more, the resistance value in the temperature range where the glass raw material is melted is low. Also, the dielectric tangent in the high frequency range can be suitably reduced. -1 If the value is less than 0.8mm, bubble defects in the glass can be suppressed. -1 Less than 0.6mm is more preferable. -1 Less than 0.5 mm is more preferable. -1 The following is particularly preferred: β-OH value is 0.1 mm -1More preferably, 0.2 mm or more -1 More preferably, 0.3 mm or more -1 The above is particularly preferred.

[0028] The alkali-free glass according to this embodiment preferably does not substantially contain alkali metal oxides such as Li2O, Na2O, and K2O. In this embodiment, "substantially does not contain alkali metal oxides" means that the glass does not contain any other than unavoidable impurities mixed in from raw materials, that is, the glass is not intentionally contained. However, a predetermined amount of alkali metal oxide may be contained in order to obtain a specific effect, i.e., to obtain an effect such as lowering the strain point, lowering the Tg, lowering the annealing point, or lowering the resistance value in the temperature range where the glass raw material is melted. Specifically, at least one selected from the group consisting of Li2O, Na2O, and K2O may be contained in a total content of 0.2% or less expressed as [Li2O] + [Na2O] + [K2O]. More preferably, it is 0.15% or less, even more preferably, it is 0.1% or less, even more preferably, it is 0.08% or less, even more preferably, it is 0.05% or less, and most preferably, it is 0.03% or less. At least one selected from the group consisting of Li2O, Na2O, and K2O may be contained in a total content of 0.001% or more expressed as mole % on an oxide basis. More preferably, it is 0.003% or more, even more preferably, it is 0.005% or more, even more preferably, it is 0.008% or more, even more preferably, it is 0.01% or less, and most preferably, it is 0.02% or more. In this specification, the total content expressed as [Li2O] + [Na2O] + [K2O] may be expressed as R2O. R indicates an alkali metal.

[0029] In order to improve the clarity of the glass, the alkali-free glass according to this embodiment may contain at least one selected from the group consisting of SnO2, Cl, and SO3, preferably in a total content of 1 mol% or less, more preferably 0.5 mol% or less, and even more preferably 0.3 mol% or less. The lower limit is 0% (not contained). In the alkali-free glass according to this embodiment, from the viewpoint of reducing bubble defects in the glass and reducing the dielectric tangent in the high frequency range, the Cl content is preferably 0.5 mol% or less, more preferably 0.4 mol% or less, even more preferably 0.3 mol% or less, even more preferably 0.2 mol% or less, and particularly preferably 0.1 mol% or less. The lower limit is 0% (substantially not contained).

[0030] In order to improve the acid resistance of the glass, the alkali-free glass according to this embodiment may contain at least one selected from the group consisting of Sc2O3, TiO2, ZnO2, Ga2O3, GeO2, Y2O3, ZrO2, Nb2O5, In2O3, TeO2, HfO2, Ta2O5, WO3, Bi2O3, La2O3, Gd2O3, Yb2O3, and Lu2O3 as a trace component. However, if the content of the trace components is too high, the uniformity of the glass decreases and phase separation is likely to occur, so the total content of the trace components is preferably 1 mol% or less. The above-mentioned trace components may be contained only one type, or two or more types.

[0031] The alkali-free glass according to this embodiment may contain up to 1 mol % of F for the purposes of improving the melting property of the glass, lowering the strain point of the glass, lowering the glass transition temperature, lowering the annealing point, etc. If the F content exceeds 1 mol %, there is a risk of increasing bubble defects in the glass.

[0032] In order to improve the meltability, clarity, formability, etc. of the glass, and to obtain absorption at a specific wavelength and improve density, hardness, bending rigidity, durability, etc., the alkali-free glass according to this embodiment may contain one or more of Se2O3, TeO2, Ga2O3, In2O3, GeO2, CdO, BeO, and Bi2O3. The total content of these is preferably 2% or less, more preferably 1% or less, even more preferably 0.5% or less, even more preferably 0.3% or less, particularly preferably 0.1% or less, particularly preferably 0.05% or less, and most preferably 0.01% or less.

[0033] In order to improve the meltability, clarity, formability, etc. of the glass and also to improve the hardness, e.g., Young's modulus, of the glass, the alkali-free glass according to this embodiment may contain rare earth oxides and transition metal oxides.

[0034] The alkali-free glass according to this embodiment may contain one or more of Sc2O3, Y2O3, La2O3, Ce2O3, Pr2O3, Nd2O3, Pm2O3, Sm2O3, Eu2O3, Gd2O3, Tb2O3, Dy2O3, Ho2O3, Re2O3, Tm2O3, Yb2O3, and Lu2O3 as rare earth oxides. The total content of these is preferably 2% or less, more preferably 1% or less, even more preferably 0.5% or less, even more preferably 0.3% or less, even more preferably 0.1% or less, particularly preferably 0.05% or less, and most preferably 0.01% or less.

[0035] The alkali-free glass according to this embodiment may contain one or more of V2O5, Ta2O3, Nb2O5, WO3, MoO3, and HfO2 as transition metal oxides. The total content of these is preferably 2% or less, more preferably 1% or less, even more preferably 0.5% or less, even more preferably 0.3% or less, even more preferably 0.1% or less, particularly preferably 0.05% or less, and most preferably 0.01% or less.

[0036] In order to improve the melting property of the glass, the alkali-free glass according to this embodiment may contain ThO2, which is an actinide oxide. The content of ThO2 is preferably 2% or less, more preferably 1% or less, even more preferably 0.5% or less, still more preferably 0.3% or less, particularly preferably 0.1% or less, still more preferably 0.05% or less, particularly preferably 0.01% or less, and most preferably 0.005% or less.

[0037] The alkali-free glass according to this embodiment preferably has a dielectric loss tangent (tan δ) of 0.006 or less at 35 GHz. If the dielectric loss tangent at 35 GHz is 0.006 or less, the dielectric loss in a high frequency region exceeding 30 GHz can be reduced. The dielectric loss tangent at 35 GHz is more preferably 0.0054 or less, even more preferably 0.005 or less, even more preferably 0.0045 or less, particularly preferably 0.004 or less, and particularly preferably 0.003 or less. Furthermore, the dielectric loss tangent at 10 GHz is preferably 0.006 or less, more preferably 0.005 or less, further preferably 0.004 or less, and most preferably 0.003 or less.

[0038] The alkali-free glass according to this embodiment preferably has a relative dielectric constant of 10 or less at 35 GHz. If the relative dielectric constant at 35 GHz is 10 or less, the dielectric loss in the high frequency range can be reduced. The relative dielectric constant at 35 GHz is more preferably 7 or less, further preferably 6 or less, and particularly preferably 5 or less. Furthermore, the relative dielectric constant at 10 GHz is preferably 5.5 or less, more preferably 5.3 or less, and even more preferably 5 or less.

[0039] Furthermore, when non-alkali glass is used for glass substrates in high frequency devices, it is required to have a high Young's modulus. If the Young's modulus is low, the glass substrate may suffer from defects such as warping, bending, or cracking after the formation of a metal (e.g., Cu) film during the device manufacturing process. Non-alkali glass with a low dielectric tangent tends to have a low Young's modulus. The alkali-free glass according to this embodiment preferably has a Young's modulus of 58 GPa or more. If the Young's modulus is within the above range, the glass substrate can be prevented from warping, bending, cracking, and other defects after the formation of a metal film, for example, a Cu film, carried out in the manufacturing process of a high-frequency device. The Young's modulus is more preferably 60 GPa or more, more preferably 62 GPa or more, even more preferably 63 GPa or more, especially preferably 64 GPa or more, even more preferably 65 GPa or more, particularly preferably 66 GPa or more, particularly preferably 67 GPa or more, and most preferably 68 GPa or more.

[0040] The alkali-free glass according to this embodiment has a specific elastic modulus of 23 GPa cm in order to suppress the amount of deformation of the glass. 3 / g or more is preferable, and 24 GPa cm 3 / g or more is preferable, and 25 GPa cm 3 / g or more is more preferable. The upper limit is not particularly limited, but for example, 32 GPa cm 3 / g or less is preferable.

[0041] The alkali-free glass according to this embodiment has a density of 2.58 g / cm 3 The density is preferably 2.57 g / cm or less. This reduces the self-weight deflection and makes it easier to handle large substrates. It also reduces the weight of devices using glass. 3 Less than 2.56 g / cm is more preferable. 3 The following is even more preferable: Note that a large substrate is, for example, a substrate with at least one side measuring 900 mm or more.

[0042] The alkali-free glass according to this embodiment has an average thermal expansion coefficient of 30×10 -7 / ° C. or more. This makes it possible to prevent the glass substrate from cracking due to an excessive difference in expansion coefficient between the glass substrate and the metal film formed thereon when the glass substrate is formed with the metal film. The average thermal expansion coefficient between 50 and 350°C is 33×10 -7 / ℃ or more is more preferable, and 35×10 -7 / ℃ or more is more preferable, and 36×10-7 / °C or more is even more preferable, and 37×10 -7 / °C or higher, most preferably 38×10 -7 / ℃ or higher. On the other hand, the average thermal expansion coefficient at 50 to 350°C is set at 43×10 in order to prevent glass from breaking during the manufacturing process of products such as high-frequency devices. -7 / °C or less is preferable. The average thermal expansion coefficient between 50 and 350°C is 42×10 -7 / ℃ or less is more preferable, and 41.5×10 -7 / ℃ or less is more preferable, and 41×10 -7 / °C or less is even more preferable, and 40.5×10 -7 / ℃ or less is especially preferable, and 40.3×10 -7 / ℃ or less is particularly preferable, and 40×10 -7 / °C or less is most preferable.

[0043] The alkali-free glass according to this embodiment has a glass viscosity of 10 2 The temperature T2 at which the glass melts is preferably 1700°C or lower. By setting T2 to 1700°C or lower, the glass melting property is excellent and the burden on the manufacturing equipment can be reduced. For example, the life of equipment such as a kiln for melting glass can be extended, and productivity can be improved. In addition, defects derived from the kiln, such as lumpy defects and Zr defects, can be reduced. T2 is more preferably 1680°C or lower, and even more preferably 1670°C or lower. T2 is preferably 1500°C or higher.

[0044] The alkali-free glass according to this embodiment has a glass viscosity of 10 4 The temperature T4 at which the glass has a viscosity of dPa·s is preferably 1290°C or lower. This provides excellent formability of the glass. In addition, for example, by lowering the temperature during glass forming, volatile substances in the atmosphere around the glass can be reduced, thereby reducing defects in the glass. Since glass can be formed at a low temperature, the burden on the manufacturing equipment can be reduced. For example, the life of equipment such as a float bath for forming the glass can be extended, and productivity can be improved. T4 is more preferably 1280°C or lower. In addition, the lower limit is not particularly limited, but for example, 1050°C or higher is preferable. T2 and T4 are measured using a rotational viscometer according to the method specified in ASTM C 965-96. 2 d Pa s or 10 4 It can be calculated as the temperature at which the viscosity becomes d·Pa·s. In the examples described below, NBS710 and NIST717a were used as reference samples for calibrating the device.

[0045] The glass transition temperature of the alkali-free glass according to this embodiment is preferably 700°C or lower. This avoids the need to increase the temperature of the annealing device, and suppresses a decrease in the life of the annealing device. The glass transition temperature is more preferably 680°C or lower, and even more preferably 670°C or lower. The glass transition temperature is preferably 600°C or higher. This makes it possible to suppress deformation and shrinkage (thermal shrinkage) of the glass plate when the glass plate is treated at high temperatures in the high-frequency device manufacturing process. The glass transition temperature is more preferably 620°C or higher, and particularly preferably 630°C or higher. Furthermore, the alkali-free glass according to this embodiment has a lower strain point, which improves the formability of the glass. The strain point is preferably 700° C. or less, more preferably 670° C. or less, and even more preferably 660° C. or less. There is no particular restriction on the lower limit of the strain point, but it is preferably, for example, 550° C. or more.

[0046] The alkali-free glass according to this embodiment preferably has a surface devitrification temperature of 1300°C or less. This provides excellent formability of the glass. It is possible to suppress the occurrence of crystals inside the glass during forming, which would otherwise cause a decrease in transmittance. It is also possible to reduce the burden on the manufacturing equipment. For example, it is possible to extend the life of equipment such as a float bath for forming the glass, thereby improving productivity. The surface devitrification temperature is further preferably 1295° C. or less, 1290° C. or less, 1285° C. or less, 1280° C. or less, 1275° C. or less, 1270° C. or less, 1265° C. or less, 1260° C. or less, 1255° C. or less, 1250° C. or less, 1245° C. or less, 1240° C. or less, 1235° C. or less, 1230° C. or less, 1225° C. or less, 1220° C. or less, 1215° C. or less, 1210° C. or less, 1205° C. or less, and 1200° C. or less in that order. The lower limit is not particularly limited, but is preferably, for example, 1000° C. or more. The surface devitrification temperature in this embodiment can be determined as follows: crushed glass particles are placed in a platinum dish, heat-treated for 17 hours in an electric furnace controlled at a constant temperature, and after the heat treatment, the maximum temperature at which crystals precipitate on the glass surface and the minimum temperature at which crystals do not precipitate are observed using an optical microscope, and the average value is taken as the surface devitrification temperature.

[0047] The alkali-free glass according to this embodiment has a glass component elution amount of 0.025 mg / cm per unit surface area when immersed in an aqueous solution containing 6 wt % HNO3 and 5 wt % H2SO4 at 45°C for 170 seconds. 2 The amount of eluted glass components is preferably 0.025 mg / cm or less. 2 If the amount of eluted glass components is less than 0.020mg / cm, the acid resistance is good. 2 The less the better, the less the better.

[0048] If the B2O3 content of alkali-free glass is increased, when the glass raw materials in a melting tank are heated with a burner or the like to melt them, a large amount of B2O3 is evaporated during melting of the glass raw materials, resulting in low productivity. On the other hand, electrical melting, in which electricity is passed directly from electrodes in a melting tank to the molten glass and the glass raw materials are melted by the generated Joule heat, forms a cold top layer on the molten glass base, which can suppress the amount of B2O3 volatilization (JP Patent Publication 5-163024). However, alkali-free glass with a low dielectric tangent tends to have a high resistance value in the melting temperature range. If the resistance value in the melting temperature range is high, the difference with the resistance value of the furnace material constituting the melting tank body becomes small, and current may also flow in the furnace material constituting the wall surface of the melting tank. If current also flows in the furnace material, problems such as the melting of glass raw materials being hindered, the furnace material being eroded, power consumption increasing, and manufacturing costs increasing (WO 2019 / 004434). In addition, when electricity is applied to the furnace material, the furnace material may be destroyed and mixed into the glass, which may cause foreign matter to be mixed into the glass product. In contrast to the above, the alkali-free glass according to this embodiment preferably has a resistance value at 1500°C of 400 Ω·cm or less. If the resistance value at 1500°C is within the above range, melting by electrical heating during glass production is possible. The resistance value at 1500°C is more preferably 300 Ω·cm or less, further preferably 250 Ω·cm or less, and even more preferably 200 Ω·cm or less. Although there is no particular lower limit, it is 10 Ω·cm or more.

[0049] In the alkali-free glass according to this embodiment, the haze value of the glass substrate having a thickness of 1 mmt is preferably 1.0% or less. This provides high uniformity in the glass, and for example, when the glass substrate is acid-washed, it is possible to suitably prevent localized unevenness from occurring on the substrate surface. This reduces the transmission loss of high-frequency signals. In the alkali-free glass according to this embodiment, the haze value of the glass substrate having a thickness of 1 mmt is more preferably 0.8% or less, more preferably 0.5% or less, and most preferably 0.4% or less, and the smaller the haze value, the better.

[0050] Due to the above-mentioned characteristics, the alkali-free glass according to this embodiment is suitable for use as a glass substrate for high-frequency devices, panel-type antennas, window glass, vehicle window glass, cover glass for touch panels, and the like. FIG. 1 is a cross-sectional view showing an example of the configuration of a circuit board for a high-frequency device. The circuit board 1 shown in FIG. 1 includes an insulating glass substrate 2, a first wiring layer 3 formed on a first main surface 2a of the glass substrate 2, and a second wiring layer 4 formed on a second main surface 2b of the glass substrate 2. The first and second wiring layers 3 and 4 form a microstrip line as an example of a transmission line. The first wiring layer 3 forms a signal line, and the second wiring layer 4 forms a ground line. However, the structure of the first and second wiring layers 3 and 4 is not limited to this. The wiring layer may be formed on only one main surface of the glass substrate 2.

[0051] The first and second wiring layers 3, 4 are layers formed of a conductor, and their thickness is usually about 0.1 to 50 μm. The conductor forming the first and second wiring layers 3, 4 is not particularly limited, and may be, for example, a metal such as steel, gold, silver, aluminum, titanium, chromium, molybdenum, tungsten, platinum, or nickel, or an alloy or metal compound containing at least one of these metals. The structure of the first and second wiring layers 3, 4 is not limited to a single-layer structure, and may be a multi-layer structure such as a laminated structure of a titanium layer and a copper layer. The method of forming the first and second wiring layers 3, 4 is not particularly limited, and may be, for example, various known forming methods such as a printing method using a conductor paste, a dipping method, a plating method, a vapor deposition method, or a sputtering method.

[0052] If a glass substrate containing the alkali-free glass according to this embodiment is used as the glass substrate 2, the dielectric loss tangent (tan δ) at 35 GHz is 0.006 or less. The relative dielectric constant of the glass substrate 2 at 35 GHz is preferably 10 or less. When the dielectric loss tangent of the glass substrate 2 at 35 GHz is 0.006 or less, the dielectric loss in a high frequency region exceeding 30 GHz can be reduced. When the relative dielectric constant of the glass substrate 2 at 35 GHz is 10 or less, the dielectric loss in a high frequency region can also be reduced. The dielectric loss tangent of the glass substrate 2 at 35 GHz is more preferably 0.0054 or less, even more preferably 0.005 or less, even more preferably 0.0045 or less, especially preferably 0.004 or less, and particularly preferably 0.003 or less. The relative dielectric constant of the glass substrate 2 at 35 GHz is more preferably 7 or less, even more preferably 6 or less, and particularly preferably 5 or less.

[0053] Further, the glass substrate 2 has main surfaces 2a, 2b and end faces. At least one of the main surfaces 2a, 2b on which the first and second wiring layers 3, 4 of the glass substrate 2 are formed preferably has an arithmetic mean roughness Ra of 1.5 nm or less as a surface roughness, and more preferably, the arithmetic mean roughness Ra of both main surfaces is 1.5 nm or less. This allows the skin resistance of the first and second wiring layers 3, 4 to be reduced even when a skin effect occurs in the first and second wiring layers 3, 4 in a high frequency region exceeding 30 GHz, thereby reducing conductor loss. The arithmetic mean roughness Ra of the main surfaces 2a, 2b of the glass substrate 2 is more preferably 1.0 nm or less, and even more preferably 0.5 nm or less. The main surface of the glass substrate 2 refers to the surface on which the wiring layer is formed. When a wiring layer is formed on one main surface, it is sufficient that the value of the arithmetic mean roughness Ra of the one main surface satisfies 1.5 nm or less. In this specification, the surface roughness Ra refers to a value according to JIS B0601 (2001).

[0054] The surface roughness of the main surfaces 2a and 2b of the glass substrate 2 can be achieved by polishing the surface of the glass substrate 2 as necessary. For example, polishing using an abrasive containing cerium oxide or colloidal silica as a main component and a polishing pad; polishing using a polishing slurry containing an abrasive and an acidic or alkaline dispersion medium and a polishing pad; polishing using an acidic or alkaline etching solution, etc. can be applied to the surface of the glass substrate 2. These polishing processes are applied according to the surface roughness of the raw plate of the glass substrate 2, and for example, preliminary polishing and finish polishing may be applied in combination. In addition, it is preferable to chamfer the edge of the glass substrate 2 in order to prevent the glass substrate 2 from breaking, cracking, or chipping due to the edge during the process flow. The chamfering form may be any of C-chamfering, R-chamfering, thread chamfering, etc.

[0055] By using such a glass substrate 2, the transmission loss of the circuit board 1 at 35 GHz can be reduced, specifically to 1 dB / cm or less. Therefore, the characteristics such as quality and strength of high frequency signals, particularly high frequency signals exceeding 30 GHz, and further high frequency signals of 35 GHz or more, are maintained, so that a glass substrate 2 and a circuit board 1 suitable for high frequency devices handling such high frequency signals can be provided. In other words, the characteristics and quality of high frequency devices handling such high frequency signals can be improved. The transmission loss of the circuit board 1 at 35 GHz is more preferably 0.5 dB / cm or less.

[0056] The shape of the glass plate including the alkali-free glass according to this embodiment is not particularly limited, but the thickness is preferably 0.7 mm or less. If the thickness of the glass plate is 0.7 mm or less, when it is used as a glass substrate for a high-frequency device, the high-frequency device can be made thinner and smaller, and the production efficiency can be improved. In addition, the ultraviolet transmittance is improved, and the manufacturability can be improved by using an ultraviolet curing material in the device manufacturing process. The thickness of the glass plate is more preferably 0.6 mm or less, more preferably 0.5 mm or less, even more preferably 0.4 mm or less, even more preferably 0.3 mm or less, even more preferably 0.2 mm or less, and particularly preferably 0.1 mm or less. In addition, the lower limit is about 0.01 mm.

[0057] When the glass plate is used as a large substrate, at least one side is preferably 900 mm or more, more preferably 1000 mm or more. Although there is no particular upper limit, the size of one side is usually 4000 mm or less. The glass plate is preferably rectangular.

[0058] Next, a method for producing a glass plate containing alkali-free glass will be described. When producing a glass plate, a melting process for heating glass raw materials to obtain molten glass, a fining process for removing bubbles from the molten glass, a forming process for forming the molten glass into a plate shape to obtain a glass ribbon, and a slow cooling process for slowly cooling the glass ribbon to room temperature are performed. Alternatively, the molten glass may be formed into a block shape, slowly cooled, and then cut and polished to produce a glass plate.

[0059] In the melting process, raw materials are prepared to obtain a target glass composition, and the raw materials are continuously charged into a melting furnace and heated to preferably about 1450°C to 1750°C to obtain molten glass. Since the alkali-free glass according to this embodiment has a low resistance in the temperature range for melting the glass raw materials, for example, around 1500°C, it is preferable to use an electric melting furnace as the melting furnace and melt the glass by electrical heating. However, electrical heating and heating by a burner may be used in combination.

[0060] The raw materials may also include oxides, carbonates, nitrates, hydroxides, chlorides, and other halides. When the molten glass comes into contact with platinum during the melting or fining process, minute platinum particles may dissolve into the molten glass and become mixed into the resulting glass sheet as foreign matter. However, the use of a nitrate raw material has the effect of preventing the generation of platinum foreign matter.

[0061] As the nitrate, strontium nitrate, barium nitrate, magnesium nitrate, calcium nitrate, etc. can be used. The use of strontium nitrate is more preferable. The particle size of the raw material can be appropriately selected from raw materials with a large particle size of several hundred μm that does not leave any residue in the solution, to raw materials with a small particle size of about several μm that does not scatter during raw material transportation and does not aggregate as secondary particles. Granules can also be used. The moisture content of the raw material can be appropriately adjusted to prevent the raw material from scattering. The β-OH value, the oxidation-reduction degree of Fe (redox [Fe 2+ / (Fe 2+ +Fe 3+ )) can also be appropriately adjusted.

[0062] The next fining step is a step of removing bubbles from the molten glass obtained in the melting step. In the fining step, a defoaming method under reduced pressure may be applied, or the temperature may be higher than the melting temperature of the raw materials to remove bubbles. SO3 or SnO2 may be used as a fining agent. As the SO3 source, a sulfate of at least one element selected from Al, Na, K, Mg, Ca, Sr, and Ba is preferable, and an alkaline earth metal sulfate is more preferable. Among them, CaSO4·2H2O, SrSO4, and BaSO4 are particularly preferable because they have a significant effect of enlarging bubbles.

[0063] As a clarifying agent in the defoaming method by reduced pressure, it is preferable to use a halogen such as Cl or F. As a Cl source, a chloride of at least one element selected from Al, Mg, Ca, Sr, and Ba is preferable, and an alkaline earth metal chloride is more preferable, among which SrCl2·6H2O and BaCl2·2H2O are particularly preferable because they have a significant effect of increasing bubble size and have a small deliquescence. As an F source, a fluoride of at least one element selected from Al, Na, K, Mg, Ca, Sr, and Ba is preferable, and an alkaline earth metal fluoride is more preferable, among which CaF2 is even more preferable because it has a significant effect of increasing the solubility of the glass raw material.

[0064] Tin compounds, such as SnO2, generate O2 gas in molten glass. In molten glass, SnO2 is reduced to SnO at a temperature of 1450°C or higher, generating O2 gas and having the effect of making bubbles grow larger. In the manufacture of glass sheets, glass raw materials are heated to about 1450 to 1750°C to melt, so that bubbles in the molten glass become larger more effectively. When SnO2 is used as a clarifier, it is preferable to prepare the raw materials so that the tin compound is contained in an amount of 0.01% or more in terms of SnO2 relative to the total amount of the matrix composition of 100%. If the SnO2 content is 0.01% or more, it is preferable because a clarification effect is obtained when the glass raw materials are melted, more preferably 0.05% or more, and even more preferably 0.10% or more. If the SnO2 content is 0.3% or less, it is preferable because the occurrence of coloring and devitrification of glass is suppressed. The content of the tin compound in the glass, calculated as SnO2 with respect to 100% of the total amount of the glass matrix composition, is more preferably 0.25% or less, further preferably 0.2% or less, and particularly preferably 0.15% or less.

[0065] The next forming step is a step of forming the molten glass from which bubbles have been removed in the fining step into a sheet shape to obtain a glass ribbon. As the forming step, a known method of forming glass into a sheet shape can be applied, such as a float method in which molten glass is made to flow onto a molten metal such as tin to form a sheet shape to obtain a glass ribbon, an overflow downdraw method (fusion method) in which molten glass is made to flow downward from a trough-shaped member, and a slit downdraw method in which molten glass is made to flow down from a slit. Among these, the float method or fusion method is preferred from the viewpoint of no polishing or light polishing.

[0066] Next, the annealing process is a process of cooling the glass ribbon obtained in the forming process to room temperature under controlled cooling conditions. In the annealing process, the glass ribbon is cooled to become a glass ribbon, and then annealed to room temperature under predetermined conditions. The annealed glass ribbon is cut to obtain a glass plate.

[0067] If the cooling rate R in the slow cooling process is too large, distortion is likely to remain in the glass after cooling. In addition, the equivalent cooling rate, which is a parameter that reflects the fictive temperature, becomes too high, and as a result, the shrinkage of the glass cannot be reduced. Therefore, it is preferable to set R so that the equivalent cooling rate is 800°C / min or less. The equivalent cooling rate is more preferably 400°C / min or less, even more preferably 100°C / min or less, and particularly preferably 50°C / min or less. On the other hand, if the cooling rate is too small, the time required for the process becomes too long, and the productivity decreases. Therefore, it is preferable to set it to 0.1°C / min or more, more preferably 0.5°C / min or more, and even more preferably 1°C / min or more.

[0068] Here, the definition and evaluation method of the equivalent cooling rate are as follows. A glass sample is prepared by processing a glass of the target composition into a rectangular parallelepiped of 10 mm x 10 mm x 0.3 to 2.0 mm. The glass sample is held at strain point +1700°C for 5 minutes using an infrared heating electric furnace, and then cooled to room temperature (25°C). At this time, multiple glass samples are prepared by changing the cooling rate in the range of 10°C / min to 1000°C / min.

[0069] Using a precision refractive index measuring device (e.g., Shimadzu Devices KPR2000), the refractive index n of multiple glass samples at the d line (wavelength 587.6 nm) was measured. d The measurement may be performed using the V-block method or the minimum deviation method. d By plotting against the logarithm of the cooling rate, n d Obtain a calibration curve.

[0070] Next, we compared n samples of glass with the same composition that were actually produced through processes such as melting, molding, and cooling. d is measured by the above-mentioned measurement method. d The corresponding cooling rate (referred to as an equivalent cooling rate in this embodiment) is obtained from the above calibration curve.

[0071] The present invention is not limited to the above embodiment. Modifications and improvements are permitted within the scope of the present invention. For example, when manufacturing the glass plate according to the present embodiment, the glass may be formed into a plate shape by a press molding method in which molten glass is directly formed into a plate shape.

[0072] In addition, when manufacturing the glass plate according to the present embodiment, in addition to the manufacturing method using a melting tank made of refractory material, a crucible made of platinum or an alloy mainly composed of platinum (hereinafter referred to as platinum crucible) may be used as the melting tank or fining tank. When a platinum crucible is used, the melting step involves preparing raw materials so as to obtain the composition of the glass plate to be obtained, and heating the platinum crucible containing the raw materials in an electric furnace, preferably to about 1450°C to 1700°C. A platinum stirrer is inserted and the mixture is stirred for 1 to 3 hours to obtain molten glass.

[0073] In the forming step in the manufacturing process of a glass plate using a platinum crucible, the molten glass is poured onto, for example, a carbon plate or into a mold to form a plate or block. In the slow cooling step, the glass is typically held at a temperature of about Tg+50°C, then cooled to near the strain point at about 1 to 10°C / min, and then cooled to room temperature at a cooling rate at which no distortion remains. After cutting into a predetermined shape and polishing, a glass plate is obtained. In addition, the glass plate obtained by cutting may be heated to, for example, about Tg+50°C, and then slowly cooled to room temperature at a predetermined cooling rate. In this way, the equivalent cooling temperature of the glass can be adjusted.

[0074] A circuit board 1 using the alkali-free glass according to this embodiment as the glass substrate 2 is suitable for high-frequency devices that handle high-frequency signals, particularly high-frequency signals exceeding 30 GHz, and further high-frequency signals of 35 GHz or higher, and can reduce the transmission loss of such high-frequency signals and improve the characteristics of the high-frequency signals, such as their quality and strength. A circuit board 1 using the alkali-free glass according to this embodiment as the glass substrate 2 is suitable for high-frequency devices (electronic devices) such as semiconductor devices used in communication devices such as mobile phones, smart phones, personal digital assistants, and Wi-Fi devices, surface acoustic wave (SAW) devices, radar parts such as radar transceivers, and antenna parts such as liquid crystal antennas and panel-type antennas. That is, the present invention relates to a glass substrate for high frequency devices containing the alkali-free glass according to this embodiment, as well as a panel type antenna containing the alkali-free glass according to this embodiment.

[0075] The alkali-free glass according to the present invention can also be suitably applied to other products for the purpose of reducing transmission loss of high-frequency signals. That is, the present invention also relates to window glass, vehicle window glass, and touch panel cover glass that contain such an alkali-free glass. Glass sheets containing alkali-free glass can stably transmit and receive radio waves in high frequency bands and are not easily damaged or destroyed, so they are also suitable for window glass, vehicle window glass, and touch panel cover glass. As a vehicle window glass, for example, a window glass for an autonomous vehicle is more preferable. EXAMPLES

[0076] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. Examples 1 to 43 and Examples 49 to 61 are Examples, and Examples 44 to 48 are Comparative Examples.

[0077] [Examples 1-61] A glass plate having the composition shown in Tables 1 to 5, Table 11, and Table 12 (mol % based on oxide), a thickness of 1.0 mm, a shape of 50×50 mm, and an arithmetic mean roughness Ra of the main surface of 1.0 nm was prepared. The glass plate was produced by a melting method using a platinum crucible. Raw materials such as silica sand were mixed so as to obtain glass having the composition shown in Tables 1 to 5, Tables 11, and Table 12, and a batch of 1 kg was prepared. The raw materials were placed in a platinum crucible and heated in an electric furnace at a temperature of 1650° C. for 3 hours to melt the raw materials, thereby obtaining molten glass. For melting, a platinum stirrer was inserted in the platinum crucible and stirred for 1 hour to homogenize the glass. The molten glass was poured onto a carbon plate and formed into a plate shape, and then the plate-shaped glass was placed in an electric furnace at a temperature of about Tg+50° C. and held for 1 hour. The temperature of the electric furnace was lowered to Tg-100°C at a cooling rate of 1°C / min, and then the glass was allowed to cool to room temperature. The glass was then cut and polished to form a plate, thereby obtaining a glass plate.

[0078] For the glass plates of Examples 1 to 48, the average thermal expansion coefficient at 50 to 350°C, density, glass transition temperature, Young's modulus, specific elastic modulus, T2, T4, β-OH value, specific dielectric constant at 10 GHz or 35 GHz, dielectric loss tangent at 10 GHz or 35 GHz, surface devitrification temperature, acid resistance, haze value, and resistivity at 1500°C are shown in Tables 6 to 12. The haze value is an index of phase separation of glass. Also, blanks in the tables mean that no measurement was performed.

[0079] The methods for measuring each physical property are shown below. (density) The density of a glass lump of about 20 g containing no bubbles was measured by the Archimedes method. (Average thermal expansion coefficient) Measurements were made using a differential thermal dilatometer in accordance with the method specified in JIS R3102 (1995). The measurement temperature range was 50 to 350°C, and the units were ppm / °C or x10 -7 Expressed as / °C. (glass transition temperature) The measurements were performed using the thermal expansion method according to the method specified in JIS R3103-3 (2001). (Young's Modulus) Glass with a thickness of 0.5 to 10 mm was measured by the ultrasonic pulse method according to the method specified in JIS Z2280 (1993). The unit is GPa. (Specific elastic modulus) The Young's modulus measured by the above method is divided by the density measured by the above method to obtain the specific elastic modulus (GPa cm 3 / g) was calculated. (T2) The viscosity was measured using a rotational viscometer according to the method specified in ASTM C 965-96. 2 The temperature T2 (°C) at which the viscosity reached d·Pa·s was measured. (T4) The viscosity was measured using a rotational viscometer according to the method specified in ASTM C 965-96. 4 The temperature T4 (℃) at which the viscosity reached d·Pa·s was measured. (Dielectric constant, dielectric tangent) Measurements were performed using a cavity resonator and a vector network analyzer according to the method specified in JLS R1641 (2007). The measurement frequency was 10 GHz or 35 GHz, which is the resonant frequency of the air in the cavity resonator. (Surface devitrification temperature) The glass was crushed and classified using a test sieve so that the particle size was in the range of 2 to 4 mm. The obtained glass cullet was ultrasonically cleaned in isopropyl alcohol for 5 minutes, washed with ion-exchanged water, dried, placed in a platinum dish, and heat-treated for 17 hours in an electric furnace controlled at a constant temperature. The heat treatment temperature was set at 10°C intervals. After the heat treatment, the glass was removed from the platinum dish and observed under an optical microscope for the maximum temperature at which crystals precipitated on the surface of the glass and the minimum temperature at which no crystals precipitated. The maximum temperature at which crystals precipitate on the glass surface and the minimum temperature at which crystals do not precipitate were each measured once. (If it is difficult to determine whether crystals precipitate, measurements may be taken twice.) The maximum temperature at which crystals precipitate on the glass surface and the minimum temperature at which crystals do not precipitate were averaged to determine the surface devitrification temperature. (acid resistance) The glass sample was immersed in an acid solution (6 mass% HNO3 + 5 mass% H2SO4, 45°C) for 170 seconds, and the amount of glass components dissolved per unit surface area (mg / cm 2 The amount of eluted glass components was 0.02 mg / cm 2 If it is below this, the acid resistance is good. (β-OH value) The absorbance of the glass sample was measured for light with wavelengths of 2.75 to 2.95 μm, and the maximum absorbance value β max The β-OH value was calculated by dividing by the thickness (mm) of the sample. (Resistivity at 1500℃) The resistivity of the molten glass was measured in the temperature range of 1350 to 1700°C. The molten glass was prepared by mixing each component to obtain a predetermined composition and melting it at a temperature of 1650°C in a platinum crucible. When melting the glass, the glass was stirred using a platinum stirrer to make it homogenous. Next, the resistivity of the molten glass was measured while it was kept at a temperature of 1500°C by the method described in the following document: "Method of Measuring the Electrical Conductivity of Ionic Melts, Ota Yoshio, Miyanaga Mitsuru, Morinaga Kenji, Yanagase Tsutomu, Journal of the Japan Institute of Metals, Vol. 45, No. 10 (1981) pp. 1036-1043" (Haze value) The haze value of the glass was measured using a haze meter (manufacturer: Suga Test Instruments Co., Ltd., model: HZ-V3 Hazemeter). The haze value was measured using a glass plate with a thickness of 1 mm and mirror polished on both sides. A haze value of 35% or less was considered to be a good product.

[0080] [Table 1]

[0081]

Table 2

[0082]

Table 3

[0083]

Table 4

[0084]

Table 5

[0085]

Table 6

[0086]

Table 7

[0087]

Table 8

[0088]

Table 9

[0089]

Table 10

[0090]

Table 11

[0091] [Table 12]

[0092] The glasses of Examples 1 to 43, which are working examples, are partially unmeasured, but all of them have an average thermal expansion coefficient of 30×10 at 50 to 350° C. -7 / ℃~40×10 -7 / ℃, density 2.58g / cm 3 The results satisfied many of the following ranges: glass transition temperature 700°C or less, Young's modulus 58GPa or more, T2 1500~1700°C, T4 1290°C or less, dielectric tangent at 35GHz 0.006 or less, and resistance at 1500°C 400Ω·cm or less. Additionally, the haze value measurement confirmed that there was no phase separation. When Al2O3-(MgO+CaO+SrO+BaO) is greater than -3 and less than 2, the surface devitrification temperature is 1300°C or less, and the acid resistance tends to be good. When Al2O3-(MgO+CaO+SrO+BaO) is 2 or more, the surface devitrification temperature tends to exceed 1300°C. When the value of Al2O3 / B2O3 is 0.49 or more, the Young's modulus of the glass tends to be high. When SrO / (MgO+CaO+SrO+BaO) is 0.64 or more, the surface devitrification temperature of the glass tends to be low. Glass with B2O3 less than 15% and Al2O3 / B2O3 value greater than 1.4 has a dielectric tangent of more than 0.006 at 35 GHz, and the dielectric loss in the high frequency region cannot be reduced. In addition, the glass transition temperature is greater than 700°C. On the other hand, glasses with an Al2O3 / B2O3 value of 0.35 or less had poor acid resistance. Phase separation was also confirmed from the haze value measurement results. Glasses with a B2O3 content of more than 24% and an Al2O3 / B2O3 value of more than 1.4 had poor acid resistance. Phase separation was also confirmed from the haze value measurement results. Furthermore, the Young's modulus was less than 58 GPa. The glasses of Examples 49 to 52, which are working examples, are glasses in which the Cl content and β-OH value were changed based on the glass composition of Example 30. These show that increasing the β-OH value may relatively reduce the dielectric tangent, and that increasing the Cl content may increase the dielectric tangent. The glasses of Examples 53 to 61, which are working examples, are glasses in which the Li2O content and the Na2O content are changed based on the glass composition of Example 30. When the Li2O content and the Na2O content increase, the resistivity at 1500°C decreases. Furthermore, Li2O can reduce the resistivity at 1500°C while maintaining a low dielectric tangent.

[0093] Although the present invention has been described in detail and with reference to specific embodiments, it is apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on Japanese patent applications filed on April 12, 2019 (Patent Application No. 2019-076423), June 28, 2019 (Patent Application No. 2019-120828), and November 27, 2019 (Patent Application No. 2019-214690), the contents of which are incorporated herein by reference. [Industrial Applicability]

[0094] The alkali-free glass according to the present embodiment has excellent acid resistance and can reduce the dielectric loss of high-frequency signals. A glass plate containing such an alkali-free glass is useful for high-frequency electronic devices that handle high-frequency signals of over 10 GHz, particularly over 30 GHz, and even over 35 GHz, such as glass substrates for communication devices, frequency filter components such as SAW devices and FBARs, bandpass filters such as waveguides, SIW (Substrate Integrated waveguide) components, radar components, antenna components (particularly liquid crystal antennas that are considered to be optimal for satellite communications), window glass, and window glass for vehicles. [Explanation of symbols]

[0095] 1: Circuit board 2: Glass substrate 2a, 2b: Main surface 3,4: Wiring layer

Claims

1. Molar percentage based on oxide: Yes 2 61~70%, <h2 style=";text-align:left;direction:ltr">Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 5~11% B 2 O 3 21.9% or less, MgO 0.2-10%, CaO 0.1-7%, SrO 0-3.3%, BaO 0-3%, Contains 0 to 0.1% ZnO; Formula (A) is [Al 2 O 3 ] / [B 2 O 3 The value of the formula (A) is 0.41 or more and 0.65 or less, The formula (B) is [MgO] + [CaO] + [SrO] + [BaO], and the value of the formula (B) is 8 or more and 11.5 or less.

2. Formula (C) is [Al 2 O 3 ] - ([MgO] + [CaO] + [SrO] + [BaO]), The alkali-free glass according to claim 1, wherein the value of formula (C) is −3 to 2%.

3. Formula (C) is [Al 2 O 3 ] - ([MgO] + [CaO] + [SrO] + [BaO]), The alkali-free glass according to claim 1, wherein the value of formula (C) is −3 to 0%.

4. Formula (C) is [Al 2 O 3 ] - ([MgO] + [CaO] + [SrO] + [BaO]), The alkali-free glass according to claim 1, wherein the value of the formula (C) is −3 to −0.5%.

5. Formula (C) is [Al 2 O 3 ] - ([MgO] + [CaO] + [SrO] + [BaO]), The alkali-free glass according to claim 1, wherein the value of formula (C) is −3 to −1%.

6. The alkali-free glass according to claim 1 or 2, wherein the value of the formula (A) is 0.54 or more and 0.65 or less.

7. Fe 2 O 3 The alkali-free glass according to claim 1 or 2, containing 1 mol % or less of Fe calculated as an alkali-free glass.

8. The β-OH value of the glass is 0.05 mm. -1 More than 1.0 mm -1 The alkali-free glass according to claim 1 or 2, wherein:

9. [Li 2 O] + [Na 2 O] + [K 2 The alkali-free glass according to claim 1 or 2, wherein the total content of [O] is 0 to 0.2 mol %.

10. SnO 2 , Cl and SO 3 The alkali-free glass according to claim 1 or 2, containing 1 mol % in total or less of at least one selected from the group consisting of:

11. S.C. 2 O 3 , TiO 2 , ZnO, Ga 2 O 3 , GeO 2 , Y 2 O 3 , ZrO 2 , Nb 2 O 5 , In 2 O 3 , TeO 2 , HfO 2 , Ta 2 O 5 , W.O. 3 , Bi 2 O 3 , La 2 O 3 , Gd 2 O 3 , Yb 2 O 3 , and Lu 2 O 3 The alkali-free glass according to claim 1 or 2, containing 1 mol % in total or less of at least one selected from the group consisting of:

12. The alkali-free glass according to claim 1 or 2, containing 1 mol % or less of F.

13. The alkali-free glass according to claim 1 or 2, which has a dielectric loss tangent at 35 GHz of 0.006 or less.

14. 3. The alkali-free glass according to claim 1, which has a resistivity of 400 Ω·cm or less at 1500° C.

15. 3. The alkali-free glass according to claim 1, which has a resistivity at 1500° C. of 300 Ω·cm or less.

16. The alkali-free glass according to claim 1 or 2, having a Young's modulus of 58 GPa or more.

17. Density is 2.58 g / cm 3 The average thermal expansion coefficient at 50 to 350°C is 30 x 10 -7 / ℃~40×10 -7 The alkali-free glass according to claim 1 or 2, wherein the temperature is 0.15 to 1.5° C.

18. Glass viscosity is 10 2 The temperature T2 at which the glass viscosity becomes dPa·s is 1500 to 1700°C, and the glass viscosity is 10 4 The alkali-free glass according to claim 1 or 2, wherein the temperature T4 at which the viscosity becomes dPa·s is 1290° C. or lower.

19. 3. The alkali-free glass according to claim 1, which has a glass transition temperature of 700° C. or lower or a strain point of 700° C. or lower.

20. The alkali-free glass according to claim 1 or 2, having a surface devitrification temperature of 1,300° C. or lower.

21. H.N.O. 3 6% by weight and H 2 SO 4 When immersed for 170 seconds in an aqueous solution at 45° C. containing 5% by weight of 2 The alkali-free glass according to claim 1 or 2, wherein:

22. 22. A glass plate comprising the alkali-free glass according to any one of claims 1 to 21, the glass plate having main surfaces and end faces, wherein at least one of the main surfaces has an arithmetic mean roughness Ra of 1.5 nm or less.

23. The glass plate according to claim 22, having at least one side of 900 mm or more and a thickness of 0.7 mm or less.

24. 24. The glass sheet according to claim 22 or 23, produced by a float process or a fusion process.

25. A glass substrate for a high frequency device comprising the alkali-free glass according to any one of claims 1 to 21.

26. A panel-type antenna comprising the alkali-free glass according to any one of claims 1 to 21.

27. A window glass comprising the alkali-free glass of any one of claims 1 to 21.

28. A vehicle window glass comprising the alkali-free glass according to any one of claims 1 to 21.

29. A cover glass for a touch panel comprising the alkali-free glass according to any one of claims 1 to 21.

Citation Information

Patent Citations

  • Low dielectric constant glass fiber

    JP1995010598A

  • Method for manufacturing windowpane for vehicle with coating film

    JP2011256060A

  • Low-CTE alkali-free boroaluminosilicate glass composition and glass articles thereof

    JP2015512852A

  • Low dielectric loss glasses for electronic devices

    JP2022522986A

  • Method for producing magnetic disk and method for producing glass substrate for information recording medium

    WO2011136027A1