Aqueous preparation containing at least one aqueous hydrophobing agent for producing aqueous coating agents with improved early rain resistance

By combining hydrophobizing agents and water-soluble cationic polymers, the coating compositions achieve improved initial rain resistance and storage stability, addressing the limitations of existing technologies in aqueous coatings.

JP2024138216APending Publication Date: 2024-10-08EVONIK OPERATIONS GMBH
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2024019124
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-02-27
Filing Date
2024-02-13
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Aqueous coating compositions face challenges in achieving early rain resistance, particularly in high humidity and low temperature conditions, due to delayed drying rates and issues with viscosity and yellowing, which are not adequately addressed by existing technologies.

Method used

Incorporating a hydrophobizing agent and a water-soluble cationic polymer into the coating formulations to enhance initial rain resistance and reduce viscosity increase during storage.

Benefits of technology

The combination of hydrophobizing agents and water-soluble cationic polymers improves the initial rain resistance and storage stability of coatings, providing a smoother and more resistant surface with reduced viscosity changes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138216000001_ABST
    Figure 2024138216000001_ABST
Patent Text Reader

Abstract

To provide an aqueous formulation for producing a coating composition with early water resistance, a produced coating composition and a production method.SOLUTION: The present invention provides an aqueous formulation that has at least one aqueous hydrophobizing agent and at least one water-soluble cationic polymer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention provides an aqueous formulation comprising at least one hydrophilic hydrophobizing agent for producing an aqueous coating composition having improved rainfastness. [Background technology]

[0002] The drying speed of water-based coating compositions depends on temperature and humidity. When humidity is low, the drying speed is often fast, and in some cases even faster than that of solvent-based coating compositions. However, at high humidity and low temperature, such as in the morning and evening, before, during, or after rain, the drying speed is obviously slower because the evaporation of water is delayed. Such coatings only become rainproof after a very long drying time. The initial rainproofness or rainproofness of water-based coating compositions before they are completely dried is particularly desirable for exterior applications, such as paints for buildings, bridges, ships, and road markings, and exterior primers.

[0003] To achieve such initial weather resistance or weatherproofing, there are various principles involved in practice.

[0004] In one variant of the so-called flocculation principle, the coating composition contains an anionically stabilized binder, a polyamine and ammonia as a volatile base that evaporates after application of the coating composition, resulting in flocculation of the binder during drying (US 5527853, EP 0594321, EP 0728822, EP 0409459). In another variant, the coating composition also contains an ionically stabilized binder. The flocculation is carried out by spraying an acid or salt solution simultaneously with the coating composition (WO 94 / 29391, EP 0200249, US 4571415, US 5403393). A change in viscosity at the surface of the coating composition can be achieved by applying a thickener to the fresh coating to increase the viscosity, or by applying a base containing a thickener to the fresh coating, as disclosed, for example, in EP 0721003. However, due to the lower pH, the thickening agent is not activated.

[0005] EP 0804514 describes a fast-drying aqueous coating composition comprising an anionically stabilized aqueous emulsion and a polyimine. The addition of a polyimine to a coating composition based on an anionically stabilized aqueous emulsion has the disadvantage that the mixture tends to yellow as soon as it dries. This is especially true when using emulsions based on vinyl acetate copolymers. For decorative exterior applications, this yellowing of the coating causes an undesirable change in shade.

[0006] Furthermore, the charge of polyimines, i.e., the flocculation, is pH dependent. At higher pH values, the charge balance of polyimines gradually shifts from the cationic to the neutral region, leading to a loss of efficacy. However, modern coating compositions are often set at a relatively high pH to reduce microbial growth while reducing the amount of biocide used.

[0007] Also known is EP 1250388, which describes a fast-drying aqueous coating composition comprising at least one aqueous binder. The fast-drying aqueous coating composition further comprises at least one water-soluble quaternary poly(allylamine) and a non-ionic surfactant. However, a drawback is that the viscosity increases during storage. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] U.S. Patent No. 5,527,853 [Patent Document 2] European Patent No. 0594321 [Patent Document 3] European Patent No. 0728822 [Patent Document 4] European Patent No. 0409459 [Patent Document 5] International Publication No. 94 / 29391 Brochure [Patent Document 6] European Patent No. 0200249 [Patent Document 7] U.S. Pat. No. 4,571,415 [Patent Document 8] U.S. Pat. No. 5,403,393 [Patent Document 9] European Patent No. 0721003 [Patent Document 10] European Patent No. 0804514 [Patent Document 11] European Patent No. 1250388 Summary of the Invention [Problem to be solved by the invention]

[0009] It would therefore be desirable to provide an aqueous formulation for producing a coating composition having early water resistance that does not suffer from the shortcomings known in the prior art. [Means for solving the problem]

[0010] To solve this problem, aqueous formulations have been proposed which contain at least one hydrophobizing agent and at least one water-soluble cationic polymer.

[0011] Quite unexpectedly, it was found that the combination of hydrophobizing agent and water-soluble cationic polymer improves initial rain resistance.The coatings made with the aqueous formulation according to the present invention have improved initial rain resistance compared to conventional coatings.Advantageously, the aqueous coating composition according to the present invention further shows less viscosity increase during storage.

[0012] The skilled person knows that the hydrophobicity of a coating can be increased by adding a hydrophobizing agent. In this way, the coating and thus the substrate can be protected from the penetration of water. A hydrophobic coating or surface can be characterized by measuring the contact angle of a water drop, which should be between 90 degrees and 180 degrees ("Water-based silicone resin coating systems for facades: fundamentals, formulations, practical applications, problem solutions", Wolfgang Schultze, 2nd edition, expert-verlag 2002, p. 18). For example, the contact angle can be measured using an optical contact angle measuring device in combination with a contour analysis system according to DIN 55660.

[0013] Typically, the hydrophobizing agent is introduced into the finished dispersion of the millbase in the form of an aqueous emulsion made with an emulsifier, into which the binder is then further stirred. Such paints and primers initially have a relatively high water absorption capacity for a period of time (the "wash-off period") after application, and therefore have limited early water resistance.

[0014] Most hydrophobizing agents are based on organosilicon compounds, used individually or in combination. Examples include alkoxysilanes, silicone oils, silicone resins, and siliconates (see also Wassrige Siliconharz-Beschichtungssysteme fur Fassaden: Grundlagen, Formulierungen, Anwendung in der Praxis, Problemlosungen, Wolfgang Schultze, 2nd edition, expert-verlag 2002, pp. 69-74).

[0015] The alkoxysilane is preferably a compound of formula (I). R 1 a Si(OR 2 ) b Formula (I) (In the formula, a is 0 or more and 2 or less, b is 2 or more and 4 or less, and the sum of a+b is 4, R 1 is a saturated or unsaturated alkyl group having 1 to 8 carbon atoms, or an organic moiety having 1 to 8 carbon atoms and 1 to 2 nitrogen or oxygen atoms, or an aromatic moiety having 6 to 20 carbon atoms, R 2 is an alkyl or acyl group having 1 to 8 carbon atoms.

[0016] Preferred alkyl groups are methyl, ethyl, propyl, isopropyl, n-butyl, s-butyl, and t-butyl. Preferred aromatic moieties are phenyl moieties. Preferred substituents R 1 R is a methyl or phenyl group, or a mixture of methyl and phenyl groups. 2 Preferred alkyl groups are methyl, ethyl, propyl, isopropyl, n-butyl, s-butyl or t-butyl. Preferred alkoxysilane is octyltriethoxysilane.

[0017] The silicone oil is preferably a compound of formula (II). R 3 O(Si(R 4 )2O) n R 3 Formula (II)

[0018] In the formula, R 3 are independently a hydrogen atom, or a trimethylsilyl group or an alkyl group, such as a methyl group or an ethyl group. 4 are independently the same or different linear or branched, saturated, monounsaturated or polyunsaturated alkyl groups having 1 to 20 carbon atoms, or an organic moiety having 1 to 8 carbon atoms and 1 to 2 nitrogen or oxygen atoms, or an organosilicon moiety having 1 silicon atom, 1 to 15 carbon atoms and 1 to 4 oxygen atoms, or an aromatic moiety having 6 to 20 carbon atoms. 4 is preferably a methyl group, a 3-aminopropyl group, an N-2-(aminoethyl)-3-aminopropyl group, a 2-(trimethoxysilyl)ethyl group, a 2-(triethoxysilyl)ethyl group, or a phenyl group. The degree of polymerization n is 1 to 10,000, preferably 3 to 1,000, and most preferably 5 to 300.

[0019] The silicone resin is preferably a polymeric compound of formula (III). R 5 c Si(OR 6 ) d O (4-c-d) / 2 Formula (III) (In the formula, c is 0 or more and 2 or less, d is 0 or more and 4 or less, and the sum of c+d is less than 4. R 5 are independently the same or different linear or branched, saturated or mono- or polyunsaturated, aromatic hydrocarbyl groups, or organic moieties having 1 to 8 carbon atoms and 1 to 2 nitrogen or oxygen atoms. 6 is a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. 5 is preferably a methyl group, a propyl group, a phenyl group, a 3-aminopropyl group, or an octyl group. 6is preferably a hydrogen atom, or a methyl or ethyl group.

[0020] Formula (III) is the smallest unit of the average structural formula of a silicone resin.

[0021] The hydrophobizing agent is preferably an aqueous silicone resin emulsion, a silicone oil emulsion, an emulsion or microemulsion of an amino-functional silicone oil, a silane emulsion, or a mixture thereof.

[0022] The hydrophobizing agent may preferably be an aqueous emulsion based on two or more organosilicon compounds.

[0023] Generally, all commercially available hydrophobizing agents are useful, as long as they can be used in aqueous coating compositions. Commercially available hydrophobizing agents that should be mentioned include Tego Phobe® 1401, 1409, 1650, 1659, 6510 and 6600 from Evonik, Silres® BS45, BS54, BS60, BS6042, BS1001 and BS1306 from Wacker, Dowsil® IE2404, IE6683, IE6694 and Z-70 emulsions from Dow, Variphob® SR550, SR580, HP105, HP120 from CHT, Bluesil BP9710, BP9878, BP9800, BP9821, BP9900, BP9705, PB9920 from Elkem Silicones, and Graf These include Silsan® CC55, HSB, DSH, WS1800, 1300 and 1350 from Chemicals Corporation.

[0024] The water-soluble cationic polymer preferably has quaternary ammonium groups.

[0025] Suitable water-soluble cationic polymers are preferably poly[(dimethylimino)-2-butene-1,4-diyl] chloride (Polyquaternium-1), poly(diallyldimethylammonium chloride) (Polyquaternium-6), copolymers of acrylamide and quaternized dimethylammonium ethyl methacrylate, poly{bis(2-chloroethyl)ether-alt-1,3-bis[3(dimethylamino)propyl]urea} (Polyquaternium-2), hydroxyethylcellulose dimethyl diallyl ammonium chloride copolymer (Polyquaternium-4), poly(acrylamide-methacryloyloxyethyl trimethylammonium methyl sulfate) (Polyquaternium-5), poly(diallyldimethylammonium chloride-co-acrylamide) (Polyquaternium-7), quaternized hydroxyethylcellulose (Polyquaternium-10), copolymers of methyl- and stearyl dimethylaminoethyl methacrylate quaternized with dimethyl sulfate (Polyquaternium-8), Poly-N,N-(dimethylamino)ethyl methacrylate quaternized with bromoethane (Polyquaternium-9), poly(vinylpyrrolidone-co-dimethylaminoethyl methacrylate, quaternized) (Polyquaternium-11), poly(ethyl methacrylate-co-abietyl methacrylate-co-diethylaminoethyl methacrylate) quaternized with dimethyl sulfate (Polyquaternium-12), poly(ethyl methacrylate-co-oleyl methacrylate-co-diethylaminoethyl methacrylate) quaternized with dimethyl sulfate (Polyquaternium-13), poly(2-methacryloyl oxyethyltrimethylammonium methylsulfate) (Polyquaternium-14), poly(acrylamide-co-trimethylammonioethyl methacrylate chloride) (Polyquaternium-15), 3-methyl-1-vinylimidazolium chloride-N-vinylpyrrolidone copolymer (Polyquaternium-16), poly[oxy-1,2-ethanediyl(dimethyliminio)-1,3-propanediimino(1,6-dioxo-1,6-hexanediyl)imino-1,3-propanediyl(dimethyliminio)-1,2-ethanediyl dichloride] (Polyquaternium-17), poly[oxy-1,2-Ethanediyl(dimethyliminio)-1,3-propanediimino(1,9-dioxo-1,9-nonanediyl)imino-1,3-propanediyl(dimethyliminio)-1,2-ethanediyl chloride (Polyquaternium-18), poly(diallyldimethylammonium chloride-acrylic acid) (Polyquaternium-22), cellulose, ethers with α-[3-(dodecyldimethylammonio)-2-hydroxypropyl]-ω-hydroxypoly(oxy-1,2-ethanediyl) chloride (Polyquaternium-24), N-vinyl-2-pyrrolidone-3-methacrylamidopropyltrimethylammonium chloride copolymer (Polyquaternium-28), 2-propenoic acid, 2-methyl-, methyl ester, polymer with N-(carboxymethyl)-N,N-dimethyl-2-[(2-methyl-1-oxo-2-propenyl)oxy]ethaneaminium zwitterion (Polyquaternium-30), 2-acryloxyethyltrimethylammonium chloride-acrylamide copolymer (Polyquaternium-31), Polyquaternium-33), 2-propenoic acid, 2-methyl-, methyl ester, polymer of 2-(dimethylamino)ethyl-2-methyl-2-propenoate, compound with dimethyl sulfate (Polyquaternium-36), poly(2-methacryloxyethyltrimethylammonium chloride) (Polyquaternium-37), acrylic acid-acrylamide-dimethyl diallyl ammonium chloride copolymer (Polyquaternium-39), poly[oxyethylene(dimethylamino)ethylene(dimethylamino)ethyl] dichloride] (Polyquaternium-42), 3-methyl-1-vinylimidazolium methyl sulfate-N-vinylpyrrolidone copolymer (Polyquaternium-44), 3-methyl-N-vinylimidazolium methyl sulfate-N-vinylcaprolactam-N-vinyl-2-pyrrolidone copolymer (Polyquaternium-46), acrylic acid-methacrylamidopropyltrimethylammonium chloride-methyl acrylate copolymer (Polyquaternium-47), N-methacryloyloxyethyl-N,N-Dimethylammonium α-N-methylcarboxybetaine polymer (Polyquaternium-50), butyl methacrylate-2-methacryloyloxyethyl phosphorylcholine copolymer (Polyquaternium-51), N,N-dimethylacrylamide-dimethylaminoethyl methacrylate-diethyl sulfate-polyethylene glycol-dimethacrylate copolymer (Polyquaternium-52), poly(acrylamide-methacrylamidopropyl trimethylammonium chloride-acrylic acid) (Polyquaternium-53), 1-dodecane aminium, N,N-dimethyl-N-[3-[(2-methyl-1-oxo-2-propenyl)amino]propyl]-, chloride, polymer with N-[3-(dimethylamino)propyl]-2-methyl-2-propenamide and 1-ethenyl-2-pyrrolidinone (Polyquaternium-55), 2-(methacryloyloxy)ethyl-2-(trimethylammonium)ethyl phosphate-stearyl methacrylate Poly(acrylamide-acrylic acid-acryloyloxyethyl trimethylammonium chloride) (Polyquaternium-63), 2-hydroxy-3-methacryloxypropyl trimethylammonium chloride-2-methacryloxyethyl phosphorylcholine copolymer (Polyquaternium-64), cellulose, 2-[3-(dodecyldimethylammonio)-2-hydroxypropoxy]ethyl-3- (Dodecyldimethylammonio)-2-hydroxypropyl-2-hydroxyethyl-2-[2-hydroxy-3-(trimethylammonio)propoxy]ethyl-2-hydroxy-3-(trimethylammonio)propyl ether, chloride (Polyquaternium-67), methacrylamide-N-vinylimidazole-N-vinylimidazole-methosulfate-N-vinyl-2-pyrrolidone copolymer (Polyquaternium-68), 1-dodecaneaminium, N,N-Dimethyl-N-[3-[(2-methyl-1-oxo-2-propenyl)amino]propyl]-, chloride, Polymer of N-[3-(dimethylamino)propyl]-2-methyl-2-propenamide, 1-ethenylhexahydro-2H-azepin-2-one and 1-ethenyl-2-pyrrolidinone (Polyquaternium-69), 1-Propanaminium, N,N,N-trimethyl-3-[(1-oxo-2-propen-1-yl)amino]-, chloride (1:1), a polymer of N,N-dimethyl-2-propenamide, 2-hydroxyethyl-2-methyl-2-propenoate, and N,N,N-trimethyl-2-[(2-methyl-1-oxo-2-propen-1-yl)oxy]ethanaminium chloride (1:1) (Polyquaternium-84), 1H-imidazolium, 1-ethenyl-3-methyl-, chloride (1:1), 1-ethenyl-1H-imidazole, 1-ethenyl-2-pyrrolidinone, and 2 2-Methyl-2-propenoic acid and 2-ethoxyethyl-2-methyl-2-propenoic acid copolymer (Polyquaternium-86), acrylic acid-ethyl acrylate-(3-methacrylamidopropyl)trimethylammonium chloride copolymer (Polyquaternium-98), ethanaminium, N,N,N-trimethyl-2-[(2-methyl-1-oxo-2-propen-1-yl)oxy]-, chloride (1:1), butyl-2-methyl-2-propenoate and 2-ethoxyethyl-2-methyl-2-propenoate and N,N-dimethylaminopropylacrylamide-stearyl methacrylate copolymer (Polyquaternium-107), 2-propen-1-aminium, N,N-dimethyl-N-2-propen-1-yl-, chloride (1:1), polymer with 2-hydroxy-1-methylethyl-2-propenoate and 2-propenoic acid (Polyquaternium-111), quaternized polysaccharides and polysaccharide derivatives such as guar hydroxypropyl trimethylammonium chloride and hydroxypropyl guar hydroxypropyl trimethylammonium chloride, chitosan hydroxypropyl trimethylammonium chloride, starch 3-(dodecyldimethylammonio)-2-hydroxypropyl 2-hydroxy-3-(trimethylammonio)propyl ether chloride (Polyquaternium-75) and hydroxypropyl trimethylammonium chloride starch.

[0026] Poly(diallyldimethylammonium chloride) and quaternized hydroxyethyl cellulose are particularly preferred, most preferably poly(diallyldimethylammonium chloride).

[0027] The water-soluble cationic polymer preferably has an amino group, and polyethyleneimine is particularly preferred.

[0028] The weight average molecular weight of the water-soluble cationic polymer is preferably in the range of 10,000 g / mol to 2,000,000 g / mol, more preferably in the range of 20,000 g / mol to 1,000,000 g / mol, and most preferably in the range of 30,000 g / mol to 500,000 g / mol.

[0029] The aqueous formulation preferably contains from 0.05% to 5.0% by weight of cationic polymer, preferably from 0.1% to 3.0% by weight, more preferably from 0.2% to 2.0% by weight, based on the formulation.

[0030] A further invention is the use of the aqueous formulation of the present invention as an additive for producing an aqueous coating composition having improved initial rain resistance.

[0031] The present invention also provides a coating composition comprising an aqueous formulation according to the present invention.

[0032] The coating compositions, as well as the aqueous formulations according to the invention, optionally also comprise film-forming aids, pigments, fillers, thickeners, levelling agents, dispersants, wetting agents, preservatives, emulsifiers, protective colloids, and / or antifoaming agents.

[0033] The coating composition according to the present invention is preferably an exterior undercoat, paint, primer or wood coating, more preferably a synthetic resin undercoat, facade paint, road marking paint or wood protection paint.

[0034] The present invention also provides (a) first preparing an aqueous formulation comprising at least one hydrophobizing agent and at least one aqueous cationic polymer solution, the weight average molecular weight of which is in the range of 10,000 g / mol to 1,000,000 g / mol; (b) then adding at least one aqueous binder to the formulation obtained according to (a); (c) adding, as required, an emulsifier or mixture of emulsifiers, film-forming aids, pigments, fillers, thickeners, leveling agents, protective colloids, dispersants, wetting agents, preservatives and / or defoamers; A method for producing a coating composition having initial rain resistance is also provided.

[0035] Surprisingly, it has been found that coatings produced by the method according to the invention have improved initial weather resistance compared to conventional coatings.

[0036] The binder may of course also be a mixture of different binders.

[0037] The weight proportion of the binder (solid form) in the coating composition is preferably 1.0 to 50.0% by weight, more preferably 3.0 to 25.0% by weight, based on the weight of the dry materials in the coating composition.

[0038] The aqueous binder is preferably added as the last component to the mixture, along with the emulsifier or emulsifier mixture, film-forming aid, pigment, filler, thickener, leveling agent, protective colloid, dispersant, wetting agent, preservative, and / or defoamer, if used.

[0039] The binder is preferably an aqueous polymer dispersion based on homopolymers and / or copolymers.

[0040] Particularly preferred homopolymers and copolymers contain, as monomer units, at least one olefinically unsaturated monomer.

[0041] Particular preference is given to copolymers which comprise from 70% by weight to 99.7% by weight, based on the total amount of monomers, of free-radically polymerizable olefinically unsaturated compounds from the group: the acrylic and methacrylic esters of (C1-C12) monoalcohols, preferably (C1-C8) monoalcohols, such as methanol, ethanol, isopropanol, isobutanol, n-butanol, 2-ethylhexyl alcohol, vinyl aromatic monomers, such as styrene, vinyl esters of (C1-C12)-alkane monocarboxylic acids, such as vinyl acetate, vinyl propionate, vinyl n-butyrate, vinyl laurate, VeoVa® 9 and VeoVa® 10, vinyl halides, such as vinyl chloride and vinylidene chloride, α- and β-monoolefinically unsaturated nitriles, such as acrylonitrile and methacrylonitrile, alkyl esters of monoolefinically unsaturated dicarboxylic acids, such as di-n-butyl maleate and di-n-butyl fumarate. The copolymer preferably also contains from 0.3 to 10% by weight, more preferably from 0.5 to 5% by weight, based on the total amount of monomers, of α- and β-monoolefinically unsaturated mono- and dicarboxylic acids, such as acrylic acid, methacrylic acid, itaconic acid, maleic acid and fumaric acid, and their amides, optionally having substituents on the nitrogen atom, such as acrylamide, methacrylamide, N-methylolacrylamide, N-butoxymethacrylamide.

[0042] Furthermore, functional monomers can be present in the copolymer in an amount of 0% to 20% by weight, preferably 0.5% to 5% by weight, based on the total amount of monomers. Functional monomers are, for example, hydroxyl group-containing monomers such as hydroxyalkyl acrylates and hydroxyalkyl methacrylates, in particular hydroxyethyl methacrylate and hydroxypropyl methacrylate, and / or acetylacetoxy group-containing monomers which improve wet adhesion, in particular allyl acetoacetate, acetylacetoxyethyl methacrylate and acetylacetoxybutyl methacrylate, and / or crosslinking monomers such as monomers having epoxy groups and silane groups, in particular glycidyl acrylate, glycidyl methacrylate, vinyltrimethoxysilane and methacryloxypropyltrimethoxysilane, and / or nitrogen-containing monomers from the group of polymerizable monomers having amino, ureido or N-heterocyclic groups, for example dimethylaminoethyl acrylate and dimethylaminoethyl methacrylate, N-(2-methacryloylethyl)ethyleneurea, and / or keto group-containing monomers, for example diacetoneacrylamide, diacetonemethacrylamide, acrolein and 2-butanone methacrylate.

[0043] In the self-crosslinking dispersion, the keto group-containing polymer can be present in a maximum of 5% by weight, based on the total amount of monomer or di- or polyfunctional carboxylic acid hydrazide, for example adipic acid hydrazide.

[0044] The polymer dispersions used as binders are preferably anionically stabilized polymer dispersions or polymer dispersions stabilized by mixtures of nonionic and anionic stabilizers or mixtures of nonionic, anionic emulsifiers and protective colloids.

[0045] Suitable nonionic emulsifiers are, for example, the alkoxylation products of alkyl polyglycol ethers or polypropylene oxides. Useful anionic emulsifiers are primarily the alkali metal or ammonium salts of alkylsulfonates, sulfates, phosphates or phosphonates, arylsulfonates, sulfates, phosphates or phosphonates, or alkylarylsulfonates, sulfates, phosphates or phosphonates.

[0046] Suitable protective colloids are natural products, such as gum arabic, starch and alginates, modified natural products, such as cellulose derivatives, or synthetic polymers, such as polyvinyl alcohol and polyvinylpyrrolidone, or mixtures thereof.

[0047] As well as emulsifiers and protective colloids, the polymer dispersions may also contain additives, auxiliaries and / or non-copolymerizable crosslinkers, if necessary.

[0048] For the formulation of the method according to the invention it is preferable to use an aqueous formulation comprising 0.05% to 5.0% by weight, preferably 0.1% to 3.0% by weight, more preferably 0.2% to 2.0% by weight of cationic polymer.

[0049] The cationic polymer preferably has quaternary ammonium groups.

[0050] Suitable water-soluble cationic polymers are preferably poly[(dimethylimino)-2-butene-1,4-diyl] chloride (Polyquaternium-1), poly(diallyldimethylammonium chloride) (Polyquaternium-6), copolymers of acrylamide and quaternized dimethylammonium ethyl methacrylate, poly{bis(2-chloroethyl)ether-alt-1,3-bis[3(dimethylamino)propyl]urea} (Polyquaternium-2), hydroxyethylcellulose dimethyldiallylammonium chloride copolymer (Polyquaternium-3), poly(diallyldimethylammonium chloride) (Polyquaternium-4), poly(diallyldimethylammonium chloride) (Polyquaternium-5), poly(diallyldimethylammonium chloride) (Polyquaternium-6), poly(diallyldimethylammonium chloride) (Polyquaternium-7), poly(diallyldimethylammonium chloride) (Polyquaternium-8), poly(diallyldimethylammonium chloride) (Polyquaternium-9), poly(diallyldimethylammonium chloride) (Polyquaternium-10), poly(diallyldimethylammonium chloride) (Polyquaternium-11), poly(diallyldimethylammonium chloride) (Polyquaternium-12), poly(diallyldimethylammonium chloride) (Polyquaternium-13), poly(diallyldimethylammonium chloride) (Polyquaternium-14), poly(diallyldimethylammonium chloride) (Polyquaternium-15), poly(diallyldimethylammonium chloride) (Polyquaternium-16), poly(diallyldimethylammonium chloride) (Polyquaternium-17), poly(diallyldimethylammonium chloride) (Polyquaternium-18), poly(diallyldimethylammonium chloride) (Polyquaternium-19), poly(diallyldimethylammonium chloride) (Polyquaternium-21), poly(diallyldimethylammonium chloride) (Polyquaternium-22), poly(diallyldimethylammonium chloride) (Polyquaternium-16), poly(diallyldimethylammonium chloride) (Polyquaternium-1 Polyquaternium-4), poly(acrylamide-methacryloyloxyethyltrimethylammonium methylsulfate) (Polyquaternium-5), poly(diallyldimethylammonium chloride-co-acrylamide) (Polyquaternium-7), quaternized hydroxyethylcellulose (Polyquaternium-10), copolymer of methyl- and stearyl dimethylaminoethyl methacrylate quaternized with dimethyl sulfate (Polyquaternium-8), poly-N,N-(dimethylamino)ethyl methacrylate quaternized with bromoethane (Polyquaternium-9). -9), poly(vinylpyrrolidone-co-dimethylaminoethyl methacrylate, quaternized) (Polyquaternium-11), poly(ethyl methacrylate-co-abietyl methacrylate-co-diethylaminoethyl methacrylate) quaternized with dimethyl sulfate (Polyquaternium-12), poly(ethyl methacrylate-co-oleyl methacrylate-co-diethylaminoethyl methacrylate) quaternized with dimethyl sulfate (Polyquaternium-13), poly(2-methacryloyloxyethyltrimethylammonium methyl sulfate) (Polyquaternium-14), poly(acrylamide-co-trimethylammonioethyl methacrylate chloride) (Polyquaternium-15), 3-methyl-1-vinylimidazolium chloride-N-vinylpyrrolidone copolymer (Polyquaternium-16), poly[oxy-1,2-ethanediyl(dimethyliminio)-1,3-propanediimino(1,6-dioxo-1,6-hexanediyl)imino-1,3-propanediyl(dimethyliminio)-1,2-ethanediyl dichloride] (Polyquaternium-17), poly[oxy-1,2-Ethanediyl(dimethyliminio)-1,3-propanediimino(1,9-dioxo-1,9-nonanediyl)imino-1,3-propanediyl(dimethyliminio)-1,2-ethanediyl chloride (Polyquaternium-18), Poly(diallyldimethylammonium chloride-acrylic acid) (Polyquaternium-22), Cellulose, α-[3-(dodecyldimethylammonio)-2-hydroxypropyl]-ω-hydroxypoly(oxy-1,2-ethanediyl)ether, chloride (Polyquaternium-24), N-vinyl-2-pyrrolidone-3-methacrylamidopropyltrimethylammonium chloride copolymer (Polyquaternium-28), 2-propenoic acid, 2-methyl-, methyl ester, polymer with N-(carboxymethyl)-N,N-dimethyl-2-[(2-methyl-1-oxo-2-propenyl)oxy]ethaneaminium zwitterion (Polyquaternium-30), 2-acryloxyethyltrimethylammonium chloride-acrylamide copolymer (Polyquaternium-31), Polyquaternium-33), 2-propenoic acid, 2-methyl-, methyl ester, polymer of 2-(dimethylamino)ethyl-2-methyl-2-propenoate, compound with dimethyl sulfate (Polyquaternium-36), poly(2-methacryloxyethyltrimethylammonium chloride) (Polyquaternium-37), acrylic acid-acrylamide-dimethyl diallyl ammonium chloride copolymer (Polyquaternium-39), poly[oxyethylene(dimethylamino)ethylene(dimethylamino)ethyl] dichloride] (Polyquaternium-42), 3-methyl-1-vinylimidazolium methyl sulfate-N-vinylpyrrolidone copolymer (Polyquaternium-44), 3-methyl-N-vinylimidazolium methyl sulfate-N-vinylcaprolactam-N-vinyl-2-pyrrolidone copolymer (Polyquaternium-46), acrylic acid-methacrylamidopropyltrimethylammonium chloride-methyl acrylate copolymer (Polyquaternium-47), N-methacryloyloxyethyl-N,N-Dimethylammonium-α-N-methylcarboxybetaine polymer (Polyquaternium-50), Butyl methacrylate-2-methacryloyloxyethyl phosphorylcholine copolymer (Polyquaternium-51), N,N-Dimethylacrylamide-Dimethylaminoethyl methacrylate diethyl sulfate-Polyethylene glycol dimethacrylate copolymer (Polyquaternium-52), Poly(acrylamide-methacrylamidopropyltrimethylammonium chloride-acrylic acid) (Polyquaternium-53), 1-Dodecane aminium, N,N-dimethyl-N-[3-[(2-methyl-1-oxo-2-propenyl)amino]propyl]-, chloride, polymer with N-[3-(dimethylamino)propyl]-2-methyl-2-propenamide and 1-ethenyl-2-pyrrolidinone (Polyquaternium-55), 2-(methacryloyloxy)ethyl-2-(trimethylammonium)ethylphosphate-stearyl methacrylate copolymer (Polyquaternium-61), poly(acrylamide-acrylic acid-acryloyloxyethyltrimethylammonium chloride) (Polyquaternium-62), Polyquaternium-63), 2-hydroxy-3-methacryloxypropyltrimethylammonium chloride-2-methacryloxyethyl phosphorylcholine copolymer (Polyquaternium-64), cellulose, 2-[3-(dodecyldimethylammonio)-2-hydroxypropoxy]ethyl-3-(dodecyldimethylammonio)-2-hydroxypropyl-2-hydroxyethyl-2-[2-hydroxy-3-(trimethylammonio)propoxy]ethyl-2-hydroxy-3-(trimethylammonio)propyl ether, chloride (Polyquaternium-67) ), methacrylamide-N-vinylimidazole-N-vinylimidazole methosulfate-N-vinyl-2-pyrrolidone copolymer (Polyquaternium-68), 1-dodecaneaminium, N,N-dimethyl-N-[3-[(2-methyl-1-oxo-2-propenyl)amino]propyl]-, chloride, polymer with N-[3-(dimethylamino)propyl]-2-methyl-2-propenamide, 1-ethenylhexahydro-2H-azepin-2-one and 1-ethenyl-2-pyrrolidinone (Polyquaternium-69), 1-propaneaminium, N,N,N-trimethyl-3-[(1-oxo-2-propen-1-yl)amino]-, chloride (1:1), polymer of N,N-dimethyl-2-propenamide, 2-hydroxyethyl-2-methyl-2-propenoate, and N,N,N-trimethyl-2-[(2-methyl-1-oxo-2-propen-1-yl)oxy]ethanaminium chloride (1:1) (Polyquaternium-84), 1H-imidazolium, 1-ethenyl-3-methyl-, chloride (1:1), polymer of 1-ethenyl-1H-imidazole, 1-ethenyl-2-pyrrolidinone, and 2-methyl-2-propenoic acid (Polyquaternium-85). Polyquaternium-86), acrylic acid-ethyl acrylate-(3-methacrylamidopropyl)trimethylammonium chloride copolymer (Polyquaternium-98), ethanaminium, N,N,N-trimethyl-2-[(2-methyl-1-oxo-2-propen-1-yl)oxy]-, chloride (1:1), polymer with butyl-2-methyl-2-propenoate and 2-ethoxyethyl-2-methyl-2-propenoate (Polyquaternium-99), poly[(dimethyliminio)(2-hydroxy-1,3-propanediyl)(dimethyliminio)-1,6-hexanediyl dichloride] (Polyquaternium-100), 2-methacryloyloxyethyl phosphorylcholine-3-N,N-dimethylaminopropylacrylamide-stearyl methacrylate copolymer (Polyquaternium-107), 2-propen-1-aminium, N,N-dimethyl-N-2-propen-1-yl-, chloride (1:1), polymer with 2-hydroxy-1-methylethyl-2-propenoate and 2-propenoic acid (Polyquaternium-111), quaternized polysaccharides and polysaccharide derivatives, e.g. The compound is selected from guar hydroxypropyl trimethyl ammonium chloride and hydroxypropyl guar hydroxypropyl trimethyl ammonium chloride, chitosan hydroxypropyl trimethyl ammonium chloride, starch 3-(dodecyl dimethyl ammonio)-2-hydroxypropyl 2-hydroxy-3-(trimethyl ammonio) propyl ether chloride (Polyquaternium-75) and hydroxypropyl trimethyl ammonium chloride starch.

[0051] The cationic polymer is preferably selected from poly(diallyldimethylammonium chloride) and quaternized hydroxyethyl cellulose. Most preferred is poly(diallyldimethylammonium chloride).

[0052] In the process according to the invention it is preferred to use a water-soluble cationic polymer containing amino groups, more preferably polyethyleneimine.

[0053] The aqueous binder is preferably added as the last component to the mixture.

[0054] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. [Brief description of the drawings]

[0055] [Figure 1] Figure 1 is an example of a photograph of the surface of a facade paint. [Diagram 2] Figure 2 is an example of a photograph of the surface of a facade paint. [Diagram 3] Figure 3 is an example of a photograph of the surface of a facade paint. [Figure 4] Figure 4 is an example of a photograph of the surface of a facade paint. [Diagram 5] Figure 5 is an example of a photo of the surface of a facade paint. EXAMPLES

[0056] method Gel Permeation Chromatography (GPC) The described method is not an absolute method. Instead, a calibration is required. The calibration is performed using a commercially available poly-2-vinylpyridine standard with a linear structure and characterized by an independent absolute method. Equipment: Agilent 1100 from Agilent Technologies, precolumn: PSS NOVEMA Max, 10 μm, guard, ID 8.00 mm × 50.00 mm, column: PSS NOVEMA Max Ultrahigh, 10 μm, ID 8.00 mm × 300.00 mm, temperature 35 °C, eluent: 0.1 M NaCl, 0.1 vol.% TFA (aq), flow rate 1 mL / min, sample concentration 3 g / L. RI detector, molar mass range 620-2,890,000 g / mol. -1 Evaluation against poly-2-vinylpyridine standards.

[0057] Viscosity measurement Viscosity was measured according to DIN 53019-1 using an Anton Paar MR301 rheometer with cone / plate geometry at 100 s -1 Measured at a shear rate of

[0058] Additional Terms When values ​​are reported in % in the context of this specification, they are weight % values ​​unless otherwise stated. In the case of compositions, percentages are percentages of the total composition unless otherwise defined. When average values ​​are stated in the following examples, they are numerical averages unless otherwise stated. When drying the coating below, this is also carried out at a pressure of 101325 Pa, a temperature of 20° C., and an ambient relative humidity of about 40%, unless otherwise stated.

[0059] Materials and Equipment - RM10W roller mixer, manufactured by CAT - Black PVC film (Leneta) - Coatmaster 509MC film applicator, manufactured by Erichsen -ZAF2010 box-type coating bar, Zehntner - HPP110eco environmental control cabinet, manufactured by Memmert - Sigma Siloxane All Seasons Ink, manufactured by PPG - Spray bottle with pump atomizer, Technical Treatments - Dispermat with 30mm dispersion disc, VMA Getzmann - TEGO Phobe® 1650, manufactured by Evonik - TEGO Phobe® 1409, manufactured by Evonik

[0060] Experimental Example 1. Preparation of the aqueous formulation according to the invention 1.1 Cationic polymer solution Table 1 shows the commercial aqueous cationic polymer solutions used and their weight-average molecular weight Mw measured by GPC (items P1-P4). Since the quaternized hydroxyethyl cellulose is available in powder form, it was necessary to prepare aqueous polymer solutions. For this purpose, 100% polymer in powder form was mixed manually with demineralized water in a 50 mL screw-cap bottle using a spatula and placed on a RM10W roller mixer for 24 h. As a result, a homogeneous and transparent solution containing 20 wt. % of the cationic polymer (item P5) was obtained. Table 1: Cationic polymer solutions used

[0061] [Table 1]

[0062] 1.2 Hydrophobizing agent used The following commercially available hydrophobizing agents were used: -TEGO Phobe (registered trademark) 1650, manufactured by Evonik → (H1) -TEGO Phobe (registered trademark) 1409, manufactured by Evonik → (H2)

[0063] To prepare the aqueous formulation according to the invention, 100 g of H1 was weighed into a 180 mL polyethylene cup, followed by dropwise addition of the cationic polymer solution of Table 1 according to the concentration of Table 2, while stirring at 500 rpm with a Dispermat. Table 2: Recipes for formulations of the present invention containing H1

[0064] [Table 2]

[0065] 2. Measurement of initial rain resistance of facade paint 2.1 Manufacturing of facade paints Items 1 and 2 from Table 3 were placed in a 180 mL polyethylene cup and homogenized with a Dispermat equipped with a 30 mm dispersing disk for 5 minutes at 800 rpm. Items 3-7 were then added with stirring and mixed for 10 minutes. The speed was increased to 1500 rpm during this period. Next, the sequence of items 8-13 was added and dispersed at 2500 rpm. After 30 minutes, the dispersing disk was replaced with a paddle stirrer. The speed was reduced to 800 rpm and items 14 and 15 were added and mixed. Finally, the binder (item 16) and thickener (item 17) were added with stirring. The mixture was stirred at 1000 rpm for a further 10 minutes. After 24 hours, the initial rain resistance was measured. Table 3: Facade paint recipes

[0066] [Table 3]

[0067] 2.2 Measurement of initial rain resistance Using a box-type coating bar with a 200 μm slit and a Coatmaster 509MC film applicator, a film of the façade paint and a film of the comparative façade paint were applied onto the black Leneta film at a speed of 15 mm / s. The coated films were then placed in an environmental control cabinet, previously adjusted to a temperature of 8°C and a humidity of 80%. The films were allowed to dry in the cabinet for 20 minutes. Immediately afterwards, the films were fixed at a 45° angle and sprayed five times with 5.0 mL of demineralized water each time using a spray bottle. The water was allowed to drain completely. The applications were allowed to dry for 24 hours under standard laboratory conditions and then visually evaluated.

[0068] The comparative examples used were the comparative facade paints VF1, VF2 and VF3.

[0069] VF1 was prepared according to the recipe in Table 3 without the use of a hydrophobizing agent or the cationic polymer of item 15.

[0070] VF2 was prepared according to the recipe in Table 3 using only 4.8 wt% H1 and no cationic polymer from item 15.

[0071] VF3 was prepared using an additional 0.10 g of cationic polymer solution P4 according to the recipe in Table 3. P4 was then added to the comparative facade paint under stirring according to the process regime of Example 1 of EP 1 250 388.

[0072] The surface of VF1 was found to be heterogeneous and had numerous cracks. In addition, the surface showed numerous thick white runoff marks that reached the bottom edge of the Leneta film (see Figure 1). The initial rain resistance of VF1 was rated as very poor.

[0073] The surface of VF2 was also found to be inhomogeneous and slightly cracked. In addition, the surface showed numerous thick white runoff marks that reached the bottom edge of the Leneta film (see Figure 2). The initial rain resistance of VF2 was rated as poor.

[0074] The surface of VF3 was found to be smooth, homogenous, and free of cracks. In addition, the surface showed a few thick white runoff marks that did not reach the bottom edge (see Figure 3). The initial rain resistance of VF3 was rated as moderate.

[0075] The early rain resistance of the facade paint according to the invention was compared with the comparative facade paints VF1, VF2 and VF3. For a more understandable representation, VF1=1 (very bad), VF2=2 (bad) and VF3=3 (medium).

[0076] Table 4 shows the results of the initial rain resistance of the facade paints according to the invention. It was found that the facade paints F1 to F3 according to the invention have a smooth, homogeneous surface without cracks and have individual thin white runoff marks that do not reach the bottom. F4 and F5 show a smooth, homogeneous surface without cracks and have individual thin funnel-shaped slightly milky / cloudy to translucent runoff marks that do not reach the bottom. For this purpose, reference is made to Fig. 4 and Fig. 5 by way of example.

[0077] Examples of facade paint surface photographs are shown in Figures 1 to 5. Table 4: Visual evaluation of initial rain resistance

[0078] [Table 4]

[0079] Thus, it was shown that the combination of the hydrophobizing agent and the water-soluble cationic polymer improves the initial rain resistance. The coatings produced using the aqueous formulation according to the present invention had improved initial rain resistance compared to coatings not containing a hydrophobizing agent and a water-soluble cationic polymer, coatings containing only a hydrophobizing agent, and coatings produced by a conventional method containing only a water-soluble cationic polymer.

[0080] 2.3 Early weather resistance of other formulations of the present invention Analogous to 1.2, formulations according to the invention based on H2 with P4 were prepared in two concentrations, see Table 5. Then, analogous to 2.1, the corresponding facade paints were prepared according to Table 3. The results of the initial rain resistance measurements are shown in Table 6. Table 5: Recipes of formulations of the present invention containing H2 and P4

[0081] [Table 5]

[0082] Table 6: Initial rain resistance with different hydrophobizing agents

[0083] [Table 6]

[0084] It has been shown that synergistic effects occur with other hydrophobizing agents as well.

[0085] 2.4 Measurement of viscosity during storage The viscosity of the facade paints was measured to assess the storage stability. For this purpose, the viscosity was measured using the facade paint F4 according to the invention, as well as VF3 and VF4 as comparative examples. VF4 was produced without H1, and P4 was added to the comparative facade paints according to Example 1 of EP 1250388.

[0086] The facade paints were stored at 50°C and the viscosity was measured at room temperature after 24 hours, one week and two weeks. The results are shown in Table 7. Table 7: Viscosity during storage

[0087] [Table 7]

[0088] It was found that the viscosity of the facade paint according to the invention, produced with the formulation according to the invention, increased much less during storage than the comparative example, so that a positive statement can be made regarding the storage stability of the facade paint.

Claims

1. An aqueous formulation comprising at least one hydrophilic hydrophobizing agent and at least one water-soluble cationic polymer.

2. 2. The aqueous formulation of claim 1, wherein the cationic polymer has quaternary ammonium groups.

3. The aqueous formulation of claim 1 , wherein the cationic polymer comprises amino groups.

4. 4. The aqueous formulation of claim 2 or claim 3, wherein the cationic polymer is selected from poly(diallyldimethylammonium chloride), quaternized hydroxyethyl cellulose, and polyethyleneimine.

5. 5. The aqueous formulation according to any one of claims 1 to 4, wherein the weight average molecular weight of the water-soluble polymer is in the range of 10,000 g / mol to 2,000,000 g / mol, more preferably in the range of 20,000 g / mol to 1,000,000 g / mol, most preferably in the range of 30,000 g / mol to 500,000 g / mol.

6. 6. The aqueous formulation according to any one of claims 1 to 5, comprising from 0.05% to 5.0% by weight of said cationic polymer, preferably from 0.1% to 3.0% by weight, more preferably from 0.2% to 2.0% by weight of the formulation.

7. 7. The aqueous formulation according to any one of claims 1 to 6, wherein the hydrophobizing agent is an aqueous silicone resin emulsion, a silicone oil emulsion, an emulsion or microemulsion of an amino-functional silicone oil, a silane emulsion, or a mixture thereof.

8. Use of the aqueous formulation according to any one of claims 1 to 7 as an additive for producing an aqueous coating composition having initial rain resistance.

9. A coating composition comprising the aqueous formulation according to any one of claims 1 to 7.

10. 10. The coating composition of claim 9 which is an exterior basecoat, paint, primer or wood coating.

11. (a) first preparing an aqueous formulation comprising at least one hydrophobizing agent and at least one aqueous cationic polymer solution, the weight average molecular weight of which is in the range of 10,000 g / mol to 1,000,000 g / mol; (b) then adding at least one aqueous binder to the formulation obtained according to (a); (c) adding, if necessary, an emulsifier or mixture of emulsifiers, film-forming aids, pigments, fillers, thickeners, leveling agents, protective colloids, dispersants, wetting agents, preservatives and / or defoamers; A method for producing a coating composition having initial rain resistance.

12. 12. The method according to claim 11, wherein the weight percentage of binder relative to the weight of dry material in the coating composition is 1.0 to 50.0% by weight, preferably 3.0 to 25.0% by weight.

13. 13. The method of claim 11 or claim 12, wherein the aqueous formulation comprises from 0.05% to 5.0% by weight of the cationic polymer, preferably from 0.1% to 3.0% by weight, more preferably from 0.2% to 2.0% by weight of the formulation.

14. The method according to any one of claims 11 to 13, wherein the cationic polymer has quaternary ammonium groups or amino groups.

15. 15. The method of claim 14, wherein the cationic polymer is selected from poly(diallyldimethylammonium chloride), quaternized hydroxyethyl cellulose, and polyethyleneimine.

16. The method according to any one of claims 11 to 15, wherein the binder is an aqueous polymer dispersion based on homopolymers and / or copolymers.

17. The method of claim 16, wherein the homopolymers and copolymers comprise, as monomer units, at least one olefinically unsaturated monomer.

18. 18. The method according to claim 11, wherein, when an emulsifier or emulsifier mixture, film-forming aid, pigment, filler, thickener, leveling agent, protective colloid, dispersant, wetting agent, preservative and / or defoamer is used, the aqueous binder is added to the mixture as the last component.

Citation Information

Patent Citations

  • Method of applying a road marking composition

    EP0200249A1

  • Aqueous coating compositions

    EP0409459A2

  • Aqueous composition

    EP0594321A1

  • Water dilutable paint for road markings

    EP0721003A2

  • Aqueous paint composition

    EP0728822A2