Preparation and application of guanidyl ionic porous organic polymer for extracting gold from water

By developing guanidine-based ionic porous organic polymer materials, using their electrostatic interactions and structural design, the kinetics and selectivity problems of existing adsorbents when removing gold ions in water are solved, and efficient and reusable gold is achieved Ion capture and recovery.

CN119039545AActive Publication Date: 2024-11-29BEIJING UNIV OF CHEM TECH

Patent Information

Application Number
CN202411045798.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-29
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

When removing gold ions in water, existing adsorbents have problems such as slow adsorption kinetics, poor selectivity and poor recyclability, and poor water stability of metal organic frame materials may lead to secondary pollution.

Method used

The guanidine ionic porous organic polymer material was developed. By introducing guanidine groups into the skeleton, the cationic covalent organic frame material Ionic-COFs and the porous ionic polymer PiP-1 were designed, and its positive ionic covalent organic is used. The structure of the framework and porous ionic polymers efficiently captures gold ions through electrostatic interactions and optimizes their performance through anion exchange process.

Benefits of technology

Gold ion capture with high selectivity, high stability and rapid adsorption kinetics is achieved, and the material can be reused, suitable for gold recovery in waste electronic equipment, significantly improving the removal efficiency and recovery efficiency of gold ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

The invention discloses preparation and application of a guanidyl ionic porous organic polymer capable of extracting gold from water, and belongs to the related fields of porous organic polymer materials and the like. The preparation method comprises the following steps: reacting an ionic guanidine hydrochloride monomer serving as a basic organic connector with an aromatic ring substituted triazinyl derivative ligand (TFBT), and carrying out anion exchange to synthesize four guanidyl ionic covalent organic framework materials (Ionic-COF-X, X: Cl <->, Br <->, AcO <-> and SO4 < 2->) with different counter ions. An ionic guanidine hydrochloride monomer is taken as a basic organic connector to react with an aromatic ring substituted benzimidazole derivative ligand (BDBI) to obtain a guanidyl porous ionic polymer material (PiP-1), the guanidyl porous ionic polymer material (PiP-1) is respectively applied to adsorption and removal of gold ions in a solution, and the guanidyl porous ionic polymer material (PiP-1) has extremely high saturated adsorption capacity and can be used for adsorbing and removing gold ions in the solution. And the gold adsorption material shows rapid adsorption kinetics, high selectivity and recyclability, and has the potential of adsorbing gold in practical application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of porous organic polymer materials, and in particular relates to the preparation of a novel guanidine-based ion-type porous organic polymer material. The porous organic polymer can be used to adsorb and remove gold ions in water. Background Art

[0002] Gold (Au) is a precious metal with scarce reserves. Due to its excellent physical and chemical properties, it is widely used in electronic devices and catalysis. The separation of gold from ore is complicated and usually requires the use of highly toxic cyanide, which will cause serious environmental pollution and high energy consumption (Angew. Chem. Int. Ed. 2017, 56, 9331–9335). Recycling gold from discarded electronic devices can avoid a huge waste of resources and help protect the environment.

[0003] Traditional pyrometallurgy has high energy consumption and serious pollution. It is relatively simple to recover gold from discarded electronic equipment by hydrometallurgy. First, the gold in the electronic equipment is leached into Au (III) ions using acid or alkali, and then separated and purified by coprecipitation, solvent extraction, ion exchange and adsorption. Among them, coprecipitation and solvent extraction are prone to secondary pollution, ion exchange is complicated and costly, and adsorption is simple to operate and low in cost, and is widely used in the field of precious metal recovery. At present, many adsorbents such as activated carbon and ion exchange resins have been developed. However, these adsorbents have problems such as slow adsorption kinetics, poor selectivity, and poor recyclability (Macromol.Mater.Eng.2022,307,2100761). Metal organic framework materials (MOFs) are also used as adsorbents, but their water stability is poor and metal ions may be leached to cause secondary pollution (Angew.Chem.Int.Ed.2024,e202402205). Therefore, the development of new adsorbents with high selectivity, high stability and fast adsorption kinetics is of great significance for the removal of gold from wastewater.

[0004] Porous organic polymers (POPs) are organic materials with regular pore structures formed by covalent bonds of light elements such as C, H, O, N, and S. They have good stability and strong designability, and are widely used in adsorption separation, sensing, semiconductors, catalysis, and other fields. Ionic covalent organic frameworks (iCOFs) and porous ionic polymers (PiPs) are important branches of POPs. Their positive / negative charges are fixed on the framework, and they capture target ions through electrostatic interactions. Adjusting their counterions can change their specific surface area, pore structure, and internal environment of the pores. They have high designability, making them widely used in precious metal recovery, pollutant adsorption and removal, and other fields.

[0005] However, there are few reports on the application of iCOFs and PiPs materials in capturing gold ions. The three nitrogen atoms of guanidine are combined with the central carbon atom of the cation, thus having a positive delocalized charge and a strong ability to bind anions. By introducing guanidine groups into the framework, its ability to capture Au can be effectively enhanced. To this end, we used ionic guanidine hydrochloride as an organic linker and utilized its charged active N + site, synthesized two types of guanidine-based ionic porous organic polymer materials, namely the cationic covalent organic framework material Ionic-COFs and the porous ionic polymer PiP-1. Ionic-COFs exhibit extremely high gold adsorption capacity, fast adsorption kinetics, excellent selectivity and reusability, and can successfully and efficiently recover gold from CPU. This work shows that Ionic-COFs can be used as a useful platform for high-performance gold recovery. Compared with Ionic-COFs, the PiP-1 material skeleton has a higher charge density and therefore has a higher adsorption capacity. To date, there have been few reports on the application of PiPs materials in gold ion capture. This invention provides new ideas for the application of PiPs materials in the field of gold recovery.

[0006] At present, there are no research reports or patent disclosures at home and abroad on the application of guanidine-based ionic porous organic polymer materials in the adsorption and removal of gold ions in wastewater. Summary of the invention

[0007] The first object of the present invention is to provide a method for synthesizing a guanidine-based ion-type porous organic polymer material. The porous organic polymer material can be a covalent organic framework material with high crystallinity or a porous polymer material with an amorphous structure;

[0008] The second object of the present invention is to provide an application of the guanidine-based ionic porous organic polymer material for removing gold from water by adsorption.

[0009] To achieve the above purpose, the technical solution adopted by the present invention specifically includes the following contents:

[0010] The first aspect of the present invention provides a method for preparing a guanidine-based ionic covalent organic framework material, comprising the following steps:

[0011] (1) The aromatic ring-substituted triazine derivative ligand TFBT and triaminoguanidine hydrochloride TG Cl The reaction components are placed in a Pyrex tube, and a solvent is added to mix evenly by ultrasonication. Then, an AcOH aqueous solution is added as a catalyst, and mixed evenly by ultrasonication. The mixture is then frozen-vacuumed-thawed for three cycles and sealed under a nitrogen atmosphere. After returning to room temperature, the mixture is heated to react completely under sealed conditions. The product is washed with organic solvents such as dichloromethane, 1,4-dioxane and tetrahydrofuran, and then Soxhlet extracted with tetrahydrofuran overnight. Finally, the crude product is dried overnight in vacuum to obtain Ionic-COF-Cl.

[0012] Or (2) dispersing the above-obtained Ionic-COF-Cl in a saturated solution of anionic sodium salt (NaBr, Na2SO4 and CH3COONa, etc.), heating and stirring to exchange Cl ions with corresponding different anions, repeating this anion exchange process three times, filtering to obtain a powdered solid, washing with deionized water and anhydrous ethanol, and vacuum drying overnight to obtain a guanidine-based ionic covalent organic framework material with different anion exchanges; that is, finally obtaining Inoic-COF-X, where X is an anion, such as an anion selected from Cl, Br, SO4 and AcO.

[0013] Further, in step (1), TFBT and TG Cl The molar ratio is: 1:1.

[0014] Furthermore, in step (1), the solvent is a mixed solvent of N,N-dimethylacetamide and o-dichlorobenzene.

[0015] Furthermore, in the step (1), the solvent is a mixed solvent of N,N-dimethylacetamide and o-dichlorobenzene in a volume ratio of 1-9:9-1 (preferably 1:1).

[0016] Furthermore, in step (1), the concentration of the AcOH aqueous solution is 3 mol / L to 12 mol / L, preferably 6 mol / L.

[0017] Furthermore, in the step (1), the ultrasonic time is 1 to 30 minutes, and the freeze-vacuum-thaw cycle method is: freezing the reactants with liquid nitrogen, evacuating the air, and thawing them with nitrogen.

[0018] Furthermore, in the step (1), the temperature of the temperature-raising reaction is between 40 and 200° C., and the reaction time is between 1 and 10 days.

[0019] Furthermore, in the step (2), the heating temperature is 20-120°C.

[0020] Furthermore, in the step (2), the stirring time is 1-10 hours.

[0021] The synthetic route of the present invention is as follows:

[0022]

[0023] The aromatic ring substituted triazine derivative ligand (TFBT) has the structural formula:

[0024] in represents an aromatic ring, an aromatic heterocyclic ring such as O / S / Se / N, wherein the aromatic ring is benzene, biphenyl, naphthalene, anthracene, phenanthrene, etc.;

[0025] like Selected from wait.

[0026] The substituent X on Inoic-COF-X can be Br, AcO, SO4 or other anions.

[0027] The second aspect of the present invention provides a study on the adsorption thermodynamics, kinetics, selectivity and cyclic regeneration of gold by the product Ionic-COF-Cl obtained in the above step (1), comprising the following steps:

[0028] Weigh an appropriate amount of tetrachloroauric acid trihydrate (HAuCl4·H2O), add an appropriate amount of deionized water to dissolve, and prepare tetrachloroauric acid aqueous solutions with different Au(III) concentrations. The exact initial concentration C0 of Au(III) in the prepared solution is determined by inductively coupled plasma optical emission spectroscopy (ICP-OES).

[0029] ① Adsorption thermodynamics: Take the same volume of tetrachloroauric acid aqueous solution containing different initial concentrations of Au(Ⅲ) and place it in a bottle, add the same mass of Ionic-COF-Cl material as Au(Ⅲ) adsorbent, add magnetic particles and stir at room temperature. After the adsorption reaches equilibrium, let it stand, extract the supernatant with a syringe, filter the mixture with a disposable needle filter, and then determine the concentration of Au(Ⅲ) in the solution after adsorption equilibrium by ICP-OES. e Calculate the equilibrium adsorption amount q of Ionic-COF-Cl at each concentration e .

[0030] ② Adsorption kinetics: Take an appropriate amount of tetrachloroauric acid aqueous solution containing a certain initial Au(Ⅲ) concentration, add an appropriate amount of Ionic-COF-Cl as an Au(Ⅲ) adsorbent, add a magnetic particle and stir at room temperature. Draw the mixture with a syringe at a certain interval, filter it with a disposable needle filter, and then measure the Au(Ⅲ) concentration C in the solution at that time by ICP-OES. t Calculate the removal rate R of Au(Ⅲ) at each time e (%).

[0031] ③ Adsorption selectivity: First, a mixed solution containing Au(III) and several competing metal ions such as Cu(II), Co(II), Na(I), Mg(II), K(I), Fe(III), Al(III), Ni(II), Zn(II), etc. was prepared. The initial concentrations of all metal ions were the same, and the accurate concentrations were determined by ICP-OES. Take an appropriate amount of Ionic-COF-Cl as an adsorbent and add it to the above solution. After adding a magnetic particle, mix and stir at room temperature. After the adsorption reaches equilibrium, let it stand, extract the supernatant with a syringe, filter the mixed solution with a disposable needle filter based on water, and then determine the concentrations of Au(III) and several other competing metal ions in the solution after adsorption equilibrium by ICP-OES and calculate the removal rate R e (%).

[0032] ④ Cyclic regeneration: Take an appropriate amount of aqueous solution of tetrachloroauric acid containing a certain initial Au(Ⅲ) concentration, add an appropriate amount of Ionic-COF-Cl as an Au(Ⅲ) adsorbent, add a magnetic particle and mix and stir at room temperature, filter with a water-based disposable needle filter, and determine the Au(Ⅲ) in the solution after adsorption equilibrium by ICP-OES. Collect the adsorbent, wash with deionized water, mix the collected solid with a solution containing thiourea (1M) and HCl (1M), add a magnetic particle and mix and stir at room temperature, filter and wash with anhydrous ethanol, and finally vacuum dry to obtain a regenerated adsorbent. The regenerated Ionic-COF-Cl is used for the next cycle of adsorption. Calculate the removal rate R of Ionic-COF-Cl for Au(Ⅲ) e (%).

[0033] Furthermore, in step ④, the volume ratio of thiourea to HCl is 1-9:9-1 (preferably 1:1).

[0034] The third aspect of the present invention provides the use of the product Ionic-COF-Cl obtained in step (1) above in the adsorption and removal of Au in electronic waste liquid, comprising the following steps:

[0035] First, cut the gold end slices of the discarded printed circuit board and soak them in aqua regia. Then, dilute the leachate with deionized water and NaOH solution to acidity, filter the diluted leachate, remove the circuit board residue and take a sample, and determine the metal ion concentration in the filtrate by ICP-OES. Add an appropriate amount of Ionic-COF-Cl to the filtrate, add a magnetic particle and mix at room temperature, filter with a disposable needle filter, and determine the metal concentration in the solution after adsorption equilibrium by ICP-OES and calculate the removal rate of metal ions by Ionic-COF-Cl R e (%).

[0036] Further, the leachate is diluted to pH=1-6, preferably 2.

[0037] A fourth aspect of the present invention provides a method for preparing a guanidine-based porous ionic polymer material, comprising the following steps:

[0038] (1) The aromatic ring-substituted benzimidazole derivative ligand (BDBI) and triaminoguanidine hydrochloride (TG Cl ) as a reactant is placed in a Pyrex tube, wherein the substituted aromatic ring is selected from benzene ring, furan, thiophene, selenophene, pyridine and other aromatic heterocyclic rings; a solvent is added for ultrasonic mixing, and then an AcOH aqueous solution is added as a catalyst, ultrasonic mixing is uniform, and then freeze-vacuum-thaw cycles are performed three times, and the tube is sealed under a nitrogen atmosphere. After returning to room temperature, the temperature is raised under sealed conditions to react completely. The product is washed with organic solvents such as dichloromethane, 1,4-dioxane and tetrahydrofuran, and then Soxhlet extraction is performed overnight with a solvent such as tetrahydrofuran, and finally vacuum dried overnight to obtain a crude product, which is recorded as PiP-1.

[0039] Further, in step (1), BDBI and TG Cl The molar ratio is: 1.5:1.

[0040] Furthermore, in step (1), the solvent is a mixed solvent of N,N-dimethylacetamide and mesitylene.

[0041] Furthermore, in the step (1), the solvent is a mixed solvent of N,N-dimethylacetamide and mesitylene in a volume ratio of 1 to 9:9 to 1 (preferably 1:1).

[0042] Furthermore, in step (1), the concentration of the AcOH aqueous solution is 3 mol / L to 12 mol / L, preferably 6 mol / L.

[0043] Furthermore, in the step (1), the ultrasonic time is 1 to 30 minutes, and the freeze-vacuum-thaw cycle method is: freezing the reactants with liquid nitrogen, evacuating the air, and thawing them with nitrogen.

[0044] Furthermore, in the step (1), the temperature of the temperature-raising reaction is between 40 and 200° C., and the reaction time is between 1 and 10 days.

[0045] The synthetic route of the present invention is as follows:

[0046]

[0047] The aromatic ring substituted benzimidazole derivative ligand (BDBI) has the structural formula:

[0048] in represents an aromatic ring, an aromatic heterocyclic ring such as O / S / Se / N, wherein the aromatic ring is benzene, biphenyl, naphthalene, anthracene, phenanthrene, etc.;

[0049] like Selected from wait.

[0050] The substituent X on PiP-1 can be F, Cl, Br, I or other anions.

[0051] The fifth aspect of the present invention provides a study on the adsorption thermodynamics, kinetics, selectivity and cyclic regeneration of gold by the product PiP-1 obtained in the above step (1), comprising the following steps:

[0052] (1) Adsorption thermodynamics: Take the same volume of aqueous solution of tetrachloroauric acid containing different initial concentrations of Au(III) and place it in a bottle. Add the same mass of PiP-1 material as Au(III) adsorbent, add a magnetic particle and stir at room temperature. After the adsorption reaches equilibrium, let it stand, extract the supernatant with a syringe, filter the mixture with a disposable needle filter, and then measure the concentration of Au(III) in the solution after adsorption equilibrium by ICP-OES. e Calculate the equilibrium adsorption amount (q e ).

[0053] (2) Adsorption kinetics: Take an appropriate amount of aqueous solution of tetrachloroauric acid containing a certain initial Au(III) concentration, add an appropriate amount of PiP-1 as an Au(III) adsorbent, add a magnetic particle and stir at room temperature. Draw out the mixture with a syringe at regular intervals, filter it with a disposable needle filter, and then measure the Au(III) concentration C in the solution at that time by ICP-OES. t Calculate the removal rate R of Au(Ⅲ) at each time e (%).

[0054] (3) Adsorption selectivity: First, a mixed solution containing Au(III) and several competing metal ions such as Cu(II), Co(II), Na(I), Mg(II), K(I), Fe(III), Al(III), Ni(II), Zn(II), etc. was prepared. The initial concentrations of all metal ions were the same, and the exact concentrations were determined by ICP-OES. Take an appropriate amount of PiP-1 as an adsorbent and add it to the above solution. After adding a magnetic particle, mix and stir at room temperature. After the adsorption reaches equilibrium, let it stand, extract the supernatant with a syringe, filter the mixed solution with a disposable needle filter based on water, and then determine the concentrations of Au(III) and several other competing metal ions in the solution after adsorption equilibrium by ICP-OES and calculate the removal rate R e (%).

[0055] (4) Recyclability: Take an appropriate amount of aqueous solution of tetrachloroauric acid containing a certain initial Au(III) concentration, add an appropriate amount of PiP-1 as an Au(III) adsorbent, add a magnetic particle and mix and stir at room temperature, filter with a water-based disposable needle filter, and determine the Au(III) in the solution after adsorption equilibrium by ICP-OES. Collect the adsorbent, wash with deionized water, mix the collected solid with a solution containing thiourea (1M) and HCl (1M), add a magnetic particle and mix and stir at room temperature, filter and wash with anhydrous ethanol, and finally vacuum dry to obtain a regenerated adsorbent. The regenerated PiP-1 is used for the next cycle of adsorption. Calculate the removal rate R of PiP-1 for Au(III) e (%).

[0056] Furthermore, in step (4), the volume ratio of thiourea to HCl is 1-9:9-1 (preferably 1:1).

[0057] The advantages of the present invention are:

[0058] 1) The present invention designs and synthesizes a series of ionic covalent organic framework materials Ionic-COF-X (X = Cl, Br, SO4 and AcO) with different anions, and studies the effects of different counter anions on the adsorption of gold.

[0059] 2) The saturated adsorption capacity of Ionic-COF-Cl prepared by the present invention for gold is as high as 1270.76 mg g -1 , and exhibited fast adsorption kinetics, high selectivity, and recyclability.

[0060] 3) The Ionic-COF-Cl prepared in the present invention can be applied to the recovery of gold from waste circuit boards, indicating that it can achieve effective recovery of gold in practical applications.

[0061] 4) The saturated adsorption capacity of the porous ionic polymer PiP-1 prepared by the present invention is as high as 1530.9 mg g-1 , and exhibits rapid adsorption kinetics, high selectivity and recyclability. The present invention lays an important foundation for the application of PiPs materials in the field of gold recovery. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 The powder X-ray diffraction pattern of the guanidine-based ionic covalent organic framework material (Ionic-COF-Cl) prepared in Example 1;

[0063] Figure 2 The infrared (FTIR) spectrum of the guanidine-based ionic covalent organic framework material (Ionic-COF-Cl) prepared in Example 1;

[0064] Figure 3 The X-ray photoelectron spectroscopy (XPS) spectrum of the guanidine-based ionic covalent organic framework material (Ionic-COF-Cl) prepared in Example 1;

[0065] Figure 4 The guanidine-based ionic covalent organic framework material (Ionic-COF-Cl) prepared in Example 1 13 C solid-state NMR spectrum;

[0066] Figure 5 This is a scanning electron microscope (SEM) image of the guanidine-based ionic covalent organic framework material (Ionic-COF-Cl) prepared in Example 1;

[0067] Figure 6 This is a transmission electron microscope (TEM) image of the guanidine-based ionic covalent organic framework material (Ionic-COF-Cl) prepared in Example 1;

[0068] Figure 7 Thermogravimetric analysis (TGA) curve of the guanidine-based ionic covalent organic framework material (Ionic-COF-Cl) prepared in Example 1;

[0069] Figure 8 The nitrogen adsorption-desorption curve and pore size distribution diagram of the guanidine-based ionic covalent organic framework material (Ionic-COF-Cl) prepared in Example 1;

[0070] Fig. 9 The powder X-ray diffraction pattern of the guanidine-based ionic covalent organic framework material Ionic-COF-X (X = Cl, Br, SO4 and AcO) prepared in Example 1 and Example 2;

[0071] Fig.10 The infrared (FTIR) spectra of the guanidine-based ionic covalent organic framework materials Ionic-COF-X (X = Cl, Br, SO4 and AcO) prepared in Examples 1 and 2;

[0072] Fig.11 The nitrogen adsorption-desorption curves and pore size distribution diagrams of the guanidine-based ionic covalent organic framework materials Ionic-COF-X (X = Cl, Br, SO4 and AcO) prepared in Examples 1 and 2;

[0073] Fig.12 The adsorption isotherms of Au(III) for the guanidine-based ionic covalent organic framework materials Ionic-COF-X (X = Cl, Br, SO4 and AcO) prepared in Examples 1 and 2;

[0074] Fig.13 The powder X-ray diffraction pattern of the guanidine-based ionic covalent organic framework material (Ionic-COF-Cl) prepared in Example 1 before and after the adsorption of gold;

[0075] Fig.14 This is a TEM image of the guanidine-based ionic covalent organic framework material (Ionic-COF-Cl) prepared in Example 1 after capturing gold;

[0076] Fig.15 The XPS total spectrum of the guanidine-based ionic covalent organic framework material (Ionic-COF-Cl) prepared in Example 1 before and after capturing gold, and the XPS high-resolution spectrum of Au 4f;

[0077] Fig.16 The adsorption isotherm of Au(III) on the guanidine-based ionic covalent organic framework material (Ionic-COF-Cl) prepared in Example 1;

[0078] Fig.17 The adsorption kinetic curve of Au(III) by the guanidine-based ionic covalent organic framework material (Ionic-COF-Cl) prepared in Example 1;

[0079] Fig.18 The adsorption selectivity of the guanidine-based ionic covalent organic framework material (Ionic-COF-Cl) prepared in Example 1 for Au (III);

[0080] Fig.19 The adsorption cyclic regeneration of Au(III) by the guanidine-based ionic covalent organic framework material (Ionic-COF-Cl) prepared in Example 1;

[0081] Fig. 20 The practical application of the guanidine-based ionic covalent organic framework material (Ionic-COF-Cl) prepared in Example 1 in the recovery of gold from electronic waste;

[0082] Fig.21This is the infrared (FTIR) spectrum of the guanidine-based porous ionic polymer material PiP-1 prepared in Example 4;

[0083] Fig. 22 The guanidine-based porous ionic polymer material PiP-1 prepared in Example 4 13 C solid-state NMR spectrum;

[0084] Fig.23 The powder X-ray diffraction pattern of the guanidine-based porous ionomer material PiP-1 prepared in Example 4;

[0085] Fig.24 This is a scanning electron microscope (SEM) image of the guanidine-based porous ionomer material PiP-1 prepared in Example 4;

[0086] Fig.25 This is a transmission electron microscope (TEM) image of the guanidine-based porous ionomer material PiP-1 prepared in Example 4;

[0087] Fig.26 This is a thermogravimetric analysis (TGA) curve of the guanidine-based porous ionomer material PiP-1 prepared in Example 4;

[0088] Fig. 27 The nitrogen adsorption-desorption curve and pore size distribution diagram of the guanidine-based porous ionic polymer material PiP-1 prepared in Example 4;

[0089] Fig.28 This is a transmission electron microscope (TEM) image of the guanidine-based porous ionic polymer material PiP-1 prepared in Example 4 after gold adsorption;

[0090] Fig.29 The XPS total spectrum of the guanidine-based porous ionic polymer material PiP-1 prepared in Example 4 before and after capturing gold, and the XPS high-resolution spectrum of Au 4f;

[0091] Fig.30 The adsorption isotherm of Au(III) by the guanidine-based porous ionic polymer material PiP-1 prepared in Example 4;

[0092] Fig.31 The adsorption kinetics curve of Au(III) by the guanidine-based porous ionic polymer material PiP-1 prepared in Example 4;

[0093] Fig.32 The adsorption selectivity of the guanidine-based porous ionic polymer material PiP-1 prepared in Example 4 to Au(III);

[0094] Fig.33 The adsorption cyclic regeneration property of Au(III) by the guanidine-based porous ionic polymer material PiP-1 prepared in Example 4. DETAILED DESCRIPTION

[0095] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0096] Example 1

[0097] The preparation method of the guanidine-based ionic covalent organic framework material (labeled as Ionic-COF-Cl) synthesized by the TFBT ligand containing biphenyl is as follows:

[0098] 2,4,6-tris-(4-formyl-biphenyl-4-yl)-1,3,5-triazine (0.03 mmol) and triaminoguanidine hydrochloride (TG Cl ) (0.03mmol) was placed in a Pyrex tube (10mL) as a reaction component, and N,N-dimethylacetamide / o-dichlorobenzene (DMAc / o-DCB, v / v=1:1, 1.0mL in total) was added as a solvent. After ultrasonication for 10 minutes, 6M AcOH (0.1mL) was added as a catalyst, and ultrasonication was continued for 5 minutes. Then, the Pyrex tube was placed in liquid nitrogen for rapid freezing while nitrogen was passed through it, and the tube was thawed in a nitrogen atmosphere after the vacuum pump was evacuated for two minutes. After the above three cycles of freezing-evacuation-thawing, the air in the Pyrex tube was completely removed and it was sealed under a nitrogen atmosphere. After returning to room temperature, it was transferred to a vacuum drying oven and heated at 120°C to 150°C for reaction for 3 to 7 days, avoiding disturbance during the period. After the reaction is completed, the mixture in the Pyrex tube is filtered with filter paper, washed with dichloromethane, 1,4-dioxane and tetrahydrofuran in sequence, and then subjected to Soxhlet extraction with tetrahydrofuran for 12 to 48 hours. Finally, the mixture is dried in an oven to obtain a final product as a yellow solid.

[0099] Figure 1 The XRD pattern of Ionic-COF-Cl shows that Ionic-COF-Cl has high crystallinity and regular crystal structure, and the stacking mode of Ionic-COF-Cl is determined to be AB stacking. Figure 2 The infrared spectrum of Ionic-COF-Cl is given. Figure 3 The XPS spectra and Figure 4 The solid state NMR carbon spectrum given proves the successful formation of the C=N bond and the successful construction of the organic unit. Figure 5 The SEM images showed that Ionic-COF-Cl was in the form of nanofibers. Figure 6 TEM images show that their uniform diameter is about 100 nm and their surface is rough and scaly. Figure 7 The TGA curves show that Ionic-COF-Cl has good thermal stability. Figure 8 The nitrogen adsorption-desorption curve shows that the specific surface area of ​​ion-COF-Cl is 452.9 m 2 g -1 The main pore size distribution is around 1.18nm, which is a microporous material.

[0100] Example 2

[0101] The products synthesized by anion exchange process using the biphenyl-containing guanidine-based ionic covalent organic framework material (Ionic-COF-Cl) in Example 1 were labeled as Ionic-COF-Br, Ionic-COF-SO4 and Ionic-COF-AcO.

[0102] Here are the steps:

[0103] 100 mg of Ionic-COF-Cl was dispersed in 10 mL of saturated solution of the corresponding sodium salt (NaBr, Na2SO4 and CH3COONa), and the mixture was heated and stirred at 60°C for 5 hours. After this anion exchange process was repeated three times, a yellow powdery solid was obtained by filtration, washed with deionized water and anhydrous ethanol, and dried in vacuum at 100°C overnight to obtain Ionic-COF-Br, Ionic-COF-SO4 and Ionic-COF-AcO, respectively.

[0104] Fig. 9 It is shown that the differences in the diffraction patterns and positions of Ionic-COF-Br, Ionic-COF-AcO, and Ionic-COF-SO4 are negligible compared to Ionic-COF-Cl. Fig.10 The FTIR spectra showed that the characteristic peaks of Ionic-COFs before and after anion exchange remained almost unchanged in position and intensity. Fig.11 The BET surface areas of Ionic-COF-Cl, Ionic-COF-Br, Ionic-COF-AcO, and Ionic-COF-SO4 are 452.9, 507.5, 394.5, and 372.6 m 2 g -1 , with microporous characteristics.

[0105] Example 3

[0106] The adsorption performance of Au(III) was tested using the Ionic-COF-X (X = Cl, Br, SO4 and AcO) in the above Examples 1 and 2.

[0107] Fig.12The maximum adsorption capacity of Au(III) for Ionic-COF-Br, Ionic-COF-AcO and Ionic-COF-SO4 after anion exchange was 793.7 mg g -1 , 694.4mg g -1 and 757.6 mg g -1 . Fig.13 The XRD patterns of Ionic-COF-Cl before and after adsorption of Au(III) are given. Diffraction peaks corresponding to the gold (111), (200), (220) and (311) crystal planes appear at 38.2°, 44.4°, 64.6° and 77.6°, indicating that Ionic-COF-Cl can successfully capture gold ions and reduce them to zero-valent gold. Fig.14 The TEM image shows that the gold nanoparticles are evenly dispersed on the Ionic-COF-Cl material. Fig.15 The characteristic peak of Au 4f appears in the spectrum after adsorption, indicating that gold has been successfully captured by Ionic-COF-Cl. The intensity of the characteristic peak of zero-valent gold in the XPS high-resolution spectrum of Au 4f is significantly higher than that of Au(III), indicating that most of the gold ions captured by Ionic-COF-Cl are reduced to gold. Fig.16 The maximum adsorption capacity q of Ionic-COF-Cl for gold was calculated based on the adsorption thermodynamic results. max 1270.8 mg g -1 , better than most materials. Fig.17 It was shown that Ionic-COF-Cl reached adsorption equilibrium in less than 20 min and the removal efficiency was about 98% after 40 min, indicating that Ionic-COF-Cl can effectively remove AuCl4 from aqueous solution. - ion. Fig.18 It is shown that Ionic-COF-Cl still has excellent selectivity for Au(III) in the presence of various interfering metal ions. Fig.19 It was shown that the recovery rate of Ionic-COF-Cl in five cycles was above 95%, indicating that it has good regeneration and reuse as a gold adsorbent material. Fig. 20 It is shown that Ionic-COF-Cl has a gold removal efficiency higher than 99% in the leachate of discarded circuit boards, making it a useful material for recovering gold from real electronic waste.

[0108] Example 4

[0109] The preparation method of the guanidine-based porous ionic polymer material (labeled as PiP-1) synthesized from the BDBI ligand containing a benzene ring as described above, the synthesis steps are as follows:

[0110] 4,7-bis(4-formylphenyl)-1,3-dimethyl-1H-benzo[d]imidazol-3-ium bromide (0.0375 mmol) and triaminoguanidine hydrochloride (TG Cl ) (0.025mmol) was placed in a 10mL Pyrex tube as a reactant, N,N-dimethylacetamide / mesitylene (DMAc / mesitylene, v / v=1:1, 1.0mL in total) was added as a solvent, the mixture was ultrasonicated for 10 minutes, and 6M AcOH solution (0.1mL) was added as a catalyst, and ultrasonicated again for 5 minutes. Then, the Pyrex tube was placed in liquid nitrogen for rapid freezing during the process of passing nitrogen gas, and the tube was thawed in a nitrogen atmosphere after the vacuum pump was evacuated for two minutes. After the above three cycles of freezing-evacuating-thawing, the air in the Pyrex tube was completely removed, and it was tightened and sealed under a nitrogen atmosphere. After the reaction tube returned to room temperature, it was transferred to a vacuum drying oven and heated at 120°C to 150°C for reaction for 3 to 7 days, avoiding disturbance during the period. After the reaction is completed, the mixture in the Pyrex tube is filtered with filter paper, washed with dichloromethane, 1,4-dioxane and tetrahydrofuran in sequence, and then Soxhlet extraction is performed with tetrahydrofuran for 12 to 48 hours, and finally dried in an oven to obtain the final product as a yellow solid. Fig.21 The infrared spectrum of PiP-1 is given. Fig. 22 The solid-state NMR carbon spectrum given proves that the PiP-1 material was successfully connected and formed through imine bonds. Fig.23 The XRD pattern shows no sharp peaks in the 2-40° test range, indicating that the PiP-1 material does not have a crystalline structure. Fig.24 SEM images and Fig.25 The TEM images show that the PiP-1 material has uniform morphology and even distribution, and is stacked in the form of spherical particles. Fig.26 The TGA curve shows that PiP-1 material has good thermal stability. Fig. 27 The BET specific surface area of ​​PiP-1 is 80.4 m 2 g -1 The pore size is mainly distributed at 1.36nm, which is a typical microporous material.

[0111] Example 5

[0112] The PiP-1 in the above-mentioned Example 4 was used to test the adsorption performance of Au(III).

[0113] Fig.28 TEM images show that gold nanoparticles are uniformly dispersed on the PiP-1 material. Fig.29A new peak corresponding to Au appeared in the XPS spectrum, indicating that Au had been adsorbed around the skeleton of PiP-1. In addition, the XPS spectrum of Au 4f showed that the gold adsorbed by PiP-1 mainly existed in the form of Au(0) and Au(Ⅲ), which once again proved the reduction effect of PiP-1 on Au(Ⅲ). Fig.30 The results of adsorption thermodynamic experiments show that the maximum saturation adsorption capacity of PiP-1 for gold is q max 1519.7 mg g -1 , which is superior to most of the porous materials reported so far. Fig.31 It was shown that the gold removal efficiency of PiP-1 gradually reached equilibrium within thirty minutes, and the final gold removal efficiency was higher than 99%, indicating that it is a highly potential gold adsorbent. Fig.32 The results show that the removal efficiency of Au(III) by PiP-1 is much higher than that of other competing metal ions, indicating that the presence of competing metal ions has little effect on the specific capture of gold by PiP-1. Fig.33 It shows that after five cycles, the gold recovery rate of PiP-1 is above 99%, indicating that it has good regeneration and recycling properties.

[0114] The above embodiments are merely examples for clearly illustrating the present invention, and should not be construed as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be varied. All variations made within the scope of protection of the independent claims of the present invention are within the scope of protection of the present invention.

Claims

1. A method for preparing a guanidine-based ionic porous organic polymer material, characterized in that: The following steps are involved: (1) Triaminoguanidine hydrochloride TG Cl The aromatic ring-substituted triazine derivative ligand TFBT is added to the solvent and ultrasonically dispersed uniformly, and then an AcOH aqueous solution is added as a catalyst and ultrasonically mixed uniformly, and then subjected to a freeze-vacuum-thaw cycle, the temperature is raised under a sealed condition to react completely, and the product is filtered, washed, purified by extraction, and vacuum dried to obtain a guanidine-based ionic covalent organic framework material Ionic-COF-Cl with high crystallinity; or (2) dispersing the above-obtained Ionic-COF-Cl in a saturated solution of anionic sodium salt NaX, heating and stirring to exchange Cl ions with corresponding different anions, repeating this anion exchange process three times, filtering to obtain a powdered solid, washing with deionized water and anhydrous ethanol, and vacuum drying overnight to obtain a guanidine-based ionic covalent organic framework material with different anion exchanges; that is, finally obtaining Inoic-COF-X, where X is an anion such as Cl, Br, SO4, and AcO; The aromatic ring substituted triazine derivative ligand (TFBT) has the structural formula: in represents an aromatic ring, an aromatic heterocyclic ring such as O / S / Se / N, wherein the aromatic ring is benzene, biphenyl, naphthalene, anthracene, phenanthrene, etc.; 2. A method for preparing a guanidine-based ionic porous organic polymer material, characterized in that: The following steps are involved: Triaminoguanidine hydrochloride TG Cl and the aromatic ring-substituted benzimidazole derivative ligand BDBI are added to the solvent for ultrasonic dispersion, and then an AcOH aqueous solution is added as a catalyst for ultrasonic mixing, and then subjected to a freeze-vacuum-thaw cycle, the temperature is raised under a sealed condition to react completely, and the product is filtered, washed, purified by extraction, and vacuum dried to obtain a guanidine-based porous ionic polymer material PiP-1; The aromatic ring substituted benzimidazole derivative ligand (BDBI) has the structural formula: in represents an aromatic ring, an aromatic heterocyclic ring such as O / S / Se / N, wherein the aromatic ring is benzene, biphenyl, naphthalene, anthracene, phenanthrene, etc.; The substituent X on PiP-1 is a different anion, such as F, Cl, Br, I or other anions.

3. The method according to claim 1, characterized in that: Triaminoguanidine hydrochloride (TG Cl ) is a linker, and the structural formula of the guanidine-based ionic covalent organic framework material is as follows: in represents an aromatic ring, an aromatic heterocyclic ring such as O / S / Se / N, wherein the aromatic ring is benzene, biphenyl, naphthalene, anthracene, phenanthrene, etc.; Substituent X is Cl - Br - ,AcO - 、SO4 2- Anions.

4. The method according to claim 2, characterized in that: Triaminoguanidine hydrochloride TG Cl is a connector, and the structural formula of the guanidine-based porous ionic polymer material is as follows: in represents an aromatic ring, an aromatic heterocyclic ring such as O / S / Se / N, wherein the aromatic ring is benzene, biphenyl, naphthalene, anthracene, phenanthrene, etc.; Substituent X is Cl - Br - ,AcO - 、SO4 2- Anions.

5. The method according to claim 1 or 2, characterized in that: Triaminoguanidine hydrochloride TG Cl The molar ratio of the aromatic ring substituted triazine derivative ligand TFBT is 1 to 10:1, preferably 1:1; Triaminoguanidine hydrochloride TG Cl The molar ratio of the aromatic ring substituted benzimidazole derivative ligand BDBI is 1 to 10:1, preferably 2:3; The reaction solvent is a mixed solvent of N,N-dimethylacetamide and o-dichlorobenzene, and the volume ratio of N,N-dimethylacetamide to o-dichlorobenzene is 1-9:9-1 (preferably 1:1); The concentration of the added AcOH solution is 3 mol / L to 12 mol / L, preferably 6 mol / L.

6. The method according to claim 1 or 2, characterized in that: In the step (1), the ultrasonic time is 1 to 30 minutes, and the freeze-vacuum-thaw cycle method is: the reactants are frozen with liquid nitrogen, vacuumed, and thawed by nitrogen; the sealed reaction conditions are under nitrogen atmosphere or vacuum conditions.

7. The method according to claim 1 or 2, characterized in that: The temperature of the reaction is 40 to 200° C., and the reaction time is 1 to 10 days.

8. The method according to claim 1 or 2, characterized in that: After filtering, washing is performed with dichloromethane, 1,4-dioxane and tetrahydrofuran in sequence, and then Soxhlet extraction is performed with an organic solvent for 1 to 5 days. Finally, vacuum drying is performed to obtain a guanidine-based ionic covalent organic framework material.

9. The guanidine-based ionic porous organic polymer material obtained according to the method of claim 1 or 2.

10. Use of the guanidine-based ionic porous organic polymer material obtained by the method according to claim 1 or 2 for adsorbing and removing gold ions in a solution, or for separating gold ions from a variety of metal ions.

11. The use according to claim 10, characterized in that: The guanidine-based ionic porous organic polymer material is added into a solution containing Au(III), mixed and stirred to adsorb the gold ions therein.

Citation Information

Patent Citations

  • Nonazide gas generating compositions

    CA2242614A1

  • Guanidine collector for reinforcing floatation recovery of gold and silver in high alkali environment

    CN101816982A

  • Preparation method of cation covalent organic framework and application of cation covalent organic framework in adsorbing gold

    CN115197382A

  • Ionic covalent organic framework with guanidine salt and nitrogen-rich sites, preparation method of ionic covalent organic framework and application of ionic covalent organic framework in adsorption of bivalent copper in wastewater

    CN115785363A

  • Room-temperature ionic liquid for separating gold as well as preparation method and application of room-temperature ionic liquid

    CN117924120A

Cited By

  • Thiourea-based aromatic porous organic polymer as well as preparation method and application thereof

    CN119823340A

  • A thioureido-based aromatic porous organic polymer and a preparation method and application thereof

    CN119823340B