Electrolyte material and methods of formation
Halide-based solid electrolytes with controlled impurity phases and optimized structures address the limitations of current electrolytes, offering improved ionic conductivity and stability for solid-state lithium batteries.
Patent Information
- Application Number
- JP2024104311
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-30
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-05-17
AI Technical Summary
Current solid electrolyte materials for solid-state lithium batteries face challenges such as high synthesis temperatures, brittleness, low ionic conductivity, and safety concerns, particularly with oxide, sulfide, and polymer electrolytes, necessitating the development of safer and more conductive alternatives.
Development of halide-based solid electrolyte materials with controlled impurity phases and optimized crystal structures, formed through a novel synthesis process that includes ammonium-containing halides and controlled stoichiometric ratios, enhancing properties like ionic conductivity and electrochemical stability.
The halide materials exhibit improved ionic conductivity, mechanical deformability, and electrochemical stability, making them suitable for solid-state lithium batteries with enhanced safety and performance.
Smart Images

Figure 2024138315000001_ABST
Abstract
Description
[Technical field]
[0001] The following describes a solid electrolyte material and a method for forming the same, specifically, a method for forming the same comprising at least two US20130232633A1 - Solid electrolyte material containing halide material containing halide anion and method for forming same - Google Patents The law is the subject of this study. [Background technology]
[0002] Solid-state lithium batteries offer a novel alternative to conventional methods by allowing for a lithium metal anode. They offer higher energy density and faster recharge times compared to conventional lithium-ion batteries. It is expected that this will reduce safety concerns. , oxides, halides, sulfides, fluorides, and solid polymer electrolytes.
[0003] Oxide-based materials are considered to be safe and have good chemical and electrochemical stability. The synthesis of these compounds generally involves high temperatures of over 1000-1200°C. Oxide-based materials are typically dense, stiff, and brittle, with resistances up to 1.0 mS / cm Ionic conductivity at room temperature (IC RT ).
[0004] Halide compounds, such as chlorides and bromides, are generally safe and have good chemical properties. and electrochemical stability, deformability at room temperature, and plasticity, and are relatively compatible with the active electrode material. Halides are generally hygroscopic and tend to form hydrates or or undergoes hydrolysis when exposed to moisture. Li3YCl6(LYC) and Li3YB Halide solid electrolytes such as r6(LYB) are based on high energy ball milling They are synthesized using solid-phase synthesis methods. Furthermore, they do not require expensive binary halide reactants and / or high Because warm annealing is used, the synthesis poses challenges for mass production applications.
[0005] Fluorides are very similar to oxides in terms of physical, chemical, and electrochemical properties. Generally, IC less than 1mS / cm is used. RT It has a value.
[0006] Sulfides have relatively high ionic conductivity. For example, IC RT is 25 mS / cm Although the commercially relevant sulfide or thiophosphate solid electrolytes can be as high as 2-1 0 mS / cm can be achieved. Sulfide materials are mechanically softer and more deformable. However, sulfide materials tend to have low electrochemical stability and are prone to accidental water and thermal It has raised safety concerns due to the risk of releasing toxic H2S gas when reacting with Furthermore, the high surface area sulfide solid electrolyte powders reduce their reactivity even at ambient humidity. This poses a particularly high H2S hazard due to increased
[0007] Solid polymer electrolytes containing lithium salts generally have relatively low IC RT Value and electricity It has pneumatic and chemical stability.
[0008] There is a continuing need in industry for improved solid electrolyte materials. [Brief description of the drawings]
[0009] The present disclosure may be better understood and its numerous features may be better understood by reference to the accompanying drawings, in which: and advantages will be apparent to those skilled in the art. [Figure 1A] FIG. 1A includes a diagram containing XRD pattern readings of the halide material. [Figure 1B] FIG. 1B includes a diagram containing XRD pattern readings of the halide material. [Diagram 2] FIG. 2 includes diagrams containing XRD pattern readings of additional halide materials. [Diagram 3] FIG. 3 includes a flow chart illustrating a process for forming a solid electrolyte material, according to one embodiment. [Figure 4] FIG. 4 includes a cross-sectional partial view of an exemplary electrochemical device. [Diagram 5] FIG. 5 contains the cyclic voltammetry VA diagrams of the battery samples. [Figure 6] FIG. 6 contains the cyclic voltammetry VA diagrams of the battery samples. [Figure 7A] FIG. 7A includes a diagram of an exemplary electrochemical device according to embodiments herein. [Figure 7B] FIG. 7B includes a diagram of an exemplary electrochemical device according to embodiments herein. [Figure 8] FIG. 8 includes a plot of Cl concentration versus ionic conductivity for a halide material according to one embodiment. [Figure 9A] FIG. 9A includes diagrams containing XRD pattern readings of additional halide materials. [Figure 9B] FIG. 9B includes diagrams containing XRD pattern readings of additional halide materials. [Figure 10] FIG. 10 includes an illustration of a formation process according to one embodiment. [Figure 11A] FIG. 11A includes a diagram of the electrochemical stability of halide materials. [Figure 11B] FIG. 11B includes a diagram of the electrochemical stability of the halide materials.
[0010] Skilled artisans will appreciate that elements in the figures are illustrated for simplicity and clarity and are not necessarily drawn to scale. It should be understood that the drawings are not to scale. For example, the dimensions of some of the elements in the drawings are not necessarily to scale. In some cases, elements may be exaggerated relative to other elements to help improve understanding of the disclosed embodiments. The use of the same reference symbols in different drawings indicates similar or identical items. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The following description in combination with the figures is provided to aid in the understanding of the teachings disclosed herein. The following discussion focuses on specific implementations and embodiments of the teachings. The points are provided to help explain the teachings and do not provide any indication as to the scope or applicability of the teachings. It should not be construed as a limitation.
[0012] As used herein, "comprises" and "comprising" "includes," "including," "has," "has The term "having," or any other variation thereof, is intended to cover a non-exclusive inclusion. For example, a process, method, article, or apparatus that includes a list of features is intended to The present invention is not necessarily limited to those features, and may not be limited to those features not expressly listed or otherwise. The present disclosure may include other features specific to a process, method, article, or apparatus. Unless otherwise stated, "or" refers to an inclusive or and not an exclusive or. For example, condition A or B is satisfied by one of the following: A is true (and A exists) and B is false (or does not exist), A is false (or does not exist) and B is true is (or exists), and both A and B are true (or exist).
[0013] The use of "a" or "an" refers to the elements and components described herein. This is done merely for convenience and to give a general idea of the scope of the invention. This description includes one or at least one, but Unless it is clear that the singular form is intended to include the plural, It should be read in reverse.
[0014] Unless otherwise defined, all technical and scientific terms used herein are defined by the principles of the present invention. The term "material" has the same meaning as commonly understood by a person skilled in the art to which the present invention pertains. The methods and examples are illustrative only and are not intended to be limiting.
[0015] Embodiments herein relate to solid electrolyte materials that include halide materials. In this embodiment, the halide material comprises at least two halide anions, at least one and at least one other metal element. The solid electrolyte material may include a quaternary halide material. In another embodiment, the solid electrolyte material The material is a halo material having one or more improved properties compared to conventional metal halide materials. For example, halide materials may have improved purity, crystal structure characteristics, and the like. In another example, halide materials may have improved ionic conductivity, electrical conductivity, or both. The material has a molecular conductivity, a mechanical property, an electrochemical thermodynamic stability, or any combination thereof. In embodiments, the solid electrolyte material may be an electrolyte, a coating, a catholyte, and / or may be used to form the anolyte, or another component of an electrochemical device. In such applications, solid electrolyte materials have been used due to their improved properties, such as improved interfacial contact and wettability. Due to its properties, it may be particularly suitable for forming a catholyte or an anolyte. In some embodiments, the solid electrolyte material may be a suitable component of a solid-state lithium battery.
[0016] Further embodiments relate to methods of forming solid electrolyte materials that include halide materials. The method allows for improved formation of solid electrolyte materials, resulting in solid electrolyte materials having improved properties. The method can facilitate the formation of electrolyte materials. It may be suitable for mass production in a good format.
[0017] In one embodiment, the solid electrolyte material is Li 3-x-f M f RE 1-y Me k y (Cl 1-u-p-q Br u F p I q ) 6-x+y*(k-3) Halides represented by material, the halide material comprising at least two halide anions, 1<=x<=1, 0<=y<=1, 0<=u<1, 0<=p<=1 / 3, 0<=q<=1 / 6, 0<(u+p+q)<1, and 0<=f<=0.3.
[0018] The halide anion is an element selected from the group consisting of F, Cl, Br, and I. Possibly. M can include at least one alkali metal other than Li. In certain examples, M is one selected from the group consisting of Na, K, Cs, Rb, and Fr. In another example, M can be Na, K, Cs, or any of the above alkali metal elements. In a more specific example, M may be Na or K. In a more specific example, M is at least one of Na or or K, or combinations thereof.
[0019] RE: Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb At least one rare earth metal selected from the group consisting of , Dy, Ho, Er, Tm, Yb, and Lu. For example, RE may be Sc, Y, La, Gd, or any of the above. In another example, RE may be any combination of Y, Ce, Specific examples include Gd, Er, La, Yb, or combinations thereof. , RE, Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, It may consist of one or more elements selected from the group consisting of Ho, Er, Tm, Yb, and Lu. In a more specific example, RE is Ce, Gd, Er, La, Yb, or a combination thereof. In another more specific example, RE can be Y, Gd, or a combination thereof. In an even more specific example, RE may consist of Y or Gd.
[0020] Me may be at least one metal element different from RE. For example, For example, Me is a group IIIB element, a group IVB element, V, Cr, Mn, Fe, Co, Ni, and C. u, Zn, Zr, Al, Sn, Pb, Bi, Sb, Mg, Ca, Ga, or Ge In another example, Me may be one or more elements selected from the group consisting of Y, Ce, G d, Er, Sm, Eu, Pr, Tb, Al, Zr, La, Yb, Mg, Zn, Sn, Mg , and Ca, or any combination thereof. At least one element selected from the group consisting of Gd, Yb, Zr, Zn, Mg, Al, and Ca. In more specific examples, Me can be Gd, Zr, Hf, Zn, or As used herein, the family of elements is defined as Han dbook of the Elements, 8th ed., 1998.
[0021] Me may have a valence k. When Me contains more than one metal element, k is the valence of each Me It can be the average of the sum of the valences of the metallic elements. For example, Me is an isovalent metal that divides trivalent and tetravalent elements into In another example, when Me is a divalent element and When tetravalent elements are present in equimolar amounts, k=(2+4) / 2=3. In certain embodiments, k is , 2 or 3 or 4 or 5.
[0022] In one embodiment, the halide material may have improved purity. The halide materials have one or more reduced contents compared to the corresponding conventional halide materials. As used herein, the corresponding conventional halide materials may have impurity phases of , which has the same formula as the halide materials of the embodiments herein, but is intended to refer to halide materials formed by processes other than those described herein. In one embodiment, the impurity phase may be unreacted starting materials, by-products, halide materials, or or products resulting from the decomposition of intermediate products, or any combination thereof. In a further embodiment, the impurity phase may include binary halides, ternary halides, , oxyhalides, oxynitrides, or any combination thereof. obtain.
[0023] In one embodiment, the halide materials have a higher thermal conductivity than conventional corresponding halide materials. , and may contain a reduced total content of binary halide phases. The binary halides are Li, M, In one embodiment, the metal element may include a cation selected from the group consisting of Me and RE. The halogenide material shall contain binary halogens with a total content of not more than 9% by weight based on the total weight of the halogenide material. Logenide phase, 8% by weight or less, 7% by weight or less, 6% by weight or less, 5% by weight or less, 4% by weight or more or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or 0.5% by weight or less in total. Total content of halide materials, including parent halide phases, not exceeding 10% by weight based on the total weight of the halide materials In another aspect, the halide material may include a binary halide phase of At least 0.0005% by weight, at least 0.001% by weight, less than 0.0005% by weight based on the total weight of the material at least 0.005% by weight, at least 0.01% by weight, or at least 0.05% by weight At least 0.05% by weight of the total halide material, such as the total content of binary halide phases. In a further embodiment, the halogen phase may comprise a total content of 0.0001% by weight of a binary halide phase. The nitride material may include any of the minimum and maximum percentages shown herein. In certain embodiments, the halide material may include a binary halide phase having a total content in the range of , may be essentially free of binary halide phases.
[0024] The content of one or more impurity phases that may be present in a halide material is determined by the Using well-known techniques such as powder X-ray diffraction analysis or innovative laser Raman mapping X-ray diffraction analysis shows that the content of impurity phases is the total content of the halide material. It may be particularly suitable if it is at least 1% by weight.
[0025] In one embodiment, the binary phase may include one or more alkali metal halide phases. In an embodiment, the halide material has a total content of 7% by weight or less based on the total weight of the halide material. Amount of alkali metal halide phase, not more than 6% by weight based on the total weight of the halide material, 5 times % by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or 0.5% by weight or less % total content of alkali metal halide phases. The halide material should contain at least 0.0005% by weight based on the total weight of the halide material. at least 0.001% by weight, at least 0.005% by weight, at least 0.01% by weight, or Halide phases, such as alkali metal halide phases with a total content of at least 0.05% by weight. Alkali metal halides with a total content of at least 0.0001% by weight based on the total weight of the material In a further example, the halide material may include a halide phase having the minimum and maximum Alkali metal halides in the range of total content including any of the maximum percentages In certain instances, the halide material may essentially comprise an alkali metal halide phase. It is not necessary to include it in the
[0026] In certain embodiments, the halide material is 7 times as heavy as the total weight of the halide material. The lithium halide phase may contain a total content of up to Li The liquid may include one or more of a Cl phase, a LiBr phase, a LiI phase, and a LiF phase. In the case of halide materials, the total content is 6% by weight or less based on the total weight of the halide materials. Lithium halide phase, not more than 5% by weight, not more than 4% by weight based on the total weight of the halide material or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or 0.5% by weight or less in total content In some cases, the halide material may include a lithium halide phase. At least 0.0005% by weight, at least 0.001% by weight, less than 0.0005% by weight based on the total weight of the material at least 0.005% by weight, at least 0.01% by weight, or at least 0.05% by weight At least one lithium halide phase, based on the total weight of the halide material, such as the total content of lithium halide phase In a further embodiment, the lithium halide phase may have a total content of 0.0001% by weight. The halogenated material may have any of the minimum and maximum percentages shown herein. In certain embodiments, the lithium halide phase may have a total content in the range including: The material may be essentially free of a lithium halide phase.
[0027] In one embodiment, the binary phase is a YX3 phase, where X represents a halide anion. In one embodiment, the halide material may include one or more rare earth halide phases. 9% by weight or less, 8% by weight or less, 7% by weight or less, 6% by weight or less, based on the total weight of the compound material; 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or 0.5 % total content of rare earth elements, such as rare earth halide phases with a total content of 10% by weight or less In another embodiment, the halide material may include a halide-like phase. At least 0.0005% by weight, at least 0.001% by weight, at least at least 0.005% by weight, at least 0.01% by weight, or at least 0.05% by weight At least 0.01% by weight of the total halide material, including rare earth halide phases. In a further embodiment, the rare earth halide phase may have a total content of 0.001% by weight. The nitride material may include any of the minimum and maximum percentages shown herein. In certain embodiments, the rare earth halide phase may have a total content in the range of may be essentially free of rare earth halide phases.
[0028] In certain embodiments, the binary halide phase is YCl, YBr, YI, or Y In one embodiment, the halogen compound may include one or more YX3 phases, such as one or more phases of F3. The amount of halogenide materials is not more than 9% by weight, not more than 8% by weight, not more than 7% by weight, based on the total weight of halogenide materials. % or less, 6% by weight or less, 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1 % or less, or a total content of YX3 phase of 0.5% or less by weight In another embodiment, the halide material may comprise a total of 100% YX3 phase. At least 0.0005% by weight, at least 0.001% by weight, at least A total content of 0.005% by weight, at least 0.01% by weight, or at least 0.05% by weight At least 0.0001% by weight based on the total weight of the halide material, such as a YX3 phase in an amount In a further embodiment, the halide material may comprise a YX3 phase having a total content of The total content of the YX3 phase is within the range including any of the minimum and maximum percentages. In certain embodiments, the halide material may be essentially free of YX3 phases. .
[0029] In one embodiment, the halide materials have a higher thermal conductivity than conventional corresponding halide materials. , may contain a reduced content of one or more oxyhalide phases. may include a cation of a metal element selected from the group consisting of M, Me, and RE. In such a case, the halide material may contain no more than 6% by weight of oxyhalogens based on the total weight of the halide material. Halide phase, not more than 5% by weight, not more than 4% by weight, not more than 3% by weight based on the total weight of halide material % or less, 2% or less, 1% or less, or 0.5% or less of total oxyhalogenated The total content of oxyhalogens is not more than 7% by weight based on the total weight of the halide materials, such as the In another embodiment, the halide material may comprise a halide phase. At least 0.0005% by weight, at least 0.001% by weight, at least 0.0 0.05% by weight, at least 0.01% by weight, or at least 0.05% by weight of total At least 0.0001 by weight of the total halide material, such as a hydroxyhalide phase In a further embodiment, the halide material may comprise an oxyhalide phase having a total content of oxyhalide phase of 100% by weight. The fee is within the range of minimum and maximum percentages set forth herein. In certain embodiments, the halide material may include an oxyhalide phase. It may be essentially free of dihalide phase.
[0030] The total content of impurity phases that may not be soluble in water is determined using the water method described below. The concentration of the halide material can be determined by dissolving 50 g of the material in distilled H2O. The solution can be filtered through a 0.2 micron Millipore filter. The insoluble material may be collected and weighed. The collected insoluble material may be present in the halide material. This may include hydrated forms of water-insoluble impurities present in halide materials. At least the majority of the soluble impurities are rare earth oxyhalides, rare earth oxides, M The collected cations may be oxyhalides of MeO, MeO oxyhalides, or any combination thereof. The weight of the insoluble material collected is used to determine the total content of water-insoluble impurities in the halide material. As an example, the insoluble impurity phase of the metal oxyhalide MeOX can be used. The precipitated hydrated impurity form can be represented by MeX(OH)2, and MeOX The content of is expressed by the formula C MeOX =C MeOHX ×(MW MeOX / MW MeOHX ) where C MeOX The weight content of MeOX relative to the weight of the halide material C represents the quantity MOHX is the weight of precipitated MeX(OH)2 relative to the weight of halide material. represents the weight content of MeOX represents the molar mass of MeOX, and MW MeOHX but, The molar mass of MeX(OH)2 is shown. The synthesis of halide materials may involve melting and solidification. In some cases, trace amounts of organic residues may be present on the surfaces of the building blocks of the halide materials. The organic residue is carbon concentrated on the surface of the block and can be removed with a scalpel. Trace amounts of carbon can be used to synthesize one or more of the elements used to synthesize the halide materials. It may be present in the feed and may result from the thermal decomposition of organic impurities.
[0031] In one embodiment, the halide material includes a reduced content of water insoluble impurity phases. In one embodiment, the halide material is 0.1 weight percent based on the total weight of the halide material. % or less, 0.09% by weight or less, 0.08% by weight or less, 0.07% by weight or less, 0.05% by weight % or less, 0.04% by weight or less, 0.03% by weight or less, 0.01% by weight or less, 0.008% by weight % by weight or less, 0.006% by weight or less, 0.004% by weight or less, or 0.003% by weight or less Any water-insoluble impurities with a total content of less than 0.11% by weight based on the total weight of the halide material In another embodiment, the halide material may include a phase of At least 0.0003% by weight, at least 0.0005% by weight, at least 0.00 1% by weight, at least 0.005% by weight, at least 0.01% by weight, at least 0.0 13% by weight, at least 0.015% by weight, at least 0.02% by weight, at least 0. 0.03% by weight, or an insoluble impurity phase with a total water content of at least 0.05% by weight. Water-insoluble impurities with a total content of at least 0.0001% by weight based on the total weight of the fluorinated material In a further aspect, the halide material may include a phase having the minimum and maximum values set forth herein. The total content of the water-insoluble impurity phase may range anywhere from 0.01 to 0.05%. In certain embodiments, the halide material may be essentially free of water-insoluble impurity phases. In some cases, the majority of the water-insoluble impurity phase is composed of rare earth oxyhalides, Me oxyhalides, oxyhalides, rare earth oxides, oxides of Me, or any combination thereof In another example, the water insoluble impurity phase may include one or more phases of rare earth oxyhalogenides. compounds, oxyhalides of Me, rare earth oxides, oxides of Me, or any combination thereof The composite may consist essentially of one or more phases of the combination.
[0032] In one embodiment, the oxyhalide phase includes one or more rare earth oxyhalides. In one embodiment, the halide material is present in an amount of 7% by weight or less, 6% by weight or less, % or less, 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or may contain rare earth oxyhalide phases with a total content of 0.5 wt.% or less. The total content of rare earth oxyhalide phases is 0.01% by weight based on the total weight of the halide material. 2% by weight lower, less than 0.12% by weight, less than 0.11% by weight, less than 0.10% by weight, 0.0 9% by weight or less, 0.07% by weight or less, 0.05% by weight or less, or 0.03% by weight or less, etc. % or less by weight of rare earth oxyhalide phase. the halide material is at least 0.0005% by weight based on the total weight of the halide materials; At least 0.001% by weight, at least 0.005% by weight, at least 0.01% by weight %, or at least 0.02% by weight, or at least 0.05% by weight of rare earth oxynitride. At least 0.0001 weight percent of the total weight of halide materials, such as halide phases % total content of rare earth oxyhalide phase. The material may be present in any range including any of the minimum and maximum percentages set forth herein. In certain embodiments, the halide material may include a rare earth oxyhalide phase. can be represented by REOX, where X is a halogen and RE is a rare earth element. The catalyst may be essentially free of any rare earth oxyhalide phase that may be present.
[0033] In one embodiment, the halide materials have a higher thermal conductivity than conventional corresponding halide materials. , may contain a reduced total content of one or more ternary halide phases. Halides are compounds that combine two metal cations and one halide, such as alkali metal-rare earth metal halides. A compound containing one metal element and two halide anions, or one metal element and two halide anions, or both. Exemplary metal cations include those of Li, M, RE, and / or Me metal elements. In one embodiment, the halide material is a total of 6% by weight or less, 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less %, or ternary halide phases with a total content of 1% by weight or less, or 0.5% by weight or less. The ternary halide phases may have a total content of up to 7% by weight based on the total weight of the ternary halide material. In another embodiment, the halide material is at least 0. 0005% by weight, at least 0.001% by weight, at least 0.005% by weight, at least 0.01% by weight or more, or at least 0.05% by weight of ternary halide phases in total. of ternary elements with a total content of at least 0.0001% by weight based on the total weight of the halide material. In a further aspect, the halide material may include a halide phase as described herein. Ternary halides with a total content in the range including any of the minimum and maximum percentages In certain embodiments, the halide material essentially comprises a ternary halide phase. It is not necessary.
[0034] In one embodiment, the ternary phase is one or more lithium yttrium halide phases, such as a lithium yttrium halide phase. The lithium-rare earth halide phase may include a halide material. Lithium-rare earth halide phases with a total content of 7% by weight or less based on the total weight of the lithium-rare earth halide material , 5% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or 0.5% by weight or less In another embodiment, the halide material may include a lithium-rare earth halide phase having a total content of lithium. The amount of the halogenated material is at least 0.0005% by weight based on the total weight of the halogenated material, and at least 0 0.001% by weight, at least 0.005% by weight, at least 0.01% by weight, or less Halides, such as lithium-rare earth halide phases with a total content of 0.05 wt.% Lithium-rare earth halide with a total content of at least 0.0001% by weight based on the total weight of the material In a further aspect, the halide material may comprise a halide phase having a minimum of the minimum required for the present invention. and the total content of lithium-rare earth halo in the range including any of the maximum percentages. In certain embodiments, the halide material may include a lithium rare earth halide phase. The alloy may be essentially free of nitride phases.
[0035] In certain embodiments, the ternary halide phase comprises 6 Weight % or less, 5 weight % or less, 4 weight % or less, 3 weight % or less, 2 weight % or less, 1 weight % or less or a ternary halide phase containing two anions with a total content of 0.5% by weight or less, Ternary phases containing two anions with a total content of less than 7% by weight, YBr x Cl y Or Li Br x Cl y One or more ternary halide phases containing two halide anions such as In some cases, the halide material may comprise a small amount by weight of the total halide material. At least 0.0005% by weight, at least 0.001% by weight, at least 0.005% by weight %, at least 0.01% by weight, or at least 0.05% by weight of two anilines At least 0.01% by weight of the total halide material, such as a ternary halide phase containing ions. It may contain a ternary halide phase containing two anions with a total content of .0001% by weight. In some embodiments, the halide material is in the range of minimum and maximum percentages shown herein. The ternary halide phase contains two anions with a total content in the range including any of the following: In certain embodiments, the halide material is a ternary halide phase comprising two anions. It is not necessary for the composition to essentially contain
[0036] In one embodiment, the halide materials have a higher thermal conductivity than conventional corresponding halide materials. The nitride phase may include an oxynitride phase, a nitride phase, or a nitride phase having a reduced content of one or more nitride phases. The nitride phase may include one or more of the following phases: Li, M, RE, SiO, SiO, SiO2, SiO3, SiO4, SiO5, SiO6, SiO7, SiO2, SiO2, SiO2, SiO2, SiO2, SiO3, SiO4, SiO5, SiO6, SiO2 ... In one embodiment, the halo may include a cation of a metal element selected from the group consisting of , , and Me. The halogenide material shall be 6% by weight or less, 5% by weight or less, or 4 times the total weight of the halide material. % by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or 0.5% by weight or less A total content of nitrogen not exceeding 7% by weight based on the total weight of the halide material, including nitride-based phases in an amount In another embodiment, the halide material may comprise a halide-based phase. At least 0.0005% by weight, at least 0.001% by weight, at least 0.0 0.05% by weight, at least 0.01% by weight, or at least 0.05% by weight of nitrogen At least 0.0001% by weight total of halide-based phases, based on the total weight of the halide materials. In a further aspect, the halide material may include a nitride-based phase of any of the above-mentioned compositions. The total content of nitride phases is within a range including any of the minimum and maximum percentages set forth above. In certain embodiments, the halide material may be essentially free of nitride-based phases. stomach.
[0037] In one embodiment, the halide materials have a higher thermal conductivity than conventional corresponding halide materials. , reduced content of REO x N y The oxynitride phase may include one or more oxynitride phases, such as an oxynitride phase. may include a cation of a metal element selected from the group consisting of Me and RE. , halide materials are 6% or less by weight, 5% or less by weight based on the total weight of halide materials , 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or 0.5% by weight or less Total content of oxynitride phases, etc., not exceeding 7% by weight based on the total weight of the halide material In another aspect, the halide material may include an amount of an oxynitride phase. At least 0.0005% by weight, at least 0.001% by weight, at least A total content of 0.005% by weight, at least 0.01% by weight, or at least 0.05% by weight At least 0.0001 weight percent of the total weight of the halide material, such as an oxynitride phase % total content of oxynitride phases. In a further aspect, the halide material may comprise the oxynitride phases described herein. Oxynitride having a total content in a range including any of the minimum and maximum percentages shown in In certain embodiments, the halide material is essentially free of oxynitride phases. This is also fine.
[0038] In one embodiment, the halide materials have a higher thermal conductivity than conventional corresponding halide materials. , reduced content of REC x N y The carbon nitride phase may include one or more carbon nitride phases, such as the carbon nitride phase. may include a cation of a metal element selected from the group consisting of Me and RE. , halide materials are 6% or less by weight, 5% or less by weight based on the total weight of halide materials , 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or 0.5% by weight or less Total content of carbon nitride phases, etc., not more than 7% by weight based on the total weight of the halide material In another aspect, the halide material may include a carbon nitride phase in an amount of 0.1 to 0.5% by weight of the total halide material. At least 0.0005% by weight, at least 0.001% by weight, at least A total content of 0.005% by weight, at least 0.01% by weight, or at least 0.05% by weight at least 0.0001 weight percent based on the total weight of the halide material, such as a carbon nitride phase % total content of carbon nitride phase. In a further aspect, the halide material may comprise The total content of carbonitride is within the range including any of the minimum and maximum percentages shown in In certain embodiments, the halide material is essentially free of carbon nitride phases. This is also fine.
[0039] In one embodiment, the halide materials have a higher thermal conductivity than conventional corresponding halide materials. , reduced content of rare earth nitride (e.g., REN (rare-earth nitride)) phase, etc. The nitride phase may include one or more nitride phases. The nitride phase may be selected from the group consisting of Li, M, Me, and RE. In one embodiment, the halide material may include a cation of a selected metal element. 6% by weight or less, 5% by weight or less, 4% by weight or less, 3% by weight or less, based on the total weight of the compound material; halo, such as nitride phases, with a total content of 2 wt. % or less, 1 wt. % or less, or 0.5 wt. % or less The nitride material may have a total content of nitride phases of up to 7% by weight based on the total weight of the nitride material. In the present specification, the halide materials are at least 0.0005% by weight of the total halide materials. %, at least 0.001%, at least 0.005%, at least 0.0 Halide materials, such as nitride phases with a total content of 1% by weight, or at least 0.05% by weight The nitride phase may have a total content of at least 0.0001% by weight relative to the total weight of the material. In some embodiments, the halide material is in the range of minimum and maximum percentages shown herein. In certain embodiments, the halogen atom may include a nitride phase having a total content in the range including any of the above. The nitride material is essentially free of at least one rare earth nitride phase and an Me metal nitride phase. In another particular embodiment, the nitride phase, when present in the halide material, is Alternatively, the phase may be essentially free of a cation of the metal element Me. In the present invention, the halide material is essentially free of rare earth nitride phases and Me metal nitride phases. Good too.
[0040] In one embodiment, the halide material is 6% by weight based on the total weight of the halide material. 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, 0. Impurity phases with a total content of 5% by weight or less, 0.3% by weight or less, or 0.1% by weight or less. 15% by weight or less, 14% by weight or less, 13% by weight or less based on the total weight of the halide material; 12% by weight or less, 10% by weight or less, 9% by weight or less, 8% by weight or less, 7% by weight or less, etc. In another embodiment, the halide material may include impurity phases having a total content of 6% by weight or less. At least 0.0005% by weight, based on the total weight of the halogenated material, at least 0.001 %, at least 0.005%, at least 0.01%, or at least 0. 0.5% by weight of impurity phases, etc., based on the total weight of the halide material In a further embodiment, the halide material may contain impurity phases with a total content of 0.0001% by weight. The fee is within the range of minimum and maximum percentages set forth herein. It may contain impurity phases.
[0041] In certain embodiments, the halide material may be a binary halide phase, a ternary halide phase, The phase may be essentially free of oxide, oxynitride, and oxyhalide phases. In embodiments, the halide material may consist essentially of a single phase. The material has the formula Li 3-x-f M f RE 1-y Me k y (Cl 1-u-p-q Br u F p I q ) 6-x+y*(k-3) and an impurity phase, The total content may be at most 0.5 mol % or at most 0.3 mol %.
[0042] In one embodiment, the halide material is a compound that promotes improved properties of the halide material. The crystal structure characteristics may include specific crystal structure characteristics that can be used to determine the crystal structure of the crystal, lattice system, , space group, one or more unit cell parameters including unit cell volume, values of a, b, c, or Any combination of the number of atoms in the unit cell, stacking order, atomic vacancies, vacancy occupancy rate, or any combination thereof Any combination of the above may be mentioned.
[0043] In one embodiment, the halide material is monoclinic, trigonal, hexagonal, or orthorhombic. In certain embodiments, the halide material may include a crystal structure of the monoclinic space group. In a particular example, the halide material may include a crystal structure represented by the formula: The crystal structure may include a crystal structure represented by the intermetallic group.
[0044] In another particular embodiment, the halide material is R3,
[0045]
number
[0046]
number
[0047]
number
[0048] In another particular embodiment, the halide material is represented by a hexagonal space group. The hexagonal crystal structure may include P6, P61, P65, P62, P64, and P6 3.
[0049]
number
[0050]
number
[0051] In certain embodiments, the halide material is at the atomic level, at the nanometer level, or both, including mixed crystalline interphases. The closest interatomic distance is usually less than 0.5 nm, and the nanometer range is 1 nm. In one aspect, the halogenated The material comprises a first crystalline phase having a first crystal structure represented by a first space group and a second crystalline phase having a second space group. and a second crystalline phase having a different second crystal structure represented by a space group of
[0052] In certain embodiments, the halide material is represented by a rhombohedral lattice space group. A first crystalline mesophase having a first crystal structure and a monoclinic space group such as C2 / m In a particular example, the halide material may include a second crystalline mesophase represented by:
[0053]
number
[0054]
number
[0055] For example, the first crystalline mesophase may have a first crystalline structure represented by a hexagonal space group. The second crystalline mesophase may have a second crystalline mesophase represented by a trigonal or orthorhombic space group. In certain instances, the second crystalline mesophase may have a crystalline structure.
[0056]
number
[0057]
number
[0058] In one embodiment, the halide material has a unit cell smaller than that of Li3YBr6. In certain embodiments, the halide material may include a crystal structure comprising Li3YBr6. In another particular embodiment, the crystal structure may be similar to, but have a smaller unit cell volume. The halide material peaks are in the powder diffraction pattern of Li3YBr6. The powder X-ray diffraction peaks are shifted to higher angles compared to the corresponding peaks in With reference to FIG. 1A, the Cu K-alpha radiation The typical halide materials Li3YBr3Cl3 and Li3Y Powder XRD patterns of Br4Cl2 and Li3YBr6 are shown. The corresponding peaks for Li3Cl3 and Li3YBr4Cl2 are more prominent than those for Li3YBr6. The shift is towards higher values of 2-theta.
[0059] In another embodiment, the halide material is similar to Li3YCl6, but with a larger In a particular example, the halide material may include a crystal structure having a large unit cell volume. The peaks in the Li3YCl6 powder diffraction pattern are compared to the corresponding peaks in the Li3YCl6 powder diffraction pattern. , the powder X-ray diffraction (XRD) pattern may be shifted to a smaller angle. Referring to the Cu K-alpha radiation, a representative halide material Powder XRD of Li3YBr2Cl4, Li3YBr1Cl5, and Li3YCl6 The pattern is shown. The corresponding peaks for Li3YBr1Cl5 are In comparison, the XRD pattern of Li3YBr4Cl2 is shifted to a smaller value of 2theta. The turn may suggest that the halide contains a mixed mesophase.
[0060] In a particular example, the halide material has a thermal conductivity of 13°, measured with Cu K-alpha radiation. The XRD pattern may include at least two peaks in the range of .about.15 degrees 2-theta. Referring to FIG. 2, Li 3-x Y(Cl 1-u Br u ) 6-x The three samples of Cu K- The alpha XRD pattern is shown. Sample 202, with u of 0.59±0.03, It shows one peak in the 2θ range of 13° to 15°. u is 0.38±0.0 Samples 204 and 206, which are 0.3 and 0.31±0.03, respectively, are in the two-axis range of 13° to 15°. The data shows two peaks.
[0061] In another embodiment, the halide material promotes improved properties of the halide material. The average diffraction crystallite size may include a specific average diffraction crystallite size that can be determined by the method of the present invention. Also referred to as the coherent X-ray scattering area size, halide-based materials X-ray diffraction analysis and Scherrer's equation L = (Kλ) / (β cosθ) (where L is the average diffraction represents the crystallite size, and K is a dimensionless number with values close to 1 and typical values between 0.9 and 1. is the dimensionless shape factor, λ is the X-ray wavelength, and β is the Half-width in radians after subtracting instrumental line broadening. where θ is the Bragg angle) obtain.
[0062] In one embodiment, the halide material is at least 20 nm, at least 25 nm, Average diffracting crystallite size of at least 30 nm, at least 35 nm, or at least 40 nm In another embodiment, the halide material may include at most 500 nm, at most 400 nm, at most 300 nm, at most 200 nm, or at most 100 nm In a further aspect, the halide material may include a crystallite size of at least one of the minimum sizes set forth herein. The mean diffracting crystallite size may include a range including any of the values and maximum values.
[0063] In one embodiment, the solid electrolyte material is an improved version of the halide material and the solid electrolyte material. The material may include a halide material containing a certain amount of Cl that can promote improved properties. In embodiments, (1-upq) is at least 0.12, at least 0.15, at least at least 0.17, at least 0.20, at least 0.23, at least 0.25, at least at least 0.27, at least 0.29, at least 0.33, at least 0.36, at least at least 0.43, at least 0.48, at least 0.50, at least 0.54, or less In another embodiment, (1-upq) is at most 0.92, at most 0.87, at most 0.83, at most 0.80, at most 0.77, at most At most 0.99, such as 0.75, at most 0.70, or at most 0.66 In a further embodiment, (1-upq) can be as low as 0.97. It may be in a range including any of the lower and maximum values.
[0064] In certain embodiments, the solid electrolyte material is Li 3-x-f M f RE 1-y Me k y ( Cl 1-u-p-q Br u F p I q ) 6-x+y*(k-3) The halogens represented by wherein u is greater than 0. More specifically, the halide material may be , may contain Br in a specific amount that can promote improved properties of halide materials. In one embodiment, u is at least 0.12, at least 0.15, at least 0.17, At least 0.2, at least 0.23, at least 0.25, at least 0.27, a little At least 0, such as at least 0.29, at least 0.32, or at least 0.34. In another embodiment, u can be at most 0.85, at most 0.83, at most 0.1. 0.8, at most 0.77, at most 0.75, at most 0.7, at most 0.67, at most 0.65, at most 0.62, at most 0.6, at most 0.57, at most 0. 54, at most 0.52, at most 0.49, at most 0.45, or at most 0.42 In another embodiment, u can be any of the minimum and maximum values set forth herein. The range may be inclusive.
[0065] In another embodiment, the halide material promotes improved properties of the halide material. The amount of Cl to the amount of Br may include a specific ratio (1-upq) / u, which may be used to In one embodiment, the ratio of (1-upq) / u is at least 0.06, at least 0.1, At least 0.2, at least 0.3, at least 0.4, at least 0.5, at least At least 0.6, at least 0.7, at least 0.8, at least 0.9, at least 1.0 , at least 1.2, at least 1.3, at least 1.4, at least 1.5, less at least 1.6, at least 1.7, at least 1.8, at least 1.9, or at least In another embodiment, (1-upq) / u may be at least 0.03, such as 2.0. The ratios are 9 or less, 8.6 or less, 8.3 or less, 8 or less, 7.7 or less, 7.4 or less, 7 or less, 6.5 or less, 6.2 or less, 6 or less, 5.5 or less, 5 or less, 4 or less, 3 or less, 2 or less, or In a further embodiment, the ratio of (1-upq) / u is less than or equal to 1.4. The range may be within any of the minimum and maximum values set forth.
[0066] In a further embodiment, the halide material is an aniline halide material consisting of Cl and Br. In a particular example, the halide material may include Li 3-x RE 1-y Me k y ( Cl 1-u Br u ) 6-x+y*(k-3) where u>0. For certain applications, 0.08<=u<=0.67. The fee is Li 3-x Y(Cl 1-u Br u ) 6-x In certain applications, In some embodiments, u may be at least 0.55 or at most 0.45. 0.2<=u<=0.45.
[0067] After reading this disclosure, one of ordinary skill in the art will appreciate that the properties of the halide materials of the embodiments herein are consistent with those of the halide materials of the present invention. the amount of one or more of the halide anions, their ratio, the crystal structure of the halide material, or can be adjusted or regulated by carefully controlling any combination of them. It will be appreciated that in one embodiment, when both Br and Cl are present, B Carefully control the amount of r and / or Cl and / or the ratio (1-upq) / u This allows the halide material to have a layered crystal structure similar to Li3YBr6, Li3YC Improved ionic conductivity compared to Li3YBr6 and improved electrical conductivity compared to Li3YBr6. In another embodiment, the halogen-containing polymer may include halogen-containing polymers having a halogen-containing structure and a halogen-containing polymeric structure. The nitride material may include Br and Cl and may include the mixed crystalline mesophase described in the embodiments herein. The halide materials may have a crystal structure that includes an improved ion exchange ratio compared to Li3YCl6. have ionic conductivity and improved electrochemical and thermodynamic stability compared to Li3YBr6 .
[0068] In another embodiment, when 0 < u < 0.33, the halide material has a crystal structure including a hexagonal / trigonal crystal structure similar to Li3YCl6, in particular improved ionic conductivity and mechanical deformability at low temperatures (i.e., below 200 °C), and improved electrochemical and thermodynamic stability compared to Li3YBr6. Such halide materials may be particularly suitable for certain applications such as the manufacture of lightweight batteries due to their reduced density compared to Li3YBr6 . .
[0069] In certain embodiments, a halide material represented by Li 3-x-f M f RE 1-y Me k y (Cl 1-u-p-q Br u F p I q ) 6-x+y*(k-3) . More specifically, the halide material may include F in a particular amount that can promote the improved properties of the halide material. In one aspect, p can be at least 0.04, such as at least 0.06, at least 0.08, at least 0.09, at least 0.10, at least 0.12, at least 0.14, at least 0.15, at least 0.17, at least 0.2, or at least 0.22. In another aspect , p can be at most 0.31, at most 0.29, at most 0.27, at most 0.25 , at most 0.22, at most 0.20, at most 0.18, at most 0.16, at most is at most 0.33, such as at most 0.14, at most 0.12, or at most 0.10 obtained. In another aspect, p can be in the range including either the minimum or the maximum value shown herein and can be within the range.
[0070] As an example of the halide material, Li3Me 3+ Cl 6(1-p) F 6p can be mentioned, where 0 < p < 0.58. In a specific example, Me can include In and more specifically, can consist of In. The solid solution of the chloride - fluoride halide phase can have a crystal structure represented by the space group C2 / m and can have improved ionic conductivity compared to Li3InF6 and Li3 InCl6.
[0071] In another embodiment, the halide material can include a specific ratio (1 - u - p - q) / p of the amount of Cl to the amount of Br that promotes improved properties of the halide material In one aspect, the ratio (1 - u - p - q) / p is at least 0.5, such as at least 0.7, at least 0.9, at least 1.0, at least 1.2, at least 1.4, at least 1.5, at least 1.6, at least 1.7, at least 1.8, at least 1.9, at least 2.0, at least 2.2, at least 2.4, at least 2.6, at least 2.8, at least 3.0, at least 3.2, at least 3.4, or at least 3.6. In another aspect, the ratio (1 - u - p - q) / p is at most 24, such as at most 21, at most 19 at most 17, at most 15, at most 13, at most 12, at most 11, at most 9, at most 8, at most 6, or at most 5. In a further aspect, the ratio (1 - u - p - q) / p can be in a range including any of the minimum and maximum values stated herein.
[0072] In one embodiment, the halide material has the formula Li a M a’ Me b Me' b’ X c X' c ’ M can be represented by at least one element other than Li, as described in the above embodiment. In a particular example, M is selected from the group consisting of Na, K, and Cs. It can be at least one element of.
[0073] Me is a group IIIB element, a group IVB element, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Al, In, Sn, Pb, Bi, S The element may be at least one element selected from the group consisting of B, Mg, Ca, Ga, and Ge. In certain instances, Me can be an RE as discussed in the embodiments herein.
[0074] Unlike Me, Me' does not include group IIIB elements, group IVB elements, V, Cr, Mn, Fe , Co, Ni, Cu, Zn, Zr, Al, In, Sn, Pb, Bi, Sb, Mg, Ca, In a particular example, the element may be at least one element from the group consisting of Me ' may be at least one element from rare earth elements, Zr, and Fe.
[0075] X can be at least one halogen, and X' can be at least one halogen other than X. In a particular example, X can be at least one element selected from the group consisting of Cl, Br, and F. In another particular example, X' can be at least one of the elements Br and F. could be.
[0076] In another embodiment, the solid electrolyte material is Li a M a’ Me b Me' b’ X c X' c’ where a≧a′, b≧b′, and c≧c′. In particular, the halide materials, as described in the embodiments herein, contain low levels of 1 In yet another embodiment, the solid electrolyte material may include Li a M a’ M e b Me' b’ X c X' c’ and the halide material may include a halide material represented by The anions of the material may be in a single phase.
[0077] In one embodiment, the halide material may include at least four elements. In an embodiment, the halide material is formed by adjusting the stoichiometric ratio of two or more elements. In certain embodiments, the same portion of the crystal structure may have a crystallographic phase transition that can be induced by The stoichiometric ratio of elements in the halide material determines the properties that the material possesses, e.g., ionic conductivity, electrical conductivity, The composition may have improved properties, including improved biological stability, compatibility, etc., or any combination thereof. After reading this disclosure, one of skill in the art would understand that Li and M are located at the same crystallographic site. It will be understood that Me and Me' may be present at the same crystallographic site, X and X' can be present at the same crystallographic site. In one example, the stoichiometry of Me and Me' is ratio, or the stoichiometric ratio of Li and M, or the stoichiometric ratio of X and X', or Any combination of these may be tailored to improve one or more properties of the halide material. In a particular example, X can be Cl and X' can be Br, and the chemistry of X and X' can be The stoichiometric ratio is Li for the halide material. + Ionic conductivity, electrochemical In another particular example, M is Na. The stoichiometric ratio of Li and M can be adjusted to improve ionic conductivity. In another example, Me can be Y and Me' can be In, and the stoichiometry of Me and Me' is The proportion of cations can be adjusted to improve the ionic conductivity of the halide material.
[0078] The halide material may have a crystallographic phase transition boundary on the compositional phase diagram. The crystallographic phase transition boundary is called the morphotropic phase boundary. In one embodiment, the crystallographic phase transition occurs when the stoichiometry of Me and Me′ is In particular, halide materials can be induced by changes in the stoichiometric ratios b / (b+b'). , (b / (b+b')) t * 0.84~(b / (b+b')) t * 1.16 Stoichiometric Model In the above formula, (b / (b+b')) t At room temperature (i.e., 2 2°C) on the composition phase diagram. In certain embodiments, b>b'>0 , c≧0, c′≧0, and (c+c′)>0. In another embodiment, Me and Me′ are At least one of them may include the RE discussed in the embodiments of the present disclosure. In certain embodiments, Me can include RE and Me' can include another tetravalent or a trivalent element. In a more specific embodiment, Me includes Y. Me' can be Zr. More specifically, Me can be , Y, and Me' can be Zr.
[0079] In one embodiment, the halide material is modified by changing the stoichiometric ratio of X and X′. In particular, halide materials may have a crystallographic phase transition that can be induced, such as c / (c+c') But (c / (c+c')) t * 0.84~(c / (c+c')) t * 1.16 Composition Phase Diagram In the above stoichiometric range, (c / (c+c')) t But room temperature (i.e., 22° C.) corresponds to a crystallographic phase transition boundary on a composition phase diagram. , c≧c′>0, b≧0, b′≧0, and (b+b′)>0. X may be Cl, and X' may be Br. In a particular embodiment, X can be Cl and X' can be Br. At least one of M′ and M′ may be an RE as discussed in the embodiments of the present disclosure. In a more specific embodiment, one of M and M′ can be Y.
[0080] In another embodiment, the halide material is modified by changing the stoichiometric ratio of Li and M. In particular, halide materials can have a crystallographic phase transition that can be induced by a / (a+a' ) is (a / (a+a')) t * 0.84~(a / (a+a')) t * Chemical equivalent of 1.16 In the theoretical range, a phase transition may occur, where a / (a+a') t At room temperature (i.e. , 22° C.) on the crystallographic phase diagram. a>0 and a'>0. In a particular embodiment, a>a'. Another particular embodiment In the above, M can include Na. In a more specific embodiment, M can include Na It could be.
[0081] In one embodiment, the halide material is a crystallographic phase transition material that includes transitions across a crystallographic phase transition boundary. In another embodiment, the crystallographic phase transition may involve one or more characteristic changes in the crystal structure. Examples of crystal structure characteristics include changes to the unit cell volume, space group, and The crystal system, one or more features of the XRD pattern, or any combination thereof may be mentioned. can.
[0082] In one embodiment, the halide material is monoclinic, trigonal, hexagonal, or orthorhombic. The crystallographic phase transition may involve a transition from one of the crystalline systems to another. In a further embodiment, the halide material is a crystalline material that includes a transition from a layered structure to a non-layered structure. For example, a crystallographic phase transition may include a crystallographic phase transition from monoclinic to trigonal. In a further embodiment, the crystallographic phase transition may include the C2 / m The transition from the space group R-3m or R-3m to the space group P-3m1 or Pnma can be mentioned. In yet another embodiment, the crystallographic phase transition may include a cubic close packed to hexagonal close packed structure. A transition to a packed structure can be mentioned.
[0083] In a further embodiment, the crystallographic phase transition includes a transition from a non-lamellar structure to another non-lamellar structure. In yet another embodiment, the crystallographic phase transition may include a non-layered structure. In a particular example, the crystallographic phase transition can be from a crystalline structure to a layered structure. , R3c to R3m. Another specific example is the crystallographic phase transition As for the conversion from the P-3m1 or Pnma space group to the C2 / m or R-3m space group, Examples of such measures include:
[0084] In a further embodiment, when the halide material has a crystallographic phase transition, certain The crystal structure characteristics of the halide material may not change. For example, the XRD patterns of the halide material Examples of phase transitions include those that represent an increase or decrease in unit cell volume. Certain other XRD features may remain unchanged. In a particular example, the halide material is Crystallographic phase transitions and XRD patterns, including the absence of a peak between ~13° 2theta It may include a turn.
[0085] In one embodiment, the halide material is converted to a fluorine-containing material without changing the elements of the halide material. As discussed above, the stoichiometric ratio of the elements can be adjusted. The proportion of elements can be expressed in terms of mol % or at %.
[0086] In one embodiment, the halide material may be stoichiometric. The halide material may be non-stoichiometric. For example, the halide material may have The phase may contain vacancies which replace some of the elements present in the alloy and maintain the electrical neutrality of the phase within the range.
[0087] In one embodiment, the halide material is Li a-f M a’ RE b Me' kb’ (Cl c Br c’ ) 6-f+(k-3)*b’ where (a+a')= 3, -1≦f≦1, (c+c′)=1, and (b+b′)=1. In certain embodiments, The halide material may include X and X', where c>c' and 0.63≦c / ( c+c')≦0.98.
[0088] In another embodiment, the halide material is Li 3-f RE b Me' k b’ (Cl c B r c’ ) 6-f+(k-3)*b’ where 0≦f≦0.3, ( c+c′)=1, (b+b′)=1, b>0, and b′≧0. ' can be 0. Specific examples of halide materials include Li3Y1(Cl c Br c ’ )6, where 0.63≦c / (c+c′)≦0.87. In embodiments, b>b'>0. Specific examples of halide materials include Li 3-f Y b Me' k b’ (Cl c Br c’ ) 6-f+(k-3)*b’ In the formula: k=3 or 4, and 0.65≦c / (c+c')≦0.98. A more specific example is Li 3-b’ Y b Zr b’ (Cl c Br c’ ) List 6 where 0.72≦c / (c+c')≦0.98. A more specific example is Li 3-f Y b Yb b’ (Cl c Br c’ ) 6-f List of where 0.65≦c / (c+c')≦0.89. A more specific example of this is Li 3-f Y b In b’ (Cl c Br c’ ) 6-f List where 0.69≦c / (c+c′)≦0.95.
[0089] A more specific example of a halide material is Li3Y1(Cl 0.8 Br 0.2 ) 6. Li3Y1(Cl 0.67 Br 0.33 )6, Li3Y1(Cl 0.79 Br 0.2 1)6, Li3Y1(Cl 0.62 Br 0.38 )6, Li 2.95 (Y 0.95 Zr0 .05 )(Cl 0.9 Br 0.1 )6, Li3(Y 0.95 Yb 0.05 )1(Cl 0. 83 Br 0.17 )6, Li3(Y 0.95 In 0.05 )1(Cl 0.9 Br 0.1 ) Six can be mentioned.
[0090] Figure 8 shows the Li3YCl c Br c C in mol% for ionic conductivity of As shown, Cl is at the crystallographic phase transition boundary (see FIG. 8). The percentage of halogenated carbon at the polyvinyl chloride (MPB) is 75 mol %. The nitride material shows a layered crystal structure of LYB until the mol% of Cl is increased to 75 mol%. The halide material may have a crystal structure similar to that of When it is 75 mol %, it can have a crystal structure similar to the non-layered crystal structure of LYC.
[0091] As shown in FIG. 8, when the Cl concentration is increased to about 63 mol%, the halogen The ionic conductivity of the nitride material can be increased to approximately 2 ms / cm. , the Cl concentration is approximately 65 mol% (referred to as "LYBC-65" in FIG. 8) and When the LYBC-80 concentration was adjusted to 80 mol% (referred to as "LYBC-80" in FIG. 8), the halogen The ionic conductivity of the nitride material can be greater than 2 ms / cm. When the ionic conductivity of the halide material is adjusted to the range of 50% to 87mol%, may be at least 2.08 mS / cm or at least 2.20 mS / cm, which is The ionic conductivity is unexpectedly higher than that of
[0092] LYB promotes higher ionic conductivity of LYB than LYC with a non-layered crystal structure. It has a layered crystal structure. The Cl concentration is in the range of 63 mol% to less than 75 mol%. In the case of LYB, the crystal structure of the halide material is distorted and typically It is highly likely that the layer structure is not the normal structure. When the Cl concentration is 75 mol% to 87 mol%, In this case, the halide material has a non-layered crystal structure. As a result, it may be less preferable than the layered structure of LYB due to its higher ionic conductivity. When the halide material has a crystalline structure, it has an ionic conductivity significantly higher than that of LYB. It is unexpected that the ZnO nanoparticles can have high conductivity.
[0093] FIG. 9A shows the Cu K-alpha radioisotope pattern overlaid with the XRD pattern of Li3YCl6. The typical halide material Li3Y(Cl 0.79 Br 0.2 1) Includes a powder XRD pattern of 6. The XRD peaks of a representative halide material are: The peaks are shifted to smaller angles compared to the corresponding peaks in the powder XRD pattern of Li3YCl6. Referring to FIG. 9B, a representative halo measured with Cu K-alpha radiation is The halogenide material Li3Y(Cl 0.67 Br 0.33 )6 powder XRD pattern , combined with the XRD pattern of Li3YBr6. The corresponding peaks are shifted to larger values of 2θ compared to Li3YBr6. Li3Y(Cl 0.67 Br 0.33 )6 is observed to be a single-phase halide material. It is possible.
[0094] In one embodiment, the halide material is Li 3-f RE b Me' k b’ X 6-f+( k-3)*b’ where -1≦f≦1, and (b+b')=1. In certain embodiments, k=3. For example, Me can include In. In another particular embodiment, RE can include Y. For the halide materials, 0.67≦b / (b+b')≦0.93. Yes, Li 3-f Y b In b X 6-f Examples include:
[0095] In another embodiment, the halide material is Li a M a It can be expressed by REX6. In the formula, a>a'>0, (a+a')=3, and 0.942≦a / (a+a')≦0. 958. In one embodiment, M can include Na. In another embodiment, R E can include Y. In another embodiment, X can include Cl. In certain embodiments, the halide material is Li a Na a’ Represented by YCl6 and 0.942≦a / (a+a')≦0.958.
[0096] A more specific example of a halide material is Li3(Y 0.85 In 0.15 ) C l6 and (Li 0.955 Na 0.045 )3YCl6 can be mentioned as an example.
[0097] In one embodiment, the halide material has the formula Li a M a’ RE b Me' b’ Cl c X' c’ where Me may have a smaller ionic radius than RE. In an embodiment, RE can be Y. In one embodiment, Me, which has a smaller ionic radius, is When b'=0, the crystallographic phase transition of the halide material from a non-layered to a layered crystal structure. For example, the crystallographic phase transition from Pnma or P-3m1 to C2 / In another example, the crystallographic phase transition may be a transition to C2 / c or C3 / m. In a further embodiment, the crystallographic phase transition is from orthorhombic to monoclinic crystallography. The transition can be controlled by adjusting the stoichiometric ratio of RE and Me. / (b+b')) t * 0.84 t * 1.16 If b / (b+b')>(b / (b+b')), then the halide material has t * 1.1 6 and b / (b+b')<(b / (b+b')) t * Significantly higher than 0.84 Examples of Me include divalent elements, trivalent elements, and The specific element Me may be a valence element, a tetravalent element, or any combination thereof. Examples include Yb, SC, In, Zr, Ga, or any combination thereof. This can be done.
[0098] In one embodiment, the halide material has the formula Li a M a’ RE b Me' b’ Cl c X' c’ and X′ may have a larger ionic radius than Cl. In the formula, X' can be Br, I, or a combination thereof. In embodiments, RE can be Y. In further embodiments, X' has a larger ionic radius. By adjusting the stoichiometric ratio of Cl and X', when c'=0, the halo It can promote the crystallographic phase transition of the fluoride material from a non-layered structure to a layered crystalline structure. The halogenated material is (c / (c+c')) t * 0.84 <c / (c+c’)<(b / (b +b')) t * If 1.16, then (c / (c+c')) t * 0.84>c / (c+c ') and c / (c+c')>(b / (b+b')) t * Compared to 1.16, They may have properties such as significantly improved ionic conductivity.
[0099] In another embodiment, the halide material has the formula Li a M a’ RE b Me' b’ Cl c X ' c’ where M has an ionic radius greater than Li. In the above, M can be Na, K, Cs, Cu, or a combination thereof. In certain embodiments, RE can be Y. In further embodiments, the larger ionic radius can be M, when a'=0, converts the non-layered structure of the halide material to a layered crystal structure or It may promote a crystallographic phase transition to another non-layered structure. For example, the crystallographic phase transition is P Examples include the transition from nma or P-3m1 to C2 / m or C2 / c. The transition is from an orthorhombic to a cubic elpasolite or monoclinic crystal structure. In certain embodiments, the transition can adjust the stoichiometric ratio of Li to M. In particular, halide materials can be controlled by (a / (a+a')) t * 0.8 4 t * If it is 1.16, then (a / (a+a ')) t * 0.84>a / (a+a') and a / (a+a')>(a / (a+a')) t * Significantly improved ionic conductivity and electrochemical stability compared to 1.16 , compatibility, or any combination thereof.
[0100] In one embodiment, the halide material has the formula Li a M a’ RE b Me' b’ Cl c X' c’ where Me may have a larger ionic radius than RE. In an embodiment, RE can be Y. In one embodiment, Me, which has a larger ionic radius, is When b'=0, the halide material from a non-layered structure to a layered or another non-layered crystal structure. For example, the crystallographic phase transition of Pnma or P-3 Another example is the transition from m1 to C2 / m or C2 / c. The transition can include a transition from orthorhombic to monoclinic crystallography. The crystallographic phase transition can be controlled by adjusting the stoichiometric ratio of RE and Me. In particular, (b / (b+b')) t * 0.84 ) t * 1.16, the halide material has a b / (b+b')>(b / (b+b' )) t * 1.16 and b / (b+b')<(b / (b+b'))t * If it is 0.84 As compared to Me, Me may have significantly improved properties, including ionic conductivity. , divalent elements, trivalent elements, tetravalent elements, or any combination thereof. Specific examples of Me include Bi, La, Ce, Gd, or any combination thereof. Some examples include:
[0101] In one embodiment, the halide material has the formula Li a M a’ RE b Me' b’ Cl c X' c’ and X′ may have a smaller ionic radius than Cl. In the above, X' can include F. In certain embodiments, RE can be Y. In a further embodiment, X' having a smaller ionic radius is in the stoichiometric ratio of Cl to X'. By adjusting the coupling, the non-layered structure of the halide material can be transformed into a layered structure when c'=0. In particular, halide materials may be favored for their crystallographic phase transformation into a layered or other non-layered crystal structure. , (c / (c+c')) t * 0.84 <c / (c+c’)<(b / (b+b’)) t * 1 If .16, then (c / (c+c')) t * 0.84>c / (c+c') and c / (c +c')>(b / (b+b')) t * A noticeable improvement compared to 1.16 , ionic conductivity, electrochemical stability, compatibility, or any combination thereof. may have:
[0102] In one embodiment, the crystallographic phase transition boundary is, by way of example only, Li 3-x*k (Y 1-x M e k+ x )(Cl c Br c’ )6, the following halide materials are used: The MBP of a halide material can be determined by the formula [c / (c+c')] t =0.7 5+12 * (δ * x) in which Me k+ The ionic radius of is r, r=r_Y 3+* (1-δ), and r_Y 3+ But, Y 3+ is the ionic radius of the or by adjusting the substitution of Me' by Li' The MPB of halide materials with crystallographic phase transitions induced by the It can be determined.
[0103] In one embodiment, the halide material is a specific phase that includes a crystallographic phase transition boundary on a compositional phase diagram. In one embodiment, the band range may include a crystalline phase within the band range of Li and M. one of Me and Me', or one of X and X'; The range of concentrations of elements in the material can be expressed as: Crystals with element concentrations in the range of 0.84 to 1.16 times the element concentrations at the crystallographic phase transition boundary In particular, the stoichiometric ratio of elements may vary depending on the crystallographic phase transition of the halide material. In certain embodiments, the halide material may be tailored to promote improved performance and properties. It may consist essentially of crystalline phases within a particular band range. For example, The anions may be present in the same phase. As discussed in the embodiments herein, halides The material may have a low content of impurities or may be essentially free of impurities. For example, the level of impurities can be below levels detectable using conventional detection methods. Thus, "consisting essentially of a single phase" means that the halide material is a complex of the halide material. In addition to the main phase of the compound, the halide material may contain low levels of impurity phases. Impurity phases are intended to mean that the composition may be free of impurity phases. In the present specification, the impurity phase may also be referred to as a parasitic impurity phase.
[0104] In one embodiment, the halide material provides improved properties of the solid electrolyte material and / or The composition may include a specific density that may facilitate performance. In one embodiment, the density is at least 2.5 g / cm m 3 , at least 2.7 g / cm 3 , at least 2.9 g / cm 3 , at least 3.1g / cm 3 , at least 3.3 g / cm 3 , or at least 3.5 g / cm 3 2. 3g / cm 3 In another embodiment, the halide material may be greater than 3.5 g / cm 3 below , 3.4g / cm 3 Below, 3.3g / cm 3 or less than 3.1g / cm 3 3, such as .8g / cm 3 In another aspect, the halide material may have a density of less than The density may be in a range that includes any of the minimum and maximum values shown. In this state, the density of the halide material is less than that of Li3YBr6 and is closer to that of Li3YCl6. The densities may be higher than 100%.
[0105] In one embodiment, the halide materials are significantly improved compared to Li3YBr6. In another embodiment, the halide material may have a solid The thermodynamic and electrochemical stability values can promote improved properties of the electrolyte material. Thermodynamic and electrochemical stability values are obtained using the following cyclic voltammetry method: or linear sweep voltammetry method. The active layer (i.e., working electrode) can be made of two layers: carbon and a halide material. The separator layer may be made of a halide material. The counter electrode layer may be made of an indium halide material. It can be made of indium metal or a lithium-indium alloy. The voltage of the working electrode corresponding to the electrolyte can gradually increase and at the same time, the oxidation current increases to a peak indicating the oxidation of the electrolyte. The onset of the peak can be measured relative to the x-axis. The offset of 0.62V can be obtained by linear extrapolation of the rise, in volts. In addition to peak onset values, thermodynamic and electrochemical stability values were obtained and standardized with respect to the indium counter electrode potential. It can be converted to a quasi-Li / Li+ potential.
[0106] In one embodiment, the thermodynamic and electrochemical stability value is at least 3.60 V, at least 3 It may be greater than 3.57V, such as 3.62V, 3.65V, or at least 3.71V. In this embodiment, the halide material is 4.50V or less, 4.30V or less, 4.19V or less, 4.15V or less, 4.10V or less, 3.85V or less, 3.80V or less, 3.75V or less, or a thermodynamic, electrochemical stability value of 3.71 V or less. The oxide material may have a thermodynamic range that includes any of the minimum and maximum values set forth herein. The electrochemical stability values may include:
[0107] In another embodiment, the halide materials have a higher thermal conductivity than conventional corresponding halide materials. For example, improved ionic conductivity in the bulk, including lithium ionic conductivity, may be achieved. The bulk ionic conductivity may be measured at room temperature (i.e., 22° C.). , ionic conductivity is greater than 0.05 mS / cm, greater than 0.15 mS / cm, at least 0.3 m S / cm, at least 0.5mS / cm, at least 0.8mS / cm, at least 0. 9 mS / cm, at least 1.1 mS / cm, at least 1.5 mS / cm, or less In another embodiment, the halide material has a conductivity of at most 1.9 4.5 mS / cm, at most 1.8 mS / cm, or at most 1.7 mS / cm, Less than mS / cm, Less than 3.4mS / cm, Less than 2.8mS / cm, Less than 2.0mS / cm In another embodiment, the halide material may include a bulk ionic conductivity measured at 22° C. The material may be in bulk in a range that includes any of the minimum and maximum values set forth herein. It may have an on conductivity.
[0108] In further embodiments, the electrolyte materials of the embodiments herein are, in particular, halide materials. However, the crystallographic phase diagram includes a specific boundary including the morphotropic phase boundary (MPB). When the crystalline phase is within the band range, the ionic conductivity can be further improved. , halide materials have a resistivity of at least 1.8 mS / cm, at least 1 .85mS / cm, at least 1.87mS / cm, at least 2.0mS / cm, at least Ionic conductivity in bulk of at least 2.08 mS / cm, or at least 2.45 mS / cm In another embodiment, the halide material may have a conductivity of at most 6.5 mS / cm, at most At most 6.1mS / cm, at most 5.8mS / cm, at most 5.3mS / cm, at most 5.1mS / cm, at most 4.7mS / cm, at most 4.4mS / cm, at most 4 .1mS / cm, at most 3.9mS / cm, at most 3.6mS / cm, at most 3. 2mS / cm, at most 3.0mS / cm, at most 2.8mS / cm, or at most 2 In another embodiment, the bulk ionic conductivity is 0.5 mS / cm measured at 22° C. The halide material may be in a range including any of the minimum and maximum values set forth herein. The bulk ionic conductivity may be
[0109] As used herein, bulk ionic conductivity refers to the ionic conductivity of a pressed powder of an electrolyte material. Electrochemical impedance spectroscopy applied to high density pellets formed by The high density pellet can be measured by using a stainless steel electrode. The measurement can be performed under a hydrostatic pressure of approximately 300 MPa. , may be applied to the high density pellet at frequencies ranging from 7 MHz to 1 Hz with an amplitude of 50 mV. Bulk ionic conductivity may be measured at 22° C. In an embodiment, bulk ionic conductivity versus temperature To aid in understanding certain characteristics of electrolyte materials, such as their ionic conductivity at activated For example, a lower activation energy can reduce the This may suggest that the ionic conductivity varies less with increasing pressure. To determine the ionic conductivity of the bulk, IC(T) was measured at temperatures between 22°C and 150°C. = A × exp(-Ea / RT) and an Arrhenius plot can be constructed based on the equation where A is the pre-exponential constant, Ea is the activation energy in eV, and R is the is the universal constant that converts degrees Kelvin in V, and T is the temperature in degrees Kelvin. The slope of the lot line can be used to determine the activation energy. The activation energy can be in the range of 0.2 eV to 0.5 eV.
[0110] Referring to FIG. 3, a process for forming a solid electrolyte material including a halide material is shown. 300 is shown.
[0111] Process 300 differs from conventional solid-phase syntheses for forming complex halide materials. Conventional processes utilize high energy ball milling or metal halide A mixture of solid reactants (e.g., simple metal halides) at temperatures near or below the melting point of the reactant Solid-state reactions are carried out by directly heating the mixture (the mixture is heated to a temperature of 100° C.). The probability of achieving 100.00% completion of the reaction decreases as the reaction proceeds. This would theoretically take an infinite amount of time. Due to the incomplete reaction of the materials, the conventional solid-state synthesis based on high-energy ball milling The resulting reaction products are higher concentrations of simple metal halides (e.g., lithium halides). It is understood that the catalyst may contain impurities such as tungsten and / or yttrium halides.
[0112] Furthermore, the conventional synthesis of complex halides based on the ammonium-halide route It is noteworthy that it may not be applicable to form complex metal halides. Traditionally, metal halides have been used as starting materials. Some trivalent metal halides and tetravalent metal halides, especially rare earth halides, are stable metal halide hydrates. The complete removal of water molecules from these hydrates tends to form By increasing the temperature, it is possible to obtain a higher concentration of undesirable metal oxides. This may result in the formation of metal oxyhalides or metal oxyhydrate halide compounds. Halide hydrates and metal oxyhalides, especially those containing rare earth metals, are quite Stable compounds, where X is a halogen other than Cl, such as Li3RE(OX)Cl3 The formation of complex compound phases containing high concentrations of Li is unlikely. Compounds such as these are not stable and will likely decompose into simpler compounds.
[0113] The process described in the embodiments of the present disclosure overcomes the problems set forth above.
[0114] The process 300 may include one or more of Li, M, RE, Me, or any combination thereof. A mixture of starting materials containing the above metal compounds is formed in a stoichiometric or non-stoichiometric ratio. The metal compound may be non-hygroscopic. In particular, the starting material may be Ammonium halides, NH4X, where X is Cl, Br, I, F, or any of the foregoing. Any combination may be used. The starting material may be an aqueous solution, an alcoholic solution, or a solution of other polar molecules. The mixture may further include an acid, such as hydrochloric acid or hydrobromic acid, to facilitate acidic synthesis in the reaction mixture.
[0115] In an exemplary embodiment, the metal compound is an oxide, carbonate, sulfate, hydrate, hydroxide, or the like. The salts may include salts of oxalates, acetates, nitrates, or any combination thereof. The heat generating material may be, for example, MeO k Contains oxides containing Other examples include lithium carbonate, sodium carbonate, cesium carbonate, Fe(OH)2, and or Fe(CO3), or any combination thereof. It can be done.
[0116] Referring to FIG. 3, a process 300 includes, as shown in block 302, An exemplary ammonium-containing halide may include forming an ammonium-containing halide from Halides include (NH4) z RE 1-y Me k y (Cl 1-u-p-q Br u F p I q ) 3+z+y*(k-3) , (NH4) z RE 1-y Me k y (Cl 1-u Br u ) 3+z+y*(k-3) , (NH4) z RE 1-y Me k y (Cl 1-p F p ) 3+ z+y*(k-3) , (NH4) z RE 1-y Me k y (Cl) 3+z+y*(k-3) , (NH4) z RE 1-y Me k y (Br) 3+z+y*(k-3) , (NH4) z RE 1-y Me k y (I) 3+z+y*(k-3) or a combination thereof. In certain embodiments, 0.33<=z<=5. Forming the ammonium-containing metal halide material may be carried out in a liquid medium, such as an acidic solution. Exemplary acids include hydrochloric acid, hydrobromic acid, hydrofluoric acid, hydroiodic acid, or any combination thereof. In a further example, any combination of ammonium-containing metal halides may be used. Forming the nitride material may be carried out under certain drying conditions.
[0117] In one embodiment, forming the ammonium-containing metal halide material comprises at most 2 For example, the temperature may be at least 20° C., at least 40° C., at least At least 50°C, at least 70°C, at least 90°C, at least 110°C, or at least In another example, the temperature may be at most 140° C. In another example, the temperature may be at most 200° C., at most 180° C., at most 160° C. In a further example, the ammonium-containing metal halide The article may be formed at a temperature range including any of the minimum and maximum values set forth herein. It is possible.
[0118] In an exemplary synthesis of halide materials, two ammonium-containing metal halides are and one halide anion, and the halide anion of the embodiments herein may be At least one exemplary synthesis can be used to form a halogenide material. The process involves treating an ammonium-containing metal halide to form a metal halide. Reactions between metal halides having different halide anions can be carried out. For example, Li3Y Br6 and Li3YCl6 are formed separately and then mixed to produce Li3YC, as described in more detail below. l 6(1-u) Br 6u The following reaction can be carried out using Li2CO3, Y2O 3. Li3YBr was prepared in a mixture of starting materials containing HBr, NH4Br, and HO. 6 can be formed. 3 * Li2CO3+Y2O3+12 * HBr+10 * H2O→2 * YBr3(H2O )8+6 * LiBr+3 * CO2 6 * NH4Br+2 * YBr3(H2O)8+6 * LiBr → 2 * (NH4)3YB r6+6 * LiBr+16 * H2O
[0119] The above reaction mixture was heated at 140°C under reduced pressure to remove water, and the following reaction took place in the solid state: This can promote the response. 2 * (NH4)3YBr6+6 * LiBr → 2 * Li3YBr6+6 * NH4Br
[0120] The reaction mixture may be further heated at 550° C. to sublime the ammonium bromide.
[0121] Li3YCl6 contains Y2O3, Li2CO3, H2O, NH4Cl, and HCl. It can be formed from a mixture of starting materials including: Y2O3+3 * Li2CO3+10 * H2O+12* HCl → 2 * YCl3(H2O )8+6 * LiCl+3 * CO2 2 * YCl3(H2O)8+6 * LiCl+6 * NH4Cl→2 * (NH4)3YC l6+6 * LiCl+16 * H2O
[0122] The reaction mixture was heated at 140°C under reduced pressure to remove water and the following reaction took place in the solid state: This can be promoted. 2 * (NH4)3YC16+6 * LiCl → 2 * Li3YCl6+6 * NH4C1
[0123] The reaction mixture may be further heated at 550° C. to sublime the ammonium chloride.
[0124] After formation, the Li3YCl6 phase may be mixed with the Li3YBr6 phase in a stoichiometric ratio, and nitrogen The solid-state reaction was carried out under dry conditions in an inert atmosphere such as oxygen to obtain Li3YCl (1-u)*6 Br 6*u can be formed.
[0125] In one particular example, Li3Y(Cl 1-u Br u 6) Forming a mass of material from a solid-state reaction Alternatively, the milling may be carried out in a neutral atmosphere of N2 or Ar to form a powder.
[0126] In a further embodiment, an ammonium-containing metal halide is formed to provide the method of the present invention. This can promote the formation of the halide material of the embodiment. As an example, Li3YCl c X 'c’ Using a halide material represented by (NH 33 Li3Y Br9 and (NH3)3Li3YCl9 were produced using the raw materials described in the embodiments of this specification. In one embodiment, the solutions are mixed and dried at 100 to 170° C. In certain embodiments, the halide compound may be added to the mixture to allow evaporation of the water and acid. The solid-state reaction of the NH3Cl and NH3Br from the charge occurs in parallel at relatively low temperatures. For example, a flux containing LiCl and NH4Cl may be used to It can be formed at temperatures below the fumarolic point. NH4Br can sublime at temperatures above 350°C. Without wishing to be bound by any theory, it is believed that the presence of ammonium halide Li3YCl at relatively low temperatures c X c The formation of a final phase having a uniform distribution throughout the final phase may be achieved. It helps to create a consistent c / c' ratio in the final product, whereas conventional solid-phase synthesis This results in a relatively high variance in the ratio, so that the final product usually contains different c / c' ratios. This is a hybridization reaction using conventional solid-state reactions of LYC and LYB powders, since they may have multiple phases. It should be noted that this may be advantageous over the synthesis of halogenide powders.
[0127] In another embodiment, the sublimation of ammonium may be followed by cooling. In particular, the cooling may be carried out by: It must be carefully controlled to avoid segregation of the crystalline phase of the halide material. In this embodiment, the cooling rate is greater than 40° C. / hour, at least 60° C. / hour, at least 7 0° C. / hour, at least 90° C. / hour, or at least 100° C. / hour, at least 15 It may be 0° C. / hr, or up to 200° C. / hr, such as at least 180° C. / hr. 10 is a halide material, Li3Y(C 0.6 5Br 0.35 ) 6, 1 includes an exemplary process diagram for forming a The ammonium-containing LYB solution and the ammonium-containing LYC solution are formed and combined, and then reacted. Drying of the reaction mixture is carried out at approximately 120° C. Heat the reaction mixture to approximately 550° C. The solid-state reaction is carried out while simultaneously sublimating the ammonium. Accelerated cooling is then performed after sublimation. The halide material Li3YC 4.5 Br 1.5 has a single phase.
[0128] Those skilled in the art will appreciate that additional alkali metal compounds, such as Na2CO3 or NaCl, may be added to the starting material. It is understood that Li can be partially substituted for the Li in the halide material by adding it to the mixture. Similarly, another RE or Me metal compound, such as Fe2O3, may be added to the mixture to It can also substitute for Y in the halide materials.
[0129] In applications, the reaction mixture is sieved to remove larger particles from the solid-state reactants. The larger particles may be from the starting material, residual particles from the starting material, carbon, or other materials. The present invention may include impurities associated with any of the above in any combination.
[0130] In another exemplary synthesis, an ammonium-containing ternary halide is used directly to form a halogen atom. With reference to the exemplary synthesis reaction above, (NH4)3 YCl6 and (NH4)3YBr6 were formed separately, followed by (NH4)3YCl6 and Li The reaction mixture of Cl was combined with the reaction mixture of (NH4)3YBr6 and LiBr in aqueous solution. A mixture containing the four reactants may be dried together to give LiY in a solid-state reaction. (Cl 1-u Br u ) 6. Sublimation of ammonium halide can form 5 It may be carried out at 50°C.
[0131] After sublimation of the ammonium halide, cooling is performed to form the halide material. For example, cooling can be performed in air, dry air, or in a nitrogen atmosphere. For example, at most 100°C, at most 70°C, at most 50°C, or at most 30°C. Cooling temperatures of less than 200° C. may be applied. In certain embodiments, cooling is achieved by drying at room temperature. It may be carried out in ambient air. Optionally, Ar or N2 may be used to aid in cooling. .
[0132] In another embodiment, the compound comprises at least two halide anions in any given ratio. The ammonium-containing metal halide may be formed in a single step. The ternary halides are mixed in stoichiometric or non-stoichiometric ratios to produce ammonium halides. The ammonium halides can be melted in the presence of ammonium salts. In one example, each ternary halide contains two metal cations and one The halide anions may include three different halide anions, and the halide anions may be different between the ternary halides. In certain instances, the ternary halide may include two halide anions. The metal cations may be the same or different between the ternary halides. The typical heating temperature is up to 600 to help melt the material and promote reactions in the solid state. The heating temperature may further aid in the escape of ammonium from the halide material. Heating can be carried out in a neutral atmosphere of nitrogen or argon. Cooling can be carried out to remove the halogens. The nitride material may be allowed to solidify.
[0133] An exemplary synthesis process is shown below. The reactions shown are Li3YCl6, Li3Y Ammonium-containing metal halides in one step from starting materials including Br6 and NH4Br One skilled in the art can use various ratios of starting materials to form halogenides. It will be appreciated that halide materials can be formed having predetermined ratios between the anions of the compounds. It will be. Li3YCl6+Li3YBr6+6 * NH4Br→2 * (NH4)3Li3YCl 3Br6
[0134] Ammonium halide can be sublimated at a heating temperature of 250°C to 650°C. In this method, a dopant material such as a Me compound is added to the melt to form one of the halide materials. The substitution of the above metal elements can be promoted. The reaction is carried out on quartz, alumina, silica-alumina, B The controlled melting can be carried out in crucibles made of N, vitreous carbon, or graphite. Cooling may be applied to the melt to solidify the halide material.
[0135] In certain embodiments, the cooling rate is controlled to promote a particular crystal growth rate. Allows for the growth of single crystals with macroscopic sizes such as large 10 cm single crystal blocks For example, cooling can be performed by applying an external heat field at a cooling rate of 10°C / hour to 50°C / hour. The crystal growth rate can be at least 0.2 mm / hour and at least 0. 3 mm / hour, or at least 0.5 mm / hour. The long speed is at most 8mm / hour, at most 6mm / hour, at most 5mm / hour, It may be at most 10 mm / hour, such as at most 3 mm / hour, or at most 1 mm / hour. do.
[0136] In another particular embodiment, the crystal growth rate is adjusted to promote the growth of polycrystalline crystals by: at least 8 mm / hour, at least 10 mm / hour, at least 15 mm / hour, or The growth rate may be relatively fast, such as at least 20 mm / hour. is at most 80mm / hour, at most 70mm / hour, at most 60mm / hour, The rate of change may be at most 50 mm / hour, or at most 40 mm / hour.
[0137] In certain embodiments, the solidification is performed in order to promote the growth of crystals having a particular crystal orientation. This can be accomplished by applying a thermal gradient to the melt zone. A crucible with a ratio of >5 can be used to facilitate the solidification of the block under a thermal gradient. This process may be particularly suitable for crystals that are anisotropic. In a particular example, the crystallization rate is greater than 10°C / cm. A strong thermal gradient such as above may be applied.
[0138] In another embodiment, the crystals that are anisotropic with respect to magnetic permeability or dielectric constant, oriented crystal growth, are This can be done using a strong permanent magnetic field, solidification under a strong electric field, or any combination thereof. do.
[0139] In another particular embodiment, the pellets are elongated in the crystallographic direction and have a higher ionic conductivity. For example, single crystal pellets have a specific crystallographic orientation. In a further example, the ceramic halide material may be prepared by casting. The oriented multi-layer structure may be formed by feeding, compressing, pressing, heating, molding, or any combination thereof. The formation of crystalline halide materials may be promoted. In certain instances, Using single crystal pellets of the crystalline halide, oriented ceramic halide materials can be formed. Optionally, an X-ray goniometer may be used to identify the crystal orientation. Using a supporting seed layer with a lattice parameter close to that of the oriented ceramic material, Solidifying in a medium can help maintain the oriented polycrystalline structure.
[0140] Single crystal halide materials form in smaller chunks of a few millimeters. Or dense blocks or large indentations up to tens of centimeters in size. In an exemplary application, the single crystals are milled to form a fine powder of single crystal particles. In a further example, the single crystal ingot or block may be sliced into thin sheets. For example, the thin sheet may have a thickness of 5 microns to 500 microns. The crystallographic direction having the highest conductivity can be through the thickness of the thin sheet. The crystals can be sliced. For example, halide materials can be oriented. has higher ionic conductivity than the different crystallographic orientations <hkl>(or <hklm>) and the thickness of the slice is <HKL> (or <hklm>) crystallographic orientation.
[0141] In certain instances where incompatible melting occurs, the resulting parasitic phase is the upper Parasitic phases may be removed from the solidified ingot, such as by grinding the ingot. In the case of dopant, it can be at most 10 vol.% of the crystal. Excessive amounts of dopant material are added to the melt. Adding excess LiX or NaX helps to reduce the formation of parasitic phases, for example in autoclaves containing excess LiX or NaX. This may help promote the formation of stoichiometric single-phase crystals under autoflux conditions.
[0142] Forming halide materials using crystal growth can be achieved by using Li, RE, Me, or M It helps to further reduce one or more unreacted simple halide phases containing e metal elements. The process simply obtains a form of halide material essentially free of metal halide phases. This can promote the development of
[0143] In another embodiment, ammonium-containing halides are mixed and co-melted to form crystalline halides. For example, ammonium-containing halides may be formed using the methods described herein. A reaction mixture containing an ammonium-containing halide, which may be formed separately as described in the embodiments. The mixture may be combined, dried, and co-melted. In a particular example, the above exemplary synthesis reaction may be For reference, (NH4)3YCl6 and (NH4)3YBr6 were separately formed, and then (NH The reaction mixture of (NH4)3YCl6 and LiCl was dissolved in water and cooled to room temperature. The reaction mixture containing the four reactants may be combined and heated together to dryness. The halide material is then melted and reacted in a solid-state reaction at temperatures up to 600°C. Li3Y(Cl 1-u Br u ) 6 can be formed. Sublimation can occur at elevated temperatures. In some cases, the ammonium halide phase can reach temperatures up to 80°C. The solidification can be removed by decomposition at a higher temperature, such as at 0° C. It may be carried out as described.
[0144] The removal of ammonium halide is carried out by removing the ammonium halide from the halide material. The ammonium halide can be monitored by collecting and weighing it. In some cases, a certain amount of the ammonium halide phase may be removed completely. For example, heating may cause the ammonium halide portion to remain in the ammonium halide material. To allow partial or complete sublimation and / or decomposition, temperatures in the range of 350°C to 800°C are used. The reaction can be carried out at 35° C. for at least 15 minutes and at most 24 hours. Decomposition occurs when undesirable substances such as water, CO2, ammonia, and halogens are released by evaporation. This can be useful in removing unwanted reaction products.
[0145] In one embodiment, the halide material is essentially free of ammonium halide phase. In at least one embodiment, the halide material may be At least 10 ppm, at least 100 ppm, at least 300 ppm by weight of the total material ppm, at least 2 ppm, such as at least 500 ppm, at least 0.5 wt. %, or at least 0.2% by weight based on the total weight of the halide material, such as at least 1% by weight. Alternatively or additionally, the composition may contain a specific content of residual ammonium halide in terms of percent by volume. The halide material may be at most about 3% by weight based on the weight of the halide material. The halide material contains up to 5% by weight of ammonium halide. The inclusion of an ammonium fluoride phase helps improve the ionic conductivity of the halide material. Note that it is possible.
[0146] After cooling and / or solidification, the halide material is formed, as shown in block 304. It can be done.
[0147] The corresponding Halide materials typically contain higher impurity contents and Stockbarger, Gradient Freezing, Czochralski, or Bagdasarov (water When used to grow crystals according to the process of Bridgman et al. It is more likely to melt and the crystals that form have a higher content of impurities and parasitic phases Possible. Using simple compounds as starting materials in the melt to directly grow crystals. This can also result in higher contents of impurities and parasitic phases. The parasitic phase is LiX and Me k+ X k and the like, wherein X is a halogen. The process described in the embodiments herein is similar to the corresponding conventional halogen Facilitates the formation of halide materials having improved purity compared to halogenide materials. It is worth noting that the higher purity can reduce the amount of halogens. In certain embodiments, the halogenide material may be provided with a halogen atom or a halogen atom. The oxide material consists of a single phase.
[0148] In a further embodiment, the halide material is Me, such as YN. x N k , LiN3, etc. x In one example, the impurities may include metal nitrides containing N, N, or any combination thereof. , metal nitride Me x N k The content of is at most 0.1 weight percent of the halide material. % by volume, at most 500 ppm, at most 300 ppm, at most 100 ppm, at most 50 ppm, at most 40 ppm, at most 30 ppm, at most 20 ppm, or more It may be at most 0.3% by weight based on the weight of the halide material, such as at most 10 ppm. In another example, the metal nitride Me x N k The content is small relative to the weight of the halide material. halogens, such as at least 0.5 ppm, at least 1 ppm, or at least 2 ppm; In another embodiment, the metal nitride may be at least 0.2 ppm by weight of the metal nitride material. Me x N k The content of is within a range including any of the minimum or maximum values shown in this specification. It could be in the vicinity.
[0149] In one example, metal nitride M x The N content is at most 100% by weight of the halide material. 0.1% by weight, at most 500 ppm, at most 300 ppm, at most 100 ppm, At most 50 ppm, at most 40 ppm, at most 30 ppm, at most 20 ppm, or at most 0.3% by weight based on the weight of the halide material, such as at most 10 ppm. In another example, the metal nitride M x The N content is based on the weight of the halide material. At least 0.5 ppm, at least 1 ppm, or at least 2 ppm In another embodiment, the metal nitride may be at least 0.2 ppm by weight of the metal nitride material. Monster M x The N content is within a range including any of the minimum and maximum values shown in this specification. It could be in the vicinity.
[0150] In one example, the total metal nitride content is at most 0.5% by weight of the halide material. 1% by weight, at most 500 ppm, at most 300 ppm, at most 100 ppm, at most 50 ppm, at most 40 ppm, at most 30 ppm, at most 20 ppm, or At most 0.3% by weight based on the weight of the halide material, such as at most 10 ppm. In another example, the total metal nitride content may be less than the weight of the halide material. Halides, such as at least 0.5 ppm, at least 1 ppm, or at least 2 ppm In another embodiment, the total amount of metal nitrides is at least 0.2 ppm by weight of the material. The content can be in a range including any of the minimum or maximum values set forth herein. .
[0151] In this disclosure, alkali nitrides and Me x N k The content of metal nitrides such as The complex metal halides can be hygroscopic, so the The conductive materials can be dissolved in water. Metal nitrides are not hygroscopic and can be dissolved in aqueous solutions. After filtration, the metal nitrides can be collected and analyzed. It can be detected using X-ray diffraction analysis. At contents below 0.2% by weight, LECO is used It can be done.
[0152] In one embodiment, the halide material may include a crystal structure that includes stacking faults. Defects are in the crystal structure caused by a shift in the position of an occupied atom or the position of a vacant atom. It refers to defects in the crystal structure that result in disordering of the crystallographic planes in the crystal structure.
[0153] In certain embodiments, the halide material is a material that promotes improved properties of the halide material. The stacking faults can be detected by X-ray powder diffraction. This can result in changes in the X-ray diffraction pattern, particularly non-uniform broadening of certain X-ray diffraction peaks. In this disclosure, stacking faults can be identified by X-ray powder diffraction analysis of halide-based materials. , and Boulineau et al., which are incorporated herein by reference in their entireties. al.,Solid State Ionics 180(2010)1652-165 According to the stacking fault quantification method described by [9], T OPAS4.2 or FullProf (version 7.30, released in March 2020) Software such as TOPAS 4.2 or FullProf version 7.3 DIFFaX stains caused by using another version or software equivalent to 0 can be determined by using the eigenvalues of the α- and β-terminal valences of the α-terminal valences and the Rietveld refinement. The quantification method is to simulate the X-ray diffraction patterns of halide-based powders. The simulation may include fitting a lattice model to define the primary blocks of the crystal structure. These primary blocks may consist of slabs and inter-slab spaces. The primary blocks are then stacked according to one of two or more possible stacking vectors. The exclusive occurrence of only one of the stacking vectors results in full stacking, i.e. 0% The change in the stacking vector in the stacking direction of the crystal structure causes stacking faults. Fitting the simulation to the X-ray diffraction patterns of halide-based materials is the process of varying one or more parameters of a crystal structure (also called "parameter refinement"). (known as a method for identifying and defining stacking faults) and implementing a least squares difference minimization algorithm. and quantifying.
[0154] In further embodiments, the halide material is at least 25%, at least 30%, At least 40%, at least 50%, at least 60%, at least 70%, at least At least 20% stacking faults, such as at least 80%, or at least 90% stacking faults. In certain embodiments, the stacking of atomic layers may be completely disordered. For example, the crystal structure may contain 100% stacking faults. In another embodiment, the stacking faults are , at most 95%, at most 92%, at most 90%, at most 85%, at most 80% , at most 75%, or at most 70%, etc. The structure may be any of the minimum and maximum percentages shown herein. In a particular example, the solid electrolyte material may include stacking faults in a range of at least 50 % stacking faults. The solid electrolyte material is a halide material having more than 50% and at most 100% stacking faults. may include.
[0155] In one embodiment, the halide material is a powder, such as a particle of a complex metal halide. In one embodiment, the powder has a particle size of at least 0.3 microns, at least 0. 5 microns, or at least 1 micron, such as an average particle size of at least 0.1 microns ( In another embodiment, the average particle size is at most 1 mm, at most 800 microns. Ron, at most 500 microns, at most 200 microns, at most 100 microns, At most 50 microns, at most 10 microns, at most 5 microns, or at most 1 micron In certain instances, the powder may be within the minimum or maximum values set forth herein. In another aspect, the powder may comprise particles having an average particle size inclusive of any of the following ranges: It may comprise particles or weakly agglomerated particles.
[0156] In a further aspect, the particles promote improved formation and performance of the electrolyte and / or electrode. For example, the particles may be spherical or elongated. In another example, the particles may have the shape of rods, flakes, or needles. The halogenide material can be selected according to the 2D or 1D anisotropy in ionic conductivity. do.
[0157] In another embodiment, the powder is in the form of an electrolyte and / or electrode having improved ionic conductivity. The particles may include particles having a particular average aspect ratio of length:width that promotes the formation of the nanoparticles. The average aspect ratio is at least 1.2, at least 1.5, at least 2, at least At least 1, such as 2.3, at least 2.5, at least 2.8, or at least 3 In another example, the average aspect ratio may be at most 30, at most 25, at most 22, at most 20, at most 15, at most 12, at most 10, at most 8, at most The particles may be as small as 5, or as large as 4. Furthermore, the particles may be within the minimum and maximum values set forth herein. The average aspect ratio may range from any of the above.
[0158] In another embodiment, the halide material may be single crystalline. The crystal may be in the form of a single crystal sheet, a single crystal film, a single crystal block, a single crystal ingot, or in another form. In a further embodiment, the halo The oxidized material may be a ceramic material. The ceramic material may be made up of ceramic particles, monoliths, or the like. The material may include, for example, crystalline particles, crystalline particles, or any combination thereof.
[0159] In another embodiment, the halide material has a crystallographic alignment that has a higher ionic conductivity. For example, the halide material may be oriented as an oriented single crystal or as an oriented ceramic. It could be Mick.
[0160] In one embodiment, the solid electrolyte comprises any of the halogens described in the embodiments herein. In certain applications, the solid electrolyte material may comprise a halide material. In at least one application, the solid electrolyte material is a mixture of another material in addition to the halide material. For example, alternative materials may include solid state electrolyte materials other than the halide materials. The material may include a material, an electronic conductive material, an additive, an active electrode material, or a combination thereof. Cut.
[0161] In one embodiment, the composite ionically conductive layer may include a solid electrolyte material and an organic material. The organic material may be a binder material, a polymer electrolyte material, or a combination thereof. In another example, the composite ion-conducting layer may include a plasticizer, a solvent, or the like. Exemplary organic materials include polytetrafluoroethylene (poly tetrafluoroethylene, PTFE), polyvinylidene fluoride, PVdF), fluorinated rubber, polypropylene, ethylene-propylene-diene monomer (et hylene-propylene-diene monomer, EPDM), sulfonated EPDM, natural butyl rubber ( natural butyl rubber (NBR), paraffin wax, polypropylene carbonate, Polyisobutylene, Polyvinylpyrrolidone, Polymethylmethacrylate, Poly(propylene Poly(vinyl oxide), Poly(vinylidene fluoride), Poly(acrylonitrile) , poly(dimethylsiloxane), poly[bis(methoxyethoxyethoxide)-phospha Zene], polyethylene carbonate, polypropylene glycol, polycaprolactone, Poly(trimethylene carbonate), hydrogenated nitrile butadiene rubber, poly(ethylene acetate) vinyl acetate), high density polyethylene, low density polyethylene, polyurethane, or any of these In another example, the composite ion conductive layer may include a lithium salt. Exemplary lithium salts include LiSbF6, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), LiC(S O2CF3)3, LiAsF6, LiClO4, LiPF6, LiBF4, LiCF3S O3, or any combination thereof.
[0162] In one embodiment, the catholyte material may include a solid electrolyte material that includes a halide material. The catholyte material may also include a cathode active material. An example of a cathode active material is: Lithium-containing transition metals, such as, but not limited to, Li(NiCoAl)O2 and LiCoO2 transition metal oxides, transition metal fluorides, polyanions, and fluorinated polyanion materials, and transition Metal sulfides, transition metal oxyfluorides, transition metal oxysulfides, transition metal oxynitrides, etc. or any combination thereof. In a particular example, the catholyte material may include The cathode may include particles of cathode active material, at least some of the particles being coated with a solid electrolyte material. In a more specific example, at least a portion of the surface of each particle of the cathode active material may be In another more specific example, the cathode active material may be coated with a solid electrolyte material. Most or all of the surfaces of the particles of the material may be coated with the solid electrolyte material.
[0163] In another embodiment, the anolyte material may include a solid electrolyte material that includes a halide material. The anolyte may also include an active material. Exemplary anode active materials include synthetic graphite. Graphite, graphite carbon fiber, resin-burned carbon, pyrolysis vapor-grown carbon, coke, mesocarbon Mesocarbon microbeads (MCMB), furfuryl alcohol derivatives Fatty carbon, polyacene, pitch-based carbon fiber, vapor-grown carbon fiber, natural graphite, Carbon materials such as graphitizable carbon, metallic materials including lithium metal, lithium alloys, etc. , oxides, nitrides, tin compounds, silicon compounds, or combinations thereof. In some cases, the anolyte material may include an electronically conductive additive. Examples of materials include carbon fiber, carbon powder, stainless steel fiber, and nickel-coated graphite. In a particular example, the positive The electrolyte material may include particles of an active material, at least some of the particles being coated with a solid electrolyte material. In a more specific example, at least a portion of the surface of each particle of the active material may be In another more specific example, the particles of the active material may be coated with a solid electrolyte material. Most or all of the surfaces may be coated with a solid electrolyte material.
[0164] In further embodiments, the solid electrolyte material is a catholyte layer, an anolyte layer, or an electrolyte layer; or combinations thereof. The optical fiber may be a component of an optical fiber optical device.
[0165] In another embodiment, a structure, such as a portion of an electrochemical device, may include a solid electrolyte layer, an electrode layer, and an intermediate layer disposed between the solid electrolyte layer and the electrode layer, At least one of the electrode layers may include a solid electrolyte material. The chemical device may include a solid-state lithium battery. Referring to FIG. , an electrolyte layer 402, and an intermediate layer 406 disposed between the electrode layer 404 and the electrolyte layer 402. A cross-sectional portion of an exemplary solid-state battery 400 is shown, including an intermediate layer 40. 6 may include a solid electrolyte material. In a particular example, the electrode layer 404 may include an anode layer. The intermediate layer 406 can include an anolyte layer adjacent to the anode layer. In another particular example, the electrode layer 404 can include a cathode layer, The intermediate layer 406 can include a catholyte layer adjacent to the cathode layer.
[0166] The intermediate layer 406 may be at most 400 microns, at most 300 microns, at most 20 At most 50, such as 0 microns, at most 100 microns, or at most 50 microns can include a thickness of 0 microns. Additionally, or alternatively, the intermediate layer is at least 5 microns , can have a thickness of at least 8 microns, at least 10 microns, at least 12 microns, or at least 20 microns. Further, in certain examples, the thickness of the intermediate layer can be in a range including either of the minimum and maximum values shown herein .
[0167] FIG. 7A includes a diagram showing a portion of an electrochemical device 700 according to an embodiment, including a solid electrolyte layer 704 including a solid electrolyte material of an embodiment herein that covers an electrode layer . In particular, the solid electrolyte material can include a halide material including at least one of Cl and F, and optionally another halogen element such as Br, I, or both. Examples of the electrode layer can include a cathode layer including a cathode active material, and at least a portion of the cathode active material can be in contact with the solid electrolyte material. As shown, the electrode layer 702 and the electrolyte layer 7 04 are in contact with each other. In certain embodiments, when a voltage is applied to the electrochemical device 700 , the solid electrolyte layer 704 can be capable of forming a concentration gradient of one or more halogen anions . For example, the solid electrolyte layer 704 can include Li3Y(Br Cl u 1-u )6, where 0 < u < 1, and when a voltage is applied, a concentration gradient of Br−, Cl - , or both can be formed. More specifically, under voltage, the solid electrolyte layer 704 can include a chlorine-deficient region proximal to the electrode layer 702, and the chlorine-deficient region can include a lower concentration of chlorine compared to a region of the solid electrolyte layer 704 away from the electrode layer 7 02 . The concentration of the halogen anion is the concentration in at% or mol% relative to the total anions is obtained.
[0168] Referring to FIG. 7B, the electrochemical device 750 includes a solid electrolyte layer 704 and an electrode layer 7 02 may be included. In a particular example, the electrode layer 702 may be a cathode layer. As shown , the electrochemical device 750 includes an intermediate layer 70 3 between the solid electrolyte layer 704 and the electrode layer 702, and at least a portion of the intermediate layer 703 may be in contact with at least a portion of the cathode active material . As shown, the intermediate layer 703 may be in contact with the solid electrolyte layer 704 and the electrode layer 702 . In a particular example, the intermediate layer 703 may include a lithium-metal halide material different from the solid electrolyte material, and the lithium-metal halide material may include at least one halogen anion that is the same as the halogen anion of the solid electrolyte material . For example, the intermediate layer may be Li M 3-x-f M f RE 1-y Me k y (Cl 1-p F p ) 6-x+y*(k- 3) and may include a lithium-metal halide represented by, where -1 <= x <= 1, 0 <= y <= 1, 0 <= p <= 1 / 3, and 0 <= f <= 0.3. In a particular embodiment , the solid electrolyte layer may include an electrolyte material including a halide material represented by Li 3-x-f M f RE 1-y Me k y (Cl 1-p F p ) 6- x+y*(k-3) , where 0 < p <= 1 / 3, and the intermediate layer is Li , 1-x-f M f RE 1-y Me k y F 4-x +y*(k-3) The lithium-metal halide may be represented by the formula: 3<=x<=0.3, 0<=y<=1, 0<=f<=0.3. A more specific example: The solid electrolyte material is Li3Y(Br u Cl 1-u ) 6, wherein <u<1であ The middle layer is Li 3(1-z) Y (1+z) Lithium-metal halide represented by Cl6 The solid electrolyte material may include a halogenide, where 0<=z<0.3. This can help stabilize the interlayer over time. For example, the solid electrolyte material can be In order to reduce the decomposition of the intermediate layer, which may be due to the depletion of halogen anions at The solid electrolyte layer 704 may serve to sustain one or more halogen anions over time. , Li in electrochemical devices + It further helps to maintain ionic current, cationic current, or both. Li + The ions are charged under a voltage such as that shown in FIG. 7B. 751.
[0169] In a further embodiment, the intermediate layer 703, when placed in contact with the cathode layer, provides improved In particular, the intermediate layer may have improved oxidative stability compared to an intermediate layer containing Li3YBr6. In certain embodiments, the intermediate layer may exhibit reduced decomposition under oxidizing conditions. - Concentration It may be possible to form a gradient in the conductivity of the intermediate layer, which allows the intermediate layer to self-passivate under cell operation. More specifically, under oxidizing conditions, the remote positions may function as an oxidation layer. Cl in position - A higher concentration of Cl compared to the concentration of - may be formed in the vicinity of the cathode layer. More specifically, Cl - The concentration of is from the surface in contact with the cathode layer to the intermediate layer. It may be reduced in the direction towards the opposite surface.
[0170] In certain embodiments, the intermediate layer 703 is adapted to improve the performance or formation of an electrochemical device. It may be a passivation layer having a certain thickness that can promote the The interlayer is at most 1 micron, at most 800 nm, at most 600 nm, at most 40 0nm, at most 300nm, at most 200nm, at most 100nm, at most 80 nm, at most 60nm, at most 50nm, at most 40nm, at most 20nm, In another example, the intermediate layer may comprise a thickness of at least 10 nm, or at most 8 nm. At least 1 nm, at least 2 nm, at least 3 nm, at least 4 nm, at least 5 nm m, may comprise a thickness of at least 10 nm, at least 20 nm, or at least 50 nm. Additionally, the intermediate layer may be in a range including any of the minimum and maximum values set forth herein. In a particular example, the intermediate layer may have a thickness of at least 2 nm and at most 5 nm. The thickness of the substrate may range from 0.1 to 10 mm.
[0171] In one embodiment, the intermediate layer may be formed in situ from a solid electrolyte material. In the present invention, an intermediate layer may be formed at the interface between the solid electrolyte material and the cathode active material. For example, the intermediate layer may be formed at an interface between particles of the cathode active material and particles of the solid electrolyte material, Particles of a cathode active material are coated with one or more particles of a solid electrolyte material. In another example, referring to FIG. 7A, at the interface between the solid electrolyte layer 704 and the electrode layer 702, The intermediate layer may be formed from a solid electrolyte material.
[0172] In a further embodiment, forming the intermediate layer comprises forming a solid electrolyte material and a cathode active material. The method may include applying a voltage to an electrochemical device, such as 700, including an interface between the In one example, the voltage may be at least 3.0V, at least 3.6V, or at least 4.0V. V, at least 4.5 V, or at least 5.0 V. So the voltage can be at most 5.1V.
[0173] In one embodiment, forming the intermediate layer comprises at least one of Cl and F. In one exemplary embodiment, the method includes partially decomposing a solid electrolyte material. The solution material is Li3Y(Br u Cl 1-u )6 Under voltage, Li3Y(Br u Cl 1-u )6 is Li3Y(Br u Cl 1-u ) undergoes electrochemical reactions that may cause partial decomposition of 6, Li3YBr at the interface 6u and Li3YCl (1-u)6 This can result in the formation of Li3YCl (1-u)6 Li3 may be formed into a thin intermediate layer in contact with the cathode active material. YBr 6u is a solid electrolyte material Li3Y(Br u Cl 1-u )6 rearranged and absorbed It can be collected.
[0174] 7A and 7B, partial decomposition of the solid electrolyte layer 704 under voltage occurs during In addition, the formation of an interlayer 703 may occur in the solid electrolyte layer 704. As shown, the cathode active material included in the electrode layer 702 may form a depletion region. The proximal region 756 has a lower concentration of C compared to the region 758 distal to the cathodically active material. It may contain l- and / or F-.
[0175] The electrolyte of an electrochemical device using the solid electrolyte material of the embodiment of the present specification, the composite ion forming an electrically conductive layer, an anode, a cathode, an anolyte, a catholyte, an intermediate layer, or another component. Known techniques may be used to achieve this. Such techniques include, but are not limited to, sting, molding, depositing, printing, pressing, heating, etc., or any combination thereof. To form a multi-layer structure, layers such as electrolyte, electrode, anolyte, and catholyte are can be formed separately and then laminated to form a multi-layer structure. A stack of layers is formed, followed by pressing, heating, drying, or any combination thereof. Further processing may be performed to form the final formed multi-layer structure.
[0176] In certain embodiments, the single crystal block or ingot is in intimate contact with the electrodes and electrolyte. To ensure contact, the cathode or may be fabricated together with the anode active material.
[0177] In another particular embodiment, single crystal blocks and ingots of halide materials are prepared by a The anolyte layer or the catholyte layer may be grown directly around the particles of the node and / or cathode active material. In one embodiment, the anolyte layer or catholyte layer is formed by dissolving the anode or cathode active material. In another embodiment, the catholyte layer or the single crystal halide material may include inclusions containing a metal. The anolyte layer is formed by the anode or cathode densely packed in a single crystal ingot or block. The material may include a photoactive material.
[0178] Many different aspects and embodiments are possible. After reading this specification, those skilled in the art will understand that these aspects and embodiments are It will be understood that these are merely illustrative examples and are not intended to limit the scope of the invention. The embodiment may be according to any one or more of the embodiments listed below.
[0179] Embodiment Embodiment 1. At least two halides selected from the group consisting of F, Cl, Br and I. Contains fluoride anion, Li 3-x-f M f RE 1-y Me k y (Cl 1-u-p-q Br u F p I q ) 6-x+y*(k-3) The solid, including halide materials represented by A biological electrolyte material, wherein -1<=x<=1, 0<=y<=1, and 0<= u<1, 0<=p<=1 / 3, 0<=q<=1 / 6, 0<(u+p+ q)<1, 0<=f<=0.3, and M is at least one alkali other than Li. RE is a rare earth element, k is the valence of Me, and Me is I Group IIB elements, Group IVB elements, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, At least one element selected from the group consisting of Al, Sn, Pb, Bi, Sb, Mg, Ca, Ga, and Ge. Another element is Me, which is different from RE in that the halide material One or more binary halide phases with a total content of not more than 10% by weight based on the total weight of the % or less in total and one or more oxyhalide phases with a total content of 7% or less by weight and at least one ternary halide phase. Embodiment 2. The halide material has no peaks between 5° and 13° 2-theta. and an X-ray diffraction pattern measured using Cu K-alpha radiation. The solid electrolyte material according to embodiment 1. Embodiment 3. The halide material is 9% by weight or less based on the total weight of the halide material. binary halide phase, 8% by weight or less, 7% by weight or less, 6% by weight or less, 5% by weight or less, 4 % by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or 0.5% by weight or less 3. The solid electrolyte material of embodiment 1 or 2, comprising a halide phase. Embodiment 4. The binary phase comprises a lithium halide phase and the halide material is a halogen Lithium halide phases not exceeding 7% by weight based on the total weight of the hydride material, not exceeding 6% by weight, % by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or 0.5% by weight or less % or less of a lithium halide phase. quality material. Embodiment 5. The binary phase comprises a rare earth halide phase and the halide material is a halogen. Rare earth halide phases not exceeding 10% by weight, 7% by weight, 5% by weight, based on the total weight of the halide material % by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or 0.5% by weight or less 5. The solid state battery according to any one of claims 1 to 4, comprising a rare earth halide phase of 0.01% or less. solute material. Embodiment 6. The halide material is 6% by weight or less based on the total weight of the halide material. Ternary halide phase, 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1 % or less by weight of a ternary halide phase, or 0.5% or less by weight of a ternary halide phase. The solid electrolyte material according to any one of claims 1 to 5, Embodiment 7. A ternary halide phase comprising a ternary phase containing two anions, the halogen The halide material contains two anions in an amount of 7% or less by weight based on the total weight of the halide material. Original halide phase, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or 0% by weight or less Any of embodiments 1-6, comprising a ternary halide phase containing 0.5 wt.% or less of two anions. 13. The solid electrolyte material according to claim 12, Embodiment 8. The ternary phase comprises a lithium-rare earth halide phase, and the halide material However, lithium-rare earth halides are not more than 7% by weight based on the total weight of the halide materials. phase, 5% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or 0.5% by weight or less 7. The solid according to any one of claims 1 to 6, comprising a lithium-rare earth halide phase of Electrolyte materials. Embodiment 9. The halide material is 6% by weight or less based on the total weight of the halide material. oxyhalide phase, 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less; 9. The method of claim 1, further comprising: 13. The solid electrolyte material according to claim 12, Embodiment 10. The oxyhalide phase comprises a rare earth oxyhalide phase, The halogenide material contains 7% by weight or less of rare earth oxyhalides based on the total weight of the halide materials. Nitride phase, 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, or any of embodiments 1 to 9, comprising 0.5 wt. % or less of a rare earth oxyhalide phase. 1. The solid electrolyte material according to claim 1. Embodiment 11. The halide material is a binary halide phase, a ternary halide phase, and and oxyhalide phases. 11. The solid electrolyte material according to any one of embodiments 1 to 10. Embodiment 12. The halide material is a binary halide phase, a ternary halide phase, and 12. The solid electrolyte according to any one of claims 1 to 11, which does not contain an oxyhalide phase. quality material. Embodiment 13. At least one selected from the group consisting of F, Cl, Br, and I in a single phase. An electrolyte material comprising a halide material containing at least two halide anions, The halogenide material is Li 3-x-f M f RE 1-y Me k y (Cl 1-u-p-q Br u F p I q ) 6-x+y*(k-3) where -1<=x<=1 and 0 <=y<=1, 0<=u<1, 0<=p<=1 / 3, 0<=q<=1 / 6, 0<(u+p+q)<1, 0<=f<=0.3, and M is less than or equal to Li. RE is a rare earth element; k is Me The valence of Me is the group IIIB elements, group IVB elements, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Al, Sn, Pb, Bi, Sb, Mg, Ca, Ga, and Ge At least one element selected from the group consisting of Me is different from RE. quality material. Embodiment 14. The halide material is monoclinic, trigonal, hexagonal, or orthorhombic. 14. The solid electrolyte material according to any one of embodiments 1 to 13, comprising a crystal structure represented by the formula: Embodiment 15. The halide material comprises a crystal structure represented by a rhombohedral space group. 15. The solid electrolyte material according to embodiment 14. Embodiment 16. A method for producing a crystalline solid having a unit cell smaller than that of Li3YBr6. 16. The solid electrolyte material according to embodiment 14 or 15. Embodiment 17. The peaks in the powder diffraction pattern of the halide material are Li3YBr6 1, which is shifted to a higher angle compared to the corresponding peak in the powder diffraction pattern. 17. The solid electrolyte material according to any one of claims 1 to 16. Embodiment 18. The halide material is Li 3-x-f M f RE 1-y Me k y (Cl 1-u-p Br u F p ) 6-x+y*(k-3) The embodiment 1 to 17 of the present invention is represented by 13. The solid electrolyte material according to claim 12, Embodiment 19. The halide material is Li 3-x-f M f RE 1-y Me k y (Cl 1-u Br u ) 6-x+y*(k-3) Any of embodiments 1 to 18, represented by 1. The solid electrolyte material according to claim 1. Embodiment 20. The halide material is Li 3-x-f M f RE 1-y Me k y (Cl 1-p F p ) 6-x+y*(k-3) where 0<=p<2. 19. The solid electrolyte material according to any one of aspects 1 to 18. Embodiment 21. The compound of embodiment 1, wherein RE comprises Y, Ce, Gd, Er, La, or Yb. 21. The solid electrolyte material according to any one of claims 1 to 20. Embodiment 22. Me is Y, Ce, Gd, Er, Sm, Eu, Pr, Tb, Al, Z r, La, Yb, Mg, Zn, Sn, Mg, Ca, or any combination thereof 22. The solid electrolyte material according to any one of embodiments 1 to 21. Embodiment 23. The solid according to any one of embodiments 1 to 22, wherein RE consists of Y. Electrolyte materials. Embodiment 24. Me is selected from the group consisting of Gd, Yb, Zr, Zn, Mg, Al, and Ca.
[0046] According to any one of the embodiments 1 to 23, wherein the at least one element selected from Solid electrolyte material. Embodiment 25. The method of embodiment 1 to 3, wherein M comprises Na or K, and M consists of Na or K. 24. A solid electrolyte material according to any one of claims 1 to 24. Embodiment 26. Wherein, u >= 0.1, u >= 0.12, u >= 0.15, u >= 0. 17, u>=0.2, u>=0.23, u>=0.25, u>=0.27, u>=0.2 9, u>=0.32, or u>=0.34, any of embodiments 1 to 19 and 21 to 25. 13. The solid electrolyte material according to claim 12, Embodiment 27. In the formula, u<=0.85, u<=0.83, u<=0.8, u<=0. 77), u<=0.75, u<=0.7, u<=0.67, u<=0.65, u<=0. 62, u<=0.6, u<=0.57, u<=0.54, u<=0.52, u<=0.4 9) Any of embodiments 1 to 19 and 21 to 25, wherein u<=0.45 and u<=0.42. The solid electrolyte material according to any one of claims 1 to 5, Embodiment 28. Wherein p>=0.04, p>=0.06, p>=0.08, p>=0 .09, p>=0.10, p>=0.12, p>=0.14, p>=0.15, p>=0 0.17, p>=0.2, or p>=0.22, 13. The solid electrolyte material according to claim 12, Embodiment 29. Wherein p<=0.33, p<=0.31, p<=0.29, p<=0 .27, p<=0.25, p<=0.22, p<=0.20, p<=0.18, p<=0 0.16, p<=0.14, or p<=0.10; 29. The solid electrolyte material according to any one of claims 1 to 28. Embodiment 30. Wherein, (1-upq)>=0.12, (1-upq)>=0 .15, (1-upq)>=0.17, (1-upq)>=0.20, (1-u -pq)>=0.23, (1-upq)>=0.25, (1-upq)>=0 .27, (1-upq)>=0.29, (1-upq)>=0.33, (1-u -pq)>=0.36, (1-upq)>=0.43, (1-upq)>=0 .48, (1-upq)>=0.50, (1-upq)>=0.54, or (1 30. The solid electrolyte according to any one of embodiments 1 to 29, wherein -upq)>=0.58. quality material. Embodiment 31. Wherein, (1-upq)<=0.97, (1-upq)<=0 .92, (1-upq)<=0.87, (1-upq)<=0.83, (1-u -pq)<=0.80, (1-upq)<=0.77, (1-upq)<=0 .75, (1-upq)<=0.70, or (1-upq)<=0.66 31. The solid electrolyte material according to any one of embodiments 1 to 30. Embodiment 32. The ratio of (1-upq) / u is at least 0.03, at least 0 .06, at least 0.1, at least 0.2, at least 0.3, at least 0.4, At least 0.5, at least 0.6, at least 0.7, at least 0.8, at least At least 0.9, at least 1.0, at least 1.2, at least 1.3, at least 1.4 , at least 1.5, at least 1.6, at least 1.7, at least 1.8, less Any of embodiments 1 to 19 and 21 to 31, wherein both are 1.9, or at least 2.0. 1. The solid electrolyte material according to claim 1. 33. The ratio of (1-upq) / u is 15 or less, 11 or less, 10 or less, 9 or less. 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, 3 or less, 2 or less, or 1.4 or less The solid electrolyte material according to any one of embodiments 1 to 19 and 21 to 32. Embodiment 34. The halide material is Li 3-x RE 1-y Me k y (Cl 1-u B r u ) 6-x+y*(k-3) where 0.08<=u<=0.67. The solid electrolyte material according to any one of embodiments 1 to 19 and 21 to 33. Embodiment 35. The halide material is Li 3-x Y(Cl 1-u Br u )6 by 35. The solid electrolyte material of embodiment 34, as represented by the formula: Embodiment 36. The compound according to embodiment 34 or 35, wherein u>=0.55 or u<=0.45. 35. The solid electrolyte material according to claim 35. Embodiment 37. Any of embodiments 34 to 36, wherein 0.2<=u<=0.45. The solid electrolyte material according to any one of claims 1 to 5, Embodiment 38. The compound according to any one of embodiments 34 to 37, wherein u<0.33. Solid electrolyte material. Embodiment 39. The halide material has at least one axially extending portion having a 2 theta angle of 13° to 15°. The experimental X-ray diffraction pattern, measured with Cu K-alpha radiation, contains two peaks. The solid electrolyte material according to any one of the first to eighteenth embodiments. Embodiment 40. The halide material is at least 20 nm, at least 25 nm, Average diffracting crystallite size of at least 30 nm, at least 35 nm, or at least 40 nm The solid electrolyte material according to any one of embodiments 1 to 39, further comprising: Embodiment 41. The halide material is at most 500 nm, at most 400 nm, The average diffraction crystallite size is at most 300 nm, at most 200 nm, or at most 100 nm. The solid electrolyte material according to any one of embodiments 1 to 40, further comprising: Embodiment 42. The halide material has a density of at least 2.3 g / cm 3 , at least 2. 5g / cm 3 , at least 2.7 g / cm 3 , at least 2.9 g / cm 3 ,at least 3.1g / cm 3 , at least 3.3 g / cm 3 , or at least 3.5 g / cm 3 Dense 42. The solid electrolyte material according to any one of embodiments 1 to 41, comprising: Embodiment 43. The halide material has a density of 3.8 g / cm 3 Below 3.5g / cm 3 below , 3.4g / cm 3 Below, 3.3g / cm 3 or less than 3.1g / cm 3 Contains the following densities: The solid electrolyte material according to any one of embodiments 1 to 42. Embodiment 44. The halide material has a voltage greater than 3.57V, at least 3.60V, or at least Thermodynamic and electrochemical stability values of 3.62 V, 3.65 V, or at least 3.71 V The solid electrolyte material according to any one of embodiments 1 to 43, comprising: Embodiment 45. The halide material is 4.30V or less, 4.19V or less, 4.15V or less or less, 4.10V or less, 3.85V or less, 3.80V or less, 3.75V or less, or 3.7 45. Any one of embodiments 1 to 44, including a thermodynamic, electrochemical stability value of 1 V or less. Solid electrolyte material. Embodiment 46. Halide materials exhibit improved electrochemical properties compared to Li3YBr6. 46. The solid electrolyte material according to any one of embodiments 1 to 45, comprising chemical stability. Embodiment 47. The halide material has a conductivity of greater than 0.15 mS / cm and at least 0.3 mS / cm, at least 0.5mS / cm, at least 0.8mS / cm, at least 0.9 mS / cm, at least 1.1 mS / cm, at least 1.5 mS / cm, or at least Any of embodiments 1 to 45, including an ionic conductivity measured at 22° C. of 1.7 mS / cm. 10. The solid electrolyte material according to claim 9, Embodiment 48. The halide material has a conductivity of less than 2.0 mS / cm and at most 1.9 mS / cm. cm, at most 1.8 mS / cm, or at most 1.7 mS / cm measured at 22 °C 46. The solid electrolyte material according to any one of embodiments 1 to 45, comprising an on-conductivity. Embodiment 49. A cathode comprising the solid electrolyte material according to any one of embodiments 1 to 48. Extreme liquid material. Embodiment 50. A method for producing a cathode comprising the steps of: 50. The catholyte material of embodiment 49, wherein the catholyte material is coated with a porous material. Embodiment 51. A positive electrode comprising the solid electrolyte material according to any one of embodiments 1 to 48. Extreme liquid material. Embodiment 52. An anode comprising particles of an anode active material, at least a portion of the particles being a solid electrolyte. 52. The anolyte material of embodiment 51, wherein the anolyte material is coated with a porous material. Embodiment 53: A layer comprising the solid electrolyte material according to any one of embodiments 1 to 48. wherein the layer comprises a catholyte layer, an anolyte layer, an electrolyte layer, or a combination thereof. Embodiment 54. A catholyte layer comprising the catholyte material of embodiment 49 or 50. Embodiment 55. An anolyte layer comprising the anolyte material of embodiment 51 or 52. Embodiment 56: A solid electrolyte comprising the solid electrolyte material according to any one of embodiments 1 to 48. a solid electrolyte layer, the halide material comprising at least one of Cl and F; an electrolyte layer; and an electrode layer including a cathode active material in contact with the solid electrolyte material; The solid electrolyte layer forms a chlorine- or fluorine-deficient region proximate the electrode layer under oxidizing conditions. The chlorine- or fluorine-deficient regions may be formed on the solid electrode layer distal to the electrode layer. The electrochemical device contains a lower concentration of chlorine or fluorine, respectively, compared to the electrolyte layer region. Chair. Embodiment 57: A solid electrolyte comprising the solid electrolyte material according to any one of embodiments 1 to 48. an electrolyte layer, an electrode layer including a cathode active material, and a layer between the solid electrode layer and the cathode active material; An electrochemical device comprising: Embodiment 58. The electrochemical device according to Embodiment 57, wherein the intermediate layer includes a cathode liquid layer adjacent to the electrode layer. Electrochemical device. Embodiment 59. The intermediate layer contains a lithium-metal halide represented by Li 3-x-f M f RE 1-y Me k y (Cl 1-p F p ) 6-x+y*(k-3) where -1 <= x <= 1, 0 <= y <= 1, 0 <= p <= 1 / 3, and 0 <= f <= 0.3. The electrochemical device according to Embodiment 57. Electrochemical device according to Embodiment 57. Embodiment 60. The solid electrolyte layer contains an electrolyte material containing a halide material represented by Li M 3-x-f M f RE 1-y Me k y (Cl 1- p F p ) 6-x+y*(k-3) where 0 < p <= 1 / 3. The intermediate layer contains a lithium-metal halide represented by Li M 1-x-f M f RE 1-y Me k y F 4-x+y*(k-3) where -0.3 <= x <= 0.3, 0 <= y <= 1, and 0 <= f <= 0.3. The electrochemical device according to Embodiment 5 7. Embodiment 61. The solid electrolyte layer contains an electrolyte material containing a halide material represented by Li3Y(Br Cl u Cl 1-u )6 where 0 < u < 1. The intermediate layer contains a lithium-metal halide represented by Li3 (1-z) (1-z) Y (1+z) Cl6 where 58. The electrochemical device of embodiment 57, wherein 0<=z<0.3. Embodiment 62. The intermediate layer is at most 1 micron, at most 800 nm, at most 60 0nm, at most 400nm, at most 300nm, at most 200nm, at most 10 0nm, at most 80nm, at most 60nm, at most 50nm, at most 40nm, 57. The method of claim 57, further comprising: and the electrochemical device according to any one of 59 to 61. Embodiment 63. The intermediate layer is at least 1 nm, at least 2 nm, at least 3 nm , at least 4 nm, at least 5 nm, at least 10 nm, at least 20 nm, or 63. The method of claim 57, further comprising the step of: Electrochemical devices. Embodiment 64. Any of embodiments 57 and 59 to 63, in which the intermediate layer is a passivation layer. 13. The electrochemical device according to claim 12, Embodiment 65. A method of forming an intermediate layer for an electrochemical device, comprising: A voltage is applied to the electrochemical device according to any one of embodiments 1 to 48. applying an electric current to the solid electrolyte material and the cathode active material, and forming an intermediate layer in contact with the cathode active material, the intermediate layer being a solid-state The intermediate layer includes a lithium-metal halide material that is different from the electrolyte material and is formed in situ. and forming a Embodiment 66. A lithium-metal halide material is used to partially decompose a solid electrolyte material. The solid electrolyte material is formed by the above-mentioned method, and the solid electrolyte material is a halogen containing at least one of Cl and F. 66. The method of embodiment 65, comprising a compound material. Embodiment 67. An electrochemical device comprising a solid electrolyte layer including a solid electrolyte material, The method further comprises forming a Cl- or F-deficient region in the solid electrolyte layer, The F-deficient region is closer to the interlayer than the region in the solid electrolyte layer farther from the interlayer. 67. The method according to embodiment 65 or 66, comprising a lower concentration of Cl- or F-, respectively. . Embodiment 68. The voltage is at least 3.0V, at least 3.6V, at least 4. Any of embodiments 65 to 67, including a voltage of 0 V, at least 4.5 V, or at least 5.0 V. The method according to any one of the above. Embodiment 69. The intermediate layer is Li 3-x-f M f RE 1-y Me k y (Cl 1-p F p ) 6-x+y*(k-3) Lithium-metal halides represented by the formula: -1<=x<=1, 0<=y<=1, 0<=p<=1 / 3, and 0<=f<=0.3. The method according to any one of embodiments 65 to 68, Embodiment 70. The electrolyte material is Li 3-x-f M f RE 1-y Me k y (Cl 1-p F p ) 6-x+y*(k-3) wherein: <p <=1 / 3, and the middle layer is Li 1-x-f M f RE 1-y Me k y F 4-x+y*( k-3) where -0.3<=x< Any one of Embodiments 65 to 69, where = 0.3, 0 <= y <= 1, and 0 <= f <= 0.3 The method according to item 1. Embodiment 71. The electrolyte material contains a halide material represented by Li3Y(Br u Cl 1-u )6, where 0 < u < 1, and the intermediate layer contains Li Y 3(1-z) Y (1+ z) A lithium-metal halide represented by Cl6, where 0 <= z < 0. 3. The method according to any one of Embodiments 65 to 70. Embodiment 72. The intermediate layer has a thickness of at most 1 micron, at most 800 nm, at most 60 0 nm, at most 400 nm, at most 300 nm, at most 200 nm, at most 10 0 nm, at most 80 nm, at most 60 nm, at most 50 nm, at most 40 nm, at most 20 nm, at most 10 nm, or at most 8 nm. The method according to any one of Embodiments 65 to 71. Embodiment 73. The intermediate layer has a thickness of at least 1 nm, at least 2 nm, at least 3 nm , at least 4 nm, at least 5 nm, at least 10 nm, at least 20 nm, or at least 50 nm. The method according to any one of Embodiments 65 to 72. Embodiment 74. A method for forming a solid electrolyte material, comprising forming a solid solution of a halide material containing at least two halide anions selected from the group consisting of F, Cl, Br, and I , wherein the halide material is Li M 3-x-f M f RE 1-y M e k y (Cl 1-u-p-q Br u F p I q ) 6-x+y*(k-3) is represented by Where -1<=x<=1, 0<=y<=1, 0<=u<1, and 0<=p <=1 / 3, 0<=q<=1 / 6, 0<=(u+p+q)<1, 0< = f <= 0.3, M is at least one alkali metal element other than Li, R E is a rare earth element, k is the valence of Me, and Me is a group IIIB element, a group IVB element, Elements, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Al, Sn, Pb, Bi At least one element selected from the group consisting of Sb, Mg, Ca, Ga, and Ge; M e is different from RE in a way. Embodiment 75. The method further comprising forming an ammonium-containing metal halide material. The method of embodiment 74. Embodiment 76. (NH4) z RE 1-y Me k y (Cl 1-u-p-q Br u F p I q ) 3+z+y*(k-3) , (NH4) z RE 1-y Me k y (Cl 1-u Br u )3 +z+y*(k-3) , (NH4) z RE 1-y Me k y (Cl 1-p F p ) 3+z+y *(k-3) , (NH4) z RE 1-y Me k y (Cl) 3+z+y*(k-3) , (N H4) z RE 1-y Me k y (Br) 3+z+y*(k-3) , (NH4) z RE 1-y Me k y (I) 3+z+y*(k-3) or a combination thereof. 76. The method of embodiment 74 or 75, comprising: Embodiment 77. The formation of an ammonium-containing metal halide is selected from the group consisting of F, Cl, B Using a predetermined ratio between at least two halogen elements selected from the group consisting of r, r, and I. 77. The method of embodiment 75 or 76, wherein the method is carried out in a single step. Embodiment 78. Forming an ammonium-containing metal halide material comprises: 78. The method of any one of embodiments 75 to 77, wherein the method is performed in Embodiment 79. The formation of an ammonium-containing metal halide material comprises the steps of: 79. The method of any one of embodiments 75 to 78, wherein the method is carried out at a temperature of 0° C. Embodiment 80. The temperature is at least 20° C., at least 40° C., at least 50° C., At least 70°C, at least 90°C, at least 110°C, or at least 140°C The method of embodiment 79. 81. The temperature is 200°C or less, 180°C or less, 160°C or less, or 140°C or less. 81. The method of embodiment 79 or 80, wherein: Embodiment 82. Any one of embodiments 78 to 81, wherein the liquid medium comprises an acidic solution. The method described. Embodiment 83. The liquid medium is hydrochloric acid, hydrobromic acid, hydrofluoric acid, hydroiodic acid, or 83. The method according to any one of embodiments 78 to 82, comprising the step of: method. Embodiment 84. Ammonium halide and and partial or complete thermal decomposition of the lithium-containing metal halide to a lithium-containing metal halide. 5 to 83. A method according to any one of claims 5 to 83. Embodiment 85. Complete synthesis of ammonium halides and lithium-containing metal halides 85. The method of embodiment 84, further comprising partial or complete separation. Embodiment 86. The halide material has at least 20% stacking faults, at least 30 %, at least 40%, at least 50%, at least 60%, at least 70%, at least 4. The present invention relates to a crystal structure having at least 80% or at least 90% stacking faults. 8. The solid electrolyte material according to any one of claims 1 to 7. Embodiment 87. The halide material is Me x N k , M x N, or a combination thereof wherein x is the valence of N and k is the valence of Me. and the total content of charge-neutral metal nitrides is at most 0.05% by weight of the halide material. 0.3% by weight of the solid electrolyte material of any one of embodiments 1 to 48 and 86. Embodiment 88.Li a M a’ Me b Me' b’ X c X' c’ The halogen represented by A solid electrolyte material comprising a nitride material, The halide material is (b / (b+b')) t * 0.84 t * 1.16 (in the formula, (b / (b+b')) t However, the crystals on the crystallographic phase diagram at a temperature of 22°C (corresponding to the boundary of the chemical phase transition) (c / (c+c')) t * 0.84 <c / (c+c’)<(c / (c+c’)) t * 1.16 (in the formula, (c / (c+c')) t However, the crystals on the crystallographic phase diagram at a temperature of 22°C corresponding to an optical phase transition), or (a / (a+a')) t * 0.84 t * 1.16 (wherein, (a / (a+a')) t However, the crystals on the crystallographic phase diagram at a temperature of 22°C (corresponding to a crystallographic phase transition) within a stoichiometric range of During the ceremony, Me is a group IIIB element, a group IVB element, V, Cr, Mn, Fe, Co, Ni, and C. u, Zn, Zr, Al, In, Sn, Pb, Bi, Sb, Mg, Ca, Ga, and Ge at least one element from the group consisting of Me' is a group IIIB element other than Me, a group IVB element, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Al, In, Sn, Pb, Bi, Sb, Mg, Ca, G at least one element selected from the group consisting of a, b, and Ge; b>=b', c>=c', and a>=a', X is at least one halogen other than X'; X' is at least one halogen; M is at least one alkali metal element other than Li; The halide material is, based on the total weight of the halide material, one or more binary halide phases with a total content of not more than 10% by weight; one or more oxyhalide phases with a total content of not more than 7% by weight; and one or more ternary halide phases having a total content of 7% by weight or less. material. Embodiment 89.Li a M a Me b Me' b’ X c X' c’ The halogens represented by A solid electrolyte material comprising a cation material, The halide material is (b / (b+b')) t * 0.84 t * 1.16 (in the formula, (b / (b+b')) t However, the crystallographic phase diagram at temperatures between 20℃ and 25℃ (corresponding to the crystallographic phase transition above), (c / (c+c')) t * 0.84 <c / (c+c’)<(c / (c+c’)) t * 1.16 (in the formula, (c / (c+c')) t However, the crystallographic phase diagram at temperatures between 20℃ and 25℃ (corresponding to the crystallographic phase transition above), or (a / (a+a')) t * 0.84 t * 1.16 (wherein, (a / (a+a')) t However, the crystallographic phase diagram at temperatures between 20℃ and 25℃ (corresponding to the crystallographic phase transition above), During the ceremony, Me is a group IIIB element, a group IVB element, V, Cr, Mn, Fe, Co, Ni, and C. u, Zn, Zr, Al, In, Sn, Pb, Bi, Sb, Mg, Ca, Ga, and Ge At least one element from the group consisting of Me' is a group IIIB element other than Me, a group IVB element, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Al, In, Sn, Pb, Bi, Sb, Mg, Ca, G at least one element selected from the group consisting of a, b, and Ge; b>=b', c>=c', a>=a', and X is at least one other than X'. at least one halogen, X' is a halogen; M is at least one alkali metal element other than Li; A solid electrolyte material in which the anions of a halide material are in a single phase. Embodiment 90. The halide material has no peak between 5° and 13° 2theta. and measuring the X-ray diffraction pattern using Cu K-alpha radiation. 81. The solid electrolyte material according to embodiment 88 or 89. Embodiment 91. The halide material is monoclinic, trigonal, hexagonal, or orthorhombic. 91. The solid electrolyte material according to any one of embodiments 88 to 90, comprising a crystal structure represented by the formula: Embodiment 92. The crystallographic phase transition comprises a transition from a layered crystal structure to a non-layered crystal structure. 92. The solid electrolyte material according to any one of embodiments 88 to 91. Embodiment 93. The crystallographic phase transition is a transition from a cubic close-packed structure to a hexagonal close-packed structure. The solid electrolyte material according to any one of embodiments 88 to 92, comprising: Embodiment 94. The crystallographic phase transition is from the C2 / m space group or the R-3m space group to the P-3m space group. 94. The solid state according to any one of embodiments 88 to 93, comprising a transition to the Pnma or Pnma space groups. Electrolyte materials. Embodiment 95. A crystallographic phase transition occurs from a non-layered crystal structure to another non-layered crystal structure or layered crystal structure. 94. The solid electrolyte material according to any one of embodiments 88 to 93, comprising a transition to a crystalline structure. Embodiment 96. The crystallographic phase transition of embodiment 88, wherein the crystallographic phase transition comprises a transition from R3c to R3m. 96. The solid electrolyte material according to any one of claims 91 to 95. Embodiment 97. The crystallographic phase transition is from the P-3m1 or Pnma space group to the C2 / m space group. Any one of embodiments 88 to 91 and 95 to 96, comprising a transition to the R-3m space group or the R-3m space group. The solid electrolyte material according to any one of claims 1 to 5. Embodiment 98. The method of any one of embodiments 88 to 97, wherein Me is at least one rare earth element. 13. The solid electrolyte material according to claim 12, Embodiment 99. Me' is at least one of the rare earth elements, In, Zr, and Fe. The solid electrolyte material according to any one of embodiments 88 to 98, wherein the elements are each an element. Embodiment 100. The method of claim 1, wherein M is at least one element selected from the group consisting of Na, K, and Cs. 100. The solid electrolyte material according to any one of embodiments 88 to 99. Embodiment 101. An embodiment in which X is at least one element selected from the group consisting of Cl and Br. The solid electrolyte material according to any one of embodiments 88 to 100. Embodiment 102. An embodiment in which X' is at least one element selected from the group consisting of Br and F. The solid electrolyte material according to any one of embodiments 88 to 101. Embodiment 103. The halide material is Li a-f M a’ RE b Me' k b’ (Cl c Br c’ ) 6-f+(k-3)*b’ wherein: a+a'=3, −1≦f≦1, c+c'=1, The solid electrolyte material according to any one of embodiments 88 to 102, wherein b+b′=1. . Embodiment 104. The halide material is Li 3-f RE b Me' k b’ (Cl c Br c’ ) 6-f+(k-3)*b’ wherein: −1≦f≦1, c+c'=1, The solid electrolyte material according to any one of embodiments 88 to 102, wherein b+b′=1. . Embodiment 105. Wherein b>0, b'>0, and 0.65≦c / (c+c')≦0. 95. The solid electrolyte material of embodiment 104, Embodiment 106. The embodiment in which RE comprises Y and Me′ comprises In, Yb, or Zr. 106. The solid electrolyte material according to claim 104 or 105. Embodiment 107. Me' is Yb, and 0.65≦c / (c+c')≦0.89. The solid electrolyte material according to any one of embodiments 104 to 106. Embodiment 108. Me' is In, and 0.69≦c / (c+c')≦0.95. The solid electrolyte material according to any one of embodiments 104 to 106. Embodiment 109. The halide material is Li3Y b Yb b’ (Cl c Br c’ )6 In the embodiment 104, the formula is represented by: 106. The solid electrolyte material according to any one of claims 106 to 107. Embodiment 110. The halide material is Li3Y b In b’ (Cl c Br c’ )6 In the embodiment 104, the formula is represented by: 109. The solid electrolyte material according to any one of 106 and 108. In an embodiment 111, Me' is Zr, and 0.72≦c / (c+c')≦0.98. The solid electrolyte material according to any one of embodiments 104 to 106. Embodiment 112. The halide material is Li 3-b’ Y b Zr b’ (Cl c Br c’ )6, wherein 0.72≦c / (c+c′)≦0.98. 04 to 106. The solid electrolyte material according to any one of claims 04 to 106. Embodiment 113. The halide material is Li 3-f RE(Cl c Br c’ ) 6-f To wherein: 0<=f<=0.3, c+c'=1, Any one of embodiments 88 to 104, wherein 0.63≦c / (c+c′)≦0.87. The solid electrolyte material according to any one of claims 1 to 5. Embodiment 114. The solid electrolyte according to embodiment 113, wherein RE includes Y. quality material. In embodiment 115, RE is Y, and 0.65≦c / (c+c′)≦0.87, or 0.66≦c / (c+c')≦0.85, or 0.67≦c / (c+c')≦0.83 115. The solid electrolyte material of embodiment 113 or 114, wherein Embodiment 116. The halide material is Li 3-f RE b Me' k b’ X 6-f+( k-3)*b’ wherein: 0<=f<=0.3, The solid electrolyte material according to any one of embodiments 88 to 104, wherein b+b′=1. . Embodiment 117. The compound according to embodiment 1, wherein 0.67≦b / (b+b′)≦0.93. 17. The solid electrolyte material according to claim 16. Embodiment 118. The embodiment in which RE contains Y, Me' contains In, and X contains Cl. 118. The solid electrolyte material according to embodiment 116 or 117. Embodiment 119. The halide material is Li 3-f RE b In b’ X 6-f By In embodiments 116 to 118, the formula is: 13. The solid electrolyte material according to claim 12, Embodiment 120. The halide material is Li3Y b In b’ Represented by X6, 118. The solid electrolyte material according to embodiment 118. Embodiment 121. The halide material is Li 3-f RE b In b’ X 6-f By The solid electrolyte material according to any one of embodiments 116 to 117, Embodiment 122. The halide material is Li a M a’ REX6, wherein , a>a'>0, a+a'=3, Any of embodiments 88 to 103, wherein 0.942≦a / (a+a′)≦0.958. 10. The solid electrolyte material according to claim 9, Embodiment 123. The solid electrolyte material of embodiment 122, wherein M comprises Na. Embodiment 124. The solid electrolyte of embodiment 122 or 123, wherein RE comprises Y. material. Embodiment 125. Any one of embodiments 122 to 124, wherein X comprises Cl. Solid electrolyte material. Embodiment 126. The halide material is Li a Na a’ Represented by YCl6, The solid electrolyte material according to any one of embodiments 122 to 124. Embodiment 127. The halide material has at least one axially extending 2-theta in the range of 13° to 15°. also includes an X-ray diffraction pattern measured with Cu K-alpha radiation, which contains two peaks, The halide material is (c / (c+c'))t * 0.84 <c / (c+c’)<(c / ( c+c'))t * If the crystallographic phase transition is within the stoichiometric range of 1.16, then c / (c+ If c')<0.75, then (c / (c+c'))t is the result at temperatures between 20°C and 25°C. 127. The method according to claim 88, wherein the phase transition corresponds to a crystallographic phase transition on a crystallographic phase diagram. Solid electrolyte material. EXAMPLES
[0180] Example 1 According to embodiments of the present invention, (NH4)3Li3YBr6 and (NH4)3Li3 Samples 1 to 8 were synthesized by forming solid solutions from YCl6. The characteristics are shown in Table 1.
[0181] At room temperature (approximately 22°C), the AC frequency is 3MHz to 10Hz and the peak voltage is 10 to 50mV. Electrochemical induction using a gold blocking electrode under the condition of a peak-to-peak sinusoidal AC voltage signal. Impedance spectroscopy was used to determine the ionic conductivity of the samples.
[0182] The ionic conductivity of the bulk grains is included in Table 1. The conductivity characteristics of the bulk grains are the most It appears at high frequencies and is associated with the lowest values of double-layer capacitance, so it is important to understand the These conductivity contributions could be separated from the grain boundaries and electrode contacts.
[0183] [Table 1]
[0184] Example 2 The following samples were formed: Sample 9 was an In / Li foil counter electrode, similar to that described in Example 1. Separators made of solid solutions of Li3YBr2Cl4 formed in a similar manner, as well as Li The working electrode was made of a mixture of 3YBr2Cl4 and carbon powder. Sample 10 was the same as Sample 9. The first charge is the same as the first charge, except that the separator is made of Li3YBr6. Cyclic voltammetry VA diagrams of samples 9 and 10 during the oxidation cycle are included in Figure 5. The cyclic voltammetry VA diagram for the second charge / oxidation cycle is included in Figure 6. The scanning speed was 0.5 mV / s and the cell area was 0.5 cm 2 It was.
[0185] Compared with sample 10, sample 9 had a higher battery life during the first and second battery charging processes. When the iron oxide exceeded the electrochemical stability threshold, it showed a significantly slower oxidative decomposition. In the first charging cycle, the oxidation peak observed in sample 10 was greater than 280 μA. When the current was applied, Sample 9 exhibited an oxidation current of less than 40 μA. In the second charge cycle / oxidation, sample 9 showed no decomposition at moderate bias. However, sample 10 still showed decomposition.
[0186] Example 3 Representative halide material samples were prepared using the process with accelerated cooling described in the embodiments herein. Briefly, ammonium-containing LYB and ammonium-containing The organic LYCs were formed in separate solutions, which were then combined and dried at 120°C. The reaction mixture was heated to 550°C, allowing the solid-state reaction and the sublimation of ammonium to proceed simultaneously. The cooling rate was approximately 100°C. Single-phase LYBC sample, LYBC-1 9, LYBC-41, LYBC-62, LYBC-67, LYBC-79, and LYBC Single-phase LYB and LYC were formed in the presence of ammonium. The ionic conductivity of the samples was measured as described in the embodiments of the present invention. In addition, samples LYBC-62, LYBC-67, and LYBC-79 showed similar results compared to LYB. It showed unexpectedly high ionic conductivity.
[0187] [Table 2]
[0188] FIG. 9A shows the powder XRD pattern of sample LYBC-79 and the reference XRD pattern of LYC. The two materials are isostructurally similar to LYBC-79 and have peaks smaller than those of LYC. The broadening of the lattice parameters is indicated by the left shift of
[0189] FIG. 9B is a powder XRD pattern of sample LYBC-67 and a reference XRD pattern of LYB. The two materials are isostructurally similar to LYBC-67 and have peaks similar to those of LYB. The lattice parameter contraction suggested by the right shift is shown.
[0190] Example 4 Representative halide materials were prepared in the same manner as described in Example 10. Improved identification of bands at the multiphase boundary (MPB) and halide materials Phase transition ranges that may enable one to have on-conductivity are included in Tables 3-5.
[0191] [Table 3]
[0192] [Table 4]
[0193] [Table 5]
[0194] Example 12 The following samples were formed and the electrochemical stability of the sample electrolytes was tested: Cell 60 The anode was an In / Li foil, LiY formed in a manner similar to that described in Example 10. (Cl 0.8 Br 0.2 )6 single-phase solid solution, and Li3Y(Cl 0. 8Br 0.2 The cell 74 contains a cathode made of a mixture of Li3 Y(Cl 0.8 Br 0.2 ) 6 was prepared in a manner similar to that described in Example 10. Li3Y(Cl 0.65 Br 0.35 Same as cell 60, except replaced with 6. The cell 69 is filled with Li3Y(Cl) to form the sample cell 69. 0.8 Br 0.2 The cell is similar to cell 60, except that LiYBr was replaced with LiYBr.
[0195] FIG. 11A and FIG. 11B show the results of cyclic voltammetry (C V) Test results of electrochemical stability of the electrolyte by the method. The voltages were measured for the Li-In anode of the tested sample. As shown, when the voltage exceeds 2.9 V, the electrolyte ( Li3YBr6) begins to decompose, which is characterized by a relatively high current in the measurement. suggested that the Li3YBr6 electrolyte has limited electrochemical stability at the tested voltages. The Li3Y(Cl) in cell 60 0.8 Br 0.2 )6 and Li3Y(Cl) in cell 74 0.65 Br 0.35 ) 6 showed significantly lower current compared to cell 69 at the same voltage. , Li3Y(Cl 0.8 Br 0.2 )6 and Li3Y(Cl0 .65 Br 0.35 This suggests a significantly improved electrochemical stability of Li3Y (Cl 0.65 Br 0.35 The decomposition of Li3YBr6 starts at a similar voltage compared to Li3YBr6. However, as characterized by the electric current, Li3Y(Cl 0.65 B r 0.35 The decomposition kinetics of Li3Y(Cl)6 is significantly slower than that of Li3YBr6. 0. 8Br 0.2 The decomposition of Li3Y(Cl 0.65 Br 0.35 )6 and Li3YBr Compared to 6, the decomposition kinetics also differ from that of Li3Y(Cl 0.65 Br 0. 35 )6 and Li3YBr6. Without wishing to be bound by any theory, However, Li3Y(Cl 0.8 Br 0.2 )6 and Li3Y(Cl 0.65 Br 0.35 The improved stability of 6 is due to the formation of a thin passivating Cl-rich layer on the cathode. This may be due to the effect.
[0196] As shown in FIG. 11B, Li3Y(Cl 0.8 Br 0.2 )6 is a voltage of 3.2 Above V, it begins to decompose, and Li3Y(Cl 0.65 Br 0.35 )6 Better electrification It shows chemical stability. Li3Y(Cl 0.8 Br 0.2 Improved electrochemical stability of 6 In particular, Li3Y(Cl) has a layered crystal structure. 0.65 Br 0.35 ) 6, Compared to , LiY(Cl 0.8 Br 0.2 Considering the higher Cl / Br ratio and non-layered crystal structure of 6, Considering this, it is unexpected.
[0197] The 3.7V of NMC cathode, the most advanced cathode for Li-In anodes The operating voltage is shown in FIG. 11B, which is 4.3 V for a Li / Li+ anode. The corresponding Li3Y(Cl 0.8 Br 0.2 )6 is the maximum capacitance at the operating voltage of the NMC cathode. Superior electrochemistry as suggested by improved degradation kinetics, characterized by low currents It can be observed that the solubility of the solubility-containing glycerol is stable.
[0198] Example 13 Sample CS13 was synthesized as follows. The target formula is Li3YCl3Br3. There were 28.23 g of Y2O3, 176.52 g of NH4Cl, and 65.13 g of L iBr, Y2O3, NH4Cl, and LiBr in a molar ratio of Y2O3:NH4Cl: LiBr=1:13.2:6 (i.e., the predetermined ratio based on the stoichiometric ratio) The amount of NH4Cl was excessive relative to the amount of Y2O3 so that it was 10 mol% more than the amount of Y2O3. The raw materials were weighed, crushed, and stored in a nitrogen atmosphere with a dew point of -80°C or less. The fine powders were mixed in a quartz crucible in air. The mixture was then cooled in a furnace that had been ventilated with N2 for 24 hours. The crucible was heated to 200 °C at a ramp rate of 50 °C per hour and held for 15 h. The temperature was then increased at 50°C per hour to 496°C in a nitrogen atmosphere and held at that temperature for 1 hour. The crucible is cooled to room temperature, approximately 25°C, and then heated at approximately 100°C per hour. The temperature was monitored using a thermocouple placed inside the crucible. The crucible containing the synthesized material was protected and the glass was placed in a moisture-free condition (dew point -80°C). The synthesized block was removed from the crucible and placed in a lobe box. The organic residues on the top surface of the block were removed. The resulting block was then cooled to room temperature under a N2 atmosphere. It was ground to a powder in a lobe box.
[0199] XRD analysis was carried out on the milled powder of sample CS13 under dry conditions. It showed the same hexagonal crystal structure as Li3YCl6 prepared by conventional methods. A Lebail refinement was performed using the lattice parameter spread function to estimate the The Br / Cl ratio was determined. The sum of Cl or Br counter anions (i.e., the sum of Cl and Br) The ratio of Br to Cl and the total of Br was 28% ± 2%, and the ratio of Cl to Cl The ratio of the sum of Br and Br was 72% ± 2%.
[0200] By processing the XRD diagrams using the FullProf software package First, the automatic routine of the winPLOTR software was used. The background of the diffractogram is extracted via the following: is used to calculate the lattice parameters (i.e., a, b, and c), the sample height correction parameter (" 0 point”), as well as the Lorentzian components related to the size and distortion of the particles in the sample. By refinement, the Lebail method implemented in the FullProf software The XRD diagram is refined using the method described above. The refinement is performed if the observed value of the chi-square parameter is less than 6. If the conversion is completed, it is considered to be fully converted.
[0201] The total content of the water-insoluble impurity phase of sample CS13 was determined as described in the embodiments herein. Briefly, 50 g of milled sample CS13 was dissolved in distilled water. The solution appeared to be visually pure, but contained 60 mg of hydrated insoluble impurities (e.g., The total amount of water-insoluble impurities (YCl(OH)2) was collected from the filter. Sample CS13 was By weight, it had a total content of 53.2 mg of water-insoluble impurities consisting of YOCl. Sample CS13 contained water-insoluble impurity phases with a total content of 0.11 wt.%.
[0202] A representative sample S14 was prepared as follows: The target formula is Li3YCl3B It was r3.
[0203] 27.71g Li2CO3, 28.23g Y2O3, 192ml 47% concentrated H 160 g of NHBr, 160 g of NHBr, and 50 g of distilled HO were measured and mixed at 95°C to obtain L A solution of i2YBr6 precursor material was formed. The solution was then filtered through a 0.2 micron Millimeter filter. The mixture was filtered through a pore filter.
[0204] Separately, 138.5 g of Li2CO3, 141.1 g of Y2O3, 687 ml of 37 % HCl, 435 g NH4Cl, and 150 g distilled H2O were measured and mixed at 95°C. The solution was then doped with 0.2 microns of Mi The mixture was filtered through an illipore filter.
[0205] Both precursor materials were dried on a rotary evaporator to give the materials in solid form. The material is ground to form a fine powder, weighed, and crushed in a nitrogen atmosphere having a dew point of -80°C or less. The mixture was mixed in a quartz crucible. The synthesis was carried out in a furnace that had been ventilated with N2 for 24 hours. The tube was heated to 540°C at a continuous ramp rate of 100°C per hour and held at 540°C for 1 hour. The crucible was cooled to room temperature, approximately 25°C, and then heated at a maximum of 100°C per hour. The temperature was monitored using a thermocouple placed inside the crucible. The crucibles containing the synthesized materials were protected and placed in a glow-box under moisture-free conditions (dew point -80°C). The synthesized block was removed from the crucible by placing it in a crucible box. The organic residues on the top surface of the block were removed. The resulting block was placed in a gas The mixture was ground to a powder in a tube box.
[0206] XRD analysis was carried out on the milled powder of sample S14 under dry conditions. The XRD spectrum showed the same hexagonal crystal structure as the Li3YCl6 prepared as above. A Lebail refinement was performed using the The ratio of Cl to the sum of Cl and Br anions was determined. The ratio of Br to the sum of Cl and Br was 20% ± 2%, and the ratio of Cl to the sum of Cl and Br was 20% ± 2%. The overall ratio was 80% ± 2%.
[0207] The total content of the water-insoluble impurity phase of sample S14 was determined as described in the embodiments herein. Briefly, 50 g of milled sample S14 was dissolved in distilled water. 9 mg of hydrated insoluble impurities corresponding to 1 g of non-hydrated water insoluble impurities were collected from the filter. Sample S14 had a total content of 0.016 wt.% based on the total weight of the halide materials. The product contained water-insoluble impurities of
[0208] Two pairs of electrodes were prepared, including a stainless steel electrode and a compressed electrolyte made from powder of sample CS13. The ionic conductivity and thickness of the electrolyte, as well as the ohmic resistance and quality of the cell, were measured. The amounts were measured and are included in Table 6.
[0209] [Table 6]
[0210] Stainless steel electrodes and a compressed electrolyte (0.98 mm thick) made from powder of sample S14 Additional symmetrical battery cells were formed containing the electrolyte. The ionic conductivity of the electrolyte was measured and is listed in Table 7. Ta.
[0211] [Table 7]
[0212] Benefits, other advantages, and solutions to problems have been described above with regard to specific embodiments. However, benefits, advantages, solutions to problems, and any benefits, advantages, or solutions that bring Any feature that may render the invention more prominent or prominent may be added to any or all of the important, essential features of the claims. The term "material" should not be construed as a necessary or essential feature of the material. Reference herein to a material is intended to mean at least one material that consists essentially of one or more of the components identified. The term "consisting essentially of" may be interpreted as including at least one embodiment. and excludes all other materials except for small amounts (e.g., impurities) The term "compositions" refers to compositions that do not significantly change the properties of a material. Alternatively, or in certain non-limiting embodiments, the compositions identified herein Any of the above may be essentially free of material not expressly disclosed. The embodiments of the present disclosure include ranges of content of certain components in the materials, and may be used to determine the composition of a given material. It will be understood that component contents total 100%.
[0213] The specification and drawings of the embodiments described herein are provided to provide a general understanding of the structure of the various embodiments. The specification and drawings are intended to provide a solution to the problems described herein. Serves as a comprehensive and comprehensive description of all elements and features of the devices and systems used It is not intended that separate embodiments be provided in combination in a single embodiment. Conversely, various embodiments that are described in the context of a single embodiment for brevity may be combined together. The features may be provided separately or in any subcombination. Reference to a range of values includes every individual value within that range. Many other embodiments are described herein. Without departing from the scope of the present disclosure, Other embodiments may be used such that structural, logical substitutions, or other changes may be made. and can be derived from the present disclosure. Accordingly, the present disclosure is intended to be illustrative and not restrictive. should be regarded as something.< / hklm> < / hklm> < / hkl>
Claims
1. At least two aniline halides selected from the group consisting of F, Cl, Br and I. Including on, Li 3-x-f M f R.E. 1-y Me k y (Cl 1-u-p-q B u F p I q ) 6-x+y*(k-3) Solid electrolyte materials, including halide materials represented by And, During the ceremony, −1<=x<=1, 0<=y<=1, 0<=u<1, 0<=p<=1 / 3, 0<=q<=1 / 6, 0<(u+p+q)<1, 0<=f<=0.3, M is at least one alkali metal element other than Li; RE is a rare earth element; k is the valence of Me; Me is a group IIIB element, a group IVB element, V, Cr, Mn, Fe, Co, Ni, C u, Zn, Zr, Al, Sn, Pb, Bi, Sb, Mg, Ca, Ga, and Ge at least one element from the group, Me being different from RE; the halide material comprises, based on the total weight of the halide material: A solid electrolyte comprising one or more water-insoluble impurity phases with a total content of 0.10% by weight or less. material.
2. At least two halogens selected from the group consisting of F, Cl, Br, and I are contained in a single phase.
1. An electrolyte material comprising a halide material containing a nitride anion, the halide material The material is Li 3-x-f M f R.E. 1-y Me k y (Cl 1-u-p-q B u F p I q ) 6-x+y*(k-3) wherein: −1<=x<=1, 0<=y<=1, 0<=u<1, 0<=p<=1 / 3, 0<=q<=1 / 6, 0<(u+p+q)<1, 0<=f<=0.3, M is at least one alkali metal element other than Li; RE is a rare earth element; k is the valence of Me; Me is a group IIIB element, a group IVB element, V, Cr, Mn, Fe, Co, Ni, or Cu. , Zn, Zr, Al, Sn, Pb, Bi, Sb, Mg, Ca, Ga, and Ge and Me is different from RE.
3. The halide material is 9% by weight or less based on the total weight of the halide material. Binary halide phases, up to 6% by weight of ternary halide phases, up to 0.10% by weight of total content 10. The method of claim 1, further comprising the step of:
3. The solid electrolyte material according to claim 2.
4. 2. The method of claim 1, wherein the halide material comprises a crystal structure represented by a rhombohedral space group.
3. The solid electrolyte material according to claim 2.
5. The crystal structure is Li 3 YBr 6 1 or 2.
3. The solid electrolyte material according to claim 2.
6. The halide material has a powder diffraction pattern peak of Li 3 YBr 6 Powder diffraction pattern 3. The method according to claim 1, wherein the peak of the turn is shifted to a higher angle compared to the corresponding peak of the turn. Solid electrolyte material.
7. The halide material is Li 3-x-f M f R.E. 1-y Me k y (Cl 1-u B u ) 6-x+y*(k-3) The solid electrolyte material according to claim 1 or 2, 。
8. The halide material is Li 3-x-f M f R.E. 1-y Me k y (Cl 1-p F p ) 6-x+y*(k-3) wherein 0<=p<2. The solid electrolyte material according to claim 1,
9. RE includes Y, Ce, Gd, Er, La, or Yb; Me includes Y, Ce, Gd, Er, Sm, Eu, Pr, Tb, Al, Zr, La, Yb, Mg, Zn, Sn, Mg, C a, or any combination thereof, wherein RE is different from Me. The solid electrolyte material described herein.
10. The halide material comprises an average diffracting crystallite size of at least 25 nm. Item 3. The solid electrolyte material according to item 1 or 2.
11. The halide material is Li 3-x R.E. 1-y Me k y (Cl 1-u B u ) 6- x+y*(k-3) where 0.08<=u<=0.
67.
4. The solid electrolyte material according to claim 3.
12. 1. An electrochemical device comprising: A solid electrolyte layer comprising the solid electrolyte material according to claim 1 or 2, a solid electrolyte layer, the oxide material including at least one of Cl and F; an electrode layer comprising a cathode active material in contact with the solid electrolyte material; The solid electrolyte layer is formed under oxidizing conditions in the vicinity of the electrode layer in a chlorine-deficient region or a fluorine-deficient region. The chlorine or fluorine deficient regions may be formed in the electrode layer. a lower concentration of chlorine or fluorine, respectively, compared to a distal region of the solid electrolyte layer; Electrochemical devices, including
13. Li a M a Me b Me' b’ X c X' c’ Including halide materials represented by , a solid electrolyte material, the halide material being (b / (b+b’)) t * 0.84<b / (b+b’)<(b / (b+b’)) t * 1.16 (in the formula, (b / (b+b')) t However, the crystallographic phase diagram at temperatures between 20°C and 25°C is (corresponding to the crystallographic phase transition above) (c / (c+c’)) t * 0.84<c / (c+c’)<(c / (c+c’)) t * 1.16 (in the formula, (c / (c+c')) t However, the crystallographic phase diagram at temperatures between 20°C and 25°C is (corresponding to the crystallographic phase transition above), or (a / (a+a’)) t * 0.84<a / (a+a’)<(a / (a+a’)) t * 1.16 (wherein, (a / (a+a')) t However, the crystallographic phase diagram at temperatures between 20°C and 25°C is (corresponding to the crystallographic phase transition above), During the ceremony, Me is a group IIIB element, a group IVB element, V, Cr, Mn, Fe, Co, Ni, C u, Zn, Zr, Al, In, Sn, Pb, Bi, Sb, Mg, Ca, Ga, and Ge At least one element from the group consisting of Me' is a group IIIB element, a group IVB element, V, Cr, Mn, Fe, other than Me; Co, Ni, Cu, Zn, Zr, Al, In, Sn, Pb, Bi, Sb, Mg, Ca, G at least one element selected from the group consisting of a, b, and Ge; b>=b', c>=c', a>=a', and X is at least one other than X'. at least one halogen, X' is a halogen; M is at least one alkali metal element other than Li; A solid electrolyte material, wherein the anions of the halide material are in a single phase.
14. The crystallographic phase transition Transition from layered to non-layered crystal structures, Transition from cubic close-packed to hexagonal close-packed structure, From the C2 / m space group or the R-3m space group to the P-3m1 or Pnma space group transitions, from a non-layered crystal structure to another non-layered or layered crystal structure; Transition from R3c to R3m, or From the P-3m1 or Pnma space group to the C2 / m space group or the R-3m space group The solid electrolyte material of claim 13, comprising a transition.
15. The halide material is Li a-f M a’ R.E. b Me' k b’ (Cl c B C’ ) 6-f+(k-3)*b’ wherein: a+a′=3, −1≦f≦1, c+c′=1, The solid electrolyte material according to claim 13 or 14, wherein b+b'=1.
Citation Information
Patent Citations
Solid electrolyte material and battery
WO2019135315A1
Solid electrolyte material and battery
WO2019135316A1
Solid electrolyte material and battery
WO2019135317A1
Solid electrolyte material and battery
WO2019135318A1
Method for producing halides