Laver net

A seaweed net with controlled surface protrusions and pores on polyester fibers addresses drying and strength issues, enhancing spore adhesion and deterring fish feeding, ensuring high-quality seaweed growth and durability.

JP2024138805AInactive Publication Date: 2024-10-09TORAY INDUSTRIES INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023049501
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing seaweed nets using vinylon fibers face challenges in drying time during low tide, leading to poor seaweed quality and reduced strength when immersed in seawater, while mixed polyester fibers result in uneven spore adhesion and increased fish feeding damage due to surface reflectance issues.

Method used

A seaweed net with polyester fibers featuring micro-sized protrusions and controlled pores on the surface and within the fiber, maintaining mechanical strength and reducing gloss to deter fish, while enhancing spore adhesion through physical catching effects.

Benefits of technology

The net achieves high spore adhesion and resistance to fish feeding damage by controlling surface roughness, pore size, and porosity, ensuring both mechanical durability and effective seaweed growth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138805000001
    Figure 2024138805000001
Patent Text Reader

Abstract

To provide a laver net having good mechanical properties and additionally both excellent laver spore adhesion properties and the ability in inhibiting damage caused by fish and the like.SOLUTION: Provided is a laver net having: a fiber surface with convex portions; an arithmetic mean roughness of the fiber surface of 1 μm or more and less than 10 μm; at least pores within a depth of 5 μm from the fiber surface layer; an average circular equivalent diameter of the pores being 5 nm or more and 80 nm or less; a porosity of 2% or more and 15% or less; and at least a part of which is made of polyester fibers.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a seaweed net. [Background technology]

[0002] Traditionally, vinylon fiber has been the main material used for seaweed nets because it is excellent for seaweed seeding and growth. One of the reasons why vinylon fiber is excellent for seaweed seeding and growth is that the fine irregularities on the fiber surface make it easy for seaweed spores to attach to the net. However, to obtain high-quality seaweed, it is necessary to dry the seaweed appropriately during growth. Specifically, when cultivating seaweed in areas with small tidal differences, it is necessary to dry the seaweed nets at low tide, but vinylon fiber is difficult to dry in a short time, which has a negative effect on seaweed growth, making it difficult to harvest high-quality seaweed.

[0003] Furthermore, although vinylon fiber has excellent fiber properties in a dry state, the fiber strength decreases when immersed in seawater, so the strength of the net decreases and it becomes more susceptible to breakage.

[0004] In order to improve these points, research is being conducted into seaweed nets made from polyester fiber, which is easy to dry and has excellent mechanical properties.

[0005] For example, it has been proposed that by using a mixed twisted yarn of vinylon fiber and polyester fiber, a seaweed net can be obtained that dries more easily and has better mechanical properties than if vinylon fiber was used alone (Patent Document 1).

[0006] In addition, a technology has been proposed in which a foaming agent is mixed into polyester resin and foaming is used to form protrusions on the surface of the fibers, thereby improving the adhesion of seaweed spores when used as a seaweed net (Patent Document 2).

[0007] Furthermore, a technology has been proposed in which a polyoxyalkylene compound is mixed into a polyester resin to increase the hydrophilicity of the seaweed net, and when the polyoxyalkylene compound naturally dissolves out of the fibers during the manufacturing process or during use, recesses are formed on the fiber surface, improving the adhesion of seaweed spores when used as a seaweed net (Patent Document 3). [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 04-335835 [Patent Document 2] JP 2004-019013 A [Patent Document 3] Japanese Patent Application Publication No. 56-061930 Summary of the Invention [Problem to be solved by the invention]

[0009] Patent Document 1 describes that in order to compensate for the loss of strength of vinylon fibers when immersed in seawater, polyester fibers with excellent mechanical properties are mixed and twisted with vinylon fibers, and that as a result, a seaweed net with less breakage and bending is obtained than a seaweed net knitted with vinylon fibers alone. However, when hydrophobic polyester fibers and hydrophilic vinylon fibers are mixed and twisted, differences in moisture content occur within the seaweed net, causing uneven adhesion rates of seaweed spores, which makes it difficult to obtain good quality seaweed.

[0010] In addition, the technology proposed in Patent Document 2 improves the adhesion of seaweed spores by forming foamed protrusions on the fiber surface by kneading a foaming agent into the polyester resin. However, since it is difficult to control the size of the protrusions formed on the fiber surface by the foaming agent, there is a problem that unevenness in the size of the protrusions occurs in the fiber axis direction, resulting in uneven growth of seaweed in the seaweed net.

[0011] In addition, the technology proposed in Patent Document 3 discloses that by kneading an easily soluble polymer into a polyester resin, minute depressions can be formed on the surface when the polymer naturally dissolves from the fiber surface during the manufacturing process or during use, and as a result, the adhesion of seaweed spores can be improved. However, the formation of minute depressions on the surface reduces the light reflectance of the fiber, which raises the problem of increasing the probability of damage caused by fish and the like.

[0012] Therefore, an object of the present invention is to provide a seaweed net that combines good mechanical properties with excellent adhesion of seaweed spores and the ability to suppress damage caused by fish and the like. [Means for solving the problem]

[0013] As a result of further investigations, the inventors have found that the excellent seaweed spore adhesion properties of vinylon fibers, which have traditionally been used in seaweed nets, are due to the anchoring effect caused by the fine irregularities on the surface of the vinylon fibers.

[0014] Furthermore, the inventors' further investigations revealed that fish and other creatures can easily recognize highly reflective and highly glossy materials in the sea, and that they react differently to the two substances. Specifically, they found that while highly reflective materials are highly wary, highly glossy materials are easily recognized as food, and therefore the highly glossy parts of the seaweed nets become the starting point of feeding damage.

[0015] However, although forming fine irregularities on the fiber surface is effective in improving seaweed spore adhesion, forming fine irregularities on the fiber surface reduces the surface reflectance of the fiber, and as mentioned above, fish and other insects become less wary of the resulting seaweed net, making it more likely for it to be eaten by the fish, so the two tend to be contradictory.

[0016] As a result of further investigations, the inventors came up with the idea of ​​forming micro-sized protrusions on the fiber surface while at the same time forming specific sized voids inside the fiber, thereby suppressing the gloss of the seaweed net through internal diffuse reflection.

[0017] Based on this knowledge, the inventors conducted intensive research to achieve the above-mentioned objective, and discovered that by setting the surface roughness of polyester fibers within a specific range, the bonding strength between attached seaweed spores is strengthened and the physical catching effect at the protrusions provides excellent adhesion of seaweed spores, and further, by forming holes in the surface layer of the fibers and setting the hole size and porosity within a specific range, a low-gloss seaweed net can be produced, resulting in a seaweed net that combines excellent adhesion of seaweed spores with the ability to inhibit feeding damage by fish and the like, and has excellent mechanical properties, thereby completing the present invention.

[0018] The present invention aims to solve the above problems, and provides the following inventions.

[0019] [1] A seaweed net made at least in part of polyester fibers, the net having a fiber surface with convex portions, an arithmetic mean roughness of the fiber surface of 1 μm or more and less than 10 μm, at least one pore being present within a depth of 5 μm from the fiber surface, an average circular equivalent diameter of the pores being 5 nm or more and 80 nm or less, and a porosity of 2% or more and 15% or less.

[0020] [2] A method for producing a seaweed net as described in [1], characterized in that the dissolution treatment forms voids in the polyester fibers without dissolving the protrusions on the fiber surface. Effect of the Invention

[0021] In addition to having excellent mechanical properties, the seaweed net of the present invention has micro-sized protrusions on the surface of the fibers that make up the seaweed net, which strengthens the bonding force between the attached seaweed spores and promotes the adhesion of the seaweed spores to the seaweed net through the physical catching effect of the protrusions.Furthermore, by having pores on the surface of the fibers and setting the pore size and porosity within a specific range, the glossiness of the seaweed net can be reduced, and the net exhibits the ability to inhibit feeding damage by fish and other organisms. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The seaweed net of the present invention is at least partially made of polyester fibers, which have convex portions on their fiber surfaces, the arithmetic mean roughness of the fiber surface being 1 μm or more and less than 10 μm, at least pores being present within a depth of 5 μm from the fiber surface, the average circular equivalent diameter of the pores being 5 nm or more and 80 nm or less, and the porosity being 2% or more and 15% or less.

[0023] The seaweed net of the present invention will be described in detail below, but the present invention is not limited to the scope described below as long as it does not exceed the gist of the present invention, and various modifications are possible without departing from the gist of the present invention.

[0024] The polyester fiber used in at least a part of the laver net of the present invention has an arithmetic mean roughness of the fiber surface of 1 μm or more and less than 10 μm. The lower limit of the arithmetic mean roughness of the fiber surface is 1 nm or more, preferably 1.5 μm or more, more preferably 2 μm or more, so that the bonding force between the attached laver spores is strong, and the convex parts have a physical catching effect, making the laver spores less likely to fall off. On the other hand, the upper limit of the arithmetic mean roughness of the fiber surface is less than 10 μm, preferably 9 μm or less, more preferably 8 μm or less, so that the specific surface area of ​​the laver net is improved, and the adhesion rate of the laver spores during seeding is improved.

[0025] In the present invention, the arithmetic mean roughness of the fiber surface refers to a value measured and calculated by the method described in Section A of the Examples section.

[0026] The polyester fiber used in at least a part of the seaweed net of the present invention has at least pores in the cross section within 5 μm depth from the fiber surface. If 1% or more of the total number of pores is not present within 5 μm depth from the fiber surface, the diffuse reflection inside the fiber becomes weak, the gloss cannot be suppressed, and the performance of suppressing feeding damage by fish, etc. cannot be exhibited.

[0027] The polyester fiber used in at least a part of the seaweed net of the present invention has an average circle equivalent diameter of pores in the fiber cross section of 5 nm to 80 nm. The lower limit of the average circle equivalent diameter of the pores in the fiber cross section is 5 nm or more, preferably 10 nm or more, and more preferably 15 nm or more, so that the diffuse reflection inside the fiber can be strengthened and the luster of the seaweed net can be suppressed, thereby exhibiting a performance of suppressing damage caused by fishes, etc. On the other hand, the upper limit of the average circle equivalent diameter of the pores in the fiber cross section is 80 nm or less, preferably 70 nm or less, and more preferably 60 nm or less, so that the seaweed net can exhibit sufficient fiber strength, is less likely to break, and has sufficient mechanical properties.

[0028] The polyester fiber used in at least a part of the seaweed net of the present invention has a porosity of 2% or more and 15% or less. By setting the lower limit of the porosity to 2% or more, preferably 3% or more, and more preferably 5% or more, the number of holes in the fiber cross section increases, the diffuse reflection inside the fiber can be strengthened, and the luster of the seaweed net can be suppressed, thereby exhibiting a performance of suppressing damage caused by fishes, etc. On the other hand, by setting the upper limit of the porosity to 15% or less, preferably 12% or less, and more preferably 10% or less, an excessive increase in the porosity of the fiber can be suppressed, sufficient fiber strength can be exhibited, and the seaweed net is less likely to break and has sufficient mechanical properties.

[0029] In the present invention, the presence of pores in the cross section of the fiber, the average equivalent circular diameter of pores and the porosity refer to values ​​measured and calculated by the method described in item B of the Examples section.

[0030] The polyester fiber used for at least a part of the seaweed net in the present invention is not particularly limited with respect to its form, and may be in any form such as monofilament, multifilament, etc. Also, it can be processed into false twist or twisted yarn in the same manner as general fibers.

[0031] The fineness of the polyester fiber used in at least a part of the seaweed net in the present invention is preferably 100 dtex or more and 3000 dtex or less. The lower limit of the fineness of the polyester fiber is preferably 100 dtex or more, more preferably 300 dtex or more, and even more preferably 500 dtex or more, which improves the productivity during spinning and improves the work efficiency during knitting since the number of fibers required for making the net thread is reduced. On the other hand, the upper limit of the fineness of the polyester fiber is preferably 3000 dtex or less, more preferably 2500 dtex or less, and even more preferably 2000 dtex or less, which makes it possible to obtain uniform cooling properties in the cooling process after spinning and to suppress deterioration of the quality of the seaweed net due to deterioration of the fiber physical properties, etc.

[0032] The cross-sectional shape of the polyester fiber used in at least a part of the seaweed net of the present invention is not particularly limited as long as it does not impair the effects of the present invention. The cross-sectional shape may be a round cross-section, or an irregular cross-section such as a triangular, flat, hexagonal, or hollow cross-section. However, a round cross-section is preferred because it has a large specific surface area and is excellent in productivity.

[0033] The polyester fiber used in at least a part of the seaweed net of the present invention may be a single component fiber made of one type of polymer, or a composite fiber made of two or more types of polymers, but composite fibers are preferred because they are more likely to produce the effects of the present invention. Composite fibers can be appropriately selected from sheath-core, sea-island, side-by-side, eccentric sheath-core, etc., but sheath-core types are preferred because of their excellent productivity and ease of management.

[0034] The seaweed net of the present invention may be a net made from a net thread containing the above-mentioned polyester fiber, or may be a net containing the above-mentioned polyester fiber separately from the net thread. When the above-mentioned polyester fiber is used as the net thread, it may be used alone, or may be mixed and twisted with hydrophobic fibers such as polyamide fibers, polyester fibers, polypropylene fibers, and polyethylene fibers.

[0035] There is no particular limitation on the type of weave of the seaweed net used in the present invention, but knotless weave net, frog weave net, Russell net, etc. are preferred.

[0036] The fineness of the net thread obtained by cutting from the seaweed net of the present invention is preferably 600 dtex or more and 18000 dtex or less. The lower limit of the fineness of the polyester fiber is preferably 600 dtex or more, more preferably 1200 dtex or more, and even more preferably 1800 dtex or more, so that the adhesion area of ​​seaweed spores is improved and seaweed productivity is improved. On the other hand, the upper limit of the fineness of the net thread is preferably 18000 dtex or less, more preferably 15000 dtex or less, and even more preferably 12000 dtex or less, so that the seaweed net is lighter and easier to handle.

[0037] The tensile strength of the net thread obtained by cutting from the seaweed net of the present invention is preferably 2.0 cN / dtex or more and 12.0 cN / dtex or less. The lower limit of the tensile strength of the net thread is preferably 2.0 cN / dtex or more, more preferably 2.5 cN / dtex or more, and even more preferably 3.0 cN / dtex or more, so that the seaweed net is less likely to break and has sufficient mechanical properties. On the other hand, the upper limit of the tensile strength of the net thread is preferably 12.0 cN / dtex or less, more preferably 11.0 cN / dtex or less, and even more preferably 10.0 cN / dtex or less, so that the net can be easily cut and can be easily disposed of or reused.

[0038] In the present invention, the tensile strength of the net yarn refers to a value measured and calculated by the method described in item F of the Examples section.

[0039] Next, a method for producing the nori net and the polyester fiber used in at least a part of the nori net in the present invention will be described. Although the production method is not particularly limited and any known method can be adopted, it is preferable to adopt melt spinning, which allows for mass production while maintaining low fuzz in low-cost and long-term production, so an example will be described below.

[0040] The polyester fiber used in at least a part of the seaweed net of the present invention is composed of a core made of an alloy polymer obtained by kneading a polyester polymer and a water-soluble substance, and a sheath made of a polyester polymer mixed with fine particles for forming convex portions. The polyester fiber can be obtained by obtaining the fiber by a known melt spinning method, and then removing the water-soluble substance from the fiber by a dissolution treatment. When kneading the polyester polymer and the water-soluble substance, a compatibilizer may be used in combination as necessary. The porosity can be controlled by the mixing ratio of the water-soluble substance in the polyester polymer. For example, the porosity can be increased by increasing the mixing ratio of the water-soluble substance.

[0041] The polyester polymer used in the manufacture of the polyester fiber used in at least a part of the seaweed net of the present invention is not particularly limited as long as it is a polymer in which monomers are linked by ester bonds. Specific examples include aromatic polyesters such as polyethylene terephthalate (PET), polytrimethylene terephthalate (PPT), polybutylene terephthalate (PBT), and polyethylene naphthalate (PEN), and aliphatic polyesters such as polylactic acid. Aromatic polyesters are preferred from the viewpoint of versatility and excellent fiber formability.

[0042] The type of water-soluble substance used in the manufacture of polyester fibers used in at least a part of the seaweed net of the present invention is not particularly limited as long as it is highly soluble in the elution treatment solution and can be an alloy polymer dispersed in nano-size in the polyester polymer. Specific examples include water-soluble polymers such as polyethylene glycol, polyvinyl alcohol, polyvinylpyrrolidone, polyglycerin and their derivatives, and inorganic salts such as sodium chloride, calcium oxide and magnesium oxide. From the viewpoint of spinnability, water-soluble polymers are preferred, and among them, polyethylene glycols having a number average molecular weight of 6000 to 40000 are particularly preferred from the viewpoint of heat resistance and solubility in the elution treatment solution. The average circle equivalent diameter of the pores can be controlled by the dispersion diameter of the water-soluble substance in the polyester polymer. When a water-soluble polymer such as polyethylene glycol is used as the water-soluble substance, the dispersion diameter can be controlled by the number average molecular weight, so for example, by increasing the number average molecular weight of polyethylene glycol, the dispersion diameter becomes larger and the average circle equivalent diameter of the pores also becomes larger.

[0043] The fine particles for forming the convex portions used in the manufacture of the polyester fiber used in at least a part of the laver net of the present invention are not particularly limited as long as they do not show elution behavior when the water-soluble substance is eluted. Specific examples include inorganic fine particles such as titanium oxide, calcium carbonate, silica, kaolin, clay, and natural fine particles such as powder derived from trees, and from the viewpoint of reducing environmental load, powder derived from trees is preferred. From the viewpoint of spinnability, the particle diameter is preferably 1 μm or more and 20 μm or less. With regard to the particle diameter, the lower limit is preferably 1.5 μm or more, more preferably 2 μm or more, so that the physical catching effect at the convex portions is easily generated. On the other hand, with regard to the particle diameter, the upper limit is preferably 18 μm or less, more preferably 16 μm or less, so that the laver net has sufficient mechanical properties.

[0044] The content of the polyester-based polymer in the alloy polymer used in the production of the polyester fiber used in at least a part of the laver net in the present invention is not particularly limited as long as it is 50% by weight or more, and can be any content. From the viewpoint of fiber properties, the content of the polyester-based polymer in the alloy polymer is preferably 85% by weight or more.

[0045] There is no limitation on the method of kneading the polyester polymer, water-soluble substance, and microparticles for forming the convex portions used in the manufacture of the polyester fiber used in at least a part of the laver net in the present invention. The polyester polymer after polycondensation may be kneaded with the water-soluble substance and microparticles for forming the convex portions while it is in a molten state, or the polyester polymer may be kneaded with the water-soluble substance and microparticles for forming the convex portions while it is in a remelted state after being cooled and solidified. The polyester polymer may be directly blended with the water-soluble substance and microparticles for forming the convex portions, but in order to easily achieve the effects of the present invention, it is preferable to knead the polyester polymer with the water-soluble substance, and the polyester polymer with the microparticles for forming the convex portions separately. From the viewpoint of forcibly kneading each component, it is preferable to knead using a twin-screw extruder.

[0046] The polyester-based polymer and water-soluble substance used in the production of the polyester fiber used in at least a part of the laver net in the present invention, and the fine particles and mixed substance for forming the convex portions can be made into useful fibers by known melt spinning and drawing methods.

[0047] The seaweed net of the present invention is subjected to a dissolution treatment, in which water-soluble substances are dissolved into a treatment solution, forming pores in the fibers.

[0048] As the treatment liquid used in the elution treatment, it is preferable to use a known aqueous solution, but it is preferable to use hot water in order to form pores in the polyester fiber without eluting the convex parts. The hot water weight reduction treatment can maintain the polyester polymer constituting the fiber surface while eluting the water-soluble substance inside the fiber, and it becomes easier to form and control micro-sized convex parts on the fiber surface. It is also possible to use an alkaline solution by controlling the temperature, time, concentration, etc. so that the polyester polymer on the fiber surface layer is not reduced in weight and the formation of convex parts is not hindered. When hot water is used as the treatment liquid, the temperature of the treatment liquid is preferably 100°C or less, more preferably 80°C or less, so that pores are formed in the fiber, diffuse reflection inside the fiber and gloss on the fiber surface are both achieved, and the performance of inhibiting feeding damage by fishes and the like can be expressed. There is no particular limit on the lower limit of the treatment temperature, but it is preferable to set it to 25°C or more in order to sufficiently elute the water-soluble substance inside.

[0049] When warm water is used as the treatment liquid, the treatment time is preferably 30 minutes or less, more preferably 20 minutes or less, so that pores are sufficiently formed in the fibers. There is no particular lower limit to the treatment time, but in order to sufficiently elute the water-soluble substances inside, the treatment time is preferably 10 minutes or more.

[0050] The seaweed net of the present invention can be obtained by preparing a net thread by beam warping the polyester fiber and twisting it, and then knitting the net with a knitting machine to obtain a knitted fabric. The knitted fabric is then subjected to a dissolution treatment to form pores inside the fibers, followed by washing with water and air drying to obtain the seaweed net of the present invention. EXAMPLES

[0051] The present invention will be described in more detail below with reference to examples. The property values ​​in the examples were determined by the following methods.

[0052] A. Arithmetic mean roughness of fiber surface One hundred fibers were randomly taken from the seaweed net, and each fiber was fixed to a silicon wafer with epoxy resin so that the longitudinal direction of the fiber was parallel to the silicon wafer surface. The sample was measured using a Bruker AXS scanning probe microscope (SPM) "NanoScopeV Dimension Icon". The measurement conditions were a scanning range of 5 μm square, a scanning speed of 0.4 Hz, and tapping mode under room temperature atmospheric conditions. The fiber longitudinal direction was defined as the X axis, the direction parallel to the silicon wafer surface and perpendicular to the X axis as the Y axis, and the direction perpendicular to both the X axis and the Y axis as the Z axis. The apex of the fixed fiber in the Z axis direction was scanned with a silicon cantilever so that it was perpendicular to the longitudinal direction (X axis) of the fiber. The roundness of the fiber was corrected for the obtained AFM image, and the average absolute value of the deviation from the center plane to the surface in the height profile of the quantitative surface was calculated using the image analysis software "NanoScope Analysis 1.40". The above-mentioned measurements and calculations were carried out on 100 of the removed fibers, and the calculated average value was rounded off to the first decimal place to be used as the arithmetic mean roughness of the fiber surface.

[0053] B. Presence or absence of pores within 5 μm depth from the fiber surface in the cross section of the fiber, porosity, and average circular equivalent diameter of pores One hundred fibers were randomly taken from the seaweed net, and for each fiber, a cross-sectional section was prepared using an EOL ion milling device "IB-19520CCP" with an Ar laser while cooling with liquid nitrogen. The obtained section was sputter-coated with metal fine particles. This sample was measured using a Hitachi High-Technologies Corporation field emission scanning electron microscope (FE-SEM) "SU8020" at an acceleration voltage of 1.5 kV to observe the presence or absence of voids and voids within a depth of 5 μm from the fiber surface. The observed image was imported into the image analysis software Image-J and binarized to extract only the void region. At this time, the binarization threshold was manually adjusted while viewing the image, and set so that only the void region was extracted. After the void region was extracted in this way, the fiber cross-sectional area was measured at a depth of 1 μm. 2The porosity was calculated from the ratio of the total area of ​​all pores per fiber. The above measurements and calculations were carried out for 100 removed fibers, and the calculated average value was rounded off to the nearest tenth to obtain the porosity. In addition, the circle equivalent diameter (diameter) was calculated from the pore area of ​​each pore, and the diameter was calculated from the area of ​​each pore per 1 μm of the fiber cross section. 2 The average of the equivalent circle diameters of all pores per 100 fibers was calculated. The above measurements and calculations were carried out for 100 fibers, and the calculated average value was rounded off to the nearest tenth, and this was used as the average equivalent circle diameter of the pores on the fiber surface.

[0054] C. Intrinsic Viscosity (IV) of Polyester Polymers 10 ml of o-chlorophenol (hereinafter abbreviated as OCP) was added to 0.8 g of sample. The sample was dissolved at 160°C for 30 minutes, and then slowly cooled to obtain a measurement solution. The relative viscosity ηr of the measurement solution was calculated at 25°C using an Ostwald viscometer according to the following formula, and the intrinsic viscosity was calculated. ηr=η / η0=(t×d) / (t0×d0) Intrinsic viscosity=0.0242ηr+0.2634 Here, η is the viscosity of the polymer solution, η0 is the viscosity of the OCP, t is the drop time of the solution (sec), and d is the density of the solution (g / cm 3 ), t0: OCP fall time (sec), d0: OCP density (g / cm 3 ).

[0055] D. Number average molecular weight of polyethylene glycol 500 mg of polyethylene glycol was dissolved in 5 mL of 0.1 M sodium chloride solution, and the filtrate was filtered through a 0.45 μm cellulose filter to obtain a sample for GPC measurement. Measurements were performed using this sample under the following conditions using a Waters GPC device "Alliance 2690" to calculate the number average molecular weight. Detector: Waters 2410 refractive index detector, sensitivity 128x Column: Tosoh TSKgel G3000PWXLI Solvent: 0.1M sodium chloride solution Injection volume: 200μL Column temperature: 40℃ Standard substance: polyethylene glycol (Mw 106-10100, manufactured by AML Corporation).

[0056] E. Net thread fineness In an environment with a temperature of 20°C and a humidity of 65% RH, 1 m of fiber was randomly sampled from the seaweed net, the weight was measured, and the fineness (dtex) was calculated using the following formula.

[0057] Fineness (dtex) = weight of 1m of net thread (g) x 10,000 The measurement was carried out five times for each sample, and the calculated average value was rounded off to the first decimal place to obtain the fineness (dtex).

[0058] F. Tensile strength of netting thread Five 40cm long net thread samples were taken from random locations on the seaweed net, and a tensile test was conducted on each net thread using Orientec's UTM-III-100 under conditions of 20℃ temperature and 65%RH humidity, with an initial sample length of 25cm and a tensile speed of 30cm / min. The samples were attached with one section and one leg. The stress (cN) at the point showing the maximum load of each sample was divided by the net thread fineness (dtex), and the calculated average value for each sample was rounded off to one decimal place and used as the tensile strength (cN / dtex) of the net thread.

[0059] G. Number of seaweed spores attached per unit area (adhesiveness of seaweed spores) A 500mL beaker containing seawater and oysters carrying seaweed spores was placed in an incubator kept at 16℃, and a seaweed net sample cut into a size of 10cm length and 10cm width was hung so that it was submerged in the seawater in the beaker. Next, the beaker was irradiated with 4000 lux daylight for 8 hours a day for 5 days, after which the seaweed net sample was taken out and observed at 5 random locations of 1mm x 1mm on the sample surface using a 100x objective lens in optical transmission mode using a Keyence Corporation microscope "VHX-2000". The average number of seaweed spores attached to each area was used to make the following judgments. A: 10 or more seaweed spores attached within a 1mm x 1mm area B: 5-9 seaweed spores attached in one field of view within a 1mm x 1mm area C: Fewer than four seaweed spores attached within a 1 mm x 1 mm area.

[0060] H. Number of contacts of black porgy with seaweed net (feeding damage prevention performance) A net measuring 1.0m in length and 1.0m in width, with seaweed spores attached, was installed parallel to the sea surface in a 100m long, 100m wide, and 5.0m deep fish pen containing seawater and 100 farmed black porgy. After installation, the behavior of black porgy near the net was observed with a fixed camera for 24 hours, and the number of times the black porgy came into contact with the net was counted. If the number of contacts was less than 5,000, it was determined that the net had the ability to suppress feeding damage.

[0061] Example 1 As the core component, polyester pellets with an IV of 1.3 and polyethylene glycol with a number average molecular weight of 20,000 (PEG20000 manufactured by Sanyo Chemical Industries, Ltd.) were mixed in a ratio of 90% by weight and 10% by weight in a twin-screw mixer (TEX30α manufactured by Nippon Kosho Co., Ltd.) at a cylinder temperature of 290°C, a discharge rate of 8 kg / h, and a screw rotation speed of 110 rpm. The mixed product was discharged into cold water in the form of a strand, cooled, and immediately cut to obtain pellet-shaped mixed product pellet A. In addition, as the sheath component, pellet B was obtained by adding 5% by weight of powder derived from Abies sachalinensis (average particle size: 10 μm) to polyester pellets with an IV of 1.3 in the same manner as pellet A, and pellets A and B were then vacuum dried at 150°C for 12 hours. The mixture was then continuously fed to an extruder, melted at 290°C, and spun from a core-sheath composite spinneret (84 holes, round holes) at a core-sheath ratio (area ratio) of 80:20 at a discharge rate of 825 g / min.

[0062] The spun yarn was passed through a heating cylinder installed just below the spinneret, where the atmospheric temperature inside the cylinder was 200°C, and then 40°C cold air was blown at a speed of 30 m / min using a circular chimney to cool and solidify the yarn. Next, after cooling, a fiber oil was applied using an oiling roll, and the obtained yarn was taken up by 1GR (75°C) with a speed of 505 m / min and continuously subjected to a drawing process. The yarn that had passed through the 1GR was then drawn by continuously passing it through the 2GR with a surface temperature of 101°C and a speed of 535 m / min, the 3GR with a speed of 110°C and a speed of 1818 m / min, the 4GR with a speed of 225°C and a speed of 2651 m / min, and the 5GR with a speed of 2700 m / min without heating, without being taken up once. The yarn bundling treatment was performed between 2GR and 3GR, and the entanglement treatment was performed between 5GR and the winding device by spraying high-pressure air of 0.4 MPa and 0.5 MPa, respectively, and then the yarn was wound up on the winding device to produce a polyethylene terephthalate fiber of 1100 dtex-84f.

[0063] Next, two of the obtained drawn yarns were beam-warped to produce a strand. Next, a three-ply net yarn consisting of three of the strands was produced, and the three-ply net yarn was woven by a knotless knitting method to a mesh size of 100 mm x 100 mm. Next, the obtained knotless net was immersed in water and subjected to a dissolution treatment at 80°C for 20 minutes, after which it was washed with water and air-dried to obtain a seaweed net. The evaluation results of the fiber properties and seaweed net properties are shown in Table 1. It was confirmed that the fibers constituting the seaweed net had pores with an average circle equivalent diameter of 9 nm and a porosity of 9%, and that pores existed within a depth of 5 μm from the fiber surface layer in the fiber cross section. In addition, the fiber surface had convex parts, and the arithmetic mean roughness of the fiber surface was 5 μm. The net yarn strength of the seaweed net was 5.3 cN / dtex, and the number of seaweed spores attached was 30 / mm 2 The number of times black porgy came into contact with the seaweed net was 1,500 times, and the resulting seaweed net had excellent mechanical properties, high seaweed spore adhesion properties, and was also confirmed to have the ability to suppress feeding damage.

[0064] Example 2 Fibers and seaweed nets were obtained in the same manner as in Example 1, except that the temperature of the elution treatment after weaving was changed to 30°C. The evaluation results of the fiber properties and seaweed net properties are shown in Table 1. It was confirmed that the fibers constituting the seaweed net had pores with an average circular equivalent diameter of 7 nm and a porosity of 6%, and that the pores existed within a depth of 5 μm from the fiber surface in the fiber cross section. In addition, the fiber surface had convex portions, and the arithmetic mean roughness of the fiber surface was 5 μm. The net thread strength of the seaweed net was 6.0 cN / dtex, and the number of attached seaweed spores was 18 / mm. 2 The number of times black porgy came into contact with the seaweed net was 1,800 times, and the resulting seaweed net had excellent mechanical properties, high seaweed spore adhesion properties, and was also confirmed to have the ability to suppress feeding damage.

[0065] Example 3 Fibers and seaweed nets were obtained in the same manner as in Example 1, except that a dissolution treatment was carried out for 40 minutes after weaving. The evaluation results of the fiber properties and seaweed net properties are shown in Table 1. It was confirmed that the fibers constituting the seaweed net had pores with an average circular equivalent diameter of 9 nm and a porosity of 12%, and that pores existed within a depth of 5 μm from the fiber surface in the fiber cross section. In addition, the fiber surface had convex portions, and the arithmetic mean roughness of the fiber surface was 5 μm. The net thread strength of the seaweed net was 5.3 cN / dtex, and the number of attached seaweed spores was 10 / mm. 2 The number of times black porgy came into contact with the seaweed net was 1,500 times, and the resulting seaweed net had excellent mechanical properties, high seaweed spore adhesion properties, and was also confirmed to have the ability to suppress feeding damage.

[0066] Example 4 Fibers and seaweed nets were obtained in the same manner as in Example 1, except that 10% by weight of powder (average particle size: 10 μm) derived from Todomatsu was added to polyester pellets with an IV of 1.3 as the sheath component. The evaluation results of the fiber properties and seaweed net properties are shown in Table 1. It was confirmed that the fibers constituting the seaweed net had pores with an average equivalent circle diameter of 9 nm and a porosity of 9%, and that pores existed within a depth of 5 μm from the fiber surface in the fiber cross section. In addition, the fiber surface had convex portions, and the arithmetic mean roughness of the fiber surface was 9 μm. The net thread strength of the seaweed net was 4.5 cN / dtex, and the number of attached seaweed spores was 21 / mm. 2The number of times black porgy came into contact with the seaweed net was 1,500 times, and the resulting seaweed net had excellent mechanical properties, high seaweed spore adhesion properties, and was also confirmed to have the ability to suppress feeding damage.

[0067] Example 5 Fibers and seaweed nets were obtained in the same manner as in Example 1, except that the number-average molecular weight of the polyethylene glycol used was changed to 6000 (PEG60000S manufactured by Sanyo Chemical Industries, Ltd.). The evaluation results of the fiber properties and seaweed net properties are shown in Table 1. It was confirmed that the fibers constituting the seaweed net had pores with an average circular equivalent diameter of 5 nm and a porosity of 9%, and that the pores existed within a depth of 5 μm from the fiber surface in the fiber cross section. In addition, the fiber surface had convex portions, and the arithmetic mean roughness of the fiber surface was 5 μm. The net thread strength of the seaweed net was 7.0 cN / dtex, and the number of attached seaweed spores was 30 / mm. 2 The number of times black porgy came into contact with the seaweed net was 1,300 times, and the resulting seaweed net had excellent mechanical properties, high seaweed spore adhesion properties, and was also confirmed to have the ability to suppress feeding damage.

[0068] Example 6 Fibers and seaweed nets were obtained in the same manner as in Example 1, except that the number-average molecular weight of the polyethylene glycol used was changed to 40,000 (PEG40000S manufactured by Sanyo Chemical Industries, Ltd.). The evaluation results of the fiber properties and seaweed net properties are shown in Table 1. It was confirmed that the fibers constituting the seaweed net had pores with an average circular equivalent diameter of 25 nm and a porosity of 9%, and that the pores existed within a depth of 5 μm from the fiber surface in the fiber cross section. In addition, the fiber surface had convex portions, and the arithmetic mean roughness of the fiber surface was 5 μm. The net thread strength of the seaweed net was 4.0 cN / dtex, and the number of attached seaweed spores was 30 / mm. 2 The number of times black porgy came into contact with the seaweed net was 2,800 times, and the resulting seaweed net had excellent mechanical properties, high seaweed spore adhesion properties, and was also confirmed to have the ability to suppress feeding damage.

[0069] Example 7 Fibers and a seaweed net were obtained in the same manner as in Example 1, except that the amount of polyethylene glycol with a number-average molecular weight of 20,000 added was changed to 3 wt%. The evaluation results of the fiber properties and seaweed net properties are shown in Table 1. It was confirmed that the fibers constituting the seaweed net had pores with an average circular equivalent diameter of 9 nm and a porosity of 3%, and that the pores existed within a depth of 5 μm from the fiber surface in the fiber cross section. In addition, the fiber surface had convex portions, and the arithmetic mean roughness of the fiber surface was 5 μm. The net thread strength of the seaweed net was 8.0 cN / dtex, and the number of attached seaweed spores was 30 / mm. 2 The number of times black porgy came into contact with the seaweed net was 2,500 times, and the resulting seaweed net had excellent mechanical properties, high seaweed spore adhesion properties, and was also confirmed to have the ability to suppress feeding damage.

[0070] Example 8 Fibers and a seaweed net were obtained in the same manner as in Example 1, except that the IV of the polyester pellets used was changed to 0.7, changing the average circular equivalent diameter of the pores. The evaluation results of the fiber properties and seaweed net properties are shown in Table 1. It was confirmed that the fibers constituting the seaweed net had pores with an average circular equivalent diameter of 9 nm and a porosity of 9%, and that the pores existed within a depth of 5 μm from the fiber surface in the fiber cross section. In addition, the fiber surface had convex portions, and the arithmetic mean roughness of the fiber surface was 5 μm. The net thread strength of the seaweed net was 2.8 cN / dtex, and the number of attached seaweed spores was 30 / mm. 2 The number of times black porgy came into contact with the seaweed net was 1,500 times, and the resulting seaweed net had excellent mechanical properties, high seaweed spore adhesion properties, and was also confirmed to have the ability to suppress feeding damage.

[0071] Comparative Example 1 Fibers and a seaweed net were obtained in the same manner as in Example 1, except that no elution treatment was carried out after weaving the net. The evaluation results of the fiber properties and seaweed net properties are shown in Table 1. The fibers constituting the seaweed net had no voids. In addition, the fiber surface had convex portions, and the arithmetic mean roughness of the fiber surface was 5 μm. The seaweed net had a net thread strength of 5.8 cN / dtex, and the number of seaweed spores attached was 4 / mm. 2 The number of times black porgy came into contact with the seaweed net was 10,000 times, but the resulting seaweed net had low adhesion of seaweed spores and no damage prevention performance was confirmed.

[0072] Comparative Example 2 Fibers and a seaweed net were obtained in the same manner as in Example 1, except that the amount of polyethylene glycol with a number-average molecular weight of 20,000 added was changed to 20 wt%. The evaluation results of the fiber properties and seaweed net properties are shown in Table 1. It was confirmed that the fibers constituting the seaweed net had pores with an average circular equivalent diameter of 9 nm and a porosity of 24%, and that the pores existed within a depth of 5 μm from the fiber surface in the fiber cross section. In addition, the fiber surface had convex portions, and the arithmetic mean roughness of the fiber surface was 5 μm. The net thread strength of the seaweed net was 1.5 cN / dtex, and the number of attached seaweed spores was 30 / mm. 2 The number of times black porgy came into contact with the Nori net was 1,300 times. The resulting Nori net had high adhesion properties for Nori spores and was confirmed to have the ability to suppress feeding damage, but it had poor mechanical properties.

[0073] Comparative Example 3 Fibers and seaweed nets were obtained in the same manner as in Example 1, except that the number-average molecular weight of the polyethylene glycol used was changed to 60,000 (PEG60000S manufactured by Sanyo Chemical Industries, Ltd.). The evaluation results of the fiber properties and seaweed net properties are shown in Table 1. It was confirmed that the fibers constituting the seaweed net had pores with an average circular equivalent diameter of 90 nm and a porosity of 9%, and that the pores existed within a depth of 5 μm from the fiber surface in the fiber cross section. In addition, the fiber surface had convex portions, and the arithmetic mean roughness of the fiber surface was 5 μm. The net thread strength of the seaweed net was 1.8 cN / dtex, and the number of attached seaweed spores was 30 / mm. 2 The number of times black porgy came into contact with the Nori net was 1,500 times. The obtained Nori net had high adhesion properties for Nori spores and was also confirmed to have the ability to suppress feeding damage, but it had poor mechanical properties.

[0074] Comparative Example 4 Fibers and seaweed nets were obtained in the same manner as in Example 1, except that the number-average molecular weight of the polyethylene glycol used was changed to 4000 (PEG40000S manufactured by Sanyo Chemical Industries, Ltd.). The evaluation results of the fiber properties and seaweed net properties are shown in Table 1. It was confirmed that the fibers constituting the seaweed net had pores with an average circular equivalent diameter of 3 nm and a porosity of 9%, and that the pores existed within a depth of 5 μm from the fiber surface in the fiber cross section. In addition, the fiber surface had convex portions, and the arithmetic mean roughness of the fiber surface was 5 μm. The net thread strength of the seaweed net was 5.5 cN / dtex, and the number of attached seaweed spores was 30 / mm. 2 The number of times black porgy came into contact with the Nori net was 7,000 times. The resulting Nori net had excellent mechanical properties and high Nori spore adhesion, but no evidence of damage prevention was confirmed.

[0075] Comparative Example 5 Fibers and a seaweed net were obtained in the same manner as in Example 1, except that the amount of polyethylene glycol with a number-average molecular weight of 20,000 added was changed to 1 wt%. The evaluation results of the fiber properties and seaweed net properties are shown in Table 1. It was confirmed that the fibers constituting the seaweed net had pores with an average circular equivalent diameter of 9 nm and a porosity of 1.3%, and that the pores existed within a depth of 5 μm from the fiber surface in the fiber cross section. In addition, the fiber surface had convex portions, and the arithmetic mean roughness of the fiber surface was 5 μm. The net thread strength of the seaweed net was 5.0 cN / dtex, and the number of attached seaweed spores was 30 / mm. 2 The number of times black porgy came into contact with the Nori net was 6,000 times. The resulting Nori net had excellent mechanical properties and high Nori spore adhesion, but no evidence of damage prevention was confirmed.

[0076] [Table 1]

Claims

1. The seaweed net is at least partially made of polyester fibers having a fiber surface with convex portions, an arithmetic mean roughness of the fiber surface being 1 μm or more and less than 10 μm, at least pores being present within a depth of 5 μm from the fiber surface layer, an average circular equivalent diameter of the pores being 5 nm or more and 80 nm or less, and a porosity being 2% or more and 15% or less.

2. The method for manufacturing a seaweed net according to claim 1, characterized in that the leaching treatment forms pores in the polyester fibers without dissolving the protrusions on the fiber surface.

Citation Information

Patent Citations

  • Fiber for marine product attaching base