Method for carbon dioxide fixation
By adjusting the moisture content of hardened cementitious materials to 0.5 to 10% and using specific gas conditions, the method enhances carbon dioxide fixation in cementitious bodies, addressing the suboptimal carbonation rates in existing technologies.
Patent Information
- Application Number
- JP2023049658
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing methods for fixing carbon dioxide in cementitious hardened bodies do not specify the optimal moisture content of the hardened cementitious material, leading to suboptimal carbonation rates.
Adjusting the moisture content of the hardened cementitious material to a range of 0.5 to 10% before contacting it with a carbon dioxide-containing gas at specific temperature and humidity levels, without additional moisture supply, to enhance carbon dioxide fixation.
This method significantly increases the amount of carbon dioxide fixed per unit mass of cementitious material, optimizing the carbonation process.
Smart Images

Figure 2024138929000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for fixing carbon dioxide. [Background technology]
[0002] 2. Description of the Related Art Techniques are known for fixing carbon dioxide contained in a carbon dioxide-containing gas (for example, factory exhaust gas) in a cementitious hardened material such as waste concrete. For example, Patent Document 1 describes a method for fixing carbon dioxide, which includes a contacting step of contacting a carbon dioxide-containing gas with a powdered or granular material having a particle size of 40 mm or less made of a cementitious hardened body at a temperature of 75 to 110°C to fix the carbon dioxide contained in the carbon dioxide-containing gas in the powdered or granular material, and which is characterized in that the relative humidity of the carbon dioxide-containing gas is adjusted depending on the particle size of the powdered or granular material and the adjustment status of the moisture content of the powdered or granular material prior to the contacting step. Patent Document 2 describes a method for fixing carbon dioxide, which includes a contacting step of contacting a carbon dioxide-containing gas with a cementitious hardened body and fixing the carbon dioxide contained in the carbon dioxide-containing gas in the cementitious hardened body, wherein the carbon dioxide-containing gas is a gas having a moisture content of 1.5% or more as measured by the method described in "7. Measurement of moisture content in flue gas" of "JIS Z 8808:2013 Measurement method for dust concentration in flue gas" and a temperature of 75 to 175°C. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-131076 A [Patent Document 2] JP 2020-15659 A Summary of the Invention [Problem to be solved by the invention]
[0004] In Patent Document 1, as an example, there is described a method in which a powdered granular material made of hardened cement paste is cured in a sealed container filled with water to obtain a test specimen, which is then brought into contact with a carbon dioxide-containing gas in an atmosphere at a temperature of 100°C to carbonate the test specimen (in other words, to fix the carbon dioxide). However, Patent Document 1 does not disclose what moisture content the powdery granular material made of hardened cement paste should have in order to maximize the carbonation rate. Patent Document 2 describes that when the proportion of water vapor in the carbon dioxide-containing gas is, for example, 30% or more in volume fraction, carbon dioxide gas (carbon dioxide) can be fixed more efficiently and in large quantities in a cementitious hardened body (for example, a cement paste hardened body). However, Patent Document 2 does not disclose what water content the cementitious hardened body should have in order to maximize the carbonation rate.
[0005] An object of the present invention is to provide a method for increasing the amount of carbon dioxide fixed per unit mass of cement, which is the material of the cementitious hardened body, in a technology for fixing carbon dioxide (carbon dioxide gas) contained in a carbon dioxide-containing gas (e.g., factory exhaust gas) in a cementitious hardened body such as waste concrete. [Means for solving the problem]
[0006] As a result of intensive research to solve the above problems, the present inventors have found that the above object can be achieved by adjusting the moisture content of the cementitious hardened body to 0.5 to 10% before contacting the cementitious hardened body with a carbon dioxide-containing gas, and have completed the present invention.
[0007] The present invention provides the following [1] to [4]. [1] A method for fixing carbon dioxide, comprising a contacting step of contacting a carbon dioxide-containing gas with a cementitious hardened body to fix carbon dioxide contained in the carbon dioxide-containing gas in the cementitious hardened body, the method comprising a moisture content adjusting step of adjusting the moisture content of the cementitious hardened body to 0.5 to 10% prior to the contacting step. [2] The method for fixation of carbon dioxide according to the above [1], wherein in the contact step, a gas having a temperature of 75 to 175°C and a relative humidity of 10 to 100% is used as the carbon dioxide-containing gas. [3] The method for fixing carbon dioxide according to [1] or [2] above, wherein the cementitious hardened body is a material selected from the group consisting of recycled aggregate, waste building materials made of concrete or mortar, waste hardened cement paste, and hardened sludge generated in ready-mixed concrete, and contains 70% by mass or more of granular matter having a particle size of 50 mm or less. [4] The method for fixation of carbon dioxide according to any one of the above [1] to [3], wherein in the contact step, additional moisture is not supplied to the carbon dioxide-containing gas. Effect of the Invention
[0008] According to the present invention, even if the temperature and relative humidity of the carbon dioxide-containing gas are maintained at specific values, the amount of carbon dioxide fixed per unit mass of cement, which is the material of the cementitious hardened body, can be increased by simply adjusting the moisture content of the cementitious hardened body within a specific range. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The method for fixing carbon dioxide of the present invention includes: (A) a moisture content adjusting step of adjusting the moisture content of a cementitious hardened body to 0.5 to 10%; and (B) a contacting step of bringing a carbon dioxide-containing gas into contact with the cementitious hardened body, the moisture content of which has been adjusted in the moisture content adjusting step, to fix carbon dioxide contained in the carbon dioxide-containing gas in the cementitious hardened body. Each step will be described in detail below.
[0010] [(A) Moisture content adjustment process] This step is a step of adjusting the moisture content of the cementitious hardened body, which is the target for fixing carbon dioxide, to 0.5 to 10%. Examples of the cementitious hardened body include a hardened body made of concrete, a hardened body made of mortar, and a hardened body made of cement paste. In this specification, the term "cementitious hardened body" includes not only a completely hardened body but also a semi-hardened body (in other words, one in which hardening is in progress). In particular, from the viewpoint of promoting the utilization of waste materials, recycled aggregate, waste building materials made of concrete or mortar (waste concrete, etc.), waste hardened cement paste, and hardened sludge generated in ready-mixed concrete (completely hardened sludge or semi-hardened sludge after dehydration treatment) are preferably used in the present invention.
[0011] The cementitious hardened material preferably has a granular form (with a particle size of 0.1 mm or more) in order to increase the contact area with the carbon dioxide-containing gas and thereby increase the amount of fixed carbon dioxide. A preferred particle size distribution of the granules, from the viewpoint of increasing the amount of fixed carbon dioxide, is one in which 70% by mass or more (more preferably 80% by mass or more) of the granules have a particle size of 50 mm or less (preferably 40 mm or less, more preferably 30 mm or less, even more preferably 20 mm or less, and particularly preferably 10 mm or less). In addition, from the viewpoint of reducing the labor required for crushing the various waste materials (recycled aggregate, etc.) mentioned above to be used as cementitious hardened bodies, it is preferable that the particle size distribution of the granules is such that the proportion of particles having a particle size of 1 mm or less is 30% by mass or less (preferably 20% by mass or less). Here, the particle size of a granule refers to the maximum dimension of the granule (for example, the dimension of the major axis when the cross section is elliptical).
[0012] The water content of the cementitious hardened material is 0.5 to 10%, preferably 1 to 8%, more preferably 1.5 to 5%, further preferably 2 to 4%, and particularly preferably 2.5 to 3.5%. If the water content is less than 0.5%, the efficiency of fixation of carbon dioxide decreases. If the water content is more than 10%, the efficiency of fixation of carbon dioxide decreases. In this specification, the "moisture content" refers to the value obtained by dividing the mass of water contained in the cementitious hardened body (in other words, water adhering to the pores of the cementitious hardened body) by the mass of the cementitious hardened body (total mass including water), and is calculated by the following formula (1). Moisture content (%) = [mass of water contained in the hardened cementitious body] × 100 ÷ [total mass of the hardened cementitious body in the bone dry state and the mass of water contained in the hardened cementitious body] (1) Examples of a method for adjusting the water content of the cementitious hardened body to fall within the above-mentioned numerical range include a method of supplying water to the cementitious hardened body in an absolutely dry state, and a method of drying the cementitious hardened body having a high water content after immersion in water by heating or the like.
[0013] [(B) Contact process] This step is a step of contacting a carbon dioxide-containing gas with the cementitious hardened body whose moisture content has been adjusted in the previous step (moisture content adjusting step) to fix the carbon dioxide contained in the carbon dioxide-containing gas in the cementitious hardened body. In the present invention, when the cementitious hardened body has a moisture content adjusted to within the range of 0.5 to 10%, the cementitious hardened body is brought into contact with a carbon dioxide-containing gas, whereby the amount of carbon dioxide fixed per unit mass of cement contained in the cementitious hardened body (hereinafter sometimes abbreviated as the amount of carbon dioxide fixed) can be increased compared to the case where the moisture content is outside the range of 0.5 to 10%.
[0014] In the present invention, the carbon dioxide-containing gas means a gas that contains carbon dioxide (carbon dioxide gas), which is a gas. An example of the carbon dioxide-containing gas is factory exhaust gas. Examples of factory exhaust gases include exhaust gases from cement factories, exhaust gases from coal-fired power plants, and exhaust gases generated during exhaust treatment in paint factories. Moreover, as the exhaust gas from a factory, a highly purified gas (gas with an increased concentration of carbon dioxide gas) obtained by separating and recovering the exhaust gas from the factory can also be used. The ratio of carbon dioxide (carbonic acid gas) in the carbon dioxide-containing gas is preferably 10% or more, more preferably 30% or more, further preferably 50% or more, and particularly preferably 70% or more, as a volume fraction value. If the ratio is 10% or more, the amount of fixed carbon dioxide increases, and the effect of reducing the amount of carbon dioxide emitted into the atmosphere increases, which is preferable. Examples of gases other than carbon dioxide (carbon dioxide gas) in the carbon dioxide-containing gas include nitrogen gas, carbon monoxide, hydrocarbons, nitrogen oxides, sulfur oxides, etc. Examples of gases other than nitrogen gas (carbon monoxide, etc.) are usually contained in factory exhaust gases, etc.
[0015] The temperature of the carbon dioxide-containing gas (the temperature at the time of contact with the cementitious hardened body) is preferably 75 to 175° C., more preferably 80 to 145° C., further preferably 85 to 120° C., and particularly preferably 87 to 95° C. If the temperature is less than 75° C., the amount of carbon dioxide fixed is small. If the temperature exceeds 175° C., the amount of carbon dioxide fixed is small. For example, when a factory exhaust gas is used as a source of carbon dioxide-containing gas, if the temperature of the exhaust gas is less than 75°C or more than 175°C, the exhaust gas can be heated or cooled to adjust the temperature of the exhaust gas to a desired value within the range of 75 to 175°C, and the exhaust gas can be used as the carbon dioxide-containing gas in the contact step of the present invention. The relative humidity of the carbon dioxide-containing gas (relative humidity at the time of contact with the cementitious hardened body) is preferably 10 to 100%, more preferably 30 to 95%, further preferably 40 to 90%, and particularly preferably 50 to 80%. If the value is less than 10%, the water content of the cementitious hardened body decreases over time, and the amount of fixed carbon dioxide decreases. If the value is 95% or less, it is easy to prepare such a carbon dioxide-containing gas, and this is preferable.
[0016] In this step (contact step), there is no need to supply additional moisture to the carbon dioxide-containing gas. If the temperature and relative humidity of the carbon dioxide-containing gas are adjusted in advance to within the above-mentioned numerical ranges (75 to 175°C, 10 to 100%), a large amount of carbon dioxide can be fixed simply by contacting the carbon dioxide-containing gas whose temperature has been adjusted with the cementitious hardened body. The contact time between the cementitious hardened body and the carbon dioxide-containing gas in the contact step is preferably 10 minutes to 3 hours, more preferably 20 minutes to 2 hours 30 minutes, even more preferably 30 minutes to 2 hours, and particularly preferably 40 minutes to 1 hour 30 minutes. When the time is 10 minutes or more, the amount of carbon dioxide fixed can be increased. When the time is 3 hours or less, carbon dioxide can be fixed more efficiently.
[0017] As a means for contacting the cementitious hardened body with a carbon dioxide-containing gas, either a continuous heating furnace or a batch heating furnace can be used. Of these, a continuous heating furnace is preferably used in the present invention since it can efficiently carry out the method for fixing carbon dioxide of the present invention. Examples of continuous heating furnaces include rotary kilns (externally heated or internally heated), tunnel heating furnaces, and the like. Among these, an externally heated rotary kiln is preferably used in the present invention because it is easy to control the temperature of the internal space of the cylindrical storage section for storing the cementitious hardened body and bringing it into contact with the carbon dioxide-containing gas. An externally heated rotary kiln is one in which the outer circumferential surface of a cylindrical container for containing the material to be treated is heated from the outside using a heat source such as multiple burners, whereas an internally heated rotary kiln is one in which high-temperature gas (for example, high-temperature exhaust gas generated by waste heat in a factory) is circulated within the internal space of a cylindrical container for containing the material to be treated. The length of the cylindrical container section of the continuous heating furnace is preferably 4 to 15 m. The inner diameter of the cylindrical container of the continuous heating furnace is preferably 0.3 to 2 m. EXAMPLES
[0018] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. [Example 1] (1) Preparation of specimens made of hardened cementitious materials 100 parts by mass of ordinary Portland cement and 47 parts by mass of water were mixed to obtain a cement paste. This cement paste, water, and sand were mixed in proportions of 15.5 mass%, 7.3 mass%, and 77.2 mass% (total of the above: 100 mass%) to obtain a mortar. This mortar was filled into a formwork, cured in water for 28 days, and then demolded to obtain a hardened mortar body (dimensions: 300 mm x 300 mm x 100 mm). This hardened mortar body was crushed to obtain a crushed hardened mortar body (a test specimen made of a cementitious hardened body). The particle size distribution of the crushed material of the hardened mortar was as follows: 100% by mass had a particle size of 40 mm or less, 90% by mass or more had a particle size of 30 mm or less, 90% by mass or more had a particle size of 20 mm or less, 80% by mass or more had a particle size of 10 mm or less, and 20% by mass or less had a particle size of 1 mm or less. The crushed hardened mortar was dried by heating (temperature: 80° C.) for 12 hours and then water was added to the crushed mortar to adjust the moisture content to 0.5%.
[0019] (2) Contact with carbon dioxide-containing gas The prepared specimen (crushed pieces of hardened mortar body) and carbon dioxide-containing gas (carbon dioxide concentration: 100%) were supplied into an externally heated rotary kiln (length of cylindrical container: 5 m; inner diameter of cylindrical container: 0.55 m; manufactured by Kurimoto Iron Works), and the carbon dioxide-containing gas was brought into contact with the specimen inside the kiln. The carbon dioxide-containing gas was supplied to the externally heated rotary kiln from the opposite side to the specimen. No moisture was supplied to the externally heated rotary kiln (in other words, the carbon dioxide-containing gas supplied into the kiln). The supply rate of the specimen (crushed pieces of hardened mortar body) was 50 kg / h. The temperature inside the rotary kiln (in other words, the temperature of the carbon dioxide-containing gas inside the kiln) was adjusted to be maintained at 90°C. The residence time (time from supply to discharge) of the test specimens (crushed hardened mortar) in the rotary kiln was 60 minutes. The relative humidity inside the rotary kiln was measured using a thermo-hygrometer (HygroPalm32 manufactured by Rotronic) and was found to be 35%. (3) Calculation of the amount of fixed carbon dioxide The amount of carbon dioxide (CO2) fixed (kg) per ton (t) of cement was calculated based on the change in the bone-dry mass of the cementitious hardened body before and after contact with carbon dioxide-containing gas.
[0020] [Examples 2 to 5, Comparative Example 1] The experiment was carried out in the same manner as in Example 1, except that the water content of the cementitious hardened material was changed as shown in Table 1. The moisture content was adjusted as follows. In Example 2, the crushed hardened mortar was dried by heating (temperature: 80° C.) (treatment time: 12 hours) and then water was added to the crushed hardened mortar, thereby adjusting the moisture content to 1.0%. In Example 3, the crushed hardened mortar was used as it was without being subjected to any treatment such as heating, and had a moisture content of 3.1%. In Examples 4 and 5, drying by heating was not performed, and the moisture content was adjusted to 4.8% (Example 4) or 6.4% (Example 5) by simply adding water. In Comparative Example 1, the moisture content was adjusted to 0% by only drying by heating (temperature: 80° C.) (treatment time: 12 hours). The above results are shown in Table 1. In Table 1, the "fixed amount of carbon dioxide" does not include the amount fixed that originates from carbon dioxide contained in the atmospheric air, but only indicates the amount fixed that originates from carbon dioxide (carbon dioxide) contained in carbon dioxide-containing gas (carbon dioxide concentration: 100%).
[0021] [Table 1]
[0022] From Table 1, it can be seen that in Comparative Example 1, since the moisture content of the cementitious hardened body is 0%, the amount of carbon dioxide fixed is 42 kg per ton of cement, whereas in Examples 1 to 5, since the moisture content of the cementitious hardened body is 0.5 to 6.4%, the amount of carbon dioxide fixed is 46 to 130 kg per ton of cement, which is a larger amount of fixation than in Comparative Example 1. In particular, in Example 3, in which the moisture content of the cementitious hardened body is 3.1%, the amount of carbon dioxide fixed is 130 kg per ton of cement, which is a very large amount of fixation.
Claims
1. A method for fixing carbon dioxide, comprising a contacting step of contacting a carbon dioxide-containing gas with a cementitious hardened body to fix carbon dioxide contained in the carbon dioxide-containing gas in the cementitious hardened body, A method for fixing carbon dioxide, comprising a moisture content adjusting step of adjusting the moisture content of the cementitious hardened body to 0.5 to 10% before the contact step.
2. 2. The method for fixation of carbon dioxide according to claim 1, wherein the carbon dioxide-containing gas used in the contact step has a temperature of 75 to 175° C. and a relative humidity of 10 to 100%.
3. 2. The method for fixing carbon dioxide according to claim 1, wherein the cementitious hardened body is a recycled aggregate, a waste building material made of concrete or mortar, a waste hardened cement paste, or a hardened body of sludge generated in ready-mixed concrete, and contains 70% by mass or more of granular matter having a particle size of 50 mm or less.
4. 4. The method for fixation of carbon dioxide according to claim 1, wherein in the contact step, additional moisture is not supplied to the carbon dioxide-containing gas.
Citation Information
Patent Citations
Stabilization method of carbon dioxide
JP2020015659A
Immobilization method of carbon dioxide
JP2020131076A