Hexavalent chromium immobilizing agent and ground improvement material containing the same

The hexavalent chromium fixing agent with CaS x and SrO improves hexavalent chromium fixation and ground strength, addressing leaching issues and maintaining slurry performance in cement-based ground improvement.

JP2024139101APending Publication Date: 2024-10-09TAIHEIYO CEMENT CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023049897
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing cement-based ground improvement methods using solidification agents can lead to the leaching of harmful hexavalent chromium, and existing immobilizing agents do not adequately address this issue while maintaining the strength and pumpability of the improved ground.

Method used

A hexavalent chromium fixing agent with a chemical formula of CaS x (where x is an integer of 1 or more) containing 0.03 to 0.28 parts by mass of SrO per 100 parts by mass of a calcium-containing compound, combined with a cement-based solidifying agent, is used to enhance hexavalent chromium fixation and improve the physical properties of the ground.

Benefits of technology

The solution effectively reduces hexavalent chromium elution, maintains excellent slurry pumpability, and enhances the unconfined compressive strength of the improved ground, meeting environmental standards and performance criteria.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139101000001
    Figure 2024139101000001
  • Figure 2024139101000002
    Figure 2024139101000002
  • Figure 2024139101000003
    Figure 2024139101000003
Patent Text Reader

Abstract

To provide a hexavalent chromium immobilizing agent that is used as a material of a ground improvement material together with a cement-based immobilizing material, which can improve hexavalent chromium immobilizing performance of a ground improved by a slurry containing a ground improvement material, and can impart excellent physical properties with respect to pump pressure-feeding property of the slurry and strength (for example, uniaxial compressive strength) of a ground improved by the slurry.SOLUTION: A hexavalent chromium immobilizing agent contains a calcium-containing compound represented by chemical formula CaSx (provided that x is an integer of 1 or more), and 0.03 to 0.28 pts.mass of SrO with respect to 100 pts.mass of the calcium-containing compound. A ground improvement material contains the hexavalent chromium immobilizing agent, and a cement-based immobilizing material (for example, a material containing cement, gypsum, and blast furnace slag fine powder which is blended as necessary).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hexavalent chromium fixing agent and a ground improvement material containing the same. [Background technology]

[0002] As a method for improving soft ground, a method is known in which a slurry containing a cement-based solidification material (cement milk) is injected into the ground and mixed and stirred to increase the strength of the ground after improvement (solidification) (e.g., uniaxial compressive strength). On the other hand, when ground improvement (solidification) is carried out using cement-based solidification materials, there is a problem in that there is a possibility that harmful heavy metals may leach from the improved ground because the cement may contain trace amounts of harmful heavy metals (e.g., hexavalent chromium). In order to solve this problem, various agents for immobilizing heavy metals and the like have been proposed.

[0003] For example, Patent Document 1 describes a heavy metal immobilizing material used to prevent the elution of heavy metals contained in a material made of gypsum, the heavy metal immobilizing material containing finely divided slag as a main component. Patent Document 2 describes a treatment composition for soil contaminated with harmful heavy metals, which contains magnesium oxide and sulfide, and is characterized in that the treatment composition contains 95 to 5 mass % of magnesium oxide and 5 to 95 mass % of sulfide based on the total amount of magnesium oxide and sulfide. Furthermore, Patent Document 2 describes that the sulfide is at least one selected from calcium sulfide, calcium polysulfide, sodium sulfide, sodium polysulfide, and steel slag. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-169816 [Patent Document 2] JP 2007-105549 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a hexavalent chromium fixing agent for use as a material for a ground improvement material together with a cement-based solidification material, which can improve the hexavalent chromium fixing performance of ground improved with a slurry containing the ground improvement material, and can impart excellent physical properties with respect to the pumpability of the slurry and the strength (e.g., uniaxial compressive strength) of the ground improved with the slurry. [Means for solving the problem]

[0006] As a result of intensive research to solve the above problems, the present inventors have discovered that the chemical formula is CaS x The inventors have found that the above object can be achieved by using a hexavalent chromium fixing agent containing 100 parts by mass of a calcium-containing compound (wherein x is an integer of 1 or more) and 0.03 to 0.28 parts by mass of SrO (strontium oxide), and have completed the present invention.

[0007] The present invention provides the following [1] to [7]. [1] The chemical formula is CaS x (wherein x is an integer of 1 or more), and SrO in an amount of 0.03 to 0.28 parts by mass relative to 100 parts by mass of the calcium-containing compound. [2] A powdered ground improvement material comprising the hexavalent chromium fixing agent according to [1] above and a cement-based solidification material. [3] The powdered ground improvement material according to [2] above, wherein the cement-based solidification material contains cement and gypsum. [4] The powdered ground improvement material described in [3] above, in which the cement-based solidification material does not contain ground granulated blast furnace slag or contains ground granulated blast furnace slag in an amount of 40 mass% or less in the total amount of the cement and the gypsum. [5] A method for producing a powdery ground improvement material according to any one of [2] to [4] above, characterized in that when a slurry consisting of the powdery ground improvement material and the water is prepared using 60 parts by mass of water per 100 parts by mass of the powdery ground improvement material, the viscosity of the slurry 90 minutes after preparation (wherein the viscosity is a value measured at a temperature of 20°C in accordance with "11 Viscosity measurement method using a vibration viscometer" of "JIS Z 8803:2011 (Methods for measuring viscosity of liquids)") is 18.0 mPa s or less. [6] A possible composition for use as a Cr(VI) fixative is CaS. x (where x is an integer of 1 or more), a composition preparation step of preparing a composition (wherein the type of composition may be one or more) containing a calcium-containing compound having a molecular weight of 1.0 or more; a measurement step of measuring the amount of SrO in the composition (wherein the type of composition is two or more, each of the two or more types of compositions) prepared in the composition preparation step; and when the amount of SrO obtained in the measurement step is within a range of 0.03 to 0.28 parts by mass relative to 100 parts by mass of the calcium-containing compound, the composition (for example, when the type of composition is three, each of the three types of compositions) is determined to be 100 parts by mass. a selection step of selecting one of the compositions (e.g., one of the compositions in the case where there are three types of composition) as a hexavalent chromium fixing agent when the amount of SrO obtained in the measurement step is less than 0.03 parts by mass or more than 0.28 parts by mass relative to 100 parts by mass of the calcium-containing compound, and not selecting the composition (e.g., two of the three types) as a hexavalent chromium fixing agent; and a mixing step of mixing the composition selected as the hexavalent chromium fixing agent in the selection step, a cement-based solidification material, and water to obtain a slurry-like ground improvement material. [7] A ground improvement method using the powdery ground improvement material described in any one of [2] to [4] above, characterized in that a slurry containing the powdery ground improvement material and water is injected into the ground to be improved. Effect of the Invention

[0008] When the hexavalent chromium fixation agent of the present invention is used as a material for a ground improvement material together with a cement-based solidification material, it can improve the hexavalent chromium fixation performance of ground improved with a slurry containing the ground improvement material, and can impart excellent physical properties to the slurry in terms of pumpability and strength (e.g., uniaxial compressive strength) of the ground improved with the slurry. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The hexavalent chromium fixing agent of the present invention has the chemical formula CaS x (wherein x is an integer of 1 or more), and SrO (strontium oxide) in an amount of 0.03 to 0.28 parts by mass relative to 100 parts by mass of the calcium-containing compound.

[0010] The calcium-containing compound used in the present invention has the chemical formula CaS x (where x is an integer greater than or equal to 1.) x is preferably 1 to 6. When x is 1, the compound is called calcium sulfide. When x is 2 or greater, the compound is called calcium polysulfide. Commercially available calcium polysulfide products usually contain a compound in which x is 5 as the main ingredient (especially the active ingredient as a pesticide). In the present invention, multiple types of calcium-containing compounds may be used in combination. For example, calcium sulfide in which x is 1 and calcium polysulfide in which x is 5 may be used in combination in any mixing ratio.

[0011] The amount of SrO (strontium oxide) is 0.03 to 0.28 parts by mass, 0.03 to 0.27 parts by mass, preferably 0.04 to 0.26 parts by mass, and particularly preferably 0.05 to 0.25 parts by mass, relative to 100 parts by mass of the calcium-containing compound. If the amount is outside the range of 0.03 to 0.28 parts by mass, the amount of hexavalent chromium eluted increases. In particular, when the calcium-containing compound is calcium sulfide, the amount of SrO is preferably 0.03 to 0.15 parts by mass, preferably 0.04 to 0.12 parts by mass, and particularly preferably 0.05 to 0.10 parts by mass, relative to 100 parts by mass of the calcium-containing compound, from the viewpoint of reducing the amount of eluted hexavalent chromium.

[0012] When the calcium-containing compound is calcium polysulfide, the amount of SrO is preferably 0.10 to 0.28 parts by mass, more preferably 0.12 to 0.26 parts by mass, and particularly preferably 0.15 to 0.24 parts by mass, relative to 100 parts by mass of the calcium-containing compound, from the viewpoint of reducing the amount of eluted hexavalent chromium. SrO (strontium oxide) can be obtained, for example, by heating the raw material strontianite (main component: strontium carbonate). SrO is available as a commercial reagent.

[0013] An example of the hexavalent chromium fixing agent of the present invention is a commercially available calcium-containing compound (calcium sulfide or calcium polysulfide) containing SrO as an impurity. Such a commercially available product can be obtained, for example, by preparing a plurality of types of commercially available products, measuring the SrO content of each of the plurality of types of commercially available products, and selecting the one containing the amount of SrO within the range specified in the present invention as the hexavalent chromium fixing agent of the present invention. Another example of the hexavalent chromium fixation agent of the present invention is a mixture of a high-purity calcium-containing compound (calcium sulfide or calcium polysulfide) with a very small SrO content and SrO (e.g., a commercially available powder product made of SrO).

[0014] Next, the powdery soil improvement material containing the hexavalent chromium fixing agent of the present invention (hereinafter referred to as the powdery soil improvement material of the present invention) will be described. The powdery soil improvement material of the present invention contains the above-mentioned hexavalent chromium fixing agent and a cement-based solidification material. In the present invention, even if the hexavalent chromium fixing agent is in a liquid state, the mass ratio of the hexavalent chromium fixing agent (liquid state) to the cement-based solidification material (powder state) is very small, so the composition consisting of the hexavalent chromium fixing agent and the cement-based solidification material is regarded as being in a powder state as a whole. In the present invention, the hexavalent chromium fixing agent and the cement-based solidification material may be used in combination when used as a ground improvement material, and for example, a liquid hexavalent chromium fixing agent may be mixed with water to obtain a liquid material, and then the liquid material may be mixed with the cement-based solidification material to prepare a slurry ground improvement material. In this case, the liquid hexavalent chromium fixing agent and the cement-based solidification material as a whole combination are considered to correspond to the powder ground improvement material of the present invention. The cement-based solidification material includes cement, gypsum (added in addition to the gypsum contained in the cement), and ground granulated blast furnace slag, which is added as needed. Examples of cement include various types of Portland cement such as ordinary Portland cement, high-early-strength Portland cement, moderate-heat Portland cement, and low-heat Portland cement, mixed cements such as blast-furnace cement and fly ash cement, and ecocement.

[0015] The Blaine specific surface area of ​​the cement is preferably 2,500 to 6,000 cm 2 / g. The value is 2,500 cm 2 / g or more, the strength development of the ground improvement material is further improved. 2 When the molecular weight is 1 / g or less, the labor required for grinding during cement production does not become excessive. Examples of gypsum include anhydrite, gypsum dihydrate, and gypsum hemihydrate. The Blaine specific surface area of ​​the gypsum is preferably 2,000 to 7,000 cm 2 / g. The value is 2,000 cm 2 When the value is 7,000 cm / g or more, the reactivity of gypsum is improved. 2 When the viscosity is 100 / g or less, the strength development of the ground improvement material is further improved.

[0016] In the present invention, by using ground granulated blast furnace slag, the excellent effects of the present invention (improved hexavalent chromium fixing performance, excellent pumpability, and excellent ground strength) can be sufficiently obtained even if the amount of the hexavalent chromium fixing agent of the present invention is reduced. When ground granulated blast furnace slag is used, the Blaine specific surface area of ​​the ground granulated blast furnace slag is preferably 3,000 to 10,000 cm 2 / g. The value is 3,000 cm 2 / g or more, the strength development of the ground improvement material is further improved. 2 When the molecular weight is 1 / g or less, the material is easily available and the cost is not excessively high.

[0017] In the present invention, even if ground granulated blast furnace slag is not used, by using an appropriate amount of the hexavalent chromium fixing agent of the present invention, the excellent effects of the present invention (improved hexavalent chromium fixing performance, excellent pumpability, and excellent ground strength) can be fully obtained. In the present invention, the amount of cement in 100 parts by mass of the total amount of cement, gypsum (anhydride equivalent) and ground granulated blast furnace slag is preferably 55 to 95 parts by mass, more preferably 58 to 93 parts by mass, and particularly preferably 61 to 91 parts by mass. When the amount is 55 parts by mass or more, the strength development of the ground improvement material is further improved. When the value is 95 parts by mass or less, the amount of gypsum is large, so that the strength development of the ground improvement material is further improved.

[0018] The amount of gypsum (anhydride equivalent; CaSO4) (amount excluding gypsum contained in cement) in the total amount of cement, gypsum (anhydride equivalent) and ground granulated blast furnace slag of 100 parts by mass is preferably 3 to 18 parts by mass, more preferably 5 to 15 parts by mass, and particularly preferably 7 to 13 parts by mass. When the amount is 3 to 18 parts by mass, the strength development of the ground improvement material is further improved. The amount of ground granulated blast furnace slag in a total amount of 100 parts by mass of cement, gypsum (anhydrous equivalent) and ground granulated blast furnace slag is preferably 40 parts by mass or less, more preferably 35 parts by mass or less, and particularly preferably 30 parts by mass or less. When the amount is 40 parts by mass or less, the strength development of the ground improvement material is further improved. When ground granulated blast furnace slag is used, the amount of ground granulated blast furnace slag per 100 parts by mass of the total amount of cement, gypsum (anhydrous equivalent) and ground granulated blast furnace slag is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, even more preferably 15 parts by mass or more, and particularly preferably 20 parts by mass or more, from the viewpoint of enhancing the effect of inhibiting elution of hexavalent chromium by blending ground granulated blast furnace slag.

[0019] In the present invention, the amount of the calcium-containing compound (calcium sulfide or calcium polysulfide) contained in the hexavalent chromium fixing agent is preferably 0.05 to 1.5 parts by mass per 100 parts by mass of the cement-based solidification material (made of cement, gypsum, and ground granulated blast furnace slag mixed as necessary). When the amount is 0.05 parts by mass or more, the effect of suppressing elution of hexavalent chromium can be further improved. When the amount is 1.5 parts by mass or less, the pumpability can be further improved. In particular, the amount of calcium sulfide is preferably 0.1 to 1.5 parts by mass, more preferably 0.15 to 1.2 parts by mass, and particularly preferably 0.2 to 0.9 parts by mass, relative to 100 parts by mass of the cement-based solidifying material. The amount of calcium polysulfide is preferably 0.05 to 1.0 part by mass, more preferably 0.08 to 0.8 part by mass, and particularly preferably 0.12 to 0.6 part by mass, relative to 100 parts by mass of the cement-based solidifying material.

[0020] It is preferable that the type (e.g., type of cement) and amount (e.g., amount of cement) of the material constituting the powdery ground improvement material of the present invention be determined so that when a slurry consisting of the powdery ground improvement material and water is prepared using 60 parts by mass of water per 100 parts by mass of the powdery ground improvement material, the viscosity of the slurry 90 minutes after preparation (wherein the viscosity is a value measured at a temperature of 20°C in accordance with "11 Viscosity measurement method using a vibration viscometer" of "JIS Z 8803:2011 (Method of measuring viscosity of liquids)") is 18.0 mPa·s or less.

[0021] A preferred example of the soil improvement method using the powdery soil improvement material of the present invention is a method in which a slurry containing the powdery soil improvement material and water is injected into the ground, which is the object of improvement. The ground improvement may be carried out by injecting a slurry into the ground and mixing and stirring it, or by injecting a slurry into voids in the ground (using the ground improvement material as a grout material). As for the type of soil constituting the ground to be improved, soil from which hexavalent chromium is easily eluted is preferred, since the present invention aims to suppress the elution of hexavalent chromium. Examples of such soil include volcanic ash soil. Examples of volcanic ash soil include red soil and black soil.

[0022] Unit volume of ground (soil) (1m 3 The amount of the powdery ground improvement material per unit area is preferably 50 to 500 kg, more preferably 100 to 400 kg. When the amount is 50 kg or more, the strength of the improved ground (e.g., uniaxial compressive strength) can be increased. When the amount is 500 kg or less, excessive costs can be avoided. The amount of water used in the ground improvement method is preferably 45 to 135 parts by mass, more preferably 50 to 110 parts by mass, even more preferably 55 to 100 parts by mass, and particularly preferably 60 to 80 parts by mass, relative to 100 parts by mass of the powdery ground improvement material. When the amount is 45 parts by mass or more, the pumpability is further improved. When the amount is 135 parts by mass or less, the strength (e.g., uniaxial compressive strength) of the improved ground can be further increased. EXAMPLES

[0023] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. [A. Materials used] (a) Soil sample Two types of volcanic ash soil (akaboku soil and black soil) shown in Table 1 were used.

[0024] [Table 1]

[0025] (b) Cement Ordinary Portland cement (Blaine specific surface area: 3,450 cm 2 / g) was used. (c) Plaster Anhydrous gypsum (Blaine specific surface area: 4,850 cm 2 / g) was used. (d) Ground granulated blast furnace slag Blaine specific surface area is 4,330cm 2 A commercially available product (a cement admixture manufactured by DC Corporation; product name: Cerament) with a molecular weight of 1000 g was used.

[0026] (e) Hexavalent chromium fixative (containing calcium sulfide) As the hexavalent chromium fixing agent containing calcium sulfide, the following hexavalent chromium fixing agents A to D were used. (e-1) Hexavalent chromium fixative A Calcium sulfide powder manufactured by Kojundo Chemical Laboratory (calcium sulfide content: 99% by mass) (e-2) Hexavalent chromium fixative B Calcium sulfide powder from China (calcium sulfide content: 99% by mass) (e-3) Hexavalent chromium fixative C Calcium sulfide powder manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (calcium sulfide content: 99% by mass or more) (e-4) Hexavalent chromium fixative D Calcium sulfide powder from India (calcium sulfide content: 99% by mass)

[0027] The "amount of SrO per 100 parts by mass of calcium sulfide" in each of the hexavalent chromium fixing agents A to D is shown in Table 2. In Table 2, "parts" indicates parts by mass. The amount of SrO in Table 2 was obtained by mixing a powder of the hexavalent chromium fixing agent with water to prepare an aqueous solution, measuring the amount of Sr in the aqueous solution by ICP atomic emission spectrometry, and converting the obtained value into the mass of oxide equivalent per 100 parts by mass of calcium sulfide.

[0028] [Table 2]

[0029] (f) Hexavalent chromium fixative (containing calcium polysulfide) As the hexavalent chromium fixing agent containing calcium polysulfide, the following hexavalent chromium fixing agents E to G were used. (f-1) Hexavalent chromium fixative E Lime sulfur mixture manufactured by Miyauchi Sulfur Mixture Co., Ltd. (liquid; calcium polysulfide content: 27.5% by mass) (f-2) Hexavalent chromium fixative F Sakura Kako Co., Ltd. lime sulfur mixture (liquid; calcium polysulfide content: 27.5% by mass) (f-3) Hexavalent chromium fixative G Lime sulfur mixture manufactured by OAT Agrio (liquid; calcium polysulfide content: 27.5% by mass)

[0030] The "amount of SrO per 100 parts by mass of calcium polysulfide" in each of the hexavalent chromium fixing agents E to G is shown in Table 3. In Table 3, "parts" indicates parts by mass. The amount of SrO in Table 3 was obtained by measuring the amount of Sr in the liquid hexavalent chromium fixation agent (lime sulfur mixture) by ICP atomic emission spectrometry and converting the value obtained into the mass of oxide equivalent per 100 parts by mass of calcium polysulfide.

[0031] [Table 3]

[0032] [B. Experimental example using calcium sulfide] [Example 1] A cement-based solidification material was prepared by mixing 65 parts by mass of cement, 10 parts by mass of gypsum, and 25 parts by mass of ground granulated blast furnace slag (a total of 100 parts by mass). 0.2 parts by mass of hexavalent chromium fixing agent A (containing 0.06 parts by mass of SrO per 100 parts by mass of calcium sulfide; see Table 1) was added to 100 parts by mass of the obtained cement-based solidification material and mixed to prepare a powdered ground improvement material. To the obtained soil improvement material, water was added in an amount such that the mass ratio of water / soil improvement material was 0.60 to prepare a slurry. The viscosity of this slurry was measured at 20° C. 90 minutes after preparation in accordance with “11 Viscosity measurement method using a vibration viscometer” of “JIS Z 8803:2011 (Methods for measuring viscosity of liquids).” The viscosity was 16.5 mPa·s (pumpability: good). The pumpability was evaluated as good when the viscosity was 18.0 mPa·s or less, and as poor when the viscosity was greater than 18.0 mPa·s.

[0033] On the other hand, the prepared slurry was applied to Akaboku soil (see Table 1) at a rate of 150 kg / m 3 (The mass is the mass of the ground improvement material excluding water.) was added and mixed to obtain a simulated improved ground. The unconfined compressive strength of this simulated improved ground at 28 days of age was measured in accordance with "JIS A 1216:2020 (Unconfined compression test method for soil)". The unconfined compressive strength is 297 kN / m 2 It was. Furthermore, for this simulated improved ground, when it was 28 days old, a hexavalent chromium compound leaching test was conducted in accordance with the method described in the Ministry of the Environment Notification No. 18, "Establishing Measurement Methods for Soil Leaching Amount Survey," dated March 6, 2003, to measure the amount of hexavalent chromium compounds leached out. The amount of hexavalent chromium compounds eluted was 0.02 mg / L (elution suppression effect: good). The effect of inhibiting elution of hexavalent chromium was evaluated as good when the amount of elution satisfied the environmental standard of "0.05 mg / liter or less," and as poor when the amount of elution exceeded 0.05 mg / liter.

[0034] [Examples 2 to 4, Comparative Examples 1 to 4] As shown in Table 4, the experiment was carried out in the same manner as in Example 1, except that the types and amounts of the ground improvement materials (cement-based solidification material, hexavalent chromium fixing agent) were changed. The results are shown in Table 4. In Table 4, "Solidification material" refers to a cement-based solidification material. "Blast furnace slag" refers to ground granulated blast furnace slag. "Amount of eluted hexavalent chromium" refers to the amount of eluted hexavalent chromium compounds.

[0035] [Table 4]

[0036] From Table 4, it can be seen that in Examples 1 to 4, which used hexavalent chromium fixing agents A to B in which the amount of SrO falls within the range of 0.03 to 0.28 parts by mass as specified in the present invention, the viscosity was 18.0 mPa s or less, and the pumpability was good. In addition, the unconfined compressive strength was 291 kN / m 2 These values ​​indicate that the product has excellent performance in solidifying the ground. Furthermore, the amount of hexavalent chromium compounds eluted was 0.01-0.04 mg / L, which meets the environmental standard (hexavalent chromium compounds: 0.05 mg / L or less).

[0037] On the other hand, in Comparative Example 1, in which the hexavalent chromium fixing agent C having an SrO content of 0.01 parts by mass was used, the amount of eluted hexavalent chromium compounds was 0.06 mg / L, indicating that the hexavalent chromium suppression effect was poor. In Comparative Example 2, in which hexavalent chromium fixing agent D containing 0.33 parts by mass of SrO was used, the viscosity exceeded 18.0 mPa·s, the pumpability was poor, and the unconfined compressive strength was 212 kN / m2 The small value obtained indicates that the performance of the material in solidifying the ground is poor. In Comparative Example 3, in which no hexavalent chromium fixing agent was used, the amount of eluted hexavalent chromium compounds was 0.08 mg / L, which indicates that the hexavalent chromium suppression effect was poor. In Comparative Example 4, in which the amount of ground granulated blast furnace slag was 50 parts by mass and no hexavalent chromium fixing agent was used, the unconfined compressive strength was 145 kN / m 2 This shows that the performance of the concrete in solidifying the ground is very poor.

[0038] [C. Experimental example using calcium polysulfide] [Examples 5 to 6, Comparative Examples 5 to 8] The experiment was conducted in the same manner as in Example 1, except that the types and amounts of the ground improvement materials (cement-based solidification material, hexavalent chromium fixation agent) were changed as shown in Table 5, and the following points were changed. The simulated improved ground was prepared by adding 250 kg / m of prepared slurry (consisting of ground improvement material and water) to black soil (see Table 1). 3 (The mass is the mass of the ground improvement material excluding water.) and mixed. In addition, since the hexavalent chromium fixing agent (lime sulfur mixture containing calcium polysulfide as the main component) is liquid, it was mixed with water and then mixed with a cement-based solidification material to prepare a slurry. The results are shown in Table 5. In Table 5, the terms "solidification material," "blast furnace slag," and "amount of eluted hexavalent chromium" are the same as in Table 4. "Amount of hexavalent chromium fixing agent (parts)" indicates the amount (parts by mass) of the lime sulfur mixture, which is a liquid. The amount of hexavalent chromium fixing agent in Example 5 (1.5 parts by mass) is equivalent to 0.41 parts by mass of calcium polysulfide. The amount of hexavalent chromium fixing agent in Example 6 (0.5 parts by mass) is equivalent to 0.14 parts by mass of calcium polysulfide.

[0039] [Table 5]

[0040] From Table 5, it can be seen that in Examples 5 and 6, which used hexavalent chromium fixing agent E in which the amount of SrO is within the range of 0.03 to 0.28 parts by mass as specified in the present invention, the viscosity is 18.0 mPa s or less, and the pumpability is good. In addition, the unconfined compressive strength is 291 kN / m 2 These values ​​indicate that the product has excellent performance in solidifying the ground. Furthermore, the amount of hexavalent chromium compounds eluted was 0.02-0.04 mg / L, which meets the environmental standard value (hexavalent chromium compounds: 0.05 mg / L or less). On the other hand, in Comparative Example 5, in which the hexavalent chromium fixing agent F containing 0.69 parts by mass of SrO was used, the unconfined compressive strength was 225 kN / m 2 This shows that the performance of solidifying the ground is inferior. In Comparative Example 6, in which the hexavalent chromium fixing agent G having an SrO amount of 1.05 parts by mass was used, the viscosity exceeded 18.0 mPa·s, and it is clear that the pumpability was poor. In Comparative Example 7, in which no hexavalent chromium fixing agent was used, the amount of eluted hexavalent chromium compounds was 0.07 mg / L, which indicates that the hexavalent chromium suppression effect was poor. In Comparative Example 8, in which neither ground granulated blast furnace slag nor a hexavalent chromium fixing agent was used, the amount of hexavalent chromium compounds eluted was 0.15 mg / L, indicating that the hexavalent chromium suppression effect was poor.

Claims

1. The chemical formula is CaS x (wherein x is an integer of 1 or more), and a hexavalent chromium fixing agent comprising: a calcium-containing compound represented by the formula (1), and SrO in an amount of 0.03 to 0.28 parts by mass relative to 100 parts by mass of the calcium-containing compound.

2. A powdered ground improvement material comprising the hexavalent chromium fixing agent according to claim 1 and a cement-based solidification material.

3. The powdery ground improvement material according to claim 2, wherein the cement-based solidification material contains cement and gypsum.

4. The powdered ground improvement material according to claim 3, wherein the cement-based solidification material does not contain ground granulated blast furnace slag or contains ground granulated blast furnace slag in an amount of 40 mass% or less in the total amount of the cement and the gypsum.

5. A method for producing the powdery ground improvement material according to any one of claims 2 to 4, wherein, when a slurry consisting of the powdery ground improvement material and the water is prepared using 60 parts by mass of water per 100 parts by mass of the powdery ground improvement material, the viscosity of the slurry at a time 90 minutes after preparation (wherein the viscosity is a value measured at a temperature of 20 ° C. in accordance with "11 Viscosity measurement method using a vibration viscometer" of "JIS Z 8803: 2011 (Method for measuring viscosity of liquids)") is 18.0 mPa · s or less. The method for producing a powdery ground improvement material, characterized in that the type and amount of materials constituting the powdery ground improvement material are determined so that the viscosity is 18.0 mPa · s or less.

6. A composition that may be used as a hexavalent chromium fixative is represented by the formula CaS x (where x is an integer of 1 or more); a measuring step of measuring the amount of SrO in the composition prepared in the composition preparing step; a selection step of selecting the composition as a hexavalent chromium fixing agent when the amount of SrO obtained in the measurement step is within a range of 0.03 to 0.28 parts by mass relative to 100 parts by mass of the calcium-containing compound, and not selecting the composition as a hexavalent chromium fixing agent when the amount of SrO obtained in the measurement step is less than 0.03 parts by mass or more than 0.28 parts by mass relative to 100 parts by mass of the calcium-containing compound; a mixing step of mixing the composition selected as the hexavalent chromium fixing agent in the selection step, a cement-based solidification material, and water to obtain a slurry-like ground improvement material; A method for producing a slurry-like ground improvement material, comprising:

7. A ground improvement method using the powdery ground improvement material according to any one of claims 2 to 4, A ground improvement method comprising injecting a slurry containing the powdered ground improvement material and water into the ground to be improved.

Citation Information

Patent Citations

  • Heavy metal fixing material

    JP1999169816A

  • Treatment composition for heavy metal contaminated soil and treatment method

    JP2007105549A