Magnetic encoder

A magnetic encoder with controlled Nd-Fe-B magnet powder and resin content, along with a vernier system, addresses angular accuracy and uniformity issues, resulting in precise and reliable magnetic flux detection.

JP2024139109APending Publication Date: 2024-10-09MINEBEAMITSUMI INC

Patent Information

Application Number
JP2023049909
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing magnetic encoders using rare earth bonded magnets face challenges in achieving high angular accuracy and uniform magnetic properties due to variations in magnet powder particle sizes and distribution, leading to inconsistencies in magnetic flux detection.

Method used

A magnetic encoder design using isotropic Nd-Fe-B magnet powder with a controlled particle size range of 45 μm to 75 μm and a specific resin content of 5% to 6.5% by weight, combined with a vernier system of concentric magnetic tracks, ensures uniform magnetization and reduced variations in magnetic properties.

Benefits of technology

The solution achieves high angular accuracy and robustness by minimizing variations in magnetic flux, thereby enhancing the precision and reliability of the magnetic encoder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139109000004
    Figure 2024139109000004
  • Figure 2024139109000001
    Figure 2024139109000001
  • Figure 2024139109000002
    Figure 2024139109000002
Patent Text Reader

Abstract

To provide a magnetic encoder which has high angle accuracy.SOLUTION: A magnetic encoder is a ring-shaped magnetic encoder which contains rare earth magnet powder, and a resin cured product of a thermosetting resin, and has a magnetic track formed by magnetizing a plurality of magnetic poles at a prescribed pitch in a circumferential direction on the surface, wherein the rare earth magnet powder is isotropic Nd-Fe-B-based magnetic powder having a particle diameter of 45 μm or more and less than 75 μm, 5 wt.% or more and 6.5 wt.% or less of the resin cured product is contained, and thickness of the ring-shaped magnetic encoder is 0.2 mm or more and 1 mm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a magnetic encoder, and more particularly to a magnetic encoder using a rare earth bonded magnet. [Background technology]

[0002] Conventionally, magnetic encoders are known as a method for detecting the rotational position of a device. A rotation detection device has been proposed that includes two magnetic encoders arranged in concentric rings and having different numbers of magnetic poles, and magnetic sensors that detect the magnetic fields of the magnetic encoders, and calculates the absolute angle of the magnetic encoders based on the phase difference between the magnetic field signals detected by the magnetic sensors (see, for example, Patent Document 1).

[0003] The magnetic encoder in the rotation detection device of Patent Document 1 is configured as a rubber magnet in which an elastic member containing magnetic powder is vulcanized and bonded to a core metal made of a magnetic material, and magnetic poles are formed alternately in the circumferential direction on the elastic member to form a magnetic track. In addition, as another configuration example of the magnetic encoder, it is described that a resin molded body made of a resin containing magnetic powder is provided on a core metal made of a magnetic material, and the resin molded body may be configured as a resin magnet in which magnetic poles are formed alternately in the circumferential direction to form a magnetic track. In such rubber magnets and resin magnets, ferrite magnet powder is usually used as the magnetic powder.

[0004] In order to improve the magnetic properties of a magnetic encoder, it is preferable that the magnetic encoder contains a larger amount of magnetic material, and that the magnetic properties of the magnetic powder are higher. For this reason, the magnetic properties are improved by using rare earth magnetic powder rather than ferrite magnetic powder. Therefore, it is considered to construct the magnetic encoder, which is the object to be magnetized, from a rare earth bonded magnet.

[0005] When magnetizing multiple magnetic poles (N pole, S pole) that become the magnetic track of a magnetic encoder, a magnetizing device using a coil current method (so-called pulse magnetizing method) is generally used. This coil current method magnetizing device, for example, applies a pulse current to a field magnet part having a coil wound around a magnetizing yoke, and magnetizes the object to be magnetized by the magnetic field generated by this. However, as described in Patent Document 2, for example, if the magnetic pole width of the magnetic sensor that detects the magnetic track of the magnetic encoder is limited to 1.28 mm, it is difficult to form multiple magnetic poles by saturating magnetization with a narrow magnetic pole pitch such as 1.28 mm for the magnetic encoder that is the object to be magnetized and is configured with a rare earth bond magnet using the above pulse magnetizing method.

[0006] For this reason, a method has been proposed that enables favorable magnetization even in multi-pole magnetization by heating the object to be magnetized to above the Curie point of the magnet, and then continuously applying a magnetizing magnetic field to the object to be magnetized using a permanent magnet that serves as a field source while cooling it to below the Curie point (see, for example, Patent Document 3).

[0007] The magnetization device in Patent Document 3 describes an isotropic rare earth iron-based bonded magnet that is made by mixing isotropic magnet powder with epoxy resin, compressing it, and curing it at a specified temperature, and can effectively magnetize even multi-pole magnetization with a narrow magnetic pole pitch such as 1.28 mm. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2008-267867 A [Patent Document 2] JP 2017-32327 A [Patent Document 3] Patent Publication No. 2021-093521 Summary of the Invention [Problem to be solved by the invention]

[0009] In light of the recent rising prices of rare earth magnet powder, it is preferable to use isotropic rare earth bonded magnets, which contain a small amount of rare earth magnet powder, in magnetic encoders, although their magnetic properties are inferior to those of isotropic rare earth iron-based bulk magnets made by sintering magnet powder at a specified temperature. When using rare earth bonded magnets, the magnetizing device of Patent Document 3 can be used to preferably magnetize multiple poles with a narrow magnetic pole pitch, and costs can be reduced.

[0010] Rare earth bonded magnets are made by mixing rare earth magnet powder with thermosetting resin and compressing it to create a green body, then heat-curing the resin contained in the green body to create a cured body (thermosetting body), and magnetizing the cured body with a specified magnetic pole pitch to obtain a magnetic encoder.

[0011] Rare earth bonded magnets are composed of rare earth magnet powder, a thermosetting resin binder, and voids, with the volume ratios of each being approximately 80% magnet powder, 10% resin, and 10% voids (air holes). As magnet powder is a mixture of magnet powders with various particle sizes, it is prone to deformation after thermal curing due to moldability issues when the green body is thinned and variations in density of the green body. In addition, only the magnet powder contributes to the magnetic properties of the magnetic encoder, so it is important for the magnet powder to be distributed evenly and for the variation in magnetic properties to be small in order to increase the accuracy of the magnetic encoder.

[0012] Patent Document 3 describes that isotropic rare earth iron-based bonded magnets can be favorably magnetized even when multiple poles are magnetized with a narrow magnetic pole pitch. However, there is room for further consideration in terms of the angle accuracy of the magnetic encoder.

[0013] SUMMARY OF THE PRESENT EMBODIMENTS An object of the present invention is to provide a magnetic encoder using a rare earth bonded magnet that reduces the variation in magnetic characteristics and achieves high angular accuracy. [Means for solving the problem]

[0014] In order to solve the above-mentioned problems and achieve the object, a magnetic encoder according to one embodiment of the present invention is a ring-shaped magnetic encoder that contains rare earth magnet powder and a cured resin of a thermosetting resin, and has a magnetic track formed by magnetizing multiple magnetic poles at a predetermined pitch in the circumferential direction of the surface, wherein the rare earth magnet powder is an isotropic Nd-Fe-B based magnet powder with a particle size of 45 μm or more and less than 75 μm, the cured resin is contained in an amount of 5 wt % or more and 6.5 wt % or less, and the thickness of the ring-shaped magnetic encoder is 0.2 mm or more and 1 mm or less. Effect of the Invention

[0015] According to one aspect of the present invention, a magnetic encoder with high angular accuracy is obtained. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a diagram for explaining the magnetic encoder of the first embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. Note that the present invention is not limited to this embodiment. In addition, the components in the following embodiments include those that are replaceable and easy for a person skilled in the art, or those that are substantially the same.

[0018] <Embodiment 1> The magnetic encoder of embodiment 1 is a ring-shaped magnetic encoder that contains rare earth magnet powder and a cured resin of a thermosetting resin, and has a magnetic track formed by magnetizing multiple magnetic poles at a predetermined pitch in the circumferential direction of the surface, where the rare earth magnet powder is an isotropic Nd-Fe-B magnet powder with a particle size of 45 μm or more and less than 75 μm, the cured resin is contained in an amount of 5 wt % or more and 6.5 wt % or less, and the thickness of the ring-shaped magnetic encoder is 0.2 mm or more and 1 mm or less.

[0019] When an isotropic rare earth bonded magnet using Nd-Fe-B magnet powder is used in a magnetic encoder, if the rare earth magnet powder used contains magnet powders of various particle sizes, the manufactured magnetic encoder will have variations in the surface magnetic flux detected by each magnetic pole. As a result, the output of the magnetic sensor that detects the magnetic flux from the magnetic poles of the magnetic encoder will vary, making it difficult to improve the angular accuracy of the magnetic encoder. For this reason, in order to reduce the variation in surface magnetic flux at each location (each magnetic pole) in the entire magnetic encoder and achieve a homogeneous state, it has been found that it is effective to reduce the particle size of the rare earth magnet powder while narrowing its particle size distribution. In general, the smaller the particle size of the magnet powder, the lower the static magnetic properties (residual magnetic flux density) of the magnet powder. However, in the magnetic encoder of the first embodiment, priority is given to suppressing the variation in static magnetic properties and achieving a homogeneous state.

[0020] FIG. 1 is a diagram for explaining a magnetic encoder of the first embodiment. The magnetic encoder 1 is configured as a vernier type in which two magnetic tracks (main track 11 and sub-track 12) are formed concentrically on one axial end face. Specifically, in the axial direction, the main track 11 is magnetized in the circumferential direction at a predetermined magnetic pole pitch on the outer circumferential side, and the sub-track 12 is magnetized in the circumferential direction at a predetermined magnetic pole pitch on the inner circumferential side. When the main track 11 is magnetized with n pole pairs, the sub-track 12 is magnetized with (n-1) pole pairs. When the magnetic pole width of the magnetic sensor that detects the magnetic track of the magnetic encoder is limited, the magnetic pole pitch of the magnetic track formed in the magnetic encoder is formed to the same width as the magnetic pole width of the magnetic sensor. For example, the predetermined pitch is 0.4 mm or more and 2.4 mm or less, more specifically, 1.28 mm. In addition, the magnetic encoder 1 has non-magnetized areas 13 between the main track 11 and the sub-track 12 and on the inner circumferential side of the sub-track 12 on the end face.

[0021] The rare earth magnet powder contained in the magnetic encoder of the embodiment 1 is an isotropic Nd (neodymium)-Fe (iron)-B (boron) based magnet powder. Examples of the isotropic Nd-Fe-B based magnet powder include MQP-14-12 (product name), MQP-8-5 (product name), MQP-10-8.5HD (product name), MQP-11-8 (product name), MQP12-8HD (product name), and the like manufactured by Magnequench.

[0022] Alternatively, for example, Nd-Fe-B magnet powder produced by a rapid cooling method may be used. Specifically, an Nd-Fe-B alloy is melted by high-frequency induction heating under reduced pressure or in an argon atmosphere. The melted alloy is then sprayed onto a rotating copper roll for rapid cooling (rapid cooling) to produce ribbon-shaped strips. The strips are then broken into pieces of, for example, several mm to several tens of mm, and then crushed by a crusher or the like to obtain powder. The crushed powder is classified using a sieve with a predetermined mesh, and then heat-treated to produce rare earth magnet powder. This rare earth magnet powder is magnetically isotropic because the magnetization easy axis of each crystal grain is not aligned in one direction.

[0023] The rare earth magnet powder has a particle size of at least 45 μm and less than 75 μm. This particle size range can be adjusted by classification using a sieve with a specified mesh.

[0024] The cured thermosetting resin contained in the magnetic encoder of the first embodiment is specifically a cured epoxy resin.

[0025] The cured resin is contained in an amount of 5% by weight to 6.5% by weight in the magnetic encoder of embodiment 1. The rare earth magnet powder is contained in an amount of 93.5% by weight to 95% by weight in the magnetic encoder of embodiment 1. In addition, the rare earth magnet powder and the cured thermosetting resin are preferably mixed uniformly in the magnetic encoder of embodiment 1.

[0026] In this way, the magnetic encoder of embodiment 1 has the above thickness and contains rare earth magnet powder within the above particle size range and cured resin in the above ratio, and therefore has excellent angular accuracy and rolling strength.

[0027] Furthermore, from the viewpoint of rolling strength, it is preferable that, in the magnetic encoder of embodiment 1 (100% by weight), the cured resin is contained in an amount of 6% by weight or more and 6.5% by weight or less, and the rare earth magnet powder is contained in an amount of 93.5% by weight or more and 94% by weight or less.

[0028] The magnetic encoder of the first embodiment can be manufactured, for example, as follows. First, the rare earth magnet powder and the components constituting the cured resin in the magnetic encoder (raw material components of the cured resin) are mixed in a predetermined mixing ratio to prepare a compound. The mixing ratio of the rare earth magnet powder and the raw material components of the cured resin is considered to be the same as the ratio of the rare earth magnet powder and the cured resin in the magnetic encoder after manufacture. The raw material components of the cured resin include a thermosetting resin (e.g., epoxy resin) as a binder, and a curing agent. Furthermore, when preparing the compound, a small amount of a lubricant (e.g., calcium stearate) may be added. Specifically, the lubricant may be mixed in an amount of 0.02% by weight or more and less than 0.5% by weight with respect to the total 100% by weight of the rare earth magnet powder and the raw material components of the cured resin.

[0029] Next, the compound is filled into the cavity of the mold and compressed under a predetermined pressure to produce a doughnut-shaped green body. The green body is then removed from the mold and placed in an oven, where it is thermally cured at a predetermined temperature for a predetermined time to produce a cured body (thermosetting body) containing the rare earth magnet powder and the cured resin. It is also preferable to apply a rust prevention means to the surface of the cured body to prevent oxidation. As the rust prevention means, known means such as electrocoating and spray coating can be used.

[0030] Next, as shown in FIG. 1, a vernier system is configured in which two magnetic tracks are formed concentrically on one axial end surface of the cured body. This configuration is also shown in the figure of Patent Document 1. Specifically, in the axial direction, a main track is magnetized in the circumferential direction at a predetermined magnetic pole pitch on the outer circumferential side, and a sub-track is magnetized in the circumferential direction at a predetermined magnetic pole pitch on the inner circumferential side. When the main track is magnetized with n pole pairs, the sub-track is magnetized with (n-1) pole pairs. When the magnetic pole pitch of the magnetic sensor that detects the magnetic track of the magnetic encoder is limited, the magnetic pole pitch of the magnetic track formed on the magnetic encoder is formed to the same width as the magnetic pole width of the magnetic sensor. Magnetization is so-called magnetization, and the magnetization means can be, for example, as disclosed in Patent Document 3, a means for continuously applying a magnetizing magnetic field to the magnetized object by a permanent magnet as a field source while heating the magnetized object to a temperature above the Curie point of the magnet powder and cooling it to a temperature below the Curie point. In addition, since the sub-track is located on the inner circumference than the main track, the magnetic pole pitch is set corresponding to the inner diameter position of the detection portion of the magnetic sensor for the sub-track. In this manner, the magnetic encoder of the first embodiment is obtained.

[0031] <Embodiment 2> The magnetic encoder of the second embodiment is a ring-shaped magnetic encoder that includes rare earth magnet powder and a resin cured product of a thermosetting resin, and has a magnetic track formed by magnetizing a plurality of magnetic poles at a predetermined pitch in the circumferential direction of the surface, the rare earth magnet powder is an isotropic Nd-Fe-B magnet powder with a particle size of 45 μm or more and less than 175 μm, the resin cured product is included in an amount of 5 wt % to 6.5 wt %, and the thickness of the ring-shaped magnetic encoder is 0.2 mm to 0.4 mm. Except for the thickness of the ring-shaped magnetic encoder, the configuration and function of the components in the magnetic encoder of the second embodiment are the same as the configuration and function of the components in the magnetic encoder of the first embodiment. Therefore, detailed description will be omitted here.

[0032] The magnetic encoder of embodiment 2 also has the above thickness and contains rare earth magnet powder within the above particle size range and cured resin in the above ratio, and therefore has excellent angular accuracy and rolling strength.

[0033] <Other embodiments> This embodiment 1 is an axial type magnetic encoder having a vernier system in which two magnetic tracks are formed on a donut-shaped (ring-shaped) magnetic encoder as shown in FIG. 1, but it may also be a radial type magnetic encoder having a vernier system in which two magnetic tracks are formed on the cylindrical side surface of a hollow cylindrical magnetic encoder.

[0034] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.

[0035] [Example] <Magnetic Encoder Creation> Isotropic Nd-Fe-B magnet powder was used as the rare earth magnet powder. MQP-14-12 (product name) manufactured by Magnequench was prepared as the isotropic Nd-Fe-B magnet powder. The particle size of MQP-14-12 was classified into three groups: 75 μm or more and less than 150 μm, 45 μm or more and less than 75 μm, and 32 μm or more and less than 45 μm. In this case, the classification was performed using a sieve with a specified mesh. Next, for each of the three groups, a compound was prepared by mixing isotropic Nd-Fe-B magnet powder with raw material components for the cured resin, including an epoxy resin binder and a curing agent (manufactured by Pernock, model number XW2310), in a specified mixing ratio. Here, the mixing ratio of the rare earth magnet powder and the raw material components for the cured resin was 2.5% by weight, and the rare earth magnet powder was 97.5% by weight, with the total weight being 100% by weight. Furthermore, compounds were also prepared for the following cases: when the raw material components of the resin cured product were 5% by weight and the rare earth magnet powder was 95% by weight; when the raw material components of the resin cured product were 5.5% by weight and the rare earth magnet powder was 94.5% by weight; when the raw material components of the resin cured product were 6% by weight and the rare earth magnet powder was 94% by weight; when the raw material components of the resin cured product were 6.5% by weight and the rare earth magnet powder was 93.5% by weight; and when the raw material components of the resin cured product were 7.5% by weight and the rare earth magnet powder was 92.5% by weight. The compounds were prepared by mixing the raw material components of the resin cured product dissolved in a solvent with the rare earth magnet powder, evaporating the solvent, and then crushing and classifying the mixture. All the compounds were prepared with the same particle size, and the fluidity conditions for filling the cavity of the mold were the same. Next, the compound was filled into the cavity of the mold and compressed with a certain pressure to produce a doughnut-shaped green body. The green body had an outer diameter of Φ56 mm, an inner diameter of Φ41 mm, and a thickness of 1 mm. In addition, green bodies with thicknesses of 0.4 mm and 0.2 mm were also produced. Next, the green body removed from the mold was placed in an oven and thermally cured at a specified temperature (150°C) for a specified time to produce a cured body (thermosetting body). The cured body had an outer diameter of Φ56 mm, an inner diameter of Φ41 mm, and a thickness of 1 mm. In addition, cured bodies with thicknesses of 0.4 mm and 0.2 mm were also produced. As such, no difference in size was observed between the green body and the cured body. Next, after applying a rust prevention means (specifically, electrochemical coating) to prevent oxidation to the surface of the cured body, a vernier system was formed in which two magnetic tracks were formed concentrically on one axial end surface of the thermoset body, as shown in FIG. 1. Specifically, in the axial direction, the main track was magnetized in the circumferential direction at a predetermined magnetic pole pitch on the outer circumferential side, and the sub-track was magnetized in the circumferential direction at a predetermined magnetic pole pitch on the inner circumferential side. The main track was magnetized with 32 pole pairs, and the sub-track was magnetized with 31 pole pairs. In this embodiment, since a magnetic sensor with a magnetic pole width limited to 1.28 mm is used, the main track of the magnetic encoder was magnetized to 1.28 mm. The magnetization is so-called magnetization, and the magnetization means was, for example, as disclosed in Patent Document 3, a means for continuously applying a magnetizing magnetic field to the magnetized object by a permanent magnet as a field source while heating the magnetized object to a temperature above the Curie point of the magnet powder and cooling it to a temperature below the Curie point. Since the sub-track is located on the inner circumference than the main track, the magnetic pole pitch is set to correspond to the inner diameter position of the detection portion of the magnetic sensor for the sub-track. In this way, ring-shaped magnetic encoders (samples 1 to 54) were produced that contained rare earth magnet powder and a cured resin of a thermosetting resin, and had magnetic tracks formed by magnetizing multiple magnetic poles at a predetermined pitch around the circumferential direction of the surface.

[0036] <Evaluation method> (Moldability) The compound was filled into the cavity of a mold and compression molded into a doughnut-shaped green body, and the handleability was evaluated when the green body was removed from the mold. Specifically, when the green body was removed from the mold with an ejector pin attached to the mold, the state of cracks and chips that occurred in the green body was visually observed and evaluated as moldability. The evaluation criteria are as follows. ○: No cracks or chips ×: Cracks and chips

[0037] (Thickness precision) The cured body was taken out of the oven and the thickness was measured at eight diagonal positions with a micrometer to evaluate the thickness variation (maximum value - minimum value). The evaluation criteria were as follows: ○: Samples with a variation value of less than 0.06 mm are considered to be good. △: Samples having a variation value between 0.06 mm and 0.08 mm are rated as fair. ×: Samples with a variation value of more than 0.08 mm are unacceptable.

[0038] (Ring crushing strength) The radial crushing strength was measured based on JIS Z 2507. The evaluation criteria are as follows: ◎: Radial crushing strength is 100 MPa or more. ◯: The radial crushing strength is 60 MPa or more and less than 100 MPa. △: The radial crushing strength is 50 MPa or more and less than 60 MPa. ×: The radial crushing strength is less than 50 MPa.

[0039] (Angle accuracy) The angular accuracy of the magnetic encoder magnetized by the above-mentioned method was measured. The evaluation criteria were as follows. The angular accuracy was evaluated by attaching the magnet and IC board to a reference servo motor shaft equipped with an optical encoder (angle accuracy of ±10 seconds or less, resolution of 20 bits or more), driving the reference motor every 1 degree (360 degrees CW CCW twice), and measuring the difference between the angle output from the IC and the reference angle. The maximum-minimum width was taken as the angular error. ◎: The variation in magnetic flux is 0.05 deg. or less. ◯: The variation in magnetic flux is greater than 0.05 degrees and equal to or less than 0.07 degrees. △: The variation in magnetic flux is greater than 0.07 deg. and less than 0.1 deg. ×: The variation in magnetic flux is 0.1 deg. or more.

[0040] (comprehensive evaluation) A comprehensive evaluation was performed on Samples 1 to 54. The evaluation criteria were as follows. ○: The evaluation results for each evaluation item are only ○ or ◎. ×: The evaluation result for each evaluation item is △ or ×. The evaluation results of Samples 1 to 54 are shown in Tables 1 to 3 below. In Table 1, the magnetic powder particle size (μm) "75-150" indicates that the particle size of the isotropic Nd-Fe-B magnet powder is in the range of 75 μm or more and less than 150 μm. In Table 2, the magnetic powder particle size (μm) "45-75" indicates that the particle size of the isotropic Nd-Fe-B magnet powder is in the range of 45 μm or more and less than 75 μm. In Table 3, the magnetic powder particle size (μm) "32-45" indicates that the particle size of the isotropic Nd-Fe-B magnet powder is in the range of 32 μm or more and less than 45 μm.

[0041] [Table 1]

[0042] Table 1 shows the evaluation of the magnetic encoder of samples 1 to 18. In samples 1 to 18, the particle size of the isotropic Nd-Fe-B magnet powder is in the range of 75 μm or more and less than 150 μm. In samples 1 to 3, in which the amount of raw material components of the resin cured product is 2.5% by weight, the radial crushing strength was △. This is due to the small amount of raw material components of the resin cured product. When the sample (green body) was ejected from the mold with an ejector pin, chips and cracks occurred on the outer periphery. If the chips and cracks reach the track formation area when the sample is magnetized to form a track in the later process, the track cannot be formed. In addition, since Nd-Fe-B magnet powder is used as the rare earth magnet powder, it is prone to rust. For this reason, it is necessary to coat the surface of the sample with an anti-rust film in order to prevent oxidation, but the area where the chips and cracks have occurred does not have a uniform anti-rust film, and there is a risk of rust occurring from this area. In samples 16 to 18, in which the amount of raw material components of the resin cured product was 7.5% by weight, some of the binder leaked out of the cavity. For this reason, the angle accuracy was not evaluated. This is because the amount of raw material components of the resin cured product was too high. The angular accuracy of samples 22 to 33, which will be described later, was all rated as excellent. This is because the particle size of the isotropic Nd-Fe-B magnet powder was in the range of 45 μm or more and less than 75 μm. This is in a smaller range than the particle size range of the Nd-Fe-B magnet powder in samples 1 to 18 shown in Table 1, so there was less variation in the distribution of the magnet powder in a given area (or volume), and this is thought to be because the variation in the magnetic properties for each magnetic pole was generally also less. The angular accuracy was rated as x when the sample thickness was 1 mm. This is because the particle size of the Nd-Fe-B magnet powder was in the range of 75 μm or more and less than 150 μm. Because the particle size of the Nd-Fe-B magnet powder is large, there is a large variation in the area occupied by the magnet powder in the thickness direction in a given area, which is likely due to the large variation in the magnetic properties for each magnetic pole.

[0043] [Table 2]

[0044] Table 2 shows the evaluation of the magnetic encoders of samples 19 to 36. In samples 19 to 36, the particle size of the isotropic Nd-Fe-B magnet powder was in the range of 45 μm or more and less than 75 μm. Samples 19 to 21, in which the amount of raw material components of the cured resin was 2.5% by weight, had a fair radial crushing strength. This is because the amount of raw material components of the cured resin was too small. Also, in samples 34 to 36, in which the amount of raw material components of the cured resin was 7.5% by weight, some of the binder leaked out of the cavity. For this reason, the angular accuracy was not evaluated. This is because the amount of raw material components of the cured resin was too large. The evaluations of samples 22 to 33 other than the sample in which the amount of raw material components of the resin cured product was 2.5% by weight were all rated as ⊚ or ◯ in all items. Therefore, the overall evaluation of samples 22 to 33 shown in Table 2 was rated as ◯. The angular precision of samples 22 to 33 was evaluated as excellent. This is because the particle size of the isotropic Nd-Fe-B magnet powder was in the range of 45 μm or more and less than 75 μm. This is in a smaller range than the particle size range of the Nd-Fe-B magnet powder in samples 1 to 18 shown in Table 1, so there is less variation in the area occupied by the magnet powder in the thickness direction in a given area, which is thought to be because the variation in the magnetic properties for each magnetic pole is also small.

[0045] [Table 3]

[0046] Table 3 shows the evaluation of the magnetic encoders of Samples 37 to 54. In Samples 37 to 54, the particle size of the isotropic Nd—Fe—B magnet powder was in the range of 32 μm or more and less than 45 μm. Samples 37 to 39, which contained 2.5% by weight of the raw material component of the cured resin, had a fair radial crushing strength. This was due to the amount of raw material component of the cured resin being too small. Samples 52 to 54, which contained 7.5% by weight of the raw material component of the cured resin, had some of the binder leaking out of the cavity. For this reason, the angle accuracy was not evaluated. This was due to the amount of raw material component of the cured resin being too large. The angular accuracy of all samples other than the above samples was rated △. This is thought to be due to the small particle size of the Nd-Fe-B magnetic powder, between 32μm and 45μm. The smaller the particle size of the magnetic powder, the worse the squareness of the demagnetization curve of the magnetic powder itself, and the easier it is for the magnetic properties to deteriorate due to thermal degradation, oxidative degradation, etc., which is thought to be due to the decrease in the surface magnetic flux from the magnetic encoder. For this reason, the overall evaluation of samples 37 to 54 shown in Table 3 was all rated as ×. [Explanation of symbols]

[0047] 1 magnetic encoder, 11 main track, 12 sub track, 13 non-magnetized area

Claims

1. A ring-shaped magnetic encoder including rare earth magnet powder and a cured resin of a thermosetting resin, the magnetic encoder having a magnetic track formed by magnetizing a plurality of magnetic poles at a predetermined pitch in the circumferential direction of a surface thereof, the rare earth magnet powder is an isotropic Nd—Fe—B magnet powder having a particle size of 45 μm or more and less than 75 μm, The cured resin is contained in an amount of 5% by weight or more and 6.5% by weight or less, The thickness of the ring-shaped magnetic encoder is 0.2 mm or more and 1 mm or less. Magnetic encoder.

2. A ring-shaped magnetic encoder including rare earth magnet powder and a cured resin of a thermosetting resin, the magnetic encoder having a magnetic track formed by magnetizing a plurality of magnetic poles at a predetermined pitch in the circumferential direction of a surface thereof, the rare earth magnet powder is an isotropic Nd—Fe—B magnet powder having a particle size of 45 μm or more and less than 175 μm, The cured resin is contained in an amount of 5% by weight or more and 6.5% by weight or less, The thickness of the ring-shaped magnetic encoder is 0.2 mm or more and 0.4 mm or less. Magnetic encoder.

3. 3. The magnetic encoder according to claim 1, wherein the magnetization is performed in an axial direction.

Citation Information

Patent Citations

  • Rotation detector, and bearing with the rotation detector

    JP2008267867A

  • Bearing with rotation detector

    JP2017032327A

  • Magnetization device and magnetized object

    JP2021093521A

Cited By

  • Magnet and magnetic encoder

    WO2026230436A1