Optical laminate and display system

The optical laminate with a high-modulus support layer and directly adjacent adhesive layers addresses bubble issues in VR goggles, improving image quality by suppressing defects.

JP2024139261AInactive Publication Date: 2024-10-09NITTO DENKO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023050126
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Optical laminates used in VR goggles suffer from defects such as bubbles due to irregularities at the lamination interface, which affect image quality.

Method used

An optical laminate design featuring a polarizing member with a protective layer, a retardation member, and a support layer with an indentation modulus of 1 GPa or more, along with adhesive layers directly adjacent to the support layer to suppress bubble formation.

Benefits of technology

The design effectively reduces defects like bubbles, enhancing the reliability and image quality of optical laminates in VR goggles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139261000001_ABST
    Figure 2024139261000001_ABST
Patent Text Reader

Abstract

To provide an optical laminate with suppressed defects.SOLUTION: An optical laminate is provided, comprising: a polarizing member including an absorptive polarizing film and a protective layer provided on at least one side of the absorptive polarizing film; and a first retardation member. The optical laminate also comprises a support layer having an indentation modulus of 1 GPa or greater, and an adhesive layer provided directly next to the support layer.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical stack and a display system. [Background technology]

[0002] Image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices), are rapidly becoming widespread. In image display devices, optical members such as polarizing members and phase difference members are generally used to realize image display and to improve the performance of the image display (see, for example, Patent Document 1).

[0003] In recent years, new applications of image display devices have been developed. For example, goggles with a display (VR goggles) for realizing virtual reality (VR) have begun to be commercialized. In VR goggles, the display is enlarged for a viewer to view, so that small defects that are acceptable in optical laminates applied to conventional image display devices may become problematic in the optical laminate applied to VR goggles. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2021-103286 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide an optical laminate in which defects are suppressed. [Means for solving the problem]

[0006] [1] According to one aspect of the present invention, there is provided an optical laminate comprising a polarizing member having an absorptive polarizing film and a protective layer disposed on at least one side of the absorptive polarizing film, and a first phase difference member, the optical laminate further comprising a support layer having an indentation elastic modulus of 1 GPa or more, and an adhesive layer disposed directly adjacent to the support layer. [2] The optical laminate described in [1] above may include, in this order, a surface adhesive layer, the polarizing member, a first adhesive layer, the first phase difference member, a second adhesive layer, and a protective member. [3] In the optical laminate described in [2] above, at least one selected from the surface adhesive layer, the first adhesive layer, and the second adhesive layer may be arranged directly adjacent to the support layer. [4] The optical laminate described in [1] above may include, in this order, a surface adhesive layer, a second phase difference member, a third adhesive layer, the polarizing member, a first adhesive layer, the first phase difference member, a second adhesive layer, and a protective member. [5] In the optical laminate described in [4] above, at least one selected from the surface adhesive layer, the first adhesive layer, the second adhesive layer, and the third adhesive layer may be arranged directly adjacent to the support layer. [6] In the optical laminate according to any one of [1] to [5] above, the support layer may be a hard coat layer. [7] In the optical laminate according to any one of the above [1] to [6], the support layer may have a thickness of 0.5 μm to 15 μm. [8] In the optical laminate described in any one of [1] to [7] above, the support layer may be provided directly adjacent to the side of the polarizing member opposite to the side on which the first phase difference member is arranged. [9] In the optical laminate according to any one of the above [1] to [8], the adhesive layer disposed directly adjacent to the support layer may have an elastic modulus of 0.01 MPa to 1 MPa.

[10] According to another aspect of the present invention, there is provided a display system including the optical laminate according to any one of [1] to [9] above. Effect of the Invention

[0007] According to an embodiment of the present invention, an optical laminate in which defects such as air bubbles are suppressed can be provided. [Brief description of the drawings]

[0008] [Figure 1] 1 is a schematic diagram showing a general configuration of a display system of VR goggles according to one embodiment of the present invention. [Diagram 2] 1 is a schematic cross-sectional view showing a general configuration of an optical laminate according to one embodiment of the present invention. [Diagram 3] 1 is a schematic cross-sectional view showing a general configuration of an optical laminate according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to these embodiments. In order to clarify the description, the drawings may be schematic in terms of the width, thickness, shape, etc. of each part compared to the embodiment, but they are merely examples and do not limit the interpretation of the present invention. In addition, in the drawings, the same or equivalent elements are given the same reference numerals, and duplicate descriptions may be omitted.

[0010] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re(λ)=(nx-ny)×d, where d(nm) is the thickness of the layer (film). (3) Retardation in the thickness direction (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light of wavelength λ nm at 23° C. For example, "Rth(550)" is the retardation in the thickness direction measured with light of wavelength 550 nm at 23° C. Rth(λ) is calculated by the formula: Rth(λ)=(nx-nz)×d, where d(nm) is the thickness of the layer (film). (4) Nz coefficient The Nz coefficient is calculated by Nz=Rth / Re. (5)Angle When an angle is mentioned in this specification, the angle includes both clockwise and counterclockwise angles with respect to a reference direction. Thus, for example, "45°" means ±45°. In this specification, "substantially parallel" includes the case where the angle is within a range of 0°±10°, for example, within a range of 0°±5°, preferably within a range of 0°±3°, more preferably within a range of 0°±1°, and "substantially perpendicular" includes the case where the angle is within a range of 90°±10°, for example, within a range of 90°±5°, preferably within a range of 90°±3°, more preferably within a range of 90°±1°.

[0011] A. Display System FIG. 1 is a schematic diagram showing a schematic configuration of a display system according to one embodiment of the present invention. In FIG. 1, the arrangement and shape of each component of a display system 2 are illustrated. The display system 2 includes a display element 12, a reflective polarizing member 14, a first lens unit 16, a half mirror 18, a first phase difference member 20, a lens unit phase difference member 22, and a second lens unit 24. The reflective polarizing member 14 is disposed in front of the display surface 12a side of the display element 12, and can reflect light emitted from the display element 12. The first lens unit 16 is disposed on the optical path between the display element 12 and the reflective polarizing member 14, and the half mirror 18 is disposed between the display element 12 and the first lens unit 16. The first phase difference member 20 is disposed on the optical path between the display element 12 and the half mirror 18, and the lens unit phase difference member 22 is disposed on the optical path between the half mirror 18 and the reflective polarizing member 14.

[0012] The components arranged in front of the half mirror (in the illustrated example, the half mirror 18, the first lens section 16, the lens section phase difference member 22, the reflective polarizing member 14, and the second lens section 24) may be collectively referred to as the lens section (lens section 4).

[0013] The display element 12 is, for example, a liquid crystal display or an organic EL display, and has a display surface 12a for displaying an image. The light emitted from the display surface 12a passes through, for example, a polarizing member (typically, a polarizing film) that may be included in the display element 12, and is converted into a first linearly polarized light.

[0014] The first phase difference member 20 includes a first λ / 4 member that can convert a first linearly polarized light incident on the first phase difference member 20 into a first circularly polarized light. When the first phase difference member does not include a member other than the first λ / 4 member, the first phase difference member may correspond to the first λ / 4 member. The first phase difference member 20 may be provided integrally with the display element 12.

[0015] The half mirror 18 transmits the light emitted from the display element 12 and reflects the light reflected by the reflective polarizing member 14 toward the reflective polarizing member 14. The half mirror 18 is provided integrally with the first lens portion 16.

[0016] The lens portion phase difference member 22 includes a second λ / 4 member that can transmit light reflected by the reflective polarizing member 14 and the half mirror 18 through the reflective polarizing member 14. When the lens portion phase difference member does not include any member other than the second λ / 4 member, the lens portion phase difference member can correspond to the second λ / 4 member. The lens portion phase difference member 22 may be provided integrally with the first lens portion 16.

[0017] The first circularly polarized light output from the first λ / 4 member included in the first phase difference member 20 passes through the half mirror 18 and the first lens unit 16, and is converted into the second linearly polarized light by the second λ / 4 member included in the lens unit phase difference member 22. The second linearly polarized light output from the second λ / 4 member is reflected toward the half mirror 18 without passing through the reflective polarizing member 14. At this time, the polarization direction of the second linearly polarized light incident on the reflective polarizing member 14 is the same as the reflection axis of the reflective polarizing member 14. Therefore, the second linearly polarized light incident on the reflective polarizing member 14 is reflected by the reflective polarizing member 14.

[0018] The second linearly polarized light reflected by the reflective polarizing member 14 is converted into the second circularly polarized light by the second λ / 4 member included in the lens portion phase difference member 22, and the second circularly polarized light emitted from the second λ / 4 member passes through the first lens portion 16 and is reflected by the half mirror 18. The second circularly polarized light reflected by the half mirror 18 passes through the first lens portion 16 and is converted into the third linearly polarized light by the second λ / 4 member included in the lens portion phase difference member 22. The third linearly polarized light passes through the reflective polarizing member 14. At this time, the polarization direction of the third linearly polarized light incident on the reflective polarizing member 14 is the same as the transmission axis of the reflective polarizing member 14. Therefore, the third linearly polarized light incident on the reflective polarizing member 14 passes through the reflective polarizing member 14.

[0019] The light transmitted through the reflective polarizing member 14 passes through the second lens portion 24 and enters the eye 26 of the user.

[0020] Although not shown, the display system 2 may include an absorptive polarizing member disposed in front of the reflective polarizing member 14. The reflection axis of the reflective polarizing member and the absorption axis of the absorptive polarizing member may be disposed approximately parallel to each other, and the transmission axis of the reflective polarizing member and the transmission axis of the absorptive polarizing member may be disposed approximately parallel to each other. This allows the third linearly polarized light transmitted through the reflective polarizing member 14 to be transmitted through the absorptive polarizing member as it is.

[0021] Regarding the display system 2 above, the propagation of light from when it exits the display element 12 until it enters the user's eye 26 has been described. However, a part of the light (not shown) that exits the display element 12 and enters the half mirror 18 can be reflected by the half mirror 18, and a part of the light (not shown) that is reflected by the reflective polarizing member 14 and enters the half mirror 18 can pass through the half mirror 18.

[0022] For example, the absorption axis of the polarizing member included in the display element 12 and the reflection axis of the reflective polarizing member 14 may be arranged substantially parallel to each other or substantially orthogonally to each other. The angle formed by the absorption axis of the polarizing member included in the display element 12 and the slow axis of the first λ / 4 member included in the first retardation member 20 is, for example, 40° to 50°, may be 42° to 48°, or may be about 45°. The angle formed by the absorption axis of the polarizing member included in the display element 12 and the slow axis of the second λ / 4 member included in the lens retardation member 22 is, for example, 40° to 50°, may be 42° to 48°, or may be about 45°.

[0023] The in-plane retardation Re(550) of the first λ / 4 member is, for example, 100 nm to 190 nm, may be 110 nm to 180 nm, may be 130 nm to 160 nm, or may be 135 nm to 155 nm. The first λ / 4 member preferably exhibits an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light. The first λ / 4 member preferably satisfies the relationship of Re(450) < Re(550) < Re(650). Re(450) / Re(550) of the first λ / 4 member is, for example, 0.75 or more and less than 1, and may be 0.8 or more and 0.95 or less.

[0024] The in-plane phase difference Re(550) of the second λ / 4 member is, for example, from 100 nm to 190 nm, may be from 110 nm to 180 nm, may be from 130 nm to 160 nm, or may be from 135 nm to 155 nm. The second λ / 4 member preferably exhibits an inverse-dispersion wavelength characteristic in which the phase difference value increases in accordance with the wavelength of the measurement light. The second λ / 4 member preferably satisfies the relationship Re(450) < Re(550) < Re(650). Re(450) / Re(550) of the second λ / 4 member is, for example, 0.75 or more and less than 1, and may be 0.8 or more and 0.95 or less.

[0025] B. Optical laminate The optical laminate according to an embodiment of the present invention can include, for example, an optical member provided in the display system described in section A, and can be included in the display system as a component member of the display system. Specifically, the optical laminate according to an embodiment of the present invention includes a polarizing member having an absorption-type polarizing film and a protective layer disposed on at least one side thereof, and a first phase difference member. Further, the optical laminate according to an embodiment of the present invention can include an adhesive layer for integrating each member constituting itself and / or an adhesive layer for bonding itself to another member (also referred to as a "surface adhesive layer"). The optical laminate according to an embodiment of the present invention further includes a support layer having a predetermined indentation elastic modulus, and an adhesive layer is disposed directly adjacent to the support layer. In this specification, "directly adjacent" means directly adjacent without intervening an adhesive layer. Also, in this specification, when simply referred to as "adjacent", it includes not only being directly adjacent without intervening an adhesive layer but also being adjacent through an adhesive layer.

[0026] The preparation of the optical laminate may include laminating an adhesive layer on a component member, and during this process, small air bubbles may occur at the interface, which may become a defect. In contrast, according to an embodiment of the present invention, the adhesive layer is disposed so as to be directly adjacent to the support layer, thereby suppressing the problem of air bubbles. The reason why this effect is achieved is presumed to be as follows, without limiting the present invention in any way. That is, when laminating an adhesive layer, if there are irregularities on the surface of the member to be laminated, air bubbles may occur due to the irregularities. However, by providing a support layer having a predetermined indentation elasticity and laminating an adhesive layer on the support layer, the generation of such air bubbles can be suppressed.

[0027] FIG. 2 is a schematic cross-sectional view showing a schematic configuration of an optical laminate according to one embodiment of the present invention. The optical laminate 100A includes a surface adhesive layer 42, a polarizing member 10, a first adhesive layer 44, a first phase difference member 20, a second adhesive layer 46, and a protective member 30, in this order. In the optical laminate 100A, a support layer 50 is provided directly adjacent to the surface adhesive layer 42 side of the polarizing member 10, and the surface adhesive layer 42 is disposed directly adjacent to the support layer 50. The polarizing member 10 may correspond to a polarizing member that may be included in the display element 12 of the display system 2. The first phase difference member 20 includes a first λ / 4 member 20a, and may correspond to the first phase difference member 20 of the display system 2. For example, when the display element 12 is a liquid crystal display, the optical laminate 100A can be attached to the front (viewing side) of a liquid crystal cell via the surface adhesive layer 42, so that the polarizing member 10 can be used as the viewing side polarizing member of a liquid crystal panel including a back side polarizing member, a liquid crystal cell, and a viewing side polarizing member in that order.

[0028] FIG. 3 is a schematic cross-sectional view showing a schematic configuration of an optical laminate according to one embodiment of the present invention. The optical laminate 100B includes a surface adhesive layer 42, a second phase difference member 60, a third adhesive layer 48, a polarizing member 10, a first adhesive layer 44, a first phase difference member 20, a second adhesive layer 46, and a protective member 30, in this order. In the optical laminate 100B, a support layer 50 is provided directly adjacent to the third adhesive layer 48 side of the polarizing member 10, and the third adhesive layer 48 is disposed directly adjacent to the support layer 50. The polarizing member 10 may correspond to a polarizing member that may be included in the display element 12 of the display system 2. The first phase difference member 20 includes a first λ / 4 member 20a, and may correspond to the first phase difference member 20 of the display system 2. The second phase difference member 60 may correspond to a phase difference member that may be included in the display element 12. For example, the second phase difference member 60 includes a λ / 4 member (also referred to as a "third λ / 4 member") 60a. The angle between the absorption axis of the polarizing member 10 and the slow axis of the third λ / 4 member is, for example, 40° to 50°, may be 42° to 48°, or may be about 45°. When the display element 12 is an organic EL display, problems such as external light reflection and background reflection due to a metal layer that may be included in the organic EL display can be solved by providing the third λ / 4 member together with the polarizing member 10 in front of the organic EL panel (on the viewing side). When the second phase difference member 60 does not include any member other than the third λ / 4 member, the second phase difference member 60 may correspond to the third λ / 4 member.

[0029] 2 and 3, the first phase difference member 20 may include a member whose refractive index characteristics show the relationship nz>nx=ny (hereinafter also referred to as "first positive C plate") in addition to the first λ / 4 member 20a. In this case, in the first phase difference member 20, it is preferable that the first λ / 4 member 20a is located closer to the polarizing member 10 than the first positive C plate. The first λ / 4 member 20a and the first positive C plate may be laminated typically via an adhesive layer.

[0030] 3, the second phase difference member 60 may include a member whose refractive index characteristics show the relationship nz>nx=ny (hereinafter also referred to as a "second positive C plate") in addition to the third λ / 4 member 60a. The third λ / 4 member 60a and the second positive C plate may be laminated typically via an adhesive layer.

[0031] <Polarizing materials> The polarizing member 10 has an absorptive polarizing film 10a, a display element side protective layer 10b arranged on the side opposite to the side where the first phase difference member 20 is arranged, and a lens unit side protective layer 10c arranged on the side where the first phase difference member 20 is arranged. Either the display element side protective layer 10b or the lens unit side protective layer 10c may be omitted depending on the purpose. Preferably, the polarizing member has an absorptive polarizing film 10a and a display element side protective layer 10b.

[0032] The absorptive polarizing film is, for example, composed of a resin film containing a dichroic material. The thickness of the absorptive polarizing film is, for example, 1 μm or more and 20 μm or less, and may be 2 μm or more and 15 μm or less, 12 μm or less, 10 μm or less, 8 μm or less, or 5 μm or less.

[0033] The absorptive polarizing film may be prepared from a single layer of resin film, or may be prepared using a laminate of two or more layers.

[0034] When preparing from a single-layer resin film, for example, an absorptive polarizing film can be obtained by subjecting a hydrophilic polymer film such as a polyvinyl alcohol (PVA)-based film, a partially formalized PVA-based film, or an ethylene-vinyl acetate copolymer-based partially saponified film to a dyeing treatment with a dichroic substance such as iodine or a dichroic dye, a stretching treatment, etc. Among them, an absorptive polarizing film obtained by dyeing a PVA-based film with iodine and uniaxially stretching it is preferable.

[0035] The dyeing with iodine is carried out, for example, by immersing the PVA film in an aqueous iodine solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching may be carried out after the dyeing treatment or while the dyeing is being carried out. Alternatively, the stretching may be followed by dyeing. If necessary, the PVA film is subjected to a swelling treatment, a crosslinking treatment, a washing treatment, a drying treatment, or the like.

[0036] Examples of the laminate produced using the laminate of two or more layers include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate. The absorptive polarizing film obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate can be produced, for example, by coating a PVA-based resin solution on the resin substrate and drying the resin substrate to form a PVA-based resin layer on the resin substrate to obtain a laminate of the resin substrate and the PVA-based resin layer; and stretching and dyeing the laminate to make the PVA-based resin layer into an absorptive polarizing film. In this embodiment, preferably, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is formed on one side of the resin substrate. The stretching typically includes immersing the laminate in an aqueous boric acid solution to stretch it. Furthermore, the stretching may further include, as necessary, stretching the laminate in air at a high temperature (for example, 95° C. or higher) before stretching in the aqueous boric acid solution. In addition, in this embodiment, the laminate is preferably subjected to a drying shrinkage treatment in which the laminate is heated while being transported in the longitudinal direction, thereby shrinking the laminate by 2% or more in the width direction. Typically, the manufacturing method of this embodiment includes subjecting the laminate to an air-assisted stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order. By introducing the auxiliary stretching, even when PVA is applied onto a thermoplastic resin, it is possible to increase the crystallinity of PVA, and to achieve high optical properties. At the same time, by increasing the orientation of PVA in advance, problems such as a decrease in the orientation or dissolution of PVA when immersed in water in the subsequent dyeing and stretching steps can be prevented, and high optical properties can be achieved. Furthermore, when the PVA-based resin layer is immersed in a liquid, the disorder of the orientation of polyvinyl alcohol molecules and the decrease in the orientation can be suppressed compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of the absorptive polarizing film obtained through treatment steps in which the laminate is immersed in a liquid, such as a dyeing treatment and an underwater stretching treatment. Furthermore, the optical properties can be improved by shrinking the laminate in the width direction through drying shrinkage treatment.The obtained laminate of resin substrate / absorptive polarizing film may be used as it is (i.e., the resin substrate may be used as a protective layer for the absorptive polarizing film), or any suitable protective layer may be laminated on the peeled surface of the resin substrate / absorptive polarizing film laminate after peeling the resin substrate from the laminate, or on the surface opposite to the peeled surface, depending on the purpose. Details of the method for producing such an absorptive polarizing film are described in, for example, JP2012-73580A and JP6470455A. The entire disclosures of these publications are incorporated herein by reference.

[0037] The display element side protective layer and the lens part side protective layer are each composed of any suitable film that can be used as a protective layer for an absorptive polarizing film. Examples of materials constituting the protective layer include cellulose resins such as triacetyl cellulose (TAC), cycloolefin resins such as polynorbornene, (meth)acrylic resins, polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyolefin resins such as polyethylene, and polycarbonate resins. Representative examples of (meth)acrylic resins include (meth)acrylic resins having a lactone ring structure. (Meth)acrylic resins having a lactone ring structure are described in, for example, JP-A-2000-230016, JP-A-2001-151814, JP-A-2002-120326, JP-A-2002-254544, and JP-A-2005-146084. These publications are incorporated herein by reference.

[0038] The thickness of the protective layer is, for example, 10 μm to 80 μm, preferably 15 μm to 70 μm, and more preferably 20 μm to 50 μm.

[0039] The orthogonal transmittance (Tc) of the absorption-type polarizing member (absorption-type polarizing film) is preferably 0.5% or less, more preferably 0.1% or less, and still more preferably 0.05% or less. The single transmittance (Ts) of the absorption-type polarizing member (absorption-type polarizing film) is, for example, 41.0% to 45.0%, preferably 42.0% or more. The degree of polarization (P) of the absorption-type polarizing member (absorption-type polarizing film) is, for example, 99.0% to 99.997%, preferably 99.9% or more.

[0040] <The first λ / 4 member> The in-plane retardation Re(550) and the wavelength dispersion characteristics of the retardation value of the first λ / 4 member 20a are as described in item A. Also, in the optical laminate, the angle formed by the slow axis of the first λ / 4 member and the absorption axis of the polarizing member is, for example, 40° to 50°, may be 42° to 48°, or may be about 45°.

[0041] The first λ / 4 member preferably exhibits a refractive index characteristic of nx > ny ≧ nz. Here, "ny = nz" includes not only the case where ny and nz are exactly equal but also the case where they are substantially equal. Therefore, the case where ny < nz may occur. The Nz coefficient of the first λ / 4 member is preferably 0.9 to 3, more preferably 0.9 to 2.5, still more preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.

[0042] The first λ / 4 member is formed of any suitable material that can satisfy the above characteristics. The first λ / 4 member can be, for example, a stretched film of a resin film or an alignment solidified layer of a liquid crystal compound.

[0043] Examples of the resin contained in the resin film include polycarbonate-based resins, polyester carbonate-based resins, polyester-based resins, polyvinyl acetal-based resins, polyarylate-based resins, cyclic olefin-based resins, cellulose-based resins, polyvinyl alcohol-based resins, polyamide-based resins, polyimide-based resins, polyether-based resins, polystyrene-based resins, and acrylic-based resins. These resins may be used alone or in combination. Examples of methods for combining include blending and copolymerization. When the first λ / 4 member exhibits reverse dispersion wavelength characteristics, a resin film containing a polycarbonate-based resin or a polyester carbonate-based resin (hereinafter, sometimes simply referred to as a polycarbonate-based resin) may be suitably used.

[0044] Any suitable polycarbonate-based resin can be used as the polycarbonate-based resin. For example, the polycarbonate-based resin contains a structural unit derived from a fluorene-based dihydroxy compound, a structural unit derived from an isosorbide-based dihydroxy compound, and a structural unit derived from at least one dihydroxy compound selected from the group consisting of alicyclic diol, alicyclic dimethanol, di-, tri- or polyethylene glycol, and alkylene glycol or spiro glycol. Preferably, the polycarbonate-based resin contains a structural unit derived from a fluorene-based dihydroxy compound, a structural unit derived from an isosorbide-based dihydroxy compound, a structural unit derived from an alicyclic dimethanol and / or a structural unit derived from a di-, tri- or polyethylene glycol; more preferably, it contains a structural unit derived from a fluorene-based dihydroxy compound, a structural unit derived from an isosorbide-based dihydroxy compound, and a structural unit derived from a di-, tri- or polyethylene glycol. The polycarbonate-based resin may contain a structural unit derived from another dihydroxy compound as necessary. Details of polycarbonate-based resins that can be suitably used for the first λ / 4 member and methods for forming the first λ / 4 member are described, for example, in JP 2014-10291 A, JP 2014-26266 A, JP 2015-212816 A, JP 2015-212817 A, and JP 2015-212818 A, and the descriptions in these publications are incorporated herein by reference.

[0045] The thickness of the first λ / 4 member made of a stretched resin film is, for example, 10 μm to 100 μm, preferably 10 μm to 70 μm, and more preferably 20 μm to 60 μm.

[0046] The above-mentioned liquid crystal compound alignment solidified layer is a layer in which the liquid crystal compound is aligned in a predetermined direction within the layer, and the alignment state is fixed. The "alignment solidified layer" is a concept that includes an alignment solidified layer obtained by hardening a liquid crystal monomer as described later. In the first λ / 4 member, typically, rod-shaped liquid crystal compounds are aligned in the slow axis direction of the first λ / 4 member (homogeneous alignment). Examples of rod-shaped liquid crystal compounds include liquid crystal polymers and liquid crystal monomers. The liquid crystal compound is preferably polymerizable. If the liquid crystal compound is polymerizable, the alignment state of the liquid crystal compound can be fixed by aligning the liquid crystal compound and then polymerizing it.

[0047] The alignment solidified layer of the liquid crystal compound (liquid crystal alignment solidified layer) can be formed by performing an alignment treatment on the surface of a predetermined substrate, applying a coating liquid containing a liquid crystal compound to the surface to align the liquid crystal compound in a direction corresponding to the alignment treatment, and fixing the alignment state. Any appropriate alignment treatment can be adopted as the alignment treatment. Specifically, mechanical alignment treatment, physical alignment treatment, and chemical alignment treatment can be mentioned. Specific examples of mechanical alignment treatment include rubbing treatment and stretching treatment. Specific examples of physical alignment treatment include magnetic field alignment treatment and electric field alignment treatment. Specific examples of chemical alignment treatment include oblique deposition method and photoalignment treatment. As the treatment conditions of various alignment treatments, any appropriate conditions can be adopted depending on the purpose.

[0048] The alignment of the liquid crystal compound is performed by treating the liquid crystal compound at a temperature at which the liquid crystal compound exhibits a liquid crystal phase according to the type of liquid crystal compound. By performing such temperature treatment, the liquid crystal compound takes on a liquid crystal state and is aligned according to the alignment treatment direction of the substrate surface.

[0049] In one embodiment, the alignment state is fixed by cooling the liquid crystal compound aligned as described above. When the liquid crystal compound is polymerizable or crosslinkable, the alignment state is fixed by subjecting the liquid crystal compound aligned as described above to a polymerization treatment or crosslinking treatment.

[0050] As the liquid crystal compound, any suitable liquid crystal polymer and / or liquid crystal monomer is used. The liquid crystal polymer and the liquid crystal monomer may be used alone or in combination. Specific examples of the liquid crystal compound and the method for producing the liquid crystal alignment solidified layer are described in, for example, JP 2006-163343 A, JP 2006-178389 A, and WO 2018 / 123551 A. The descriptions in these publications are incorporated herein by reference.

[0051] The thickness of the first λ / 4 member constituted by the liquid crystal alignment solidified layer is, for example, 1 μm to 10 μm, preferably 1 μm to 8 μm, more preferably 1 μm to 6 μm, and further preferably 1 μm to 4 μm.

[0052] <First positive C plate> The thickness direction retardation Rth(550) of the first positive C plate is preferably -20nm to -200nm, more preferably -30nm to -180nm, further preferably -40nm to -160nm, and particularly preferably -50nm to -140nm. Here, "nx=ny" includes not only the case where nx and ny are strictly equal, but also the case where nx and ny are substantially equal. The in-plane retardation Re(550) of the first positive C plate is, for example, less than 10nm.

[0053] The first positive C plate may be formed of any suitable material, but is preferably composed of a film containing a liquid crystal material fixed in homeotropic alignment. The liquid crystal material (liquid crystal compound) that can be homeotropically aligned may be a liquid crystal monomer or a liquid crystal polymer. Specific examples of such liquid crystal compounds and methods for forming a positive C plate include the liquid crystal compounds and methods for forming the retardation layer described in

[0020] to

[0028] of JP-A-2002-333642. In this case, the thickness of the first positive C plate is preferably 0.5 μm to 5 μm.

[0054] <Third λ / 4 component> The in-plane retardation Re(550) of the third λ / 4 member 60a is, for example, 100 nm to 190 nm, and may be 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. The third λ / 4 member preferably exhibits an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light. The third λ / 4 member's Re(450) / Re(550) may be, for example, 0.75 or more and less than 1, or 0.8 or more and 0.95 or less. The third λ / 4 member preferably exhibits a refractive index characteristic of nx>ny≧nz. The third λ / 4 member preferably has an Nz coefficient of 0.9 to 3, more preferably 0.9 to 2.5, even more preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.

[0055] The third λ / 4 member is formed of any appropriate material that can satisfy the above characteristics. The third λ / 4 member can be, for example, a stretched resin film or an oriented and solidified layer of a liquid crystal compound. The same explanation as for the first λ / 4 member can be applied to the third λ / 4 member composed of a stretched resin film or an oriented and solidified layer of a liquid crystal compound. The first λ / 4 member and the third λ / 4 member may be members having the same configuration (e.g., forming material, thickness, optical properties, etc.) or may be members having different configurations.

[0056] <Second positive C plate> The thickness direction retardation Rth(550) of the second positive C plate is preferably -20nm to -200nm, more preferably -30nm to -180nm, further preferably -40nm to -160nm, and particularly preferably -50nm to -140nm. Here, "nx=ny" includes not only the case where nx and ny are strictly equal, but also the case where nx and ny are substantially equal. The in-plane retardation Re(550) of the second positive C plate is, for example, less than 10nm.

[0057] The second positive C plate may be formed of any suitable material, but is preferably composed of a film containing a liquid crystal material fixed in a homeotropic orientation. The same explanation as for the first positive C plate can be applied to the forming material and forming method of such a second positive C plate. The first positive C plate and the second positive C plate may be members having the same configuration (e.g., forming material, thickness, optical properties, etc.) or may be members having different configurations.

[0058] <Protective materials> The protective member 30 typically includes a substrate. The substrate may be made of any appropriate film. Examples of materials that are the main components of the film that constitutes the substrate include cellulose-based resins such as triacetyl cellulose (TAC), polyester-based, polyvinyl alcohol-based, polycarbonate-based, polyamide-based, polyimide-based, polyethersulfone-based, polysulfone-based, polystyrene-based, cycloolefin-based such as polynorbornene, polyolefin-based, (meth)acrylic-based, acetate-based, and other resins. The thickness of the substrate is preferably 5 μm to 80 μm, more preferably 10 μm to 50 μm, and even more preferably 15 μm to 40 μm.

[0059] The protective member 30 is preferably a laminated film having a substrate and a surface treatment layer. The protective member having the surface treatment layer can be disposed so that the substrate is located on the first retardation member 20 side. The thickness of the surface treatment layer is, for example, 0.5 μm to 10 μm, and may be 1 μm to 7 μm, or may be 2 μm to 5 μm. The surface treatment layer may have any appropriate function. For example, the surface treatment layer preferably has an antireflection function.

[0060] <Adhesive layer> As the adhesive layer, typically, an adhesive layer or a pressure-sensitive adhesive layer is used. The surface adhesive layer for bonding the optical laminate itself to another member is preferably a pressure-sensitive adhesive layer. The adhesive layer for bonding adjacent members together may be an adhesive layer or a pressure-sensitive adhesive layer. In one embodiment, at least one selected from the first adhesive layer, the second adhesive layer, and the third adhesive layer may be a pressure-sensitive adhesive layer, and two or three may be pressure-sensitive adhesive layers. The adhesive layer disposed directly adjacent to the support layer is preferably a pressure-sensitive adhesive layer, since it can suitably satisfy the storage modulus described below.

[0061] The storage modulus (23°C) of the adhesive layer disposed directly adjacent to the support layer is, for example, 0.01 MPa to 1 MPa, preferably 0.05 MPa to 0.5 MPa, and more preferably 0.08 MPa to 0.2 MPa. By using the surface to be bonded to the adhesive layer having such a storage modulus as the support layer, the effects of the present invention can be suitably obtained. The storage modulus can be measured, for example, by the following measurement method. <Method for measuring storage modulus> A laminate of multiple pressure-sensitive adhesive layers with a thickness of approximately 1.5 mm is used as a measurement sample. Dynamic viscoelasticity measurement is performed under the following conditions using an "Advanced Rheometric Expansion System (ARES)" manufactured by Rheometric Scientific as a measurement device, and the storage modulus at 23°C is read from the measurement results. (Measurement conditions) Deformation mode: Torsion Frequency: 1Hz Crimping load: 100g Heating rate: 5℃ / min Temperature range: -50℃~150℃ Shape: Parallel plate, 8.0mmφ

[0062] The adhesive layer may be formed of any suitable adhesive. Specific examples include acrylic adhesives, rubber adhesives, silicone adhesives, polyester adhesives, urethane adhesives, epoxy adhesives, and polyether adhesives. The adhesive contains a base resin, and may further contain various additives, such as crosslinking agents, polymerization initiators, polymerization catalysts, crosslinking catalysts, silane coupling agents, tackifiers, plasticizers, softeners, deterioration inhibitors, fillers, colorants, ultraviolet absorbers, antioxidants, surfactants, antistatic agents, etc., depending on the purpose, within a range that does not impair the characteristics of the present invention. By adjusting the type, combination, and compounding ratio of monomers forming the base resin of the adhesive; the type, combination, and compounding amount of additives (e.g., crosslinking agents); reaction temperature; reaction time, etc., an adhesive having desired characteristics according to the purpose can be prepared. The base resin of the adhesive may be used alone or in combination of two or more. As the base resin, an acrylic resin is preferably used. Specifically, the pressure-sensitive adhesive layer is preferably composed of an acrylic pressure-sensitive adhesive containing a (meth)acrylic polymer as a main component.

[0063] The thickness of the pressure-sensitive adhesive layer is, for example, 3 μm or more, preferably 5 μm or more, and for example, 50 μm or less, preferably 30 μm or less.

[0064] The adhesive layer can be formed by coating and drying an adhesive composition containing a base resin, additives such as a crosslinking agent, and a solvent. For example, the adhesive composition can be coated on a substrate such as a release liner and dried to form an adhesive layer, which can then be transferred to a target member. For example, the adhesive composition can be directly coated on a target member and dried to form an adhesive layer. Drying is typically performed by heating.

[0065] The adhesive layer may be formed of any suitable adhesive. For example, the adhesive irreversibly changes from a liquid to a solid state during the process of forming the adhesive layer, has fluidity when applied, and has the property of being cured by a curing treatment (for example, irradiation with active energy rays, heating). As the adhesive, a curable adhesive is preferably used. As the curable adhesive, an ultraviolet-curable adhesive is preferably used.

[0066] The ultraviolet-curable adhesive contains a curable monomer such as a compound having a (meth)acryloyl group or a compound having a vinyl group. A compound having a (meth)acryloyl group is preferably used. Here, the (meth)acryloyl group refers to an acryloyl group and / or a methacryloyl group.

[0067] The thickness of the adhesive layer is, for example, 0.1 μm to 5 μm, preferably 0.5 μm to 4 μm, and more preferably 1 μm to 3 μm.

[0068] <Support layer> The position of the support layer 50 in the optical laminate is not limited to the illustrated example. The support layer 50 can be disposed directly adjacent to at least one adhesive layer selected from all adhesive layers of the optical laminate. For example, the support layer can be disposed directly adjacent to at least one adhesive layer selected from the surface adhesive layer, the first adhesive layer, the second adhesive layer, and the third adhesive layer if present, preferably a pressure-sensitive adhesive layer. Since defects present in a position close to the display element tend to have a large effect on visibility, the support layer can be disposed directly adjacent to at least one selected from the surface adhesive layer, the first adhesive layer, and the third adhesive layer. The number of support layers provided in the optical laminate is, for example, 1 to 3.

[0069] The indentation modulus of the support layer is, for example, 1 GPa or more, preferably 2 GPa or more, more preferably 3 GPa to 12 GPa, and even more preferably 4 GPa to 10 GPa. By disposing the adhesive layer directly adjacent to the support layer having such an indentation modulus, the generation of air bubbles can be suitably suppressed. The indentation modulus is a value obtained by a nanoindentation method.

[0070] The hardness of the support layer is, for example, 0.05 GPa or more, preferably 0.1 GPa or more, more preferably 0.2 GPa to 2 GPa, and further preferably 0.3 GPa to 1 GPa. The above hardness is a value obtained by a nanoindentation method.

[0071] The amount of plastic deformation of the support layer is, for example, 200 nm or less, preferably 0 nm to 150 nm, more preferably 10 nm to 100 nm, and further preferably 20 nm to 80 nm. The amount of plastic deformation is a value obtained by a nanoindentation method.

[0072] The support layer may be made of any suitable material capable of forming a layer having the above-mentioned properties. For example, the support layer is a cured layer of a curable material. In one embodiment, the support layer is a hard coat layer, and may be formed by applying a support layer forming material (hard coat layer forming material) to a member (e.g., a polarizing member, a first phase difference member, a second phase difference member, a protective member) to which the adhesive layer is to be laminated, and curing the applied layer. The support layer forming material typically includes a curable compound as a layer forming component. Examples of the curing mechanism of the curable compound include a thermosetting type and a photocuring type. Examples of the curable compound include a monomer, an oligomer, and a prepolymer. Preferably, a polyfunctional monomer or oligomer is used as the curable compound. Examples of the polyfunctional monomer or oligomer include a monomer or oligomer having two or more (meth)acryloyl groups, a urethane (meth)acrylate or an oligomer of a urethane (meth)acrylate, an epoxy-based monomer or oligomer, and a silicone-based monomer or oligomer.

[0073] In one embodiment, the support layer is provided directly adjacent to the polarizing member, and is preferably provided directly adjacent to the side opposite to the side of the polarizing member where the first phase difference member is disposed. In this embodiment, the support layer can be typically formed on the surface of the protective layer of the absorptive polarizing film. When a thin absorptive polarizing film and a protective layer are bonded together via an adhesive layer, unevenness may occur on the surface of the polarizing member (protective layer surface) obtained due to shrinkage during curing. In contrast, the occurrence of such unevenness can be suppressed by bonding a protective layer with a support layer, on which a support layer has been formed in advance, to the absorptive polarizing film via an adhesive layer. Alternatively, when the absorptive polarizing film and the protective layer are bonded together by roll-to-roll bonding, unevenness may occur in the obtained polarizing member due to process foreign matter. In contrast, by forming a support layer on the surface of the protective layer of a polarizing member including an absorptive polarizing film and a protective layer bonded together via an adhesive layer, the unevenness can be filled to form a flat surface. By providing a support layer directly adjacent to the polarizing member in this manner, unevenness on the surface of the polarizing member can be suppressed, and the generation of air bubbles at the lamination interface between the uneven surface and an adhesive layer (e.g., a pressure-sensitive adhesive layer) can be effectively suppressed.

[0074] The thickness of the support layer is, for example, 0.5 μm to 15 μm, preferably 1 μm to 12 μm, and more preferably 3 μm to 10 μm.

[0075] <Method of producing optical laminate> The optical laminate can be produced, for example, by laminating each member via an adhesive layer. In one embodiment, the optical laminate can be produced by a method including producing a support layer-attached polarizing member having a polarizing member having an absorptive polarizing film and a protective layer arranged on at least one side of the film, and a support layer arranged directly adjacent to the protective layer of the polarizing member, and laminating an adhesive layer (for example, a pressure-sensitive adhesive layer) on the support layer side of the support layer-attached polarizing member. EXAMPLES

[0076] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. The thickness and retardation values ​​are values ​​measured by the following measurement methods. Unless otherwise specified, "parts" and "%" are based on weight. <Thickness> The thickness of 10 μm or less was measured using a scanning electron microscope (manufactured by JEOL, product name "JSM-7100F"), and the thickness of more than 10 μm was measured using a digital micrometer (manufactured by Anritsu, product name "KC-351C"). <Phase difference value> The phase difference value at each wavelength at 23° C. was measured using a phase difference measuring device (KOBRA manufactured by Oji Scientific Instruments Co., Ltd.).

[0077] [Manufacturing Example 1: Production of λ / 4 component A] Polymerization was carried out using a batch polymerization apparatus consisting of two vertical reactors equipped with stirring blades and a reflux condenser controlled at 100° C. Bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane 29.60 parts by mass (0.046 mol), isosorbide (ISB) 29.21 parts by mass (0.200 mol), spiroglycol (SPG) 42.28 parts by mass (0.139 mol), diphenyl carbonate (DPC) 63.77 parts by mass (0.298 mol), and calcium acetate monohydrate 1.19×10 as a catalyst. -2 Part of mass (6.78×10 -5mol) was charged. After the inside of the reactor was purged with nitrogen under reduced pressure, heating was performed with a heat medium, and stirring was started when the inside temperature reached 100 ° C. 40 minutes after the start of the temperature increase, the inside temperature was reached 220 ° C., and while controlling to maintain this temperature, the pressure was reduced and 90 minutes after reaching 220 ° C., the pressure was reduced to 13.3 kPa. Phenol vapor by-produced with the polymerization reaction was led to a reflux condenser at 100 ° C., a small amount of monomer components contained in the phenol vapor were returned to the reactor, and the uncondensed phenol vapor was led to a condenser at 45 ° C. and recovered. Nitrogen was introduced into the first reactor to restore the pressure to atmospheric pressure, and the oligomerized reaction liquid in the first reactor was transferred to the second reactor. Next, the temperature increase and pressure reduction in the second reactor were started, and the inside temperature was set to 240 ° C. and the pressure to 0.2 kPa in 50 minutes. Thereafter, polymerization was allowed to proceed until the specified stirring power was reached. When the predetermined power was reached, nitrogen was introduced into the reactor to restore pressure, and the produced polyester carbonate resin was extruded into water and the strands were cut to obtain pellets.

[0078] The obtained polyester carbonate resin (pellets) was vacuum-dried at 80°C for 5 hours, and then a long resin film having a thickness of 135μm was produced using a film-forming device equipped with a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 200mm, setting temperature: 250°C), a chill roll (setting temperature: 120-130°C) and a winder. The obtained long resin film was stretched in the width direction at a stretching temperature of 143°C and a stretching ratio of 2.8 times to obtain a stretched film (λ / 4 member A) having a thickness of 48μm. The Re(550) of the obtained stretched film was 143nm, Re(450) / Re(550) was 0.86, and the Nz coefficient was 1.12.

[0079] [Manufacturing Example 2: Preparation of protective material A] The anti-reflection layer-forming material shown below was applied to an acrylic film (thickness 40 μm) having a lactone ring structure and heated at 80° C. for 1 minute. After heating, the coating layer was irradiated with a high-pressure mercury lamp with an integrated light quantity of 300 mJ / cm 2 2 The coating layer was cured by irradiation with ultraviolet light of 1000 ohms, thereby obtaining a protective member A having an antireflection layer having a thickness of 0.1 μm.

[0080] (Anti-reflection layer forming material) 100 parts by weight of a polyfunctional acrylate mainly composed of pentaerythritol triacrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd., trade name "Viscoat #300", solid content 100% by weight), 150 parts by weight of hollow nanosilica particles (manufactured by JGC Catalysts and Chemicals Co., Ltd., trade name "Surulia 5320", solid content 20% by weight, weight average particle diameter 75 nm), 50 parts by weight of solid nanosilica particles (manufactured by Nissan Chemical Industries, Ltd., trade name "MEK-2140Z-AC", solid content 30% by weight, weight average particle diameter 10 nm), 12 parts by weight of a fluorine-containing additive (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KY-1203", solid content 20% by weight), and 3 parts by weight of a photopolymerization initiator (manufactured by BASF, trade name "OMNIRAD907", solid content 100% by weight) were mixed. To the mixture was added a mixed solvent of TBA (tertiary butyl alcohol), MIBK (methyl isobutyl ketone) and PMA (propylene glycol monomethyl ether acetate) in a weight ratio of 60:25:15 as a dilution solvent until the total solids content was 4% by weight, and the mixture was stirred to prepare an anti-reflection layer forming material.

[0081] [Production Example 3: Preparation of polarizing member A with support layer] 1. Preparation of Absorptive Polarizing Film The thermoplastic resin substrate was a long amorphous isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) having a water absorption rate of 0.75% and a Tg of about 75° C. One side of the resin substrate was subjected to a corona treatment. A PVA aqueous solution (coating solution) was prepared by adding 13 parts by weight of potassium iodide to 100 parts by weight of a PVA-based resin made by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "GOHSEFFIMER Z410") in a ratio of 9:1, and dissolving the mixture in water. The above PVA aqueous solution was applied to the corona-treated surface of a resin substrate and dried at 60° C. to form a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate. The obtained laminate was uniaxially stretched at its free end to 2.4 times its original size in the machine direction (longitudinal direction) between rolls with different peripheral speeds in an oven at 130° C. (auxiliary air stretching treatment). Next, the laminate was immersed in an insolubilizing bath (a boric acid aqueous solution obtained by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilizing treatment). Next, the film was immersed in a dye bath (an aqueous iodine solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single transmittance (Ts) of the final polarizing film would be 43.0% (dyeing process). Next, the piece was immersed in a crosslinking bath (a boric acid aqueous solution obtained by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment). Thereafter, the laminate was immersed in an aqueous boric acid solution (boric acid concentration 4.0 wt %, potassium iodide 5.0 wt %) at a liquid temperature of 70°C and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds so that the total stretch ratio was 5.5 times (underwater stretching treatment). Thereafter, the laminate was immersed in a cleaning bath (an aqueous solution obtained by mixing 4 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment). Thereafter, while drying in an oven maintained at 90°C, the laminate was brought into contact with a SUS heated roll whose surface temperature was maintained at 75°C for approximately 2 seconds (drying shrinkage treatment). The shrinkage rate of the laminate in the width direction due to the drying shrinkage treatment was 5.2%. In this manner, an absorptive polarizing film having a thickness of 5 μm was formed on the resin substrate.

[0082] 2. Preparation of protective layer with support layer The following support layer forming material was applied to an acrylic film (thickness 40 μm) having a lactone ring structure and heated at 90°C for 1 minute. After heating, the applied layer was irradiated with a high-pressure mercury lamp with an integrated light intensity of 300 mJ / cm 2 The coating layer was cured by irradiating it with ultraviolet light of 1000 nm, thereby obtaining an acrylic film having a 7 μm-thick support layer (hard coat layer) formed on one side thereof as a support layer-attached protective layer.

[0083] (Support layer forming material) A support layer forming material was prepared by mixing 50 parts of urethane acrylic oligomer (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK Oligo UA-53H"), 30 parts of a multifunctional acrylate whose main component is pentaerythritol triacrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd., product name "Viscoat #300"), 20 parts of 4-hydroxybutyl acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd.), 1 part of a leveling agent (manufactured by DIC Corporation, "GRANDIC PC4100") and 3 parts of a photopolymerization initiator (manufactured by Ciba Japan, "Irgacure 907") and diluting with methyl isobutyl ketone to a solids concentration of 50%.

[0084] 3. Preparation of Polarizing Component The above-mentioned protective layer with support layer was attached to the surface of the absorptive polarizing film of the laminate of [resin substrate / absorptive polarizing film] obtained in 1 above, via an ultraviolet-curable adhesive, so that the acrylic film was on the absorptive polarizing film side. Specifically, the curable adhesive was applied to a thickness of 1.0 μm, and the layers were attached using a rolling machine. Thereafter, UV rays were irradiated from the protective layer with support layer side to cure the adhesive. Next, the resin substrate was peeled off from the absorptive polarizing film, and an acrylic film (thickness 40 μm) having a lactone ring structure was attached to the peeled surface in the same manner as above. In this way, a polarizing member with support layer A having a structure of [support layer / acrylic film / absorptive polarizing film / acrylic film] was obtained. In the polarizing member with support layer A, the support layer is provided directly adjacent to the polarizing member (more specifically, directly adjacent to the surface of the protective layer).

[0085] [Production Example 4A: Preparation of Adhesive Layer A] A monomer mixture containing 91.5 parts of butyl acrylate, 3 parts of acrylic acid, 0.5 parts of 4-hydroxybutyl acrylate, and 5 parts of acryloylmorpholine was charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Furthermore, 0.1 parts of 2,2'-azobisisobutyronitrile as a polymerization initiator was charged together with 100 parts of ethyl acetate for 100 parts of this monomer mixture, and nitrogen gas was introduced while gently stirring to replace the atmosphere in the flask with nitrogen. The liquid temperature in the flask was kept at about 55°C and a polymerization reaction was carried out for 8 hours. Next, ethyl acetate was added to the obtained reaction liquid to adjust the solid concentration to 12% by weight, and a solution of an acrylic polymer with a weight average molecular weight (Mw) of 2.5 million was prepared. A pressure-sensitive adhesive composition was prepared by blending 100 parts of the solid content of the obtained acrylic polymer solution with 0.3 parts of a peroxide-based crosslinking agent, benzoyl peroxide (product name: Niper BMT, manufactured by Nippon Oil & Fats Co., Ltd.), 0.2 parts of a trimethylolpropane / tolylene diisocyanate adduct (product name: Coronate L, manufactured by Tosoh Corporation), and 0.2 parts of a silane coupling agent (product name: KBM403, manufactured by Shin-Etsu Chemical Co., Ltd.). The obtained adhesive composition was applied to the release surface of a release liner which was a PET film whose release surface had been treated with a release agent, and then dried to form an adhesive layer A having a thickness of 5 μm.

[0086] [Production Example 4B: Preparation of Adhesive Layer B] A monomer mixture containing 94.9 parts by weight of butyl acrylate, 5 parts by weight of acrylic acid, and 0.1 parts by weight of 2-hydroxyethyl acrylate was charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Furthermore, 0.3 parts by weight of dibenzoyl peroxide as a polymerization initiator was charged together with ethyl acetate for 100 parts of this monomer mixture, and nitrogen gas was introduced while gently stirring to replace the atmosphere in the flask with nitrogen. The liquid temperature in the flask was kept at about 60°C and a polymerization reaction was carried out for 7 hours. Next, ethyl acetate was added to the obtained reaction liquid to adjust the solid concentration to 30% by weight, and a solution of an acrylic polymer with a weight average molecular weight (Mw) of 2.2 million was prepared. A pressure-sensitive adhesive composition was prepared by blending 100 parts of the solid content of the obtained acrylic polymer solution with 0.2 parts of a peroxide-based crosslinking agent, benzoyl peroxide (product name: Niper BMT, manufactured by Nippon Oil & Fats Co., Ltd.), 0.6 parts of a trimethylolpropane / tolylene diisocyanate adduct (product name: Coronate L, manufactured by Tosoh Corporation), and 0.2 parts of a silane coupling agent (product name: KBM403, manufactured by Shin-Etsu Chemical Co., Ltd.). The obtained adhesive composition was applied to the release surface of a release liner which was a PET film whose release surface had been treated with a release agent, and then dried to form an adhesive layer B having a thickness of 15 μm.

[0087] [Example 1] The adhesive layer B was attached together with a release liner to both sides of the λ / 4 member A as a second retardation member. The release liner on one side was peeled off, and the exposed adhesive layer B was attached to the support layer side surface of the support layer-attached polarizing member A, to obtain a laminate 1 having a laminated structure of [release liner / adhesive layer B / second retardation member / adhesive layer B / support layer / polarizing member]. At this time, the lamination was performed such that the absorption axis of the absorptive polarizing film and the slow axis of the λ / 4 member A formed an angle of 45°.

[0088] The protective member A was attached to one side of the λ / 4 member A as a first retardation member via the adhesive layer B. Here, the acrylic film of the protective member A was attached to the λ / 4 member A side. This resulted in a laminate 2 having a laminated structure of [first retardation member / adhesive layer B / protective member A].

[0089] The laminate 2 was attached to the polarizing member side of the laminate 1 via the pressure-sensitive adhesive layer A. At this time, the laminate 2 was attached so that the first retardation member of the laminate 2 was located on the pressure-sensitive adhesive layer A side, and the angle between the slow axis of the λ / 4 member A of the laminate 1 and the slow axis of the λ / 4 member A of the laminate 2 was 0°. This resulted in an optical laminate A having a laminated structure of [release liner / pressure-sensitive adhesive layer B / second retardation member / pressure-sensitive adhesive layer B / support layer / polarizing member / pressure-sensitive adhesive layer A / first retardation member / pressure-sensitive adhesive layer B / protective member A]. In the optical laminate A, a support layer is provided directly adjacent to the protective layer of the absorptive polarizing film, and a pressure-sensitive adhesive layer B is disposed directly adjacent to the support layer.

[0090] <Air bubble evaluation> When the obtained optical laminate A was observed under a microscope, it was found that air bubbles of 10 μm or more were generated at the interface between the support layer and the pressure-sensitive adhesive layer B, with 1 bubble per 100 cm 2 This was within the practically acceptable range.

[0091] <Evaluation of supporting layer characteristics> The support layer-attached polarizing member A was cut into a 10 mm×10 mm square to prepare a measurement sample. Using the measurement sample, nanoindentation measurement was performed on the support layer under the following conditions. Measuring device: Hysitron Inc., product name "Triboindenter" ·Indenter used: Berkovich (triangular pyramid type) Measurement method: Single indentation measurement ·Measurement temperature: Room temperature (approx. 25℃) Indentation depth setting: 200nm Push-in speed: 20nm / s

[0092] From the measurement results, the indentation modulus (S√π / 2√A), hardness (Pmax / A), and plastic deformation were calculated using the software (triboscan) attached to the measuring device (S: contact stiffness, A: contact projected area, Pmax: maximum load). The average values ​​of N=3 were taken as the indentation modulus, hardness, and plastic deformation of the support layer. As a result, the indentation modulus of the support layer was 6.01 GPa, the hardness was 0.383 GPa, and the plastic deformation was 47.0 nm.

[0093] The present invention is not limited to the above-described embodiment, and various modifications are possible. For example, the above-described embodiment may be replaced with a configuration that is substantially the same as the configuration shown in the above-described embodiment, a configuration that provides the same action and effect, or a configuration that can achieve the same purpose. [Industrial Applicability]

[0094] The optical laminate according to the embodiment of the present invention can be suitably used in a display system such as VR goggles, for example. [Explanation of symbols]

[0095] 2 display system, 4 lens portion, 12 display element, 14 reflective polarizing member, 16 first lens portion, 18 half mirror, 20 first phase difference member, 22 second phase difference member, 24 second lens portion, 30 protective member, 42 surface adhesive layer, 44 first adhesive layer, 46 second adhesive layer, 48 third adhesive layer, 50 second phase difference member, 60 support layer, 100 optical laminate

Claims

1. An optical laminate comprising a polarizing member having an absorptive polarizing film and a protective layer disposed on at least one side of the absorptive polarizing film, and a first phase difference member, The optical laminate further includes a support layer having an indentation elastic modulus of 1 GPa or more, an adhesive layer disposed directly adjacent to the support layer; Optical laminate.

2. The optical laminate according to claim 1 , comprising, in this order, a surface adhesive layer, the polarizing member, a first adhesive layer, the first phase difference member, a second adhesive layer, and a protective member.

3. The optical stack of claim 2 , wherein at least one selected from the surface adhesive layer, the first adhesive layer, and the second adhesive layer is disposed directly adjacent to the support layer.

4. The optical laminate according to claim 1, comprising, in this order, a surface adhesive layer, a second phase difference member, a third adhesive layer, the polarizing member, a first adhesive layer, the first phase difference member, a second adhesive layer, and a protective member.

5. The optical laminate of claim 4 , wherein at least one selected from the surface adhesive layer, the first adhesive layer, the second adhesive layer, and the third adhesive layer is disposed directly adjacent to the support layer.

6. The optical laminate according to claim 1 , wherein the support layer is a hard coat layer.

7. The optical laminate according to claim 1, wherein the support layer has a thickness of 0.5 μm to 15 μm.

8. The optical laminate according to claim 1 , wherein the support layer is provided directly adjacent to the polarizing member on the side opposite to the side on which the first phase difference member is disposed.

9. 2. The optical laminate according to claim 1, wherein the adhesive layer disposed directly adjacent to the support layer has an elastic modulus of 0.01 MPa to 1 MPa.

10. A display system comprising the optical laminate according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Optical laminate

    JP2012234165A

  • Optical laminate and image display device using optical laminate

    JP2020160197A

  • Polarizing plate with phase difference layer and image display device

    JP2021099531A

  • Laminate for organic el displays and circular polarizing plate used therefor

    JP2021103286A