Method for producing diamond abrasive grains
Ultrasonic treatment of diamond abrasive grains controls internal stress, improving microfragility and crystallinity, addressing the inconsistency in existing manufacturing methods.
Patent Information
- Application Number
- JP2023050139
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing methods for manufacturing diamond abrasive grains fail to effectively control internal stress, leading to inconsistent microfragility, which affects their processing efficiency and suitability for different materials.
Applying ultrasonic waves to diamond abrasive grains to control internal stress, shifting the Raman peak position and altering microfragility, allowing for the production of diamond abrasive grains with desired properties.
Ultrasonic treatment enables the production of diamond abrasive grains with controlled microfragility and improved crystallinity, enhancing their processing efficiency and suitability for various materials.
Smart Images

Figure 2024139272000001
Abstract
Description
[Technical field]
[0001] The technology disclosed herein relates to a method for producing diamond abrasive grains. [Background technology]
[0002] In recent years, diamond abrasive grains have been widely used for grinding and polishing various materials. These diamond abrasive grains are required to have appropriate micro-friability according to the object to be processed. For example, diamond abrasive grains that frequently break into tiny scales during processing (high micro-friability) have excellent processing efficiency because they can maintain a sharp cutting edge. On the other hand, diamond abrasive grains with low micro-friability have excellent strength and can be used to properly process high-hardness products.
[0003] It is also known that diamond abrasive grains tend to fracture as their internal stress (tensile stress) increases. Here, the internal stress of diamond abrasive grains can be evaluated based on Raman spectroscopy. Specifically, when the Raman spectrum of diamond abrasive grains is obtained, a peak due to the lattice vibration of diamond crystals is observed at 1333 cm -1 The Raman peak position is confirmed near the center of the diamond abrasive grain. The diamond abrasive grain has the Raman peak position shifted to the low wavenumber side due to the introduction of internal stress or the inclusion of impurities in the crystal. Non-Patent Document 1 reports that the diamond abrasive grain to which internal stress is introduced by heat treatment has a Raman peak position shifted to the low wavenumber side, improving micro-fracturability. [Prior art documents] [Non-patent literature]
[0004] [Non-Patent Document 1] Hitoshi Kakutani et al., "Internal Strain Distribution and Microfracture Behavior of Various Single Crystal Diamonds for Cutting Tools," Proceedings of the JSPE Spring Meeting, Academic Lecture Series, 2019, P644-P645 Summary of the Invention [Problem to be solved by the invention]
[0005] The technology disclosed herein aims to control the internal stress of diamond abrasive grains by means other than heat treatment, and to produce diamond abrasive grains having the desired micro-friability depending on the object to be processed. [Means for solving the problem]
[0006] The inventor of the present invention has conducted various experiments and studies, and has surprisingly found that when ultrasonic waves are applied to diamond abrasive grains, the internal stress of the diamond abrasive grains changes. For example, when ultrasonic waves are applied to diamond abrasive grains in which strong internal stress is introduced, the internal stress is released and the Raman peak position shifts to the high wave number side. On the other hand, when ultrasonic waves are applied to diamond abrasive grains in which weak internal stress is introduced, the internal stress is introduced and the peak position shifts to the low wave number side. The inventor of the present invention thought that by utilizing this phenomenon, it is possible to easily manufacture diamond abrasive grains that have the desired micro-fracturability according to the processing object by controlling the internal stress of the diamond abrasive grains.
[0007] The manufacturing method disclosed herein is based on the above-mentioned findings and includes an internal stress control step of applying ultrasonic waves to diamond abrasive grains. This allows the internal stress of diamond abrasive grains to be changed, so that diamond abrasive grains with desired micro-fracturability can be manufactured. In addition, the manufacturing method disclosed herein also contributes to reducing the manufacturing cost of diamond abrasive grains, since it implements ultrasonic application treatment, which is less expensive than heat treatment.
[0008] In one embodiment of the manufacturing method disclosed herein, the diamond abrasive grains before the internal stress control step have a Raman spectrum of 1325 cm -1 From 1334cm -1 The average peak position of the Raman peaks that exist in the range of 1331 cm -1 The use of such diamond abrasive grains makes it easy to control the internal stress by applying ultrasonic waves.
[0009] In one embodiment of the manufacturing method disclosed herein, the internal stress control step introduces internal stress into the diamond abrasive grains. As described above, when ultrasonic waves are applied to diamond abrasive grains with weak internal stress, internal stress is introduced, so that the micro-fracturability of the diamond abrasive grains after manufacturing can be improved. As an example, the diamond abrasive grains have an average Raman peak position of 1329 cm -1 Over 1331cm -1 By using diamond abrasive grains having such a weak internal stress, an appropriate internal stress can be introduced in the internal stress control step.
[0010] In one embodiment of the manufacturing method disclosed herein, the internal stress control step releases the internal stress of the diamond abrasive grains. As described above, when ultrasonic waves are applied to diamond abrasive grains with strong internal stress, the internal stress is released, and the micro-fracturability of the diamond abrasive grains after manufacturing can be reduced. As an example, the diamond abrasive grains have an average Raman peak position of 1329 cm -1 When diamond abrasive grains having such a high internal stress are used, the internal stress is released in the internal stress control step.
[0011] In one embodiment of the manufacturing method disclosed herein, in the internal stress control step, a diamond abrasive grain is subjected to Raman spectroscopy to detect a peak at 1325 cm -1 From 1334cm -1 The average half-width of the Raman peaks that have Raman peak positions in the range of 100 to 1500 mm is reduced. According to the inventor's experiments, it has been confirmed that when ultrasonic waves are applied to diamond abrasive grains, the crystallinity of the abrasive grains also changes, and the average half-width of the Raman peaks decreases.
[0012] In addition, when the average half-width of the Raman peak is reduced as described above, the reduction in the average half-width of the Raman peak is set to 0.05 cm. -1 It is preferable to control the internal stress to 4.8 cm or more. This can favorably improve the crystallinity of the diamond abrasive grains. In addition, the average half-width of the Raman peak after the internal stress control process is 4.8 cm or less. -1It is preferable to control the above as follows. This makes it possible to realize diamond abrasive grains with particularly excellent crystallinity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] An embodiment of the technology disclosed herein will be described below. Matters other than those specifically mentioned in this specification and necessary for implementing the technology disclosed herein can be understood as design matters of a person skilled in the art based on the conventional technology in the field. The technology disclosed herein can be implemented based on the contents disclosed in this specification and the technical common sense in the field. In this specification, the expression "A to B" indicating a numerical range means "A or more and B or less" unless otherwise specified. The drawings are drawn diagrammatically, and the dimensional relationships (length, width, thickness, etc.) in the drawings do not reflect the actual dimensional relationships.
[0014] The manufacturing method disclosed herein includes an internal stress control step of applying ultrasonic waves to diamond abrasive grains. The manufacturing method will be specifically described below.
[0015] (1) Diamond abrasive grains The diamond abrasive grains are diamond particles having a predetermined hardness. The diamond abrasive grains may be natural diamond or artificial diamond. The diamond abrasive grains may contain metal elements as impurities. Examples of the metal elements include Fe, Ni, Co, Mn, Al, Ti, Cr, Zr, and V. The diamond abrasive grains may contain impurities other than the above-mentioned metal elements. Other examples of such impurities include N, B, Si, and P. These impurities may be unavoidably mixed in during the manufacturing process, or may be intentionally introduced into the abrasive grains. The diamond abrasive grains containing these metal elements have a Raman peak position shifted to the low wave number side, improving the micro-friability, making it easier to control the micro-friability to a suitable level. A suitable example of the impurity is a metal (typically a metal particle), and examples of its constituent elements include the above-mentioned metal elements. In addition, the content of the metal element relative to the total weight (100wt%) of the diamond abrasive grain is preferably 0.1wt% or more, more preferably 0.2wt% or more, even more preferably 0.3wt% or more, and particularly preferably 0.5wt% or more. On the other hand, the upper limit of the content of the metal element is not particularly limited, and may be 3wt% or less, 2wt% or less, or 1wt% or less. The content of the metal element in the diamond abrasive grain can be measured based on X-ray fluorescence analysis (XRF: X-Ray Fluorescence).
[0016] In addition, diamond abrasive grains have a Raman spectrum of 1325 cm -1 From 1334cm -1 The average peak position of the Raman peaks that exist in the range of 1331 cm -1 Less than 1330 cm -1 In the manufacturing method disclosed herein, it is preferable to prepare diamond abrasive grains in advance, whose Raman peak position is shifted to a certain degree toward the low wavenumber side by introducing metal elements. This makes it easy to control the internal stress of diamond abrasive grains to a desired value in the internal stress control process described later.
[0017] In this specification, the "Raman peak position" is measured under the following conditions. First, a commercially available microscopic Raman spectrophotometer can be used as the measuring device. The measurement conditions are, for example, set to a measurement temperature of 24°C, a calibration sample of Si, and an excitation laser wavelength of 532 nm, and other conditions are appropriately adjusted so that clear measurement results are obtained. When Raman spectroscopy of diamond abrasive grains is performed under the above conditions, a peak due to the lattice vibration of diamond crystals appears at the Raman shift of 1333 cm. -1 A Raman spectrum present in the vicinity is detected. Then, using a predetermined waveform analysis software (such as Labspec6), baseline correction, peak search and fitting are performed on this Raman spectrum, and the position of the peak top (Raman shift) is regarded as the "Raman peak position". In this specification, the "average value of the Raman peak positions" is adopted when evaluating the internal stress of diamond abrasive grains. This "average value of the Raman peak positions" is the arithmetic average of the Raman peak positions obtained at at least 500 measurement points (the number of measurement points within the same grain is constant) for 100 or more randomly selected diamond abrasive grains.
[0018] The size of the diamond abrasive grains does not limit the technology disclosed herein, and can be changed as appropriate depending on the purpose and mode of use. For example, 50 The particle size may be 0.1 μm or more, 0.5 μm or more, 1 μm or more, 5 μm or more, or 10 μm or more. 50 The particle size may be 1000 μm or less, 500 μm or less, 250 μm or less, or 100 μm or less. 50 "Particle size" is the particle size that corresponds to a cumulative frequency of 50 volume % from the small particle side in the volume-based particle size distribution based on a general laser diffraction / light scattering method (dispersion medium: water).
[0019] The shape of the diamond abrasive grains is not particularly limited, and can be appropriately selected from conventionally known shapes. For example, the diamond abrasive grains may be spherical, plate-like, or irregular (such as confetti-like). The average aspect ratio of the diamond abrasive grains may be 1 or more and 2 or less, or 1.1 or more and 1.8 or less. The "aspect ratio" in this specification can be obtained by drawing a rectangle circumscribing the abrasive grains in an electron microscope image and calculating the ratio (b / a) of the length (a) of the short side of the rectangle to the length (b) of the long side of the rectangle. The "average aspect ratio" is the arithmetic mean value of the aspect ratios of 100 or more particles.
[0020] (2) Internal stress control process The manufacturing method disclosed herein includes an internal stress control step of applying ultrasonic waves to diamond abrasive grains. According to an experiment conducted by the present inventor, it has been confirmed that when ultrasonic waves are applied to diamond abrasive grains, the internal stress of the diamond abrasive grains changes. For example, when ultrasonic waves are applied to diamond abrasive grains in which strong internal stress has been introduced, the internal stress is released and the Raman peak position shifts to the high wave number side. On the other hand, when ultrasonic waves are applied to diamond abrasive grains in which internal stress is weak, internal stress is introduced and the Raman peak position shifts to the low wave number side. Therefore, by using the method disclosed herein, diamond abrasive grains having a desired internal stress can be easily manufactured. Although it is not intended to limit the technology disclosed herein, it is speculated that the reason for this phenomenon is that in diamond abrasive grains with small internal stress, the pressure fluctuation applied by ultrasonic application remains as stress inside the abrasive grains, while in diamond abrasive grains with large internal stress, the pressure fluctuation applied by ultrasonic application acts as a force to release the internal stress.
[0021] Considering the above-mentioned mechanism of action, it is understood that the direction of change of the Raman peak position after ultrasonic application changes depending on the Raman peak position before ultrasonic application.For example, when the Raman peak position before ultrasonic application is relatively high (internal stress is small), the Raman peak position after ultrasonic application changes toward the low wave number side (introduction of internal stress).On the other hand, when the Raman peak position before ultrasonic application is relatively low (internal stress is large), the Raman peak position after ultrasonic application changes toward the high wave number side (release of internal stress).That is, in the manufacturing method disclosed here, if the Raman peak position before ultrasonic application is known, the internal stress introduced into the diamond abrasive grain after ultrasonic application can be controlled to a specific range, and diamond abrasive grain with desired micro-fracture property can be manufactured.
[0022] In addition, in the experiment conducted by the present inventor, it has been confirmed that, depending on the type of diamond abrasive grain, the Raman peak position after ultrasonic application changes to converge to a specific range.Although this does not limit the technology disclosed here, in the test example described below, when ultrasonic waves are applied under a specific condition to a certain diamond abrasive grain, the Raman peak position of the abrasive grain changes to 1329.0-1329.5 cm -1 It has been confirmed that the Raman peak position converges to the range of 1329 cm. -1 When ultrasonic waves were applied to diamond abrasive grains with a wavelength of less than 1329 cm (high internal stress), the internal stress was released and the Raman peak position shifted to the higher wavenumber side. -1 Over 1331cm -1 When ultrasonic waves were applied to the diamond abrasive grains below (weak internal stress), internal stress was introduced and the Raman peak position shifted to the lower wavenumber side. In either case, the Raman peak position of the diamond abrasive grains after ultrasonic waves was applied was 1329.0 to 1329.5 cm -1 In this way, depending on the type of diamond abrasive grain, the internal stress of the diamond abrasive grain after application of ultrasonic waves may converge to a specific range.
[0023] In addition, an example of the ultrasonic wave application device used in this process is an ultrasonic wave application device for liquids such as an ultrasonic dispersion device or an ultrasonic cleaning device. When using this ultrasonic wave application device for liquids, it is preferable to prepare an abrasive grain dispersion liquid in which diamond abrasive grains are dispersed in a predetermined dispersion medium. This allows ultrasonic waves to be applied uniformly to the diamond abrasive grains in the abrasive grain dispersion liquid. In addition, the dispersion medium at this time is preferably a low-viscosity liquid medium. This makes it easier to apply ultrasonic waves to the diamond abrasive grains in the abrasive grain dispersion liquid. Specifically, the viscosity of the dispersion medium at room temperature (20°C) may be 100 mPa·s or less, preferably 10 mPa·s or less, more preferably 7 mPa·s or less, even more preferably 5 mPa·s or less, and particularly preferably 3 mPa·s or less. On the other hand, the lower limit of the viscosity of the dispersion medium is not particularly limited, and may be 0.05 mPa·s or more, 0.1 mPa·s or more, or 0.3 mPa·s or more. Examples of dispersion media having such a viscosity include water, ethanol, 2-propanol, 1-propanol, and ethylene glycol. The ultrasonic wave application device used in this step is not limited to the above-mentioned device for liquids, and any conventional ultrasonic wave generating device can be used without particular limitation. For example, in this step, a device that directly applies ultrasonic waves to a powder material (such as an ultrasonic sieve) can also be used.
[0024] In addition, according to the inventor's experiments, it has been confirmed that controlling the internal stress of diamond abrasive grains by ultrasonic application treatment improves the crystallinity of the abrasive grains, unlike the introduction of internal stress by heat treatment. Specifically, according to the manufacturing method disclosed here, in the internal stress control process, the 1325 cm -1 From 1334cm -1 The average half-width of the Raman peaks, which have Raman peak positions in the range of 0.05 cm, is reduced. This makes it possible to realize diamond abrasive grains with excellent crystallinity and extremely high hardness. In the internal stress control process, the reduction in the average half-width of the Raman peaks is 0.05 cm. -1 or more (preferably 0.10 cm -1 More preferably, 0.15 cm -1More preferably, 0.20 cm -1 More preferably, 0.30 cm or more -1 For example, 040cm -1 It is preferable to adjust the ultrasonic application conditions so that the half-width of the Raman peak of the diamond abrasive grains after the application of ultrasonic waves is 4.8 cm or more. This can suitably improve the crystallinity of the diamond abrasive grains. More preferably, -1 It is preferable to adjust various conditions (ultrasonic output, application time, etc.) so that the following is obtained. This allows the production of abrasive grains with particularly excellent crystallinity. In this specification, the "Raman peak half-width" refers to the wavenumber width of the peak at half the intensity of the peak top of the Raman spectrum obtained by the above-mentioned procedure. In addition, the "average Raman peak half-width" is the arithmetic average of the Raman peak half-widths obtained at at least 500 measurement points (the number of measurement points within the same particle is constant) for 100 or more randomly selected diamond abrasive grains.
[0025] In addition, it is preferable to set the ultrasonic application time appropriately depending on the amount of diamond abrasive grains to be processed. As an example, the application time is preferably 1 minute or more, more preferably 2 minutes or more, and more preferably 3 minutes or more. This allows the internal stress of the diamond abrasive grains to be sufficiently shifted to the target range. On the other hand, the upper limit of the irradiation time is preferably 30 minutes or less, more preferably 10 minutes or less, and particularly preferably 7 minutes or less. This allows the reduction in manufacturing efficiency and excessive temperature rise to be suppressed. Note that ultrasonic waves may be applied continuously, or may be applied intermittently at a predetermined interval. For example, ultrasonic application processing with an application time of 1 minute may be performed multiple times (for example, 2 to 10 times). This allows the temperature rise caused by the continuous application of ultrasonic waves to be suppressed. Note that ultrasonic application processing may be performed continuously while cooling appropriately.
[0026] The output of the ultrasonic generator is also set appropriately according to the amount of diamond abrasive grains to be processed. As the output is increased, the time required for the change of internal stress tends to be shortened. As an example, the output of the ultrasonic generator is preferably 100W or more, more preferably 200W or more, even more preferably 300W or more, and particularly preferably 400W or more. On the other hand, when using the maximum output of the ultrasonic generator, the output is preferably 2000W or less, more preferably 1500W or less, even more preferably 1000W or less, and particularly preferably 800W or less. This allows efficient processing in a short time while suppressing the destruction and overheating of the abrasive grains.
[0027] The frequency of the ultrasonic waves is preferably 15kHz or more, more preferably 20kHz or more, even more preferably 22kHz or more, and particularly preferably 25kHz or more. This allows for efficient processing of abrasive grains of various particle sizes in a short time while suppressing damage and overheating of the abrasive grains. On the other hand, the frequency of the ultrasonic waves may be 1000kHz or less, preferably 500kHz or less, more preferably 120kHz or less, even more preferably 80kHz or less, and particularly preferably 40kHz or less. This allows for efficient ultrasonic processing in a short time.
[0028] In addition, in the manufacturing method disclosed herein, before carrying out the above-mentioned internal stress control process, an inspection process may be carried out to inspect the internal stress of the diamond abrasive grain to be processed. If the internal stress of the processed object is recognized in this inspection process, the Raman peak position after the internal stress control process can be predicted. In addition, by carrying out a selection process to select diamond abrasive grains that change to a desired Raman peak position after carrying out the inspection process, diamond abrasive grains having the desired micro-fracturability can be stably manufactured. In addition, in this internal stress inspection process, it is preferable to measure the Raman peak position of the Raman spectrum based on Raman spectroscopy according to the above-mentioned procedure. This allows the internal stress of the diamond abrasive grains to be accurately inspected. In addition, this internal stress inspection process does not need to be carried out for all diamond abrasive grains supplied to the internal stress control process. For example, it is preferable to carry out the internal stress inspection process when the lot of diamond abrasive grains supplied to the internal stress control process is changed. This allows the conditions of the internal stress control process to be set to appropriate conditions without significantly reducing the manufacturing efficiency.
[0029] An embodiment of the technology disclosed herein has been described above. However, the above embodiment is not intended to limit the technology disclosed herein. In other words, the technology disclosed herein may include various modifications of the above embodiment.
[0030] [Test example] Next, test examples related to the technology disclosed herein will be described. Note that the technology disclosed herein is not limited to the following test examples.
[0031] 1. Sample Preparation (1) Comparative Example 1 Comparative Example 1 in this test is a commercially available diamond abrasive grain (manufactured by Global Diamond Co., Ltd., FRM-DN 40-60). Note that, as a result of laser diffraction analysis, the D 50The particle size was 40 μm. Furthermore, the results of the component analysis based on XRF showed that the diamond abrasive grains contained 0.176 wt% Ni and 0.389 wt% Mn as impurities.
[0032] (2) Example 1 In Example 1, ultrasonic wave application treatment was performed on the diamond abrasive grains. Specifically, 3 g of the same diamond abrasive grains as in Comparative Example 1 were weighed and mixed with 100 ml of pure water to prepare an abrasive grain dispersion. Next, ultrasonic waves were applied to the diamond abrasive grains in the dispersion using an ultrasonic disperser (manufactured by SMT Corporation, model: UH-600S). This ultrasonic disperser has an output of 600 W, an oscillation frequency of 20 kHz, and a diameter of the vibrator irradiation part of 36 mm. Then, the OUTPUT of the ultrasonic disperser was set to 10 (maximum), and a treatment cycle including one minute of ultrasonic treatment and one minute of interval was repeated five times. Thereafter, the diamond abrasive grains were separated from the dispersion by filtration treatment, washed with ethanol, and then dried at room temperature. As a result, ultrasonic wave application treatment was performed on the diamond abrasive grains (Example 1).
[0033] (3) Comparative Example 2 In Comparative Example 2, the diamond abrasive grains were subjected to heat treatment. Specifically, the same diamond abrasive grains as those in Comparative Example 1 were heated in a reducing atmosphere (N2 gas containing 3% H2). The temperature rise rate in this heat treatment was set to 100°C / h, and the maximum temperature was set to 700°C. The heating time (retention time at the maximum temperature) was set to 3 hours. In this way, heat-treated diamond abrasive grains (Comparative Example 2) were produced.
[0034] (4) Comparative Example 3 In Comparative Example 3, the diamond abrasive grains were subjected to heat treatment in the same manner as in Comparative Example 2. Specifically, the diamond abrasive grains were heated according to the same procedure as in Comparative Example 2, except that the maximum temperature was changed to 1000°C.
[0035] (5) Example 2 In Example 2, ultrasonic application treatment was performed on the diamond abrasive grains after the heat treatment. Specifically, heat treatment (maximum temperature: 1000°C) was performed according to the same procedure as in Comparative Example 3, and then ultrasonic treatment was performed according to the same procedure as in Example 1. In this way, diamond abrasive grains (Example 2) that had been subjected to ultrasonic treatment after heat treatment were produced.
[0036] 2.Evaluation Test In this study, 500 Raman spectra were acquired for each example. -1 ~1334cm -1 The positions and half-widths of the Raman peaks having peak positions at and are shown in Table 1.
[0037] In this test, the position and half-width of the Raman peak were measured according to the following procedure. First, a microscopic Raman spectrophotometer (LabRAM HR Evolution manufactured by Horiba, Ltd.) was used as the measuring device. The measurement conditions were, for example, a measurement temperature of 24°C, a calibration sample of Si, an excitation laser wavelength of 532 nm, a grating of 1800 gr / mm, an exposure time of 8 seconds, and an accumulation count of 2 times. Then, baseline correction, peak search, and fitting were performed on the obtained Raman spectrum using waveform analysis software (Labspec6). Then, the position of the peak top was regarded as the "position of the Raman peak", and the wavenumber width of the peak at half the intensity of the peak top was regarded as the "half-width of the Raman peak". Then, for each of 100 randomly selected diamond abrasive grains, the peak position and half-width were measured at five non-overlapping measurement points, and the average values (average value of the Raman peak position and the average value of the Raman peak half-width) were obtained. That is, the "Raman peak position" and "Raman peak half width" in Table 1 are the average values of the measurement results at 500 measurement positions.
[0038] [Table 1]
[0039] First, the Raman peak position of Comparative Example 1 is 1329.64 cm -1 This shows that the diamond abrasive grains used in this test have a high degree of uniformity due to the presence of impurities or the introduction of stress during manufacturing. -1 ) to the lower wavenumber side.
[0040] Next, the Raman peak position of Example 1 is 1329.42 cm -1 From this, it was found that the diamond abrasive grains to which ultrasonic waves were applied had internal stresses equivalent to those of the diamond abrasive grains (Comparative Example 2) that had been heat-treated at 700°C. Next, the Raman peak position of Comparative Example 3 was 1328.66 cm -1 This is believed to be due to the fact that a very strong internal stress was introduced into the diamond abrasive grains by the heat treatment at a high temperature of 1000°C. On the other hand, in Example 2, the Raman peak position was 1329.10 cm -1 This resulted in the surprising result that when ultrasonic waves are applied to diamond abrasive grains in which extremely strong internal stress has been introduced, the internal stress is released. These results show that when ultrasonic waves are applied to diamond abrasive grains, the internal stress changes depending on the state of the diamond abrasive grains before the ultrasonic waves are applied.
[0041] In addition, when comparing Example 1 and Comparative Example 2, the positions of the Raman peaks were similar, but there was a significant difference in the half-width. Specifically, in Comparative Example 2, the half-width of the Raman peak increased. This is because the crystallinity of Comparative Example 2, which was heat-treated at 700°, was reduced by heat. On the other hand, in Example 1, in which internal stress was introduced by applying ultrasonic waves, there was no increase in the half-width of the Raman peak, and the crystallinity was high. From this, it can be expected that by controlling the internal stress of diamond abrasive grains using ultrasonic waves, diamond abrasive grains with higher hardness than conventional ones can be realized.
[0042] Although the technology disclosed herein has been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes to the specific examples exemplified above. In other words, the technology disclosed herein includes the embodiments described in items 1 to 7 below.
[0043] <Item 1> A method for manufacturing diamond abrasive grains, comprising an internal stress control step of applying ultrasonic waves to the diamond abrasive grains.
[0044] <Item 2> The diamond abrasive grains before the internal stress control step are subjected to a Raman spectroscopy-based Raman spectrum of 1325 cm -1 From 1334cm -1 The Raman peak position is in the range of 1331 cm -1 2. The method according to item 1, wherein the method is as follows:
[0045] <Item 3> 3. The manufacturing method according to claim 1 or 2, wherein the internal stress control step introduces internal stress into the diamond abrasive grains.
[0046] <Item 4> The diamond abrasive grains before the internal stress control step have a Raman peak position of 1329 cm -1 Over 1331cm -1 Item 3. The method for producing a semiconductor device according to item 3, wherein the semiconductor device is a semiconductor device.
[0047] <Item 5> The manufacturing method according to item 1 or 2, wherein the internal stress control step releases internal stress in the diamond abrasive grains.
[0048] <Item 6> The diamond abrasive grains before the internal stress control step have a Raman peak position of 1329 cm -1 6. The method according to item 5, wherein the production method is less than 50% by weight.
[0049] <Item 7> In the internal stress control step, the diamond abrasive grains are subjected to Raman spectroscopy to obtain a Raman spectrum of 1325 cm -1 From 1334cm -1 The method for producing a Raman peak having a Raman peak position in the range of
[0050] <Item 8> The reduction in the average half-width of the Raman peak in the internal stress control step is 0.05 cm -1 The above is the production method according to Item 7.
[0051] <Item 9> In the internal stress control step, the average half width of the Raman peak is 4.8 cm -1 9. The method for producing according to item 7 or 8, wherein:
Claims
1. A method for manufacturing diamond abrasive grains, comprising an internal stress control step of applying ultrasonic waves to the diamond abrasive grains.
2. The diamond abrasive grains before the internal stress control step are characterized by a Raman spectrum of 1325 cm -1 From 1334 cm -1 The average peak position of the Raman peaks that exist in the range of 1331 cm -1 The method of claim 1, wherein:
3. The manufacturing method according to claim 2 , wherein the internal stress control step introduces internal stress into the diamond abrasive grains.
4. The diamond abrasive grains before the internal stress control process had an average value of the peak positions of 1329 cm -1 1331cm or more -1 The method of claim 3, wherein:
5. The manufacturing method according to claim 2 , wherein the internal stress control step releases internal stress in the diamond abrasive grains.
6. The diamond abrasive grains before the internal stress control process had an average value of the peak positions of 1329 cm -1 The method of claim 5, wherein the
7. In the internal stress control step, the diamond abrasive grain is subjected to Raman spectroscopy. -1 From 1334 cm -1 The method according to claim 1 or 2, wherein the average half-width of a Raman peak having a Raman peak position in the range of
8. The reduction in the average half-width of the Raman peak in the internal stress control step is 0.05 cm -1 The method for producing a semiconductor device according to claim 7 .
9. In the internal stress control step, the average half width of the Raman peak is 4.8 cm -1 The method of claim 7, wherein the temperature is controlled as follows:
Citation Information
Cited By
Preparation method of long-circulation artificial graphite negative electrode material and graphite negative electrode material
CN121097074A