Capacitor
The capacitor's acicular conductive layer addresses peeling issues by enhancing anchoring, thereby reducing ESR and improving durability.
Patent Information
- Application Number
- JP2023051899
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-28
AI Technical Summary
Capacitors experience peeling between the inorganic layer and the electrode, leading to increased equivalent series resistance (ESR).
A capacitor design featuring a conductive layer with an acicular structure made of inorganic material on the surface layer, which enhances anchoring and reduces peeling between the inorganic layer and the second electrode.
The design effectively suppresses peeling and reduces ESR, resulting in a capacitor with improved durability and performance.
Smart Images

Figure 2024140647000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to capacitors. [Background technology]
[0002] Various capacitors have been proposed in the past. Claim 1 of Patent Document 1 (JP Patent Publication 2018-182106 A) describes a multilayer ceramic capacitor comprising: "a laminated chip having a substantially rectangular parallelepiped shape in which dielectric layers mainly composed of ceramic and internal electrode layers are alternately laminated, and the laminated internal electrode layers are exposed on two end faces that alternately face each other, and external electrodes formed on the two end faces, the external electrodes having a structure in which a plating layer is formed on a base layer, and at least a part of the surface of the base layer includes a region in which the height from the bottom to the peak is 0.4 μm or more and the average distance between local peaks is 0.5 μm or less."
[0003] Claim 1 of Patent Document 2 (JP 2020-35890 A) describes "a solid electrolytic capacitor comprising an anode body made of a valve metal, a dielectric layer formed on the surface of the anode body, a semiconductor layer formed on the dielectric layer, and a cathode layer formed on the semiconductor layer, wherein the semiconductor layer is composed of a p-type inorganic semiconductor." [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-182106 A [Patent Document 2] JP 2020-35890 A Summary of the Invention [Problem to be solved by the invention]
[0005] As described in Patent Document 2, a capacitor is known in which an inorganic layer is disposed between two electrodes. However, if the contact between the inorganic layer and the electrodes is insufficient, peeling occurs between the inorganic layer and the electrode layer, resulting in problems such as an increase in equivalent series resistance (ESR). In this situation, one of the objectives of the present disclosure is to provide a capacitor in which peeling is unlikely to occur between the inorganic layer (conductive layer) and the electrodes. [Means for solving the problem]
[0006] One aspect of the present disclosure relates to a capacitor including a first electrode, a dielectric layer formed on a surface of the first electrode, a conductive layer disposed on the dielectric layer, and a second electrode disposed on the conductive layer, the conductive layer having needle-like structures made of an inorganic material on a surface layer on the second electrode side. Effect of the Invention
[0007] According to the present disclosure, a capacitor in which peeling is unlikely to occur between the inorganic layer (conductive layer) and the electrode can be obtained. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic structure of an example of a capacitor according to this embodiment. [Diagram 2] FIG. 2 is a cross-sectional view illustrating a schematic view of a portion of the capacitor illustrated in FIG. [Diagram 3] FIG. 3 is a cross-sectional view that illustrates a schematic structure of another example of a capacitor according to this embodiment. [Figure 4A] FIG. 4A is a cross-sectional image of the surface of the zinc oxide layer of an example capacitor produced in Experiment 1. [Figure 4B] FIG. 4B is a cross-sectional image of the surface of the zinc oxide layer of another example of the capacitor produced in Experiment 1. [Figure 4C] FIG. 4C is a cross-sectional image of the surface of the zinc oxide layer of another example of the capacitor produced in Experiment 1. [Figure 4D]FIG. 4D is a cross-sectional image of the surface of the zinc oxide layer of another example of the capacitor produced in Experiment 1. [Diagram 5] FIG. 5 is a cross-sectional image showing an example of the measurement result of the aspect ratio of the needle-like portion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] In the following, the embodiments according to the present disclosure will be described with examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values and materials may be exemplified, but other numerical values and other materials may be applied as long as the invention according to the present disclosure can be implemented. In this specification, the description "numerical value A to numerical value B" includes numerical value A and numerical value B, and can be read as "numerical value A or more and numerical value B or less." In the following description, when the lower limit and the upper limit of numerical values related to specific physical properties or conditions are exemplified, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined as long as the lower limit is not equal to or greater than the upper limit.
[0010] (Capacitor) The capacitor according to this embodiment may be referred to as "capacitor (C)" below. Capacitor (C) includes a first electrode, a dielectric layer formed on the surface of the first electrode, a conductive layer disposed on the dielectric layer, and a second electrode disposed on the conductive layer. The conductive layer has needle-like structures made of an inorganic material on the surface layer on the second electrode side.
[0011] As a result of the investigation, the inventors of the present application have found a new method of forming a conductive layer having a needle-like structure made of an inorganic material on the surface layer. By using a conductive layer having a needle-like structure on the surface layer, it is possible to suppress peeling between the surface layer (inorganic layer) having the needle-like structure and the second electrode. Therefore, it is possible to suppress an increase in ESR due to peeling.
[0012] The conductive layer can be made of an inorganic material. Therefore, the conductive layer can be read as an inorganic layer. A preferred example of the conductive layer of the capacitor (C) does not contain an organic material (e.g., a conductive polymer). By forming the conductive layer from an inorganic material, a capacitor (C) with high heat resistance can be obtained.
[0013] A part of the needle-like structure may be embedded in the second electrode. With this configuration, the inorganic layer and the second electrode can be firmly fixed together by the anchor effect.
[0014] The average aspect ratio As in a cross-sectional image of the needle-like portion at the end of the needle-like structure may be in the range of 4.6 to 17.2 (for example, in the range of 5 to 16). The cross-sectional image is an image of a cross section parallel to the thickness direction Dt of the conductive layer. The average aspect ratio As is determined by a method described in the examples.
[0015] At least a part of the needle-shaped portion at the end of the needle-shaped structure may be curved. With this configuration, the anchor effect of the needle-shaped structure is particularly enhanced. At least a part of the needle-shaped portion may be a needle-shaped crystal. That is, the needle-shaped structure may include a needle-shaped crystal.
[0016] The conductive layer may be made of an inorganic material containing a metal oxide. In that case, the needle-like structure may be made of the metal oxide. By using a conductive layer made of an inorganic material, a capacitor with high heat resistance can be obtained.
[0017] The metal oxide may be a conductive metal oxide mainly composed of at least one selected from the group consisting of ZnO, TiO2, indium tin oxide, In2O3, SnO2, Ga2O3, MnO2, NiO2, CuInO2, CuCrO2, CuAlO2, and CuScO2, or may be a conductive metal oxide composed of at least one of the above. The metal oxide may be a conductive metal oxide mainly composed of any one selected from the above group, or may be a conductive metal oxide composed of the above. For example, the metal oxide may be a conductive metal oxide mainly composed of ZnO, or may be ZnO. Although ZnO is sometimes classified as a semiconductor, it is treated as a conductive metal oxide in this specification because it has conductivity. With respect to the metal oxide, the main component means that the content is 50% by mass or more. The content of the main component in the metal oxide may be in the range of 80 to 100% by mass, 90 to 100% by mass, or 95 to 100% by mass.
[0018] The conductive metal oxide may contain oxygen vacancies. By containing oxygen vacancies, the conductivity of the conductive metal oxide can be increased. When the conductive metal oxide is mainly composed of zinc oxide (ZnO), ZnO 1-x The main component may be zinc oxide represented by the formula (0≦x≦0.25), where x may be greater than 0.
[0019] The conductive metal oxide may contain an additive element for improving the conductivity. When the conductive metal oxide is mainly composed of ZnO, at least one element selected from the group consisting of Al, Ga, B, and In may be added to ZnO so that the content of the element is 10 atomic % or less.
[0020] When the conductive metal oxide is mainly composed of Ga2O3, at least one element selected from the group consisting of Ta and Hf may be added to Ga2O3 so that its content is 0.1 atomic % or less. When the conductive metal oxide is mainly composed of TiO2, at least one element selected from the group consisting of Nb and Ta may be added to TiO2 so that its content is 10 atomic % or less. When the conductive metal oxide is mainly composed of SnO2, Sb may be added to SnO2 so that its content is 12.5 atomic % or less. When the conductive metal oxide is mainly composed of CuCrO2, Mg may be added to CuCrO2 so that its content is 5 atomic % or less. When the conductive metal oxide is mainly composed of CuInO2, Ca may be added to CuInO2 so that its content is 3 atomic % or less.
[0021] In the capacitor (C), the first electrode may be an anode and the second electrode may be a cathode. In the capacitor (C), the first electrode may be an aluminum foil or a tantalum sintered body.
[0022] In the capacitor (C), the first electrode may have a porous portion on its surface. In this case, the dielectric layer is formed on the surface of the porous portion, and a part of the conductive layer is disposed in the voids of the porous portion. The first electrode having a porous portion on its surface may be an etched aluminum foil or a sintered body of a valve metal (e.g., a tantalum sintered body).
[0023] The conductive layer may include a first conductive layer in contact with the dielectric layer and a second conductive layer in contact with the second electrode. The conductive layer may be composed of the first conductive layer and the second conductive layer. The second conductive layer has the above-mentioned needle-like structure on the surface layer. The first conductive layer and the second conductive layer may have different compositions or the same composition. The first conductive layer and the second conductive layer may be composed of the above-mentioned conductive metal oxide. When a porous portion is present on the surface layer of the first electrode, at least a part of the first conductive layer may be formed in the recess of the porous portion.
[0024] The conductive layer may have a conductivity of 1 S / cm or more, or 10 S / cm or more. The conductive layer may have a conductivity of 10,000 S / cm or less, or 1,000 S / cm or less. The conductive layer may be an inorganic layer having a conductivity of 1 S / cm or more.
[0025] The thickness of the conductive layer is not particularly limited and may be in the range of 0.1 μm to 100 μm (for example, in the range of 1 μm to 10 μm).
[0026] (Capacitor manufacturing method) The manufacturing method according to this embodiment may be referred to as manufacturing method (M) below. According to manufacturing method (M), a capacitor (C) can be manufactured. However, the capacitor (C) may be manufactured by a method other than manufacturing method (M). The matters described for the capacitor (C) can be applied to manufacturing method (M), so duplicated descriptions will be omitted. The matters described for manufacturing method (M) may also be applied to the capacitor (C).
[0027] The manufacturing method (M) is a method for manufacturing a capacitor including a first electrode and a dielectric layer formed on the surface of the first electrode. The manufacturing method (M) includes steps (i) and (ii) in this order. These steps are described below.
[0028] Step (i) is a step of forming a conductive layer on the dielectric layer formed on the surface of the first electrode. The conductive layer is the conductive layer described for the capacitor (C). In step (i), the conductive layer is formed so that the surface layer of the conductive layer has a needle-like structure made of an inorganic material. At least the surface layer of the conductive layer can be formed by liquid phase growth. According to the liquid phase growth method, a conductive layer (a crystal layer having conductivity) can be formed by crystal growth. At this time, the surface layer having a needle-like structure can be formed by selecting the conditions of the liquid phase growth method.
[0029] When the surface layer is made of zinc oxide, a zinc oxide layer having a needle-like structure can be formed under the following conditions. First, a solution for liquid phase growth (solution growth) is prepared. Examples of the solution include an aqueous solution in which zinc nitrate and other additives are dissolved. Examples of the additives include hexamethylenetetramine, ammonia, citric acid, ammonium nitrate, aluminum nitrate, gallium nitrate, indium nitrate, and the like. When the additive element described above is added to ZnO, a compound containing the additive element may be dissolved. The pH of the solution is, for example, in the range of 6 to 11. The concentration of zinc nitrate in the solution is, for example, in the range of 0.01 mol / L to 2 mol / L. In addition, when forming a surface layer having a needle-like structure, the temperature of the first electrode is, for example, in the range of 65°C to 75°C. The temperature of the solution is, for example, 75°C or less. The temperature of the solution may be in the range of 0 to 75°C (for example, in the range of 10 to 50°C or in the range of 10 to 40°C).
[0030] If the temperature of the first electrode is high (e.g., 85°C or higher), a columnar structure is formed instead of a needle-like structure. Conventionally, when forming a zinc oxide layer, conditions have been selected that result in the formation of a dense columnar structure. However, the inventors of the present application have found that a needle-like structure can be formed at a relatively low temperature. At least the surface layer of the conductive layer described above is formed under conditions that result in the formation of a needle-like structure. The average aspect ratio As of the needle-like portion at the end of the needle-like structure can be changed by changing the temperature of the first electrode, the pH of the solution, the concentration of the solution, etc.
[0031] Before forming the zinc oxide layer, a base layer made of zinc oxide may be formed in advance. For example, the base layer made of zinc oxide may be formed by a gas phase method. Examples of the gas phase method include atomic layer deposition (ALD), sputtering, and chemical vapor deposition (CVD). The use of the base layer makes it easier to form the zinc oxide layer by a liquid phase deposition method. The ALD method is preferable because it is easy to form a layer in the recesses of the porous portion.
[0032] The conductive layer made of the conductive metal oxide can be formed by liquid phase deposition in the same manner as the zinc oxide layer, by selecting a solution appropriate for the conductive metal oxide to be formed.
[0033] The method of forming the conductive layer other than the surface layer having the needle-like structure is not limited. The conductive layer other than the surface layer may be formed by a gas phase method or a liquid phase method. Examples of the gas phase method include the gas phase method described above. The entire conductive layer may be formed by a liquid phase growth method, or the entire conductive layer may be formed under the same conditions as the conditions for forming the surface layer described above. When the entire conductive layer is formed by the liquid phase growth method, as described above, a base layer may be formed in advance on the dielectric layer. Alternatively, a first conductive layer having a certain thickness may be formed on the dielectric layer by the ALD method, and then a second conductive layer may be formed by the liquid phase growth method. In either case, the surface layer of the conductive layer is formed under conditions that form a needle-like structure. Note that even when the entire conductive layer is formed under conditions that form a needle-like structure, the conductive layer close to the dielectric layer may not have a needle-like structure due to the progress of growth.
[0034] When the conductive layer includes a first conductive layer and a second conductive layer, the first conductive layer and the second conductive layer may be formed by the same formation method or different formation methods. For example, the first conductive layer and the second conductive layer having different compositions may be formed by the same formation method. Alternatively, the first conductive layer and the second conductive layer having the same composition may be formed by different formation methods.
[0035] Step (ii) is a step of forming a second electrode on the conductive layer. At this time, the second electrode is formed on the needle-like structures on the surface of the conductive layer. As a result, the conductive layer and the second electrode are firmly fixed to each other.
[0036] The second electrode is formed using a material having electrical conductivity. The material of the second electrode is not particularly limited, and may be any material that can be used as an electrode of a capacitor. The method of forming the second electrode is not particularly limited, but it is preferable to use a method of forming the second electrode that firmly connects the conductive layer and the second electrode. For example, the second electrode may be formed by applying a conductive paste containing conductive particles. Alternatively, the second electrode may be formed by a vapor phase method, a plating method, or the like.
[0037] The second electrode may include a carbon layer and a silver particle layer laminated in order from the conductive layer side. In that case, first, a carbon paste containing conductive carbon particles is applied. Next, a silver paste containing silver particles is applied. Then, a heat treatment is performed to form a carbon layer and a silver particle layer. In this way, the second electrode is formed. Note that, if necessary, heat treatment may be performed not only after application of the silver paste but also before application of the silver paste. The carbon paste and silver paste are not limited, and known carbon paste and silver paste may be used.
[0038] Through the above steps, a capacitor element including a first electrode, a dielectric layer, a conductive layer, and a second electrode is formed. After step (ii), if necessary, a lead may be connected, or the capacitor element may be housed in an exterior body. In this manner, a capacitor (C) is obtained.
[0039] Examples of the configuration and constituent members of the capacitor (C) are described below. Known constituent members may be used for the constituent members other than those characteristic of the present disclosure.
[0040] (1st electrode) The first electrode can be formed using a valve metal, an alloy containing a valve metal, a compound containing a valve metal, or the like. These materials may be used alone or in combination of two or more. For example, aluminum, tantalum, niobium, and titanium are preferably used as the valve metal. For the first electrode, a foil of the above material (for example, a metal foil such as an aluminum foil) may be used.
[0041] The first electrode having a porous portion on its surface can be obtained, for example, by roughening the surface of a metal foil containing a valve metal. The roughening may be performed by electrolytic etching or the like.
[0042] The first electrode may be formed by sintering particles of the above material. For example, the first electrode may be a sintered body of tantalum. When the first electrode is a sintered body, a porous portion exists on the surface of the first electrode. When the first electrode is a sintered body, the capacitor (C) may include an anode wire partially embedded in the sintered body.
[0043] (Dielectric layer) The dielectric layer is an insulating layer that functions as a dielectric. The dielectric layer may be formed by anodizing a valve metal on the surface of the first electrode (e.g., a metal foil). The dielectric layer may be formed so as to cover at least a part of the first electrode. The dielectric layer is usually formed on the surface of the first electrode. When a porous portion exists on the surface of the first electrode, the dielectric layer is formed on the surface of the porous portion of the first electrode.
[0044] A typical dielectric layer includes an oxide of a valve metal. The first electrode may be formed of a valve metal, and the dielectric layer may be formed of an oxide of the valve metal. For example, when tantalum is used as the material of the first electrode, the dielectric layer may be a tantalum oxide layer. When aluminum is used as the material of the first electrode, the dielectric layer may be an aluminum oxide layer. However, the dielectric layer is not limited to these, and may be any layer that functions as a dielectric layer.
[0045] (2nd electrode) The second electrode is a layer having electrical conductivity. The second electrode may be formed using conductive carbon or metal. Specifically, the second electrode may be formed using a carbon paste containing conductive carbon particles or a metal paste containing metal particles. Alternatively, the second electrode may include a layer made of only metal (a vapor deposition layer or a metal foil). Examples of conductive carbon include graphite, carbon black, graphene flakes, and carbon nanotubes. Examples of metal paste include a silver paste containing silver particles.
[0046] The second electrode may include a first layer formed on the conductive layer and a second layer formed on the first layer. In this case, the first layer may be a carbon layer containing conductive carbon, and the second layer may be a layer formed of a metal paste.
[0047] (Leads and case) The capacitor (C) may include other components as necessary, for example, leads and an exterior body. There are no particular limitations on the leads and exterior body, and known leads and exterior bodies may be used.
[0048] (Capacitor (C) structure) The capacitor (C) may include only one capacitor element. Alternatively, the capacitor (C) may include multiple capacitor elements. For example, the capacitor element (C) may include multiple capacitor elements connected in parallel. The multiple capacitor elements (C) are usually connected in parallel in a stacked state and covered with an exterior body.
[0049] Examples of embodiments according to the present disclosure will be specifically described below with reference to the drawings. The above-mentioned components can be applied to the components of the examples described below. The examples described below can be modified based on the above description. The matters described below may be applied to the above-mentioned embodiments. In the embodiments described below, components that are not essential to the capacitor of the present disclosure may be omitted. Note that the following figures are schematic and may differ from the actual configuration.
[0050] (Embodiment 1) 1 is a cross-sectional view illustrating a capacitor in accordance with embodiment 1. Capacitor 10 illustrated in FIG.
[0051] The capacitor element 100 includes a first electrode 111, a dielectric layer 112, a conductive layer 120, and a second electrode 131. The dielectric layer 112 is formed so as to cover at least a portion of a surface of the first electrode 111. The conductive layer 120 is formed so as to cover at least a portion of the dielectric layer 112. The second electrode 131 is formed so as to cover at least a portion of the conductive layer 120. The conductive layer 120 is the conductive layer described above.
[0052] The first lead terminal 21 is connected to the first electrode 111. The second lead terminal 22 is connected to the second electrode 131 via the metal paste layer 23. The metal paste layer 23 is formed of a metal paste (silver paste) or the like. The exterior body 30 is formed so as to cover a part of the first lead terminal 21, a part of the second lead terminal 22, and the capacitor element 100. A part of the first lead terminal 21 and a part of the second lead terminal 22 are exposed from the exterior body 30 and function as terminals.
[0053] FIG. 2 is a schematic cross-sectional view of an example of a portion where the conductive layer 120 is present. FIG. 2 shows the thickness direction Dt of the conductive layer 120. The cross-sectional view of FIG. 2 is a cross-sectional view parallel to the thickness direction Dt of the conductive layer 120. The first electrode 111 of the example of FIG. 2 has a porous portion 111a on the surface. The actual porous portion 111a may have a more complicated shape, but the porous portion 111a is illustrated in a simplified form in FIG. 2. The surface layer 120a of the conductive layer 120 has a needle-like structure. However, the needle-like structure is not illustrated in FIG. 2.
[0054] Fig. 1 shows a case where capacitor 10 includes only one capacitor element 100. However, capacitor 10 may include multiple capacitor elements 100. Fig. 3 is a schematic cross-sectional view of an example of capacitor 10 including multiple capacitor elements 100. Note that in order to make the drawing easier to understand, some components are omitted from Fig. 3.
[0055] 3 includes a plurality of stacked capacitor elements 100. The plurality of capacitor elements 100 are connected in parallel.
[0056] (Additional Note) Based on the above description, the following techniques are disclosed. (Technology 1) A capacitor, A first electrode; a dielectric layer formed on a surface of the first electrode; a conductive layer disposed on the dielectric layer; a second electrode disposed on the conductive layer; The conductive layer has a needle-shaped structure made of an inorganic material on a surface layer on the second electrode side. (Technology 2) The capacitor described in Technology 1, wherein a portion of the needle-like structure is embedded in the second electrode. (Technology 3) The capacitor according to technique 1 or 2, wherein an average aspect ratio in a cross-sectional image of the needle-like portion at the end of the needle-like structure is in the range of 4.6 to 17.2. (Technology 4) 4. The capacitor according to any one of Techniques 1 to 3, wherein at least a part of the needle-like portion at the end of the needle-like structure is curved. (Technology 5) the conductive layer is made of an inorganic material containing a metal oxide, 5. The capacitor according to any one of Techniques 1 to 4, wherein the needle-like structure is made of the metal oxide. (Technology 6) The capacitor according to technology 5, wherein the metal oxide is a conductive metal oxide mainly composed of at least one selected from the group consisting of ZnO, TiO2, indium tin oxide, In2O3, SnO2, Ga2O3, MnO2, NiO2, CuInO2, CuCrO2, CuAlO2, and CuScO2. (Technology 7) The capacitor according to claim 6, wherein the conductive metal oxide contains oxygen vacancies. (Technology 8) The capacitor according to claim 6, wherein the conductive metal oxide contains an additive element for improving conductivity. (Technology 9) The capacitor according to any one of techniques 1 to 8, wherein the first electrode is an anode and the second electrode is a cathode. (Technology 10) The capacitor according to any one of Techniques 1 to 9, wherein the first electrode is an aluminum foil or a tantalum sintered body. (Technology 11) the first electrode has a porous portion on a surface layer, the dielectric layer is formed on a surface of the porous portion, 11. The capacitor according to any one of techniques 1 to 10, wherein a part of the conductive layer is disposed in the voids of the porous portion. (Technology 12) the conductive layer includes a first conductive layer in contact with the dielectric layer and a second conductive layer in contact with the second electrode; 12. The capacitor according to any one of techniques 1 to 11, wherein the second conductive layer has the needle-like structure and a composition different from a composition of the first conductive layer. EXAMPLES
[0057] The capacitor (C) according to the present disclosure will be described in more detail with reference to examples.
[0058] (Experiment 1) In experiment 1, a conductive layer (ZnO layer) was formed under different conditions and evaluated. First, an aluminum foil with a dielectric layer (aluminum oxide layer) formed on its surface was prepared. The aluminum foil used had porous parts formed on its surface by etching. The aluminum oxide layer was formed by subjecting the aluminum foil to a chemical conversion treatment.
[0059] Next, a base layer made of zinc oxide was formed on the dielectric layer by the ALD method. Next, a conductive layer made of zinc oxide (ZnO) was formed on the base layer. Specifically, the aluminum foil on which the base layer was formed was immersed in a specific solution and held for 6 hours to form a zinc oxide layer on the base layer.
[0060] The solution used was an aqueous solution of zinc nitrate hexahydrate and hexamethylenetetramine dissolved in a molar ratio of 1:1. The concentration of zinc nitrate hexahydrate in the solution was 0.05 mol / L. The pH of the solution was 6.5 to 7.5. The temperature of the solution was room temperature (approximately 24°C). During the growth of zinc oxide, a heater was placed in contact with the back side of the aluminum foil (the side opposite to the growth surface of zinc oxide) to heat the aluminum foil to a constant temperature. In experiment 1, four types of zinc oxide layers were formed by changing the temperature of the aluminum foil. Figure 4A shows a cross-sectional image of the surface of the zinc oxide layer formed when the temperature of the aluminum foil was set to 65°C. Figures 4B to 4D show cross-sectional images of the surface of the zinc oxide layer formed when the temperature of the aluminum foil was set to 75°C, 85°C, and 95°C. The cross-sectional images in Figures 4A to 4D are images of a cross section parallel to the thickness direction Dt of the conductive layer. In other words, the cross-sectional images in FIGS. 4A to 4D are images of a cross section perpendicular to the surface of the aluminum foil.
[0061] As shown in FIG. 4A to FIG. 4D, when the temperature of the aluminum foil was in the range of 65 to 75° C., a needle-like structure was formed. On the other hand, when the temperature of the aluminum foil was in the range of 85 or 95° C., a columnar structure was formed instead of a needle-like structure. As shown in FIG. 4A and FIG. 4B, the needle-like portion at the end of the needle-like structure formed was not oriented in a fixed direction, but extended in various directions. In addition, at least a part of the needle-like portion at the end of the needle-like structure was curved. Note that, when the temperature of the aluminum foil was 50° C. or less, the growth of zinc oxide was difficult to proceed, and a needle-like structure was not formed.
[0062] The average value As of the aspect ratio in the cross-sectional image of the needle-like portion at the end of the needle-like structure shown in FIG. 4A was calculated. The average value As was obtained by the following procedure. First, 22 needle-like portions at the end of the needle-like structure were arbitrarily selected in the cross-sectional image. The needle-like portion was the portion at the end of the needle-like structure that was not branched. Next, the diameter D and length L of each selected needle-like portion were obtained from the cross-sectional image. The diameter D was obtained by measuring the diameter at one arbitrary point of the needle-like portion. When the needle-like portion was curved, the length L of the needle-like portion was obtained from the entire length along the curved portion. Next, the aspect ratio of each needle-like portion was obtained from the formula aspect ratio = length L / diameter D. Then, the average value As was obtained by arithmetically averaging the obtained 22 aspect ratios. The aspect ratios of each needle-like portion are shown in FIG. 5. In FIG. 5, the needle-like portion for which the aspect ratio was obtained is shown as a rod-shaped figure. As described above, the average aspect ratio As can be determined by arbitrarily selecting and measuring 20 or more (for example, 20) needle-like portions.
[0063] The average aspect ratio As of the needle-like portions at the ends of the needle-like structures shown in Figure 4A was 4.6, and the average aspect ratio As of the needle-like portions at the ends of the needle-like structures shown in Figure 4B was 17.2.
[0064] (Experiment 2) In experiment 2, a second electrode was formed on a conductive layer (ZnO layer) formed under different conditions, and the peel resistance between the conductive layer and the second electrode was evaluated.
[0065] First, an aluminum foil having a dielectric layer formed on its surface was prepared. The aluminum foil having a dielectric layer formed on its surface was the same as that used in Experiment 1. Next, a zinc oxide layer (conductive layer) was formed on the dielectric layer by the same method and conditions as those described in Experiment 1. At this time, as described in Experiment 1, the temperature of the aluminum foil was changed to form multiple types of zinc oxide layers. Next, a second electrode was formed on the zinc oxide layer. Two types of electrodes were used for the second electrode. One second electrode was formed by laminating a carbon layer and a silver particle layer in this order on a conductive layer. The other second electrode was formed only by a silver particle layer. In this way, four types of samples A1 to A4 were produced. Furthermore, samples R1 to R4 of comparative examples were produced by the same method and conditions as those for producing samples A1 to A4, except that the base material was changed from aluminum foil to a glass substrate.
[0066] The structure of the surface of the zinc oxide layer was observed for the prepared samples. Furthermore, a peeling test of the second electrode was performed for the prepared samples. The peeling test was performed using a method called a tape peeling test. Specifically, tape was attached to the surface of the second electrode, and then the tape was peeled off, and the presence or absence of peeling of the second electrode was observed. The sample preparation conditions and the evaluation results of the peeling test are shown in Table 1.
[0067] [Table 1]
[0068] Samples A1 to A4 have the structure of the capacitor (C) according to the present disclosure. In comparative samples R1 to R4, no needle-like structures were found on the surface of the zinc oxide layer. As shown in Table 1, in samples A1 to A4, no peeling of the second electrode occurred regardless of the configuration of the second electrode. [Industrial Applicability]
[0069] The present disclosure can be used for capacitors. [Explanation of symbols]
[0070] 10: Capacitor 21: First lead terminal 22: Second lead terminal 30: Exterior body 100: Capacitor element 111: 1st electrode 111a: Porous part 112: Dielectric layer 120: Conductive layer 120a: Surface layer 131:Second electrode
Claims
1. A capacitor, A first electrode; a dielectric layer formed on a surface of the first electrode; a conductive layer disposed on the dielectric layer; a second electrode disposed on the conductive layer; The conductive layer has a needle-shaped structure made of an inorganic material on a surface layer on the second electrode side.
2. The capacitor of claim 1 , wherein a portion of the needle-like structure is embedded in the second electrode.
3. The capacitor according to claim 1 or 2, wherein the average aspect ratio in a cross-sectional image of the needle-like portion at the end of the needle-like structure is in the range of 4.6 to 17.
2.
4. The capacitor according to claim 1 or 2, wherein at least a part of the needle-like portion at the end of the needle-like structure is curved.
5. the conductive layer is made of an inorganic material containing a metal oxide, The capacitor according to claim 1 , wherein the needle-like structure is made of the metal oxide.
6. The metal oxide is ZnO, TiO 2 , indium tin oxide, In 2 O 3 , SnO 2 , Ga 2 O 3 , MnO 2 , NiO 2 , CuInO 2 , CuCrO 2 , CuAlO 2 , and CuScO 2 6. The capacitor according to claim 5, wherein the conductive metal oxide is composed mainly of at least one selected from the group consisting of:
7. The capacitor of claim 6 , wherein the conductive metal oxide comprises oxygen vacancies.
8. The capacitor of claim 6 , wherein the conductive metal oxide includes an additive element for improving electrical conductivity.
9. 3. The capacitor of claim 1, wherein the first electrode is an anode and the second electrode is a cathode.
10. 3. The capacitor according to claim 1, wherein the first electrode is an aluminum foil or a tantalum sintered body.
11. the first electrode has a porous portion on a surface layer, the dielectric layer is formed on a surface of the porous portion, The capacitor according to claim 1 , wherein a part of the conductive layer is disposed within the voids of the porous portion.
12. the conductive layer includes a first conductive layer in contact with the dielectric layer and a second conductive layer in contact with the second electrode; The capacitor according to claim 1 , wherein the second conductive layer has the needle-like structure and a composition different from a composition of the first conductive layer.
Citation Information
Patent Citations
Metal oxide structural form and its production
JP2000159599A
Conductive composition, conductive coating, capacitor and method for manufacturing the same
JP2005298563A
Solid electrolytic capacitor
JP2017103412A
Solid electrolyte film
JP2018198128A
Element for electronic component
WO2009099127A1