Wiring board and method for manufacturing the same

A CuNiTi alloy-based first metal film on the insulating layer of wiring boards enhances adhesion by addressing filler exposure issues, ensuring structural integrity and cost-effective manufacturing.

JP2024140740AActive Publication Date: 2024-10-10SHINKO ELECTRIC IND CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023052050
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

The exposure of filler on the surface of the insulating layer in wiring boards reduces the adhesion between the insulating layer and the wiring layer, leading to potential detachment issues.

Method used

A wiring board design where the insulating layer contains a resin and filler, with a first metal film formed from a CuNiTi alloy covering the exposed surface, having a Ni content of 5 wt% to 30 wt% and Ti content of 5 wt% to 15 wt%, enhancing adhesion by improving contact with the filler.

Benefits of technology

The improved adhesion between the insulating and wiring layers is achieved, reducing detachment risks and maintaining structural integrity while allowing for efficient etching of the metal film without additional costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140740000001_ABST
    Figure 2024140740000001_ABST
Patent Text Reader

Abstract

To provide a wiring board capable of improving adhesion between an insulating layer and a wiring layer.SOLUTION: A wiring board 10 has a wiring layer 22, an insulating layer 30 formed to cover a side surface of a wiring layer 22 and expose a part of an upper surface of the wiring layer 22, and a wiring layer 40 formed on the wiring layer 22 exposed from the insulating layer 30. The insulating layer 30 contains a resin 32 and a filler 33. An upper surface 30A of the insulating layer 30 has a structure in which the filler 33 is exposed from the resin 32. The wiring layer 40 has a first metal film 51 that covers the upper surface 30A of the insulating layer 30 and the upper surface of the wiring layer 22 exposed from the insulating layer 30, and metal layers 53, 54 formed on an upper layer of the first metal film 51. The first metal film 51 is formed of a CuNiTi alloy. The content of Ni contained in the first metal film 51 is 5 wt% or more and 30 wt% or less. The content of Ti contained in the first metal film 51 is 5 wt% or more and 15 wt% or less.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a wiring board and a method for manufacturing a wiring board. [Background technology]

[0002] Conventionally, wiring boards of various shapes and structures have been proposed for mounting electronic components such as semiconductor elements. As this type of wiring board, a wiring board in which a plurality of wiring layers and a plurality of insulating layers are alternately laminated by a build-up method is known (see, for example, Patent Document 1). The plurality of wiring layers are electrically connected to each other through via wiring formed in through holes that penetrate the insulating layers in the thickness direction. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-188139 A Summary of the Invention [Problem to be solved by the invention]

[0004] Incidentally, the insulating layer in the above-mentioned wiring board may contain a resin and a filler. In this case, if the filler is exposed on the surface of the insulating layer, there is a problem that the adhesion between the insulating layer and the wiring layer is reduced. [Means for solving the problem]

[0005] According to one aspect of the present invention, a semiconductor device includes a first wiring layer, an insulating layer formed to cover side surfaces of the first wiring layer and expose at least a portion of an upper surface of the first wiring layer, and a second wiring layer formed on the first wiring layer exposed from the insulating layer, wherein the insulating layer contains a resin and a filler, and the upper surface of the insulating layer has a structure in which the filler is exposed from the resin, and the second wiring layer includes a first metal film covering the upper surface of the insulating layer and the upper surface of the first wiring layer exposed from the insulating layer, and a metal layer formed on the upper layer of the first metal film, and the first metal film is formed of a CuNiTi alloy, and the Ni content of the first metal film is 5 wt% or more and 30 wt% or less, and the Ti content of the first metal film is 5 wt% or more and 15 wt% or less. Effect of the Invention

[0006] Advantageous Effects of Invention According to one aspect of the present invention, an effect is achieved in that the adhesion between an insulating layer and a wiring layer can be improved. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a wiring board according to an embodiment. [Diagram 2] FIG. 2(a) is an enlarged cross-sectional view of a portion of the wiring board of one embodiment, and FIG. 2(b) is a further enlarged cross-sectional view of the portion of the wiring board shown in FIG. 2(a). [Diagram 3] FIG. 3 is a schematic cross-sectional view showing a method for manufacturing a wiring board according to an embodiment. [Figure 4] FIG. 4 is a schematic cross-sectional view showing a method for manufacturing a wiring board according to an embodiment. [Diagram 5] 5(a) and 5(b) are schematic cross-sectional views showing a method for manufacturing a wiring board according to one embodiment. [Figure 6] 6(a) and 6(b) are schematic cross-sectional views showing a method for manufacturing a wiring board according to one embodiment. [Figure 7] FIG. 7 is a schematic cross-sectional view showing a method for manufacturing a wiring board according to an embodiment. [Figure 8]FIG. 8 is a schematic cross-sectional view showing a method for manufacturing a wiring board according to an embodiment. [Figure 9] FIG. 9 is a schematic cross-sectional view showing a method for manufacturing a wiring board according to an embodiment. [Figure 10] FIG. 10 is a schematic cross-sectional view showing a method for manufacturing a wiring board according to an embodiment. [Figure 11] FIG. 11 is a schematic cross-sectional view showing a method for manufacturing a wiring board according to an embodiment. [Figure 12] FIG. 12 is a table showing the results of the first experiment. [Figure 13] FIG. 13 is a table showing the results of the second experiment. [Figure 14] FIG. 14(a) is an enlarged cross-sectional view of a portion of the wiring board of the modified example, and FIG. 14(b) is a further enlarged cross-sectional view of a portion of the wiring board shown in FIG. 14(a). [Figure 15] FIG. 15 is a schematic cross-sectional view showing a wiring board according to a modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, an embodiment will be described with reference to the accompanying drawings. In addition, for convenience, the attached drawings may show characteristic parts in an enlarged manner to make the characteristics easier to understand, and the dimensional ratios of each component are not necessarily the same in each drawing. In addition, in the cross-sectional views, in order to make the cross-sectional structure of each member easier to understand, the hatching of some members is shown as a matte pattern, and the hatching of some members is omitted. In this specification, "planar view" refers to viewing an object from a vertical direction (up and down in the figure) such as in FIG. 1, and "planar shape" refers to the shape of an object viewed from a vertical direction such as in FIG. 1. In this specification, the "up and down direction" and "left and right direction" refer to the direction in which the symbols indicating each member in each drawing can be correctly read as the normal position.

[0009] (Overall configuration of wiring board 10) 1, the wiring board 10 has a substrate body 11. A wiring layer 20 and a solder resist layer 21 are laminated in this order on the lower surface of the substrate body 11. A wiring layer 22, an insulating layer 30, and a wiring layer 40 are laminated in this order on the upper surface of the substrate body 11.

[0010] The substrate body 11 may be a wiring structure in which insulating resin layers and wiring layers are alternately laminated. The wiring structure may have, for example, a core substrate, or may not have a core substrate. The insulating resin layer may be made of, for example, a thermosetting insulating resin. The thermosetting insulating resin may be made of, for example, an insulating resin such as an epoxy resin, a polyimide resin, or a cyanate resin. The insulating resin layer may be made of, for example, an insulating resin mainly composed of a photosensitive resin such as a phenolic resin or a polyimide resin. The insulating resin layer may contain, for example, a filler such as silica or alumina.

[0011] The wiring layer of the substrate body 11 and the wiring layer 20 may be made of, for example, copper (Cu) or a copper alloy. The solder resist layer 21 may be made of, for example, an insulating resin mainly composed of a photosensitive resin such as a phenolic resin or a polyimide resin. The solder resist layer 21 may contain, for example, a filler such as silica or alumina.

[0012] (Structure of wiring layer 20) The wiring layer 20 is formed on the lower surface of the substrate body 11. The wiring layer 20 is the bottommost wiring layer of the wiring substrate 10.

[0013] (Structure of solder resist layer 21) The solder resist layer 21 is laminated on the lower surface of the substrate body 11 so as to cover the wiring layer 20. The solder resist layer 21 is an insulating layer that is the outermost layer (here, the bottom layer) of the wiring substrate 10.

[0014] A plurality of openings 21X are formed in the solder resist layer 21 to expose parts of the lower surface of the wiring layer 20 as external connection pads P1. External connection terminals (not shown) used when mounting the wiring board 10 on a mounting board such as a motherboard are connected to the external connection pads P1.

[0015] A surface treatment layer is formed on the lower surface of the wiring layer 20 exposed at the bottom of the opening 21X, as necessary. Examples of the surface treatment layer include a gold (Au) layer, a nickel (Ni) layer / Au layer (a metal layer in which a Ni layer and an Au layer are laminated in this order), and a Ni layer / palladium (Pd) layer / Au layer (a metal layer in which a Ni layer, a Pd layer, and an Au layer are laminated in this order). Other examples of the surface treatment layer include a Ni layer / Pd layer (a metal layer in which a Ni layer and a Pd layer are laminated in this order), and a Pd layer / Au layer (a metal layer in which a Pd layer and an Au layer are laminated in this order). Here, the Au layer is a metal layer made of Au or an Au alloy, the Ni layer is a metal layer made of Ni or an Ni alloy, and the Pd layer is a metal layer made of Pd or a Pd alloy. The Au layer, Ni layer, and Pd layer may be, for example, a metal layer (electroless plating layer) formed by electroless plating or a metal layer (electrolytic plating layer) formed by electrolytic plating. The surface treatment layer may be an OSP film formed by performing an anti-oxidation treatment such as an OSP (Organic Solderability Preservative) treatment on the lower surface of the wiring layer 20 exposed in the opening 21X. The OSP film may be an organic coating such as an azole compound or an imidazole compound. When a surface treatment layer is formed on the lower surface of the wiring layer 20, the surface treatment layer functions as the external connection pad P1.

[0016] In this example, an external connection terminal is provided on the underside of the wiring layer 20, but the wiring layer 20 itself exposed at the bottom of the opening 21X, or if a surface treatment layer is formed on the underside of the wiring layer 20, the surface treatment layer itself may be used as the external connection terminal.

[0017] (Structure of wiring layer 22) The wiring layer 22 is formed on the upper surface of the substrate body 11. The wiring layer 22 is electrically connected to the wiring layer 20 via a wiring layer and a through electrode in the substrate body 11.

[0018] (Configuration of insulating layer 30) The insulating layer 30 is laminated on the upper surface of the substrate body 11 so as to cover the side surface of the wiring layer 22 and expose a part of the upper surface of the wiring layer 22. The insulating layer 30 is an outermost insulating layer provided on the outermost layer (here, the uppermost layer) of the wiring substrate 10. For example, the same insulating resin layer as the insulating resin layer used in the substrate body 11 can be used for the insulating layer 30. For example, a solder resist layer can also be used for the insulating layer 30. For example, the same material as the solder resist layer 21 can be used for the material of the solder resist layer. The thickness from the upper surface of the wiring layer 22 to the upper surface 30A of the insulating layer 30 can be, for example, about 3 μm to 30 μm.

[0019] The insulating layer 30 has a through hole 31 formed therein, which penetrates the insulating layer 30 in the thickness direction and exposes a part of the upper surface of the wiring layer 22. The planar shape of the through hole 31 can be set to any shape and any size. In this example, the planar shape of the through hole 31 is formed in a circular shape. The depth of the through hole 31 can be, for example, about 3 μm to 30 μm.

[0020] As shown in Fig. 2(a), the through hole 31 of this example is formed in a tapered shape in which the opening width (opening diameter) becomes smaller from the upper side (the upper surface 30A side of the insulating layer 30) to the lower side in Fig. 2(a). The inner wall surface of the through hole 31 is formed, for example, inclined so as to approach the center of the plane of the through hole 31 from the upper surface 30A of the insulating layer 30 to the wiring layer 22. Note that the inner wall surface of the through hole 31 does not need to be flat, and a part or the whole of the inner wall surface of the through hole 31 may be a convex curved surface or a concave curved surface. The through hole 31 is, for example, a via hole formed by a laser processing method.

[0021] As shown in FIG. 2(b), the insulating layer 30 contains a resin 32 and a large number of fillers 33. The resin 32 is formed, for example, so as to cover the surface of the fillers 33. The fillers 33 are, for example, embedded in the resin 32. As the resin 32, for example, an insulating resin mainly composed of a thermosetting resin such as an epoxy resin, a polyimide resin, or a cyanate resin can be used. The resin 32 in this embodiment is an epoxy resin. As the fillers 33, for example, a silica filler or an alumina filler can be used. The fillers 33 in this embodiment are silica fillers. The fillers 33 are, for example, formed in a spherical shape.

[0022] The surface of the insulating layer 30, here the upper surface 30A of the insulating layer 30, has a structure in which the resin 32 and the filler 33 are mixed. The upper surface 30A of the insulating layer 30 has a structure in which the filler 33 is exposed from the upper surface 32A of the resin 32. The upper surface 30A of the insulating layer 30 in this example has a structure in which a part (here, the upper part) of the filler 33 protrudes upward from the upper surface 32A of the resin 32. The filler 33 in this example is exposed from the resin 32 while remaining spherical. Therefore, the upper surface 30A of the insulating layer 30 in this example has a structure in which a part of the spherical surface of the filler 33 protrudes upward from the upper surface 32A of the resin 32. The filler 33 provided on the upper surface 30A of the insulating layer 30 is partly embedded in the resin 32 (here, the lower part) and the remaining part (here, the upper part) is exposed from the resin 32. 2(b) illustrates the structure of the upper surface 30A of the insulating layer 30, but the inner wall surface of the through hole 31 (see FIG. 2(a)) of the insulating layer 30 also has the same structure as the upper surface 30A. That is, the inner wall surface of the through hole 31 shown in FIG. 2(a) has a structure in which the filler 33 is exposed from the surface of the resin 32.

[0023] (Structure of wiring layer 40) As shown in FIG. 1, the wiring layer 40 is formed on the wiring layer 22 exposed from the through hole 31. The wiring layer 40 is, for example, the uppermost wiring layer of the wiring board 10. The wiring layer 40 functions, for example, as a pad for mounting an electronic component for electrically connecting to the electronic component. The wiring layer 40 has, for example, a via wiring 41 formed in the through hole 31, and a wiring pattern 42 electrically connected to the wiring layer 22 through the via wiring 41 and formed on the upper surface 30A of the insulating layer 30. The planar shape of the wiring layer 40 can be set to any shape and any size. The planar shape of the wiring layer 40 in this example is formed in a circular shape.

[0024] The via wiring 41 is formed, for example, so as to fill the through hole 31. The via wiring 41 is formed in the same shape as the through hole 31. The wiring pattern 42 is formed, for example, in a columnar shape so as to protrude upward from the upper surface 30A of the insulating layer 30.

[0025] 2(a), the wiring layer 40 has a first metal film 51 that covers the inner surface of the through hole 31 and the upper surface 30A of the insulating layer 30, and a second metal film 52 that covers the surface of the first metal film 51. The wiring layer 40 has a metal layer 53 that fills the through hole 31 on the inner side of the second metal film 52, and a metal layer 54 formed on the second metal film 52 and the metal layer 53 formed on the upper surface 30A of the insulating layer 30. The first metal film 51 and the second metal film 52 are seed layers. The second metal film 52 is formed of, for example, Cu.

[0026] The first metal film 51 is formed so as to continuously cover the upper surface 30A of the insulating layer 30, the entire inner wall surface of the through hole 31, and the entire upper surface of the wiring layer 22 exposed at the bottom of the through hole 31. As shown in FIG. 2(b), the first metal film 51 is formed so as to cover the surface of the insulating layer 30 where the filler 33 is exposed from the resin 32. The first metal film 51 is formed so as to cover, for example, the entire surface of the filler 33 exposed from the resin 32 in a tight contact state. The first metal film 51 is formed so as to cover, in a tight contact state, the surface of the resin 32 (the upper surface 32A in FIG. 2(b)).

[0027] The first metal film 51 is made of an alloy of Cu, nickel (Ni) and titanium (Ti), i.e., a CuNiTi alloy. The Ni contained in the first metal film 51 is a metal that has higher adhesion to the resin 32 than Cu. The Ti contained in the first metal film 51 is a metal that has higher adhesion to the filler 33 than Cu.

[0028] The Ni content in the first metal film 51 is set to be in the range of 5 wt% to 30 wt%. The Ti content in the first metal film 51 is set to be in the range of 5 wt% to 15 wt%. The Cu content in the first metal film 51 is the remainder other than Ti and Ni contained in the first metal film 51. Note that this Cu content also includes impurities present in the production of the material.

[0029] By setting the content of Ni and Ti contained in the first metal film 51 within the above-mentioned range, the adhesion to the surface of the insulating layer 30 where the filler 33 is exposed from the resin 32 can be improved. Furthermore, by setting the content of Ni and Ti contained in the first metal film 51 within the above-mentioned range, when the unnecessary portion of the second metal film 52, which is a Cu film, is etched away, the unnecessary portion of the first metal film 51 can be suitably etched away together with the second metal film 52. That is, by setting the content of Ni and Ti contained in the first metal film 51 within the above-mentioned range, the unnecessary portion of the first metal film 51 can be suitably etched away by an etching solution for Cu. Note that, as shown in the experimental results described later, when the content of Ti contained in the first metal film 51 is lower than 5 wt%, the adhesion of the first metal film 51 to the surface of the insulating layer 30 where the filler 33 is exposed from the resin 32 is reduced. Furthermore, when the content of Ti contained in the first metal film 51 is higher than 15 wt%, when the first metal film 51 is etched away together with the Cu film, a residue is generated. Furthermore, if the content of Ni in first metal film 51 is lower than 5 wt %, the adhesion of first metal film 51 to the surface of insulating layer 30 where filler 33 is exposed from resin 32 decreases.

[0030] The first metal film 51 is, for example, a sputtered film formed by a sputtering method. The thickness of the first metal film 51 can be, for example, about 30 nm to 100 nm. 2(a), the second metal film 52 continuously covers the upper surface of the first metal film 51 in a portion covering the upper surface 30A of the insulating layer 30, the side surface of the first metal film 51 in a portion covering the inner wall surface of the through hole 31, and the upper surface of the first metal film 51 in a portion covering the upper surface of the wiring layer 22. The second metal film 52 is formed so as to expose the outer side surface of the first metal film 51 in the portion covering the upper surface 30A of the insulating layer 30.

[0031] The second metal film 52 is a Cu film formed from Cu. The second metal film 52 is, for example, a sputtered film formed by a sputtering method. The thickness of the second metal film 52 can be, for example, about 300 nm to 500 nm.

[0032] The metal layer 53 is formed, for example, so as to fill the through holes 31 on the inner side than the second metal film 52. The material of the metal layer 53 may be, for example, Cu or a Cu alloy. The metal layer 53 may be, for example, an electrolytic plating layer formed by an electrolytic plating method. The metal layer 53 of this embodiment is an electrolytic Cu plating layer formed by an electrolytic Cu plating method.

[0033] The first metal film 51, the second metal film 52, and the metal layer 53 formed in the through hole 31 described above constitute the via wiring 41 of the wiring layer 40. The metal layer 54 is formed on the second metal film 52 formed on the upper surface 30A of the insulating layer 30 and on the via wiring 41 (metal layer 53). The metal layer 54 is formed continuously and integrally with the metal layer 53. For example, Cu or a Cu alloy can be used as the material of the metal layer 54. For example, an electrolytic plating layer formed by an electrolytic plating method can be used as the metal layer 54. The metal layer 54 in this embodiment is an electrolytic Cu plating layer formed by an electrolytic Cu plating method.

[0034] The metal layer 54 is formed, for example, in a columnar shape so as to protrude upward from the upper surface 30A of the insulating layer 30. The upper surface of the metal layer 54 is formed, for example, in a flat surface. The planar shape of the metal layer 54 can be set to any shape and any size. The planar shape of the metal layer 54 can be, for example, a circle with a diameter of about 15 μm to 40 μm. The thickness of the metal layer 54 can be, for example, about 2 μm to 50 μm.

[0035] The wiring pattern 42 of the wiring layer 40 is composed of the metal layer 54 described above and the first metal film 51 and second metal film 52 formed on the upper surface 30A of the insulating layer 30. It should be noted that wiring board 10 can be used upside down or placed at any angle.

[0036] (Method of Manufacturing Wiring Board 10) Next, a method for manufacturing the wiring board 10 will be described with reference to Fig. 3 to Fig. 11. Here, a method for manufacturing the insulating layer 30 and the wiring layer 40 will be described in detail. For ease of explanation, the parts that will ultimately become the components of the wiring board 10 will be described with the reference numerals of the final components.

[0037] 3, a structure is prepared in which a wiring layer 22 is formed on the upper surface of a substrate body 11. The wiring layer 22 can be formed by using various wiring formation methods such as a subtractive method or a semi-additive method.

[0038] Next, in the step shown in FIG. 4, an insulating layer 30 is formed on the upper surface of the substrate body 11 to entirely cover the wiring layer 22. For example, when a resin film is used as the insulating layer 30, the resin film is laminated on the upper surface of the substrate body 11. Then, the resin film is pressed and heat-treated at a temperature equal to or higher than the curing temperature (for example, about 130° C. to 200° C.) to cure the resin film, thereby forming the insulating layer 30. For example, a thermosetting resin film mainly composed of epoxy resin can be used as the resin film. For example, when a liquid or paste insulating resin is used as the insulating layer 30, the liquid or paste insulating resin is applied to the upper surface of the substrate body 11 by a spin coating method or the like. Then, the applied insulating resin is heat-treated at a temperature equal to or higher than the curing temperature to cure the resin, thereby forming the insulating layer 30. For example, a thermosetting resin mainly composed of epoxy resin can be used as the liquid or paste insulating resin.

[0039] 5(a), a through hole 31 is formed in the insulating layer 30 so as to penetrate the insulating layer 30 in the thickness direction and expose a part of the upper surface of the wiring layer 22. The through hole 31 is formed by, for example, CO 2 It can be formed by laser processing using a laser, a UV-YAG laser, or the like.

[0040] Next, a dry desmear process is performed to remove resin smears (resin residues) adhering to the upper surface of the wiring layer 22 exposed at the bottom of the through hole 31. The dry desmear process is a type of plasma process. For example, the dry desmear process uses carbon tetrafluoride (CF 4 ) and oxygen (O 2 ) can be performed by plasma etching using a mixed gas of the resin 32 and the filler 33. The dry desmear process is a process for micro-etching the resin 32 (see FIG. 5(b)) on the surface of the insulating layer 30. As shown in FIG. 5(b), when the dry desmear process is performed on the insulating layer 30, the resin 32 is predominantly etched out of the resin 32 and the filler 33. As a result, the filler 33 is exposed from the resin 32 on the surface of the insulating layer 30, and the resin 32 and the filler 33 are mixed together. On the surface of the insulating layer 30 in this example, the filler 33 protrudes from the surface of the resin 32. The surface roughness of the resin 32 at this time is smaller than that when the insulating layer 30 is subjected to a wet desmear process, for example.

[0041] Next, in the step shown in FIG. 6(a), a first metal film 51 is formed of a CuNiTi alloy so as to continuously cover the entire upper surface 30A of the insulating layer 30, the entire inner wall surface of the through hole 31, and the entire upper surface of the wiring layer 22 exposed at the bottom of the through hole 31. Here, by setting the Ni content in the CuNiTi alloy to a range of 5 wt% to 30 wt% and the Ti content to a range of 5 wt% to 15 wt%, the adhesion between the first metal film 51 and the insulating layer 30 can be improved. In more detail, as shown in FIG. 6(b), the adhesion between the first metal film 51 and the resin 32 can be improved, and the adhesion between the first metal film 51 and the filler 33 can be improved. That is, the adhesion of the first metal film 51 to both the resin 32 and the filler 33 can be improved. Specifically, the peel strength of the first metal film 51 to the insulating layer 30 is 0.5 kgf / cm or more. Therefore, peeling of the first metal film 51 from the insulating layer 30 can be suppressed.

[0042] The first metal film 51 can be formed by, for example, a sputtering method. By forming the first metal film 51 by using a sputtering method, the content of Ni and Ti contained in the first metal film 51 made of a CuNiTi alloy can be set accurately to the content within the desired range described above.

[0043] 7, a second metal film 52 is formed of Cu so as to cover the entire surface of the first metal film 51. The second metal film 52 can be formed by, for example, a sputtering method. By forming the second metal film 52 by a sputtering method, the second metal film 52 can be formed by using the sputtering device used when forming the first metal film 51.

[0044] 8, a resist layer 60 having an opening 61 is formed on the second metal film 52 formed on the upper surface 30A of the insulating layer 30. The opening 61 is formed so as to expose the second metal film 52 in a portion corresponding to the formation region of the metal layer 54 shown in FIG. 2(a). For example, a material having plating resistance against the electrolytic plating process in the next step can be used as the material of the resist layer 60. For example, a photosensitive dry film resist or a liquid photoresist (for example, a dry film resist or a liquid resist such as a novolac resin or an acrylic resin) can be used as the material of the resist layer 60. For example, when a photosensitive dry film resist is used, a dry film is laminated on the upper surface of the second metal film 52 by thermocompression bonding, and the dry film is patterned by a photolithography method to form the resist layer 60 having the opening 61. Note that even when a liquid photoresist is used, the resist layer 60 can be formed through the same steps.

[0045] 9, the resist layer 60 is used as a plating mask to perform electrolytic plating on the second metal film 52, using the second metal film 52 as a plating power supply layer. That is, electrolytic plating, here electrolytic Cu plating, is performed on the upper surface of the second metal film 52 exposed from the opening 61 of the resist layer 60. This process forms a metal layer 53 filling the through hole 31 on the inner side than the second metal film 52, and also forms a metal layer 54 in the opening 61. At this time, the metal layer 54 is formed integrally and continuously with the metal layer 53.

[0046] Subsequently, in a process shown in FIG. 10, the resist layer 60 shown in FIG. 9 is removed by an alkaline stripping solution (for example, an organic amine stripping solution, caustic soda, acetone, ethanol, or the like).

[0047] 11, the unnecessary second metal film 52 and the unnecessary first metal film 51 are removed by etching using the metal layer 54 as an etching mask. When the first metal film 51 is a Cu film, the unnecessary second metal film 52 can be removed by wet etching using a Cu etching solution (e.g., a sulfuric acid / peroxide aqueous solution). At this time, when the content of Ni and Ti contained in the first metal film 51 is set to the desired range described above, the unnecessary portion of the first metal film 51 and the unnecessary portion of the second metal film 52 can be simultaneously removed by using a Cu etching solution (e.g., a sulfuric acid / peroxide aqueous solution). That is, the unnecessary portion of the first metal film 51 can also be removed by the Cu etching solution for removing the unnecessary portion of the second metal film 52. As a result, it is not necessary to remove the unnecessary portion of the first metal film 51 and the unnecessary portion of the second metal film 52 using separate etching solutions, and therefore an increase in the manufacturing cost of the wiring board 10 can be suppressed.

[0048] Through the above manufacturing steps, via wiring 41 is formed, which is made up of first and second metal films 51 and 52, and a metal layer 53, formed in through hole 31. Also, wiring pattern 42 is formed, which is made up of first and second metal films 51 and 52, and a metal layer 54, formed on upper surface 30A of insulating layer 30. Then, wiring layer 40 having via wiring 41 and wiring pattern 42 is formed on wiring layer 22 exposed at the bottom of through hole 31.

[0049] (First experiment) Next, we will explain the first experimental results, which support the idea that setting the Ni and Ti content in first metal film 51 within the above-mentioned range improves the adhesion of first metal film 51 to the surface of insulating layer 30 where filler 33 is exposed from resin 32.

[0050] (Experimental conditions) First, 30 types of samples for evaluation were created. More specifically, in each sample, a first metal film 51 having a thickness of 30 nm and a Cu film having a thickness of 300 nm were sequentially laminated by a sputtering method on the upper surface 30A of the insulating layer 30 where the filler 33, which is a silica filler, was exposed from the resin 32, which is an epoxy resin. Furthermore, an electrolytic Cu plating layer having a thickness of 35 μm was laminated on the Cu film. At this time, the combinations of the Ni content and the Ti content in the first metal film 51 were set to be different from each other in each sample. Specifically, 30 (=6×5) types of samples were created by combining six types of Ni content and five types of Ti content. The six types of Ni content are 0 wt%, 5 wt%, 10 wt%, 20 wt%, 30 wt%, and 40 wt%. The five types of Ti content are 0 wt%, 5 wt%, 10 wt%, 15 wt%, and 20 wt%. The conditions other than the Ni content and Ti content in the first metal film 51 were set to be the same for all the samples.

[0051] (Cross-cut test) After the reliability test was performed on all the 30 types of samples described above, a cross-cut test was performed to evaluate the adhesion of the first metal film 51 to the upper surface 30A of the insulating layer 30. The results are shown in FIG. 12. In the reliability test, each sample was held in an atmosphere at a temperature of 125°C for 24 hours, and then held in an atmosphere at a humidity of 60% RH and a temperature of 60°C for 40 hours, and then reflow was performed three times at 265°C for each sample. In the cross-cut test, 100 squares of 1 mm square cuts were made in the electrolytic Cu plating layer in a checkerboard pattern, and adhesive tape was attached to the surface of the electrolytic Cu plating layer in the 100 square areas, and then the adhesive tape was peeled off. Then, the adhesion of the first metal film 51 to the upper surface 30A of the insulating layer 30 was evaluated by checking whether peeling occurred in the first metal film 51 due to peeling of the adhesive tape. Specifically, for samples in which peeling of the first metal film 51 did not occur as the adhesive tape was peeled off, it was determined that the adhesion of the first metal film 51 to the upper surface 30A of the insulating layer 30 was good, and this was marked with "◯" in the experimental results in Fig. 12. On the other hand, for samples in which peeling of the first metal film 51 occurred as the adhesive tape was peeled off, it was determined that the adhesion of the first metal film 51 to the upper surface 30A of the insulating layer 30 was not good, and this was marked with "X" in the experimental results in Fig. 12.

[0052] (First experimental result) As is clear from FIG. 12, when the Ti content in the first metal film 51 is low, the adhesion of the first metal film 51 to the upper surface 30A of the insulating layer 30 is low. Specifically, when the Ti content in the first metal film 51 is 0 wt%, that is, when Ti is not contained, the adhesion of the first metal film 51 to the upper surface 30A of the insulating layer 30 is low. More specifically, when the Ti content in the first metal film 51 is 0 wt%, the adhesion of the first metal film 51 to the upper surface 30A of the insulating layer 30 is low regardless of the Ni content in the first metal film 51. Also, as is clear from FIG. 12, when the Ni content in the first metal film 51 is low, the adhesion of the first metal film 51 to the upper surface 30A of the insulating layer 30 is low. Specifically, when the Ni content in the first metal film 51 is 0 wt%, that is, when no Ni is contained, the adhesion of the first metal film 51 to the upper surface 30A of the insulating layer 30 may be reduced. More specifically, when the Ni content in the first metal film 51 is 0 wt% and the Ti content in the first metal film 51 is lower than 20 wt%, the adhesion of the first metal film 51 to the upper surface 30A of the insulating layer 30 is reduced.

[0053] On the other hand, when the Ni content in the first metal film 51 is in the range of 5 wt% to 30 wt% and the Ti content is in the range of 5 wt% to 15 wt% (within the thick line frame), the adhesion of the first metal film 51 to the upper surface 30A of the insulating layer 30 is good. When the Ti content in the first metal film 51 is 20 wt%, the adhesion of the first metal film 51 to the upper surface 30A of the insulating layer 30 is good regardless of the Ni content in the first metal film 51. When the Ni content in the first metal film 51 is 40 wt% and the Ti content is 5 wt% or more, the adhesion of the first metal film 51 to the upper surface 30A of the insulating layer 30 is good.

[0054] (Second experiment) Next, we will explain the second experimental results which support the idea that first metal film 51 can be suitably removed using an etching solution for Cu by setting the Ni and Ti contents in first metal film 51 within the above-mentioned ranges.

[0055] (Etching test) As in the first experiment, 30 types of samples were created in which the combinations of the Ni content and the Ti content in the first metal film 51 were set to be different from one another. All of these 30 types of samples were etched using an etching solution for Cu, here a sulfuric acid / peroxide aqueous solution. Then, by confirming by microscope observation whether the first metal film 51 was etched away together with the Cu film by the etching process, the ease of etching away the first metal film 51 by the etching solution for Cu was evaluated. The results are shown in FIG. 13. Specifically, for samples in which no residue of the first metal film 51 was detected by microscope observation, it was determined that the first metal film 51 could be etched away by the etching solution for Cu, and the experimental results in FIG. 13 were marked with "◯". On the other hand, for samples in which residue of the first metal film 51 was detected by microscope observation, it was determined that the first metal film 51 was difficult to etch away by the etching solution for Cu, and the experimental results in FIG. 13 were marked with "X".

[0056] (Second experimental result) As is clear from FIG. 13, when the Ti content in the first metal film 51 is high, it becomes difficult to etch and remove the first metal film 51 with an etching solution for Cu. Specifically, when the Ti content in the first metal film 51 is 20 wt% or more, it becomes difficult to etch and remove the first metal film 51 with an etching solution for Cu, regardless of the Ni content in the first metal film 51. Also, as is clear from FIG. 13, when the Ni content in the first metal film 51 is high, it becomes difficult to etch and remove the first metal film 51 with an etching solution for Cu. Specifically, when the Ni content in the first metal film 51 is 40 wt% or more, it may become difficult to etch and remove the first metal film 51 with an etching solution for Cu. More specifically, when the Ni content in the first metal film 51 is 40 wt% and the Ti content in the first metal film 51 is 5 wt% or more, it becomes difficult to etch and remove the first metal film 51 with an etching solution for Cu.

[0057] On the other hand, when the Ni content in the first metal film 51 is in the range of 5 wt% to 30 wt% and the Ti content is in the range of 5 wt% to 15 wt% (within the thick line frame), the first metal film 51 can be suitably etched away with an etching solution for Cu. When the Ti content in the first metal film 51 is 0 wt%, the first metal film 51 can be suitably etched away with an etching solution for Cu, regardless of the Ni content in the first metal film 51. When the Ni content in the first metal film 51 is 0 wt% and the Ti content is 15 wt% or less, the first metal film 51 can be suitably etched away with an etching solution for Cu.

[0058] As is clear from the first and second experimental results described above, it is preferable to set the Ni content in the first metal film 51 to 5 wt% or more and 30 wt% or less, and the Ti content to 5 wt% or more and 15 wt% or less. That is, by setting the Ni and Ti contents in the first metal film 51 to the above ranges (within the thick line frame), good results can be obtained in both of the two experiments. As is supported by the two experimental results, by setting the Ni and Ti contents in the first metal film 51 to the above ranges, the adhesion of the first metal film 51 to the insulating layer 30 can be improved, and the first metal film 51 can be suitably etched away with an etching solution for Cu.

[0059] Next, the effects of this embodiment will be described. (1) The wiring board 10 has a wiring layer 22, an insulating layer 30 formed to cover the side surfaces of the wiring layer 22 and expose a part of the upper surface of the wiring layer 22, and a wiring layer 40 formed on the wiring layer 22 exposed from the insulating layer 30. The insulating layer 30 contains a resin 32 and a filler 33. The upper surface 30A of the insulating layer 30 has a structure in which the filler 33 is exposed from the resin 32. The wiring layer 40 has a first metal film 51 covering the upper surface 30A of the insulating layer 30 and the upper surface of the wiring layer 22 exposed from the insulating layer 30, and metal layers 53 and 54 formed on the first metal film 51. The second metal film 52 is formed of Cu, and the first metal film 51 is formed of a CuNiTi alloy.

[0060] According to this configuration, the first metal film 51 covering the upper surface 30A of the insulating layer 30 where the filler 33 is exposed from the resin 32 is formed of a CuNiTi alloy containing Ti, which has high adhesion to the filler 33. Therefore, even when the filler 33 is exposed from the resin 32, the first metal film 51 can be suitably adhered to the exposed filler 33. As a result, the adhesion of the first metal film 51 to the upper surface 30A of the insulating layer 30 where the resin 32 and the filler 33 are mixed can be improved compared to when the first metal film 51 is formed of an alloy not containing Ti. As a result, the adhesion between the wiring layer 40 including the first metal film 51 and the insulating layer 30 can be improved.

[0061] (2) The content of Ni contained in the first metal film 51 is set in the range of 5 wt% to 30 wt%, and the content of Ti contained in the first metal film 51 is set in the range of 5 wt% to 15 wt%. As supported by the results of the first and second experiments, by setting the content of Ni and Ti in the first metal film 51 in the above ranges, the adhesion of the first metal film 51 to the insulating layer 30 can be improved, and the first metal film 51 can be suitably etched away with an etching solution for Cu. As a result, the first metal film 51 can be etched away with an etching solution for Cu that is relatively inexpensive, and therefore an increase in the manufacturing cost of the wiring board 10 can be suppressed.

[0062] (3) Furthermore, when the second metal film 52, which is a Cu film, is etched away with an etching solution for Cu, the first metal film 51 can also be etched away at the same time with the etching solution for Cu. This eliminates the need to remove the unnecessary portions of the first metal film 51 and the unnecessary portions of the second metal film 52 with separate etching solutions, thereby preventing an increase in the manufacturing cost of the wiring board 10.

[0063] (4) The first metal film 51 is formed by a sputtering method. This makes it possible to set the content of Ni and Ti contained in the first metal film 51 made of a CuNiTi alloy to the desired content range described above with high precision.

[0064] (Other embodiments) The above embodiment can be modified as follows: The above embodiment and the following modifications can be combined with each other to the extent that no technical contradiction occurs.

[0065] The structure of the wiring layer 40 in the above embodiment can be modified as appropriate. For example, the second metal film 52 may be omitted. In this case, metal layers 53 and 54 are formed on the first metal film 51.

[0066] In the above embodiment, the via wiring 41 is formed so as to fill the through hole 31. However, the present invention is not limited to this, and for example, the via wiring 41 may be formed as a conformal via. The structure of the wiring layer 22 in the above embodiment can be modified as appropriate.

[0067] For example, as shown in FIG. 14(a), the wiring layer 22 may be embodied as a via wiring 23 penetrating the insulating layer 30 in the thickness direction. The insulating layer 30 of this modification is formed so as to cover the side surface of the via wiring 23 and expose the entire upper surface of the via wiring 23. The upper surface 30A of the insulating layer 30 of this modification is formed flush with the upper surface of the via wiring 23. The wiring layer 40 of this modification has a first metal film 51 that continuously covers the upper surface 30A of the insulating layer 30 and the upper surface of the via wiring 23 exposed from the insulating layer 30, a second metal film 52 that covers the upper surface of the first metal film 51, and a metal layer 54 that covers the upper surface of the second metal film 52. In this modification, as shown in FIG. 14(b), the first metal film 51 also covers in close contact with the upper surface 30A of the insulating layer 30 where the filler 33 is exposed from the resin 32.

[0068] In the modified example shown in FIG. 14(a), a metal film having the same function as the first metal film 51 and the second metal film 52 may also be formed on the inner wall surface of the through hole 30X that penetrates the insulating layer 30 in the thickness direction.

[0069] In the above embodiment, the upper surface 30A of the insulating layer 30 has a structure in which a part of the filler 33 protrudes upward from the upper surface 32A of the resin 32, but the present invention is not limited to this. For example, as shown in FIG. 14(b), the upper surface 32A of the resin 32 and the upper surface 33A of the filler 33 may be formed flush with each other on the upper surface 30A of the insulating layer 30. In this case, the upper surface 33A of the filler 33 exposed from the resin 32 is not spherical, but is formed as a flat surface extending in a planar direction perpendicular to the thickness direction of the insulating layer 30. The upper surface 30A of the insulating layer 30 in this modification is formed, for example, by polishing the upper surface 30A of the insulating layer 30. The polishing of the upper surface 30A of the insulating layer 30 can be performed, for example, by chemical mechanical polishing (CMP) or mechanical polishing. By such polishing, the resin 32 and the filler 33 are polished together, and the upper surface 32A of the resin 32 becomes a polished surface and the upper surface 33A of the filler 33 becomes a polished surface. Note that such polishing is performed before the first metal film 51 is formed. For example, in the example shown in FIG. 14(a), the upper surface 30A of the insulating layer 30 and the upper surface of the via wiring 23 are polished together.

[0070] The first metal film 51 in this modified example covers, for example, the upper surface 32A of the resin 32 and covers the upper surface 33A of the filler 33 exposed from the upper surface 32A of the resin 32. The first metal film 51 in this modified example covers, for example, the upper surface 32A of the resin 32 in a tight contact state and covers the upper surface 33A of the filler 33 in a tight contact state.

[0071] In the above embodiment, the resin 32 contained in the insulating layer 30 is an epoxy resin, but is not limited to this. For example, the resin 32 may be changed to a resin other than an epoxy resin. For example, the resin 32 may be changed to a polyimide resin.

[0072] In the above embodiment, the filler 33 contained in the insulating layer 30 is a silica filler, but this is not limited thereto. For example, the filler 33 may be changed to a filler other than a silica filler. For example, the filler 33 may be changed to an alumina filler.

[0073] In the above embodiment, the first metal film 51 is made of a CuNiTi alloy, which is an alloy of Cu, Ni, and Ti, but is not limited to this. For example, the first metal film 51 may be made of an alloy of Cu, Ni, and Cr by replacing Ti with a metal having higher adhesion to the filler 33 than Cu, such as chromium (Cr).

[0074] In the above embodiment, the first metal film 51 is formed by sputtering, but the present invention is not limited to this. For example, the first metal film 51 may be formed by vapor deposition or electroless plating.

[0075] In the above embodiment, the second metal film 52 is formed by sputtering, but the present invention is not limited to this. For example, the second metal film 52 may be formed by vapor deposition or electroless plating.

[0076] In the above embodiment, the wiring layer 40 is formed by a semi-additive method, but the present invention is not limited to this. For example, the wiring layer 40 may be formed by various wiring formation methods such as a subtractive method.

[0077] In the above embodiment, the wiring layer 40 is embodied as the outermost wiring layer of the wiring board 10, but the present invention is not limited to this. 15, the wiring layer 40 may be applied to a wiring layer provided in an inner layer than the outermost wiring layer 70. In this modification, the wiring layer 40 is applied to a wiring layer provided between the outermost wiring layer 70 and the wiring layer 22.

[0078] In the wiring board 10 of this modified example, an insulating layer 80 covering the wiring layer 40 is laminated on the upper surface 30A of the insulating layer 30. The insulating layer 80 may contain a resin 32 and a filler 33 (see FIG. 2(b)), similar to the insulating layer 30. The outermost wiring layer 70 is formed on the upper surface of the insulating layer 80. The wiring layer 70 may have a structure similar to that of the wiring layer 40. That is, the wiring layer 70 may have a first metal film 51, a second metal film 52, and metal layers 53 and 54 (see FIG. 2(a)).

[0079] The number of wiring layers 20, 22, 40 and insulating layer 30 in the wiring board 10 in the above embodiment, the layout of the wiring, and the like can be changed as appropriate. [Explanation of symbols]

[0080] 10 Wiring board 22 Wiring layer (1st wiring layer) 23 Via wiring (first wiring layer) 30 Insulating layer 30A top 31 Through hole 32 Resin 32A Top 33 Filler 33A Top 40 Wiring layer (2nd wiring layer) 51 First metal film 52 Second metal film 53 Metal layer 54 Metal layer

Claims

1. A first wiring layer; an insulating layer formed to cover a side surface of the first wiring layer and to expose at least a portion of an upper surface of the first wiring layer; a second wiring layer formed on the first wiring layer exposed from the insulating layer; The insulating layer contains a resin and a filler, an upper surface of the insulating layer has a structure in which the filler is exposed from the resin; the second wiring layer includes a first metal film covering an upper surface of the insulating layer and an upper surface of the first wiring layer exposed from the insulating layer, and a metal layer formed on the first metal film; the first metal film is formed of a CuNiTi alloy; the content of Ni contained in the first metal film is 5 wt % or more and 30 wt % or less, A wiring board, wherein the content of Ti in the first metal film is 5 wt % or more and 15 wt % or less.

2. the second wiring layer includes the first metal film, a second metal film covering a surface of the first metal film, and the metal layer formed on the second metal film; The wiring board according to claim 1 , wherein the second metal film is made of Cu.

3. The wiring board according to claim 1 , wherein the upper surface of the insulating layer has a structure in which a part of the filler protrudes upward from an upper surface of the resin.

4. The filler is formed into a spherical shape, The wiring board according to claim 3 , wherein the upper surface of the insulating layer has a structure in which a part of the spherical surface of the filler protrudes upward from the upper surface of the resin.

5. The wiring board according to claim 1 , wherein the upper surface of the insulating layer has a structure in which an upper surface of the resin and an upper surface of the filler are formed flush with each other.

6. the insulating layer has a through hole penetrating the insulating layer in a thickness direction and exposing a part of an upper surface of the first wiring layer; The wiring board according to claim 1 , wherein the first metal film continuously covers an upper surface of the insulating layer, an inner wall surface of the through hole, and an upper surface of the first wiring layer exposed from the through hole.

7. The resin is an epoxy resin, The wiring board according to claim 1 , wherein the filler is a silica filler.

8. forming an insulating layer that contains a resin and a filler, covers a side surface of a first wiring layer, and exposes at least a portion of an upper surface of the first wiring layer; forming a structure in which the filler is exposed from the resin on an upper surface of the insulating layer; forming a first metal film made of a CuNiTi alloy to cover an upper surface of the insulating layer and an upper surface of the first wiring layer exposed from the insulating layer; forming a second metal film made of Cu and covering a surface of the first metal film; forming a metal layer on the second metal film; and removing the first metal film and the second metal film at the portions that do not overlap the metal layer in a plan view by etching using the metal layer as a mask, the content of Ni contained in the first metal film is 5 wt % or more and 30 wt % or less, A method for manufacturing a wiring substrate, wherein the content of Ti in the first metal film is 5 wt % or more and 15 wt % or less.

9. the step of forming the insulating layer includes a step of forming a through hole penetrating the insulating layer in a thickness direction by a laser processing method and exposing a part of an upper surface of the first wiring layer; The method for manufacturing a wiring board according to claim 8 , wherein in the step of forming a structure in which the filler is exposed from the resin, a dry desmear treatment is performed on the insulating layer after the through hole is formed.

10. The method for manufacturing a wiring board according to claim 8 , wherein the upper surface of the insulating layer is polished to form a structure in which the filler is exposed from the resin.

Citation Information

Patent Citations

  • Deposition method of plating layer

    JP1997083133A

  • Wiring substrate, and method for manufacturing the same

    JP2009188324A

  • Processing method of resin substrate

    JP2016092307A

  • Wiring circuit board, semiconductor device, method of manufacturing wiring circuit board, and method of manufacturing semiconductor device

    JP2016096262A

  • Cu ALLOY WIRE AND Cu ALLOY SPUTTERING TARGET

    JP2017095770A