Inkjet recording method, and inkjet recording device

By employing titanium oxide particles coated with alumina and silica in water-based ink with controlled dynamic surface tension, the method addresses image unevenness and disturbance on non-absorbent media, ensuring uniform ink adhesion and stability across density variations.

JP2024141030AInactive Publication Date: 2024-10-10CANON KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023052457
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Inkjet recording methods on non-absorbent recording media, such as vinyl chloride and polyethylene terephthalate, suffer from image unevenness and disturbance due to the low surface energy and ink repellency, particularly in low and high-density images, despite corona treatment to enhance wettability.

Method used

The method involves using water-based ink containing titanium oxide particles coated with alumina and silica, with a specific dynamic surface tension ratio, applied after corona treatment to improve ink compatibility and viscosity control, thereby reducing image unevenness and disturbance.

Benefits of technology

The method achieves stable image recording with suppressed unevenness and disturbance on non-absorbent media by enhancing ink adhesion and viscosity control, ensuring uniformity across varying ink densities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141030000014
    Figure 2024141030000014
  • Figure 2024141030000001
    Figure 2024141030000001
  • Figure 2024141030000002
    Figure 2024141030000002
Patent Text Reader

Abstract

To provide an inkjet recording method and the like capable of recording an image in which unevenness or disturbance is suppressed regardless of an amount of ink applied.SOLUTION: Provided is an inkjet recording method in which an image is recorded on a recording medium by using aqueous ink, which has: a pretreatment process of performing corona treatment to the recording medium; and a recording process of applying the aqueous ink to at least a part of a region to which the corona treatment of the recording medium has been performed. The aqueous ink contains titanium oxide particles which are titanium oxide in which at least a part of a surface is coated by alumina and silica, and dynamic surface tension γ10 in lifetime 10 milliseconds and dynamic surface tension γ5,000 in lifetime 5,000 milliseconds which are measured by a maximum bubble pressure method satisfies the relationship of γ5,000 / γ10≥0.80.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an inkjet recording method and an inkjet recording apparatus. [Background technology]

[0002] In recent years, inkjet recording devices have come to be widely used when printing advertisements and exhibits using recording media such as paper and resin film. For example, in order to express clear color images even on transparent recording media, white ink is used in addition to black and basic color inks (hereinafter, these may be collectively referred to as color inks). Specifically, a recording method is used in which white ink is applied in advance to a location on a transparent recording medium including an area where an image is to be recorded to perform base treatment, and color inks are applied on top of that, or each ink is applied in the reverse order (so-called back printing).

[0003] When printing advertisements or exhibits, not only absorbent recording media such as paper are used, but also non-absorbent recording media made of polyvinyl chloride (PVC) or polyethylene terephthalate (PET), whose surfaces have almost no ink absorption. Therefore, even with such recording media, it is necessary to suppress bleeding of images. Hereinafter, recording media that have almost no ink absorption will also be referred to as "non-absorbent recording media."

[0004] Non-absorbent recording media have a lower surface energy than absorbent recording media such as plain paper and glossy paper for inkjet printing, and therefore have the property of easily repelling ink. Water-based inks used in inkjet printing methods are required to be able to record images regardless of the recording medium.

[0005] To date, hydrophilization treatment of recording media, such as corona treatment, has been considered in order to form images with aqueous inks on recording media, including non-absorbent recording media (see Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2019-119115 A [Patent Document 2] International Publication No. 2017 / 138439 Summary of the Invention [Problem to be solved by the invention]

[0007] The present inventors recorded images by the inkjet recording methods proposed in Patent Documents 1 and 2, and investigated various characteristics of the images. As a result, unevenness was confirmed in low-density images, and disturbance was confirmed in high-density images, and it was found that there is room for improvement in performance.

[0008] It is therefore an object of the present invention to provide an inkjet recording method capable of recording an image in which unevenness and disturbance are suppressed regardless of the amount of ink applied. It is also an object of the present invention to provide an inkjet recording apparatus for use in the inkjet recording method. [Means for solving the problem]

[0009] The above object is achieved by the present invention, which is described below. That is, the inkjet recording method according to the present invention is an inkjet recording method for recording an image on a recording medium using an aqueous ink, comprising a pretreatment step of subjecting the recording medium to a corona treatment, and a recording step of applying the aqueous ink to at least a part of the area of ​​the recording medium that has been subjected to the corona treatment, wherein the aqueous ink contains titanium oxide particles that are titanium oxide at least a part of the surface of which is coated with alumina and silica, and has a dynamic surface tension γ at a lifetime of 10 milliseconds as measured by a maximum bubble pressure method. 10 , and the dynamic surface tension γ at a lifetime of 5,000 milliseconds 5,000 But, γ 5,000 / γ 10 ≧0.80. Effect of the Invention

[0010] According to the present invention, it is possible to provide an inkjet recording method capable of recording an image in which unevenness and disturbance are suppressed regardless of the amount of ink applied. Also, according to the present invention, it is possible to provide an inkjet recording apparatus used in the inkjet recording method. [Brief description of the drawings]

[0011] [Figure 1] 1A and 1B are diagrams illustrating an example of an inkjet recording apparatus used in the inkjet recording method of the present invention, in which (a) is a perspective view of the main part of the inkjet recording apparatus, and (b) is a perspective view of a head cartridge. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in more detail below with reference to preferred embodiments. In the present invention, when the compound is a salt, the salt is present in the ink in the form of dissociation into ions, but for convenience, it is expressed as "containing a salt." Titanium oxide and titanium oxide particles may be simply referred to as "pigment." Furthermore, water-based ink for inkjet printing may be simply referred to as "ink." Physical property values ​​are values ​​at room temperature (25°C) unless otherwise specified.

[0013] Inorganic oxides such as titanium oxide react with water molecules constituting the aqueous medium in the aqueous ink to generate hydroxyl groups (hereinafter, sometimes referred to as "surface hydroxyl groups") on the surface. For this reason, in the case of aqueous inkjet inks, in order to utilize the generated surface hydroxyl groups while further improving the storage stability of the ink, the ink is generally used in a state where the ink is surface-treated with inorganic oxides such as alumina or silica. The surface hydroxyl groups of titanium oxide particles have properties specific to the inorganic oxide corresponding to the inorganic compound used in the surface treatment, and the isoelectric point, which is an indicator of the strength of the acid, differs depending on the type of inorganic compound. Therefore, although titanium oxide itself is an inorganic oxide, the surface of titanium oxide particles shows the properties of an inorganic oxide corresponding to the inorganic compound used in the surface treatment, and the surface charge of titanium oxide particles is strongly dependent on the pH of the aqueous medium, the type of surface treatment agent, and the amount of the surface treatment agent used.

[0014] The present inventors have studied the causes of image unevenness and image disturbance depending on the amount of white ink applied in the inkjet recording methods of Patent Documents 1 and 2. Corona treatment is a treatment for modifying a recording medium to be hydrophilic by irradiating the recording medium with corona discharge. By generating anionic groups such as carboxylic acid groups and hydroxyl groups on the surface of the recording medium, the wettability of the ink to the recording medium is improved, and it becomes possible to record images with aqueous ink on a wide variety of recording media, including non-absorbent recording media. However, when a low-density image is recorded using white ink on a recording medium that has been subjected to corona treatment, image unevenness may occur and an uneven image may be recorded. Since the modification treatment by corona treatment is performed by a process that has randomness, namely corona discharge, there is a limit to performing the modification treatment uniformly, and variation in the degree of hydrophilization of the recording medium (treatment unevenness) occurs. When a low-density image is recorded, the whiteness is not so high, so it is considered that the unevenness of the image is emphasized due to the unevenness of the corona treatment.

[0015] Therefore, the present inventors have re-examined the possibility of suppressing unevenness in low-density images by devising ink composition, etc. As a result, they have found that by coating the surfaces of titanium oxide particles with silica, rather than just alumina, it is possible to reduce affinity with recording media and suppress unevenness in images.

[0016] However, it has been found that even when using ink containing the above-mentioned titanium oxide particles, which can suppress unevenness in low-density images, when a high-density image is recorded using white ink, image distortion occurs due to another processing unevenness in the corona treatment. When recording a color image that shows clear color development, white ink may be used to form a base, and high concealing properties are required for the white ink. In such a case, it is preferable to apply a large amount of white ink per unit area, and the ink is likely to overflow at the edge of the area on the recording medium where the white ink is applied. It is believed that if there is unevenness in the corona treatment at the edge, the overflowing white ink will flow into the non-recording area, causing image distortion.

[0017] Conventionally, the corona treatment of a recording medium has sometimes been performed offline rather than inline. In other words, it is known that a recording medium that has been previously subjected to corona treatment is used to perform recording by a recording device other than the device that performs the corona treatment. However, it has been found that the above-mentioned problem occurs to a significant level when the corona treatment and recording are performed in a series of steps in an inkjet recording device. When the corona treatment is performed offline or some time has passed since the modification treatment, the effect of the corona treatment gradually decreases and the unevenness of the treatment is evened out to some extent, so it is assumed that the above-mentioned problem is less likely to become apparent.

[0018] The present inventors further investigated how to suppress the disturbance in a high-density image, which occurs significantly when an image is recorded following a corona treatment, and discovered that the disturbance in a high-density image can be suppressed by controlling the dynamic surface tension of the ink.

[0019] That is, the inkjet recording method of the present invention has the following features. First, the ink contains a pigment. As the pigment, titanium oxide particles in which at least a part of the surface of titanium oxide is coated with alumina and silica are used. In addition, the dynamic surface tension γ at a life time of 10 milliseconds measured by the maximum bubble pressure method is 10 , and the dynamic surface tension γ at a lifetime of 5,000 milliseconds 5,000 is γ 5,000 / γ 10 ≧0.80. Then, the ink is applied to at least a part of the region of the recording medium that has been subjected to the corona treatment. The present inventors speculate as follows about the mechanism by which the above-mentioned configuration enables recording of an image in which unevenness and disturbance are suppressed, regardless of the amount of white ink applied.

[0020] As described above, the pretreatment process involves modifying the recording medium by subjecting it to corona discharge. This process improves the wettability of the ink on the recording medium, enabling stable image recording.

[0021] The titanium oxide particles are titanium oxide particles whose surface is at least partially coated with alumina and silica. As described above, the characteristics of the surface hydroxyl groups of titanium oxide are affected by the inorganic oxide coating the surface. In the alkaline region, which is the normal liquid property of aqueous inkjet inks, the surface hydroxyl groups derived from alumina tend to be positively charged, and the surface hydroxyl groups derived from silica tend to be negatively charged. Therefore, when the ink is applied to a recording medium, the positive charge of the surface hydroxyl groups derived from alumina and the anionic groups generated by the corona treatment of the recording medium have affinity, and an image can be recorded without the ink being repelled. And, by simultaneously presenting the surface hydroxyl groups derived from silica, the affinity is moderately suppressed, and even when a low-density image is recorded, the effect of uneven processing is reduced, and a uniform image with reduced unevenness can be recorded. Even if the titanium oxide particles are coated with alumina, if they are not coated with silica, the affinity between the titanium oxide particles and the anionic groups generated on the surface of the recording medium is high, and the titanium oxide particles are affected by uneven processing. As a result, unevenness in the image occurs when a low-density image is recorded.

[0022] The ink also has a certain dynamic surface tension characteristic. Specifically, the dynamic surface tension of the ink at a life time of 10 milliseconds, measured by the maximum bubble pressure method, is γ 10 , and the dynamic surface tension of the ink at a lifetime of 5,000 milliseconds γ 5,000 is γ 5,000 / γ 10 ≧0.80. The dynamic surface tension of the ink can be considered to correspond to the change in the surface state over time when the ink is applied to the recording medium and a new interface is formed. γ 10 corresponds to the surface tension in the process of the newly formed interface becoming stable, and γ 5,000 corresponds to the state where the newly formed interface is stable. In other words, the relationship between these two points allows us to grasp the state of the newly formed interface, which can be said to grasp the degree of aggregation of components that affect viscosity, such as surfactants (hereinafter, simply referred to as components).

[0023] If the relationship of the dynamic surface tension of the ink is within the above range, it means that the above components are present in large amounts near the newly formed interface. In areas where the above components are present in large amounts, the viscosity of the liquid tends to increase locally. Therefore, near the interface, the viscosity increases suddenly, suppressing the flow of the ink. If this phenomenon is applied to the movement of the above components in high-density image recording, since the above components are present in large amounts near the interface, that is, at the edges of the image where the ink is likely to overflow, the viscosity of the ink at the edges increases suddenly, suppressing image distortion. γ 5,000 / γ 10 If the ratio is less than 0.80, the movement of the above components to the interface is slow, so that when recording a high-density image, the viscosity of the ink at the edge of the image, which is prone to overflowing, is difficult to increase. Therefore, the ink overflows due to uneven processing, causing image distortion. In this specification, the dynamic surface tension of the ink is a value measured by the maximum bubble pressure method. The method for measuring the dynamic surface tension will be described in detail later.

[0024] <Inkjet recording method and inkjet recording apparatus> The inkjet recording method of the present invention (hereinafter, also simply referred to as "recording method") is a method of ejecting ink from an inkjet recording head to record an image on a recording medium. The recording method of the present invention has a pretreatment step of subjecting the recording medium to corona treatment, and a recording step of applying ink to the recording medium on at least a part of the region of the recording medium that has been subjected to corona treatment. In the inkjet recording method of the present invention, other steps than those steps that characterize the present invention may be known steps. For example, when white ink is used as a base treatment for color inks, an image may be recorded by applying color inks (inks such as black, cyan, magenta, and yellow) so as to overlap at least a part of the region to which the white ink has been applied. Furthermore, the method may also be used for back printing, in which white ink is applied so as to overlap at least a part of the region to which the color ink has been applied.

[0025] The inkjet recording apparatus of the present invention (hereinafter, simply referred to as the "recording apparatus") is an apparatus used for ejecting ink from an inkjet recording head to record an image on a recording medium. The recording apparatus of the present invention includes a pretreatment means for subjecting the recording medium to a corona treatment, and a recording means for applying ink to the recording medium at least in a part of the area of ​​the recording medium that has been subjected to the corona treatment.

[0026] If necessary, the recorded image may be heated. Methods for ejecting ink include a method of applying mechanical energy to the ink and a method of applying thermal energy to the ink. In the present invention, it is particularly preferable to adopt a method of ejecting ink by applying thermal energy to the ink.

[0027] FIG. 1 is a diagram showing an example of an inkjet recording device used in the inkjet recording method of the present invention, in which (a) is a perspective view of the main part of the inkjet recording device, and (b) is a perspective view of a head cartridge. The inkjet recording device is provided with a conveying means (not shown) for conveying a recording medium 32, and a carriage shaft 34. A head cartridge 36 can be mounted on the carriage shaft 34. The head cartridge 36 includes recording heads 38 and 40, and is configured so that an ink cartridge 42 is set thereon. While the head cartridge 36 is conveyed along the carriage shaft 34 in the main scanning direction, ink (not shown) is ejected from the recording heads 38 and 40 toward the recording medium 32. Then, an image is recorded on the recording medium 32 by conveying the recording medium 32 in the sub-scanning direction by a conveying means (not shown).

[0028] Multi-pass printing is preferred in which the application of ink to a unit area of ​​a print medium is performed by multiple relative scans of the print head and the print medium. In particular, it is preferred to apply white ink and color ink to a unit area by different relative scans. This increases the time until the inks come into contact with each other, making it easier to suppress mixing. The unit area can be set as any area, such as one pixel or one band.

[0029] (Pretreatment process) The pretreatment step is a step of subjecting the recording medium to a corona treatment. The surface of the recording medium can be made hydrophilic by the corona treatment. Whether or not hydrophilic groups have been generated on the recording medium by the corona treatment can be determined, for example, by the presence or absence of detection of functional groups such as hydroxyl groups (-OH) and carboxylic acid groups (-COOH) in the infrared absorption spectrum of the recording medium. The corona treatment can be performed by any known method or condition as long as hydrophilic groups are generated.

[0030] The transport speed of the recording medium during corona treatment is preferably 1 mm / s or more and 500 mm / s or less. The corona discharge irradiation distance is preferably 0.5 mm or more and 10.0 mm or less to stably ensure a distance that does not interfere with the recording medium being treated. The corona discharge amount is 1 W·min / m 2 More than 100W min / m 2 It is preferable that:

[0031] As described above, in the recording process of the present invention, the pretreatment process and the recording process are carried out in series (in-line). The time interval between the pretreatment process and the recording process is preferably short. Specifically, the time interval between the pretreatment process and the recording process is preferably within 5 minutes, more preferably within 1 minute, and particularly preferably within 30 seconds. Here, the time interval between the pretreatment process and the recording process is the time from the end of the corona treatment, which is the pretreatment process, to the application of ink to the recording medium in the recording process.

[0032] (Recording medium) In the recording method and recording device of the present invention, it is preferable to use a non-absorbent recording medium (a low to non-absorbent recording medium). A low to non-absorbent recording medium is one that is capable of being held in contact with the paper for 30 msec in the Bristow method described in JAPAN TAPPI Paper and Pulp Test Method No. 51 "Liquid Absorbency Test Method for Paper and Paperboard". 1 / 2 Water absorption up to 0mL / m 2 More than 10mL / m 2 In the present invention, a recording medium that satisfies the above-mentioned condition of water absorption amount is defined as a "low to non-absorbent recording medium". A recording medium for inkjet recording having a coating layer (ink receiving layer) formed of inorganic particles (glossy paper, matte paper, etc.) and plain paper having no coating layer have a water absorption amount of 10 mL / m 2 It is an "absorbent recording medium" that exceeds this.

[0033] Examples of low to non-absorbent recording media that can be used include plastic films; recording media in which a plastic film is bonded to the recording surface of a substrate; and recording media in which a resin coating layer is provided on the recording surface of a substrate containing cellulose pulp. Among these, plastic films are preferred, and recording media in which a resin coating layer is provided on the recording surface of a substrate containing cellulose pulp are also preferred. Since the aqueous ink of the present invention can be used as a white ink, it is preferred to use a transparent or colored recording medium.

[0034] <Water-based ink> The ink used in the recording method of the present invention is an aqueous inkjet ink containing titanium oxide particles, which are titanium oxide at least partly coated with alumina and silica. This ink is preferably a white ink since titanium oxide is a white pigment. The ink also has a dynamic surface tension γ at a life time of 10 milliseconds, as measured by the maximum bubble pressure method. 10 , and the dynamic surface tension γ at a lifetime of 5,000 milliseconds 5,000 But, γ 5,000 / γ 10 The relationship is ≧0.80.

[0035] The dynamic surface tension of the ink is measured by the maximum bubble pressure method. The maximum bubble pressure method is a method in which the maximum pressure required to release a bubble formed at the tip of a probe (capillary tube) immersed in the liquid to be measured is measured, and the surface tension of the liquid is calculated from the measured maximum pressure. In the maximum bubble pressure method, when a bubble is formed at the tip of the probe, the bubble leaves the tip and a new bubble surface is formed, and the lifetime is the time from the time when the bubble leaves the tip and a new bubble surface is formed, to the time when the maximum bubble pressure (the time when the radius of curvature of the bubble is equal to the radius of the tip of the probe) is measured. The dynamic surface tension of the ink in this specification is a value measured at 25°C. The dynamic surface tension of the ink can be adjusted by the type and content of the water-soluble organic solvent and surfactant.

[0036] The dynamic surface tension of the ink at a given life time is not particularly limited as long as it satisfies the above relationship. Specifically, the dynamic surface tension of the ink at a given life time (e.g., 10 ms, 5,000 ms) is preferably 25.0 mN / m or more and 65.0 mN / m or less, and more preferably 30.0 mN / m or more and 55.0 mN / m or less.

[0037] The components constituting the ink used in the recording process and the physical properties of the ink will be described in detail below.

[0038] (Colorant) The ink contains titanium oxide particles as a coloring material (pigment) in which the surface of titanium oxide is treated with a specific inorganic oxide. In other words, the ink contains titanium oxide particles, which are titanium oxide whose surface is coated with a specific inorganic oxide. The content (mass%) of titanium oxide particles in the ink is preferably 0.10% by mass or more and 20.00% by mass or less, based on the total mass of the ink. The content (mass%) of titanium oxide particles in the ink is more preferably 1.00% by mass or more and 20.00% by mass or less, based on the total mass of the ink. In particular, the content (mass%) of titanium oxide particles in the ink is particularly preferably 1.00% by mass or more and 15.00% by mass or less, based on the total mass of the ink.

[0039] Titanium oxide is a white pigment, and has three crystal forms: rutile, anatase, and brookite. Among them, rutile titanium oxide is preferred. Titanium oxide can be industrially produced by the sulfuric acid method and the chlorine method, and the titanium oxide used in the present invention may be produced by either method.

[0040] The volume-based cumulative 50% particle diameter (hereinafter also referred to as the average particle diameter) of the titanium oxide particles is preferably 200 nm or more and 500 nm or less. In particular, the volume-based cumulative 50% particle diameter of the titanium oxide particles is more preferably 200 nm or more and 400 nm or less. The volume-based cumulative 50% particle diameter of the titanium oxide particles (D 50) is the diameter of the particle that is 50% of the total volume of the measured particles in the particle size accumulation curve, calculated from the small particle size side. 50 can be measured under the following conditions: SetZero: 30 seconds, number of measurements: 3, measurement time: 180 seconds, shape: aspheric, refractive index: 2.60. A particle size analyzer using a dynamic light scattering method can be used as the particle size distribution measuring device. Of course, the measurement conditions are not limited to those described above.

[0041] Titanium oxide that has been surface-treated with alumina and silica is used. The surface treatment is expected to suppress photocatalytic activity and improve dispersibility. In this specification, "alumina" is a general term for oxides of aluminum such as aluminum oxide. In this specification, "silica" is a general term for silicon dioxide or a substance composed of silicon dioxide. Most of the alumina and silica that coat titanium oxide are present in the form of silicon dioxide and aluminum oxide.

[0042] The ratio (mass%) of titanium oxide in the titanium oxide particles is preferably 90.00 mass% or more based on the total mass of the titanium oxide particles. The ratio (mass%) of titanium oxide in the titanium oxide particles is preferably 98.50 mass% or less based on the total mass of the titanium oxide particles. The ratio (mass%) of alumina in the titanium oxide particles is preferably 0.30 times or more and 4.00 times or less in terms of mass ratio to the ratio (mass%) of silica. In particular, the ratio is more preferably 0.50 times or more and 2.00 times or less, and particularly preferably 0.50 times or more and 1.00 times or less. If the ratio is less than 0.30 times, the ratio of silica is too high, and affinity with the recording medium is not sufficiently obtained, and image unevenness and image disturbance may not be sufficiently suppressed. On the other hand, if the ratio is more than 4.00 times, the ratio of silica is too low, and affinity with the recording medium is too high, and image unevenness and image disturbance may not be sufficiently suppressed.

[0043] The ratio of alumina and silica in titanium oxide particles, i.e., the amount of alumina and silica coating, can be measured by, for example, quantitative analysis of aluminum and silicon elements by inductively coupled plasma (ICP) emission spectrometry. In this case, it is assumed that all atoms coated on the surface are oxides, and the obtained values ​​of aluminum and silicon can be calculated by converting them to their oxides, i.e., alumina and silica. The ratio (mass%) of aluminum element in titanium oxide particles obtained by inductively coupled plasma emission spectrometry is preferably 0.34 times or more and 4.53 times or less in mass ratio to the ratio (mass%) of silicon element. When this value is converted to its oxides, i.e., alumina and silica, the ratio (mass%) of alumina in titanium oxide particles is 0.30 times or more and 4.00 times or less in mass ratio to the ratio (mass%) of silica.

[0044] Surface treatment methods for titanium oxide include wet treatment and dry treatment. For example, titanium oxide can be dispersed in a liquid medium and then reacted with a surface treatment agent such as sodium aluminate or sodium silicate to perform surface treatment, and the desired characteristics can be achieved by appropriately changing the ratio of these surface treatment agents. In addition to alumina and silica, inorganic oxides such as zinc oxide and zirconia, and organic substances such as polyols can also be used for surface treatment, as long as the effects of the present invention are not impaired.

[0045] As long as the effect of the present invention is not impaired, the ink may contain other pigments besides titanium oxide. In this case, the ink may be of a color other than white ink. The content (mass %) of the other pigments in the ink is preferably 0.10 mass % or more and 5.00 mass % or less, and more preferably 0.10 mass % or more and 1.00 mass % or less, based on the total mass of the ink.

[0046] (Surfactant) The ink preferably contains a surfactant in order to satisfy a predetermined dynamic surface tension relationship. The surfactant in the present invention is a substance composed of a hydrophobic portion (such as a hydrocarbon chain, a perfluoroalkyl group, or a siloxane structure) and a hydrophilic portion (such as an ethylene oxide group). The content (mass%) of the surfactant in the ink is preferably 0.30 mass% or more and 2.00 mass% or less based on the total mass of the ink. If the content of the surfactant is less than 0.30 mass%, the viscosity at the edge of a high-density image is unlikely to increase, and image disturbance may not be sufficiently suppressed. Even if the content of the surfactant is more than 2.00 mass%, image disturbance may not be sufficiently suppressed.

[0047] Examples of the surfactant include anionic, cationic, and nonionic surfactants. Among them, nonionic surfactants are preferable because they have little effect on the dispersion state of titanium oxide particles and can be effective in small amounts. Examples of the nonionic surfactant include polyoxyethylene alkyl ethers, polyoxyethylene fatty acid esters, polyoxyethylene alkyl phenyl ethers, acetylene glycol surfactants (e.g., ethylene oxide adducts of acetylene glycol), and silicone surfactants.

[0048] In addition, from the viewpoint of compatibility with the liquid components of the ink, it is preferable to use a first surfactant having an HLB value of 8 or more and 11 or less as the surfactant contained in the ink. The "HLB value" of the surfactant in this specification is a value obtained by the Griffin method, and is calculated based on the formula: HLB value = 20 x (formula weight of hydrophilic group of surfactant) / (molecular weight of surfactant). The HLB value obtained by the Griffin method is a physical value that indicates the degree of hydrophilicity or lipophilicity of the surfactant, and takes a value of 0 to 20. The smaller the HLB value, the higher the lipophilicity, and the larger the HLB value, the higher the hydrophilicity. One or more types of surfactants can be used in the ink. The ratio (mass %) of the first surfactant to the surfactant in the ink is preferably 0.50 times or more. By setting the ratio in the above range, the surfactant quickly moves to the edge of a high-density image, and the viscosity is locally improved, thereby more effectively suppressing image disturbance.

[0049] (Compounds having sulfonic acid groups) The ink preferably further contains a compound having a sulfonic acid group. By containing a compound having a highly ionic sulfonic acid group in the ink, the sulfonic acid group easily attracts water, so that the viscosity is likely to increase rapidly at the edge of a high-concentration image. As a result, image distortion can be more effectively suppressed. The compound having a sulfonic acid group only needs to have at least one sulfonic acid group in the molecule. The content (mass %) of the compound having a sulfonic acid group in the ink is preferably 0.10 mass % or more and 0.50 mass % or less based on the total mass of the ink. Examples of the compound having a sulfonic acid group include inorganic compounds such as potassium sulfate, sodium sulfate, and sulfuric acid; and organic compounds such as taurine.

[0050] In addition, the resin may have a sulfonic acid group. In particular, it is preferable that the resin has a sulfonic acid group, and it is more preferable that the resin particles have a sulfonic acid group. The content (mass%) of the resin particles having a sulfonic acid group is preferably 0.10 mass% or more and 10.00 mass% or less.

[0051] (Compound represented by general formula (1)) The ink may contain a compound to aid in the dispersion of titanium oxide particles. In particular, it is preferable to contain a compound represented by the following general formula (1). The content (mass%) of the compound represented by general formula (1) in the ink is preferably 0.01% by mass or more and 1.00% by mass or less, and more preferably 0.02% by mass or more and 0.50% by mass or less, based on the total mass of the ink. Furthermore, the content (mass%) of the compound represented by general formula (1) in the ink is preferably 0.002 times or more and 0.10 times or less in mass ratio to the content (mass%) of titanium oxide particles.

[0052] A part of OR1 bonded to silicon atoms in the compound represented by general formula (1) is hydrolyzed in an aqueous medium to form a silanol group. Therefore, it has affinity with the surface hydroxyl groups derived from silica on the titanium oxide particle surface. In addition to the structure capable of forming a silanol group as described above, the compound represented by general formula (1) also has a structure having n alkylene oxide groups having 2 to 4 carbon atoms as repeating units ((OR4) in general formula (1)) via X, which serves as a linking group. n ) Hereinafter, the above structure will also be referred to as an alkylene oxide chain. Since the alkylene oxide chain is hydrophilic, it extends appropriately in an aqueous medium and exhibits a repulsive force due to steric hindrance. Therefore, the compound represented by general formula (1) has the effect of assisting the dispersion of titanium oxide particles.

[0053] [ka]

[0054] (In general formula (1), R1, R2, and R3 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. Each R4 is independently an alkylene group having 2 to 4 carbon atoms. X is a single bond or an alkylene group having 1 to 6 carbon atoms. n is 6 to 24. a is 1 to 3, b is 0 to 2, and a+b=3.)

[0055] In the general formula (1), R1, R2, and R3 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, and an n-butyl group. Among these, a methyl group is preferable from the viewpoint of ease of hydrolysis. a representing the number of R1O is 1 to 3, and b representing the number of R2 is 0 to 2, and a+b=3. Among these, it is preferable that a is 3 and b is 0, that is, all three substituents of the silicon atom are R1O.

[0056] In the general formula (1), R4 is independently an alkylene group having 2 to 4 carbon atoms. Examples of the alkylene group having 2 to 4 carbon atoms include an ethylene group, an n-propylene group, an i-propylene group, and an n-butylene group. Among them, an ethylene group is preferable. The number of OR4, that is, n (average value) representing the number of alkylene oxide groups, is 6 to 24.

[0057] In the general formula (1), X is a single bond or an alkylene group having 1 to 6 carbon atoms. When X is a single bond, it means that the silicon atom and OR4 are directly bonded. Examples of the alkylene group having 1 to 6 carbon atoms include a methylene group, an ethylene group, an n-propylene group, an i-propylene group, an n-butylene group, an n-pentylene group, and an n-hexylene group. Among them, an n-propylene group is preferable.

[0058] (resin) The ink may contain a resin. Examples of the resin include acrylic resin, urethane resin, and urea resin. Of these, acrylic resin is preferred. The content (mass%) of the resin in the ink is preferably 1.00% by mass or more and 25.00% by mass or less, and more preferably 3.00% by mass or more and 15.00% by mass or less, based on the total mass of the ink. Of these, the content of 5.00% by mass or more and 15.00% by mass or less is particularly preferred.

[0059] The resin can be contained in the ink for the purpose of improving various properties of the recorded image, such as abrasion resistance and concealment. Examples of the form of the resin include block copolymers, random copolymers, graft copolymers, and combinations thereof. The resin may be a water-soluble resin that can be dissolved in an aqueous medium, or may be resin particles that are dispersed in an aqueous medium. As described above, it is preferable to use a resin having a sulfonic acid group as the compound having a sulfonic acid group, and it is more preferable to use resin particles having a sulfonic acid group. The resin particles do not need to encapsulate a coloring material.

[0060] In this specification, "a resin is water-soluble" means that when the resin is neutralized with an alkali equivalent to the acid value, the resin is present in an aqueous medium in a state in which it does not form particles whose particle size can be measured by a dynamic light scattering method. Whether or not a resin is water-soluble can be determined according to the following method. First, a liquid (resin solid content: 10 mass%) containing a resin neutralized with an alkali (sodium hydroxide, potassium hydroxide, etc.) equivalent to the acid value is prepared. Next, the prepared liquid is diluted 10 times (volume basis) with pure water to prepare a sample solution. Then, when the particle size of the resin in the sample solution is measured by a dynamic light scattering method, if particles having a particle size are not measured, the resin can be determined to be water-soluble. The measurement conditions at this time can be, for example, SetZero: 30 seconds, number of measurements: 3 times, and measurement time: 180 seconds. As a particle size distribution measurement device, a particle size analyzer using a dynamic light scattering method (for example, the product name "UPA-EX150", manufactured by Nikkiso) can be used. Of course, the particle size distribution measurement device and measurement conditions used are not limited to those described above.

[0061] The acid value of the water-soluble resin is preferably 80 mgKOH / g or more and 250 mgKOH / g or less, more preferably 100 mgKOH / g or more and 200 mgKOH / g or less. When resin particles are used, the acid value is preferably 0 mgKOH / g or more and 50 mgKOH / g or less. The weight average molecular weight of the water-soluble resin is preferably 1,000 or more and 30,000 or less, more preferably 5,000 or more and 15,000 or less. The weight average molecular weight of the resin constituting the resin particles is preferably 1,000 or more and 3,000,000 or less, more preferably 100,000 or more and 3,000,000 or less. The weight average molecular weight of the resin is a value measured by gel permeation chromatography (GPC) in terms of polystyrene.

[0062] (aqueous medium) The ink is an aqueous ink containing water as an aqueous medium. The ink may contain water or an aqueous medium that is a mixed solvent of water and a water-soluble organic solvent. As the water, it is preferable to use deionized water (ion-exchanged water). The content (mass %) of water in the ink is preferably 50.00 mass % or more and 95.00 mass % or less based on the total mass of the ink.

[0063] The water-soluble organic solvent is not particularly limited as long as it is water-soluble (preferably, dissolves in water at 25°C in any ratio). Specifically, monohydric or polyhydric alcohols, alkylene glycols, glycol ethers, nitrogen-containing polar compounds, sulfur-containing polar compounds, etc. can be used. The content (mass%) of the water-soluble organic solvent in the ink is preferably 3.00% by mass or more and 50.00% by mass or less, and more preferably 10.00% by mass or more and 40.00% by mass or less, based on the total mass of the ink. If the content (mass%) of the water-soluble organic solvent is less than 3.00% by mass, the ink may be stuck in the inkjet recording device, and sufficient sticking resistance may not be obtained. If the content (mass%) of the water-soluble organic solvent is more than 50.00% by mass, poor ink supply may occur. The water-soluble organic solvent does not include "surfactants".

[0064] (Other additives) In addition to the additives described above, the ink may contain various additives, such as a pH adjuster, an antirust agent, an antiseptic, an antifungal agent, an antioxidant, an antireducing agent, an evaporation promoter, and a chelating agent, as necessary.

[0065] (Ink properties) Since the ink is applied to the inkjet method, it is preferable to appropriately control the physical properties of the ink. The static surface tension of the ink at 25°C is preferably 10 mN / m or more and 60 mN / m or less, and more preferably 20 mN / m or more and 40 mN / m or less. The static surface tension of the ink can be adjusted by appropriately determining the type and content of the surfactant in the ink. In addition, the viscosity of the ink at 25°C is preferably 1.0 mPa·s or more and 10.0 mPa·s or less. The pH of the ink at 25°C is preferably 7.0 or more and 9.0 or less. The pH of the ink can be measured with a general pH meter equipped with a glass electrode or the like. EXAMPLES

[0066] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples in any way as long as it does not deviate from the gist of the invention. "Parts" and "%" used to describe the amounts of components are based on mass unless otherwise specified. In addition, a dispersion of titanium oxide particles is referred to as a "pigment dispersion."

[0067] <Preparation of titanium oxide particles> Commercially available titanium oxide particles that had been surface-treated in advance and titanium oxide particles prepared by surface-treating untreated titanium oxide were used. The cumulative 50% particle diameter (D 50) was measured using a particle size analyzer using dynamic light scattering (trade name "Nanotrac WaveII-EX150", manufactured by Microtrack Bell). The properties of titanium dioxide particles are shown in Table 1. In Table 1, TITANIX: JR, JR-301, JR-403, JR-405, JR-600A, and JR-800 are trade names for rutile-type titanium dioxide manufactured by Teika. TITONE R-7E is the trade name for rutile-type titanium dioxide manufactured by Sakai Chemical Industry Co., Ltd. Typec: R-780 and R-780-2 are trade names for rutile-type titanium dioxide manufactured by Ishihara Sangyo Kaisha.

[0068] (Measurement of the amount of alumina and silica coating) The ratio of alumina and silica in the titanium oxide particles, i.e., the amount of alumina and silica coating, was measured as follows. The prepared titanium oxide particles were added to nitric acid to prepare a liquid, and quantitative analysis of aluminum and silicon elements was performed using an inductively coupled plasma (ICP) emission spectrometer. In this case, it was assumed that all atoms coating the surface were in the form of oxides, and the obtained values ​​of aluminum and silicon were converted to the oxides, i.e., alumina and silica, to calculate the mass ratio.

[0069] (Titanium oxide particles 1, 6, 8, 9) Titanium oxide particles were produced by surface treatment of the titanium oxide using a wet method. Surface treatment using the wet method involves contacting untreated titanium oxide with a surface treatment agent (sodium aluminate, sodium silicate, etc.), and the amount and ratio of the surface treatment agent used were appropriately adjusted to provide a surface treatment at any ratio.

[0070] Specifically, 300 parts of rutile-type titanium oxide (trade name "TITANIX JR", manufactured by Teika Co., Ltd.) that had not been subjected to surface treatment and 700 parts of pure water were mixed with a homogenizer. Then, the temperature was raised to 90°C while stirring, and potassium hydroxide (pH adjuster) was added to adjust the pH to 10.5. Next, sodium silicate was added, and dilute sulfuric acid (pH adjuster) was added over about 1 hour to adjust the pH to 5.0. The reaction was continued for about 1 hour. Thereafter, sodium aluminate was added little by little at 90°C. At this time, in order to maintain the pH, dilute sulfuric acid was used in combination to maintain the pH at 6.0 to 8.0. After the addition of sodium aluminate, the reaction was continued for about 1 hour to obtain a dispersion. The dispersion was cooled to 25°C, and then purified by repeatedly sedimenting with a centrifuge and redispersing in ion-exchanged water, and dried at 120°C to obtain titanium oxide particles that had been subjected to surface treatment with at least one of alumina and silica. Table 1 shows the characteristics of each titanium oxide particle.

[0071] (Titanium oxide particles 2-5, 7, 10-13) Commercially available titanium oxide particles (including those that have been previously surface-treated with alumina or silica) were used as titanium oxide particles 2 to 5, 7, and 10 to 13. Table 1 also shows the properties of the titanium oxide particles. Some commercially available titanium oxide particles contain inorganic oxides such as zirconia and zinc oxide, and organic compounds such as polyols, in addition to alumina and silica, but the proportion of these is at most about 1.00%. Therefore, for convenience, the proportion of titanium oxide in the titanium oxide particles is shown as T (%) ("Titanium oxide T (%)" in Table 1).

[0072] [Table 1]

[0073] <Preparation of the compound represented by general formula (1)> The compound represented by general formula (1) was synthesized by the following procedure. The synthesis conditions and structures of the compound synthesized as the compound represented by general formula (1) and the comparative compound are shown in Tables 2 and 3, respectively. The compound represented by general formula (1) can be synthesized by allylation and hydrosilylation of a raw material (such as a polyalkylene glycol monoalkyl ether).

[0074] The raw materials, base, and solvent shown in Table 2 were placed in a three-neck flask equipped with a stirrer and a nitrogen inlet tube, and stirred at 25°C for 30 minutes. As the "sodium hydride", a paraffin dispersion of 60% sodium hydride was used, and the dispersion was used so that the amount of sodium hydride used was as shown in Table 2. Then, the bromide shown in Table 2 was added dropwise while stirring at 25°C, and stirring was continued for 12 hours after the end of the dropwise addition to obtain a solution containing the reactants. After filtering out the unreacted sodium hydride and neutralized product (sodium bromide) from the solution containing the reactants, THF was removed under reduced pressure to obtain a concentrate. The concentrate was dissolved in 500 parts of pure water, and this aqueous solution was extracted three times with 200 mL of hexane, and then extracted with 200 mL of dichloromethane. The solvent containing the product was dried by adding magnesium sulfate, and concentrated under reduced pressure to obtain each of the allylated compounds (allylation process).

[0075] The allylated raw materials and silane compounds shown in Table 2 were placed in a dry, passivated round-bottom flask equipped with a stirrer and an argon inlet tube, and stirred at 85°C. Then, 0.54 parts of an aqueous solution of 65 mmol / L chloroplatinic acid monohydrate in isopropyl alcohol was added, and the mixture was heated at 85°C for 5 hours. After the reaction was completed, the mixture was allowed to cool to 25°C, and the excess silane compounds were removed under reduced pressure. The residue was purified by column chromatography using silica gel passivated with triethoxysilane as a carrier to obtain each compound (hydrosilylation step). The eluent used for purification by column chromatography was ethyl acetate / hexane / ethanol = 85 / 15 / 5 (by volume).

[0076] [Table 2]

[0077] [Table 3]

[0078] <Preparation of pigment dispersion> 40.00 parts of titanium oxide particles shown in Table 4, a dispersant, a neutralizer (potassium hydroxide), and ion-exchanged water with a total of 100.00 parts of the components were mixed and pre-dispersed using a homogenizer. Then, dispersion treatment (main dispersion) was performed for 12 hours at 25°C using a paint shaker using 0.5 mm zirconia beads. The amount of potassium hydroxide used was appropriately adjusted so that the pH of the main dispersion was 10.5. The pH of the main dispersion was measured using a pH meter (trade name "Portable pH Meter D-74", manufactured by Horiba, Ltd.) at the time of starting the main dispersion. The zirconia beads were filtered off, and an appropriate amount of ion-exchanged water was added as necessary to prepare pigment dispersions 1 to 15 with a titanium oxide particle content of 40.00%.

[0079] [Table 4]

[0080] <Preparation of resin particles> (Resin particles 1) Resin particles having sulfonic acid groups (resin particles 1) were synthesized according to the method for preparing resin particle dispersion 1 in JP 2014-101492 A. Specifically, 35.0 parts of butyl methacrylate, 2.0 parts of n-hexadecane, and 2.0 parts of 2,2'-azobis-(2-methylbutyronitrile) were placed in a four-neck flask equipped with a stirrer, a reflux condenser, and a nitrogen gas inlet tube, and stirred for 30 minutes. 61.0 parts of a 5.0% by mass aqueous solution of polyoxyethylene cetyl ether (trade name "Nikkol BC15", manufactured by Nikko Chemicals) was dropped and stirred for 30 minutes. Then, using an ultrasonic irradiation machine S-150D digital sonifier (manufactured by Branson), dispersion was performed under conditions of 400W, 20kHz, and 3 hours, and then polymerization reaction was performed under a nitrogen atmosphere at 80°C for 4 hours.

[0081] 73.0 parts of the above liquid were heated to 70°C under a nitrogen atmosphere, and 7.9 parts of ion-exchanged water and 0.1 parts of potassium persulfate were added. 10.0 parts of butyl methacrylate, 3.0 parts of methacrylic acid, 3.0 parts of 1,4-butanediol dimethacrylate, and 3.0 parts of Aqualon KH-05 (a reactive surfactant having a sulfonic acid group, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) were mixed into this liquid, and the emulsified liquid was dropped over 1 hour, heated to 85°C, and stirred for 2 hours. After cooling to 25°C, ion-exchanged water and an aqueous solution containing potassium hydroxide equimolar to the acid value of the resin particles were added to prepare an aqueous dispersion of resin particles 1 having a sulfonic acid group with a resin particle content of 30.00%. The cumulative 50% particle diameter based on volume of resin particles 1 was 200 nm.

[0082] (Resin particles 2) A liquid containing commercially available acrylic resin particles (product name "Vinyblan 2685", manufactured by Nissin Chemical Industry Co., Ltd.) was used as the aqueous dispersion of resin particles 2. The content of resin particles 2 was 30.00%.

[0083] <Preparation of surfactant> The properties of the surfactants used in preparing the inks are shown in Table 5. In Table 5, in the column "First surfactant", whether or not it was the first surfactant was indicated by a circle or an x.

[0084] [Table 5]

[0085] <Ink Preparation> The types and amounts of each component shown in the upper rows of Tables 6 to 9 were mixed and stirred. Proxel GXL(S) (trade name) is a preservative manufactured by LONZA. Then, pressure filtration was performed using a membrane filter (manufactured by Sartorius) with a pore size of 5.0 μm to prepare each ink. In Tables 6 to 9, γ 10 , and γ 5,000indicates the dynamic surface tension at a life time of 10 milliseconds and at a life time of 5,000 milliseconds, respectively. The ion-exchanged water containing potassium hydroxide is ion-exchanged water containing potassium hydroxide for adjusting the pH of each ink to 8.0, and the remaining amount was added so that the total of the components was 100.00%. The dynamic surface tension of each ink was measured at 25°C using a dynamic surface tensiometer (product name "BUBLE PRESSURE TENSIOMETER BP-2", manufactured by KRUSS) using the maximum bubble pressure method. The ratio of the first surfactant to the surfactant is shown in the column "Ratio of the first surfactant (times)". In addition, the content of the compound represented by general formula (1) is shown in the column "Content D (%) of specific compound".

[0086] [Table 6]

[0087] [Table 7]

[0088] [Table 8]

[0089] [Table 9]

[0090] <Evaluation> The inks obtained above were evaluated for the following items. In the present invention, for each of the evaluation criteria for the following items, "AAA" to "B" were considered acceptable levels, and "C" was considered unacceptable. The evaluation results are shown in Table 10.

[0091] Each ink obtained above was filled into an ink cartridge, and the cartridge was set in an inkjet recording device (product name "PIXUS PRO-10S", manufactured by Canon) equipped with a recording head that ejects ink by thermal energy. In this embodiment, the recording duty of a solid image recorded under the condition that four ink droplets of about 3.8 ng are applied to a unit area of ​​1 / 600 inch x 1 / 600 inch is defined as 100%.

[0092] The recording medium was subjected to corona treatment using a corona surface modification evaluation device (product name "TEC-4AX", manufactured by Kasuga Electric Co., Ltd.). The conditions of the corona treatment were irradiation speed 500 mm / min, irradiation distance 1 mm, and corona discharge amount 50 W·min / m 2 The corona treatment was performed appropriately by measuring the IR spectrum of the recording medium and confirming that it had hydrophilic groups (the presence of hydroxyl groups and carboxylic acid groups). The recording medium used was a non-absorbent recording medium, product name "WINTERIOR GIY-0315" (manufactured by Lintec Sign Systems, material: polyethylene terephthalate, 30 msec from the start of contact in the Bristow method). 1 / 2 Water absorption up to 0mL / m 2 More than 10mL / m 2 The composition of Comparative Example 1 was not subjected to corona treatment.

[0093] Using the above-mentioned inkjet recording device (serial method), a pattern was recorded on the above-mentioned recording medium, with the ink recording duty of 80%, in which a total of 15 solid images of 3 x 5 were arranged. At this time, the moving speed in the main scanning direction (reciprocating scanning direction) of the carriage carrying the recording head was 12.7 cm / s. After the ink was applied, the recording medium was not transported in the sub-scanning direction (paper feed direction), and hot air at 80°C was blown for 10 seconds from a position 10 mm above the recording medium, and then the paper was discharged, and a solid image was recorded. The hot air was generated by a hot air dryer (product name "TSK hot air dryer TSK-18", manufactured by Kansai Electric Heating Co., Ltd.) and blown from a nozzle with a diameter of 4 mm. The wind speed was 30.0 m / s. This recording was performed by setting the recording medium in the recording device after the corona treatment, and it was assumed that the ink was applied continuously after the corona treatment in the inkjet recording device. Specifically, the recording process was started within 30 seconds after the corona treatment as a pretreatment process. However, in Comparative Example 2, assuming offline corona treatment, the recording medium was placed in an environment of 25°C and 1 atm for 48 hours after the corona treatment, and then recording was performed.

[0094] The above-mentioned hot air drying is not intended to dry all of the liquid components of the recorded image. This is a preliminary drying to suppress transfer or loss due to contact with the image, such as a paper press of the recording medium, when handling the recording medium in the next process after recording. Preliminary drying makes the recording medium easier to handle. After that, the obtained solid image was placed in an oven at 80°C for 6 minutes to sufficiently dry the liquid components on the surface of the recording medium, thereby obtaining an evaluation image with low density. In addition, a high-density evaluation image was obtained by carrying out the same operations as above, except that the recording duty of the ink was set to 550%.

[0095] (Suppression of image unevenness) The occurrence of image unevenness in the low-density evaluation image was visually confirmed, and the suppression of image unevenness in the low-density image was evaluated according to the evaluation criteria shown below. AAA: No image unevenness was observed in any of the images. AA: Image unevenness was observed in 1 to 2 solid images. A: Image unevenness was observed in 3 to 4 solid images. B: Image unevenness was observed in 5 to 6 solid images. C: Image unevenness was observed in 7 or more solid images.

[0096] (Image distortion suppression) The occurrence of image disturbance in the high-density evaluation image was visually confirmed, and the suppression of image disturbance in the low-density image was evaluated according to the following evaluation criteria. AAA: No image distortion due to ink overflow was observed at the edges of any of the images. AA: Image distortion due to ink overflow was confirmed in one or more but not more than two solid images. A: Image unevenness was observed in 3 to 5 solid images. B: Image unevenness was observed in 6 to 9 solid images. C: Image unevenness was observed in 10 or more solid images.

[0097] [Table 10]

[0098] The disclosure of this embodiment includes the following configurations and methods.

[0099] [Method 1] An inkjet recording method for recording an image on a recording medium using a water-based ink, comprising the steps of: a pretreatment step of subjecting the recording medium to a corona treatment; a recording step of applying the water-based ink to at least a part of the area of ​​the recording medium that has been subjected to the corona treatment, The aqueous ink contains titanium oxide particles, which are titanium oxide particles having at least a portion of their surface covered with alumina and silica, and has a dynamic surface tension γ at a life time of 10 milliseconds measured by a maximum bubble pressure method. 10 , and the dynamic surface tension γ at a lifetime of 5,000 milliseconds 5,000 But, γ 5,000 / γ 10 ≧0.80.

[0100] [Method 2] The inkjet recording method according to Method 1, wherein the proportion (mass %) of the alumina in the titanium oxide particles is 0.30 to 4.00 times the proportion (mass %) of the silica in the titanium oxide particles.

[0101] [Method 3] 3. The inkjet recording method according to claim 1, wherein the aqueous ink contains a surfactant including a first surfactant having an HLB value of 8 or more and 11 or less.

[0102] [Method 4] The inkjet recording method according to Method 3, wherein the ratio (mass %) of the first surfactant to the total surfactants in the aqueous ink is 0.50 times or more.

[0103] [Method 5] The inkjet recording method according to Method 3 or 4, wherein the content (mass %) of the surfactant in the aqueous ink is from 0.30 mass % to 2.00 mass % based on the total mass of the ink.

[0104] [Method 6] 6. The inkjet recording method according to any one of Methods 1 to 5, wherein the water-based ink further contains a resin having a sulfonic acid group.

[0105] [Method 7] 7. The inkjet recording method according to any one of Methods 1 to 6, wherein the water-based ink further contains a compound represented by the following general formula (1):

[0106] [ka]

[0107] (In general formula (1), R1, R2, and R3 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and R4 is an alkylene group having 2 to 4 carbon atoms. X is a single bond or an alkylene group having 1 to 6 carbon atoms. n is 6 to 24. a is 1 to 3, b is 0 to 2, and a+b=3.)

[0108] [Method 8] The recording medium is subjected to a Bristow method for 30 msec from the start of contact. 1 / 2 Water absorption up to 10mL / m 2 8. The inkjet recording method according to any one of Methods 1 to 7, wherein the recording medium is:

[0109] [Configuration 1] An inkjet recording apparatus used for recording an image on a recording medium using a water-based ink, comprising: a pretreatment means for subjecting the recording medium to a corona treatment; a recording means for applying the water-based ink to at least a part of the area of ​​the recording medium that has been subjected to the corona treatment, The aqueous ink contains titanium oxide particles, which are titanium oxide particles having at least a portion of their surface covered with alumina and silica, and has a dynamic surface tension γ at a life time of 10 milliseconds measured by a maximum bubble pressure method. 10 , and the dynamic surface tension γ at a lifetime of 5,000 milliseconds 5,000 But, γ 5,000 / γ 10 ≧0.80.

Claims

1. An inkjet recording method for recording an image on a recording medium using a water-based ink, comprising the steps of: a pretreatment step of subjecting the recording medium to a corona treatment; a recording step of applying the water-based ink to at least a part of the area of ​​the recording medium that has been subjected to the corona treatment, The aqueous ink contains titanium oxide particles, which are titanium oxide particles having at least a portion of their surface covered with alumina and silica, and has a dynamic surface tension γ at a life time of 10 milliseconds measured by a maximum bubble pressure method. 10 , and the dynamic surface tension γ at a lifetime of 5,000 milliseconds 5,000 But, γ 5,000 / γ 10 ≧0.

80.

2. 2. The inkjet recording method according to claim 1, wherein a ratio (mass %) of the alumina in the titanium oxide particles is 0.30 to 4.00 times the ratio (mass %) of the silica in the titanium oxide particles.

3. The inkjet recording method according to claim 1 , wherein the water-based ink contains a surfactant including a first surfactant having an HLB value of 8 or more and 11 or less.

4. The inkjet recording method according to claim 3 , wherein a ratio (mass %) of the first surfactant to the total surfactants in the aqueous ink is 0.50 times or more.

5. The inkjet recording method according to claim 3, wherein a content (% by mass) of the surfactant in the aqueous ink is from 0.30% by mass to 2.00% by mass, based on the total mass of the ink.

6. The ink-jet recording method according to claim 1 , wherein the water-based ink further contains a resin having a sulfonic acid group.

7. The inkjet recording method according to claim 1 , wherein the water-based ink further contains a compound represented by the following general formula (1): 【Chemistry 1】 (In general formula (1), R 1 , R 2 , and R 3 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; R 4 is an alkylene group having 2 to 4 carbon atoms; X is a single bond or an alkylene group having 1 to 6 carbon atoms; n is 6 to 24; a is 1 to 3, b is 0 to 2, and a+b=3.

8. The recording medium is 1/2 The amount of water absorbed is 10 mL / m 2 The ink jet recording method according to claim 1, wherein the recording medium is:

9. An inkjet recording apparatus used for recording an image on a recording medium using a water-based ink, comprising: a pretreatment means for subjecting the recording medium to a corona treatment; a recording means for applying the water-based ink to at least a part of the area of ​​the recording medium that has been subjected to the corona treatment, The aqueous ink contains titanium oxide particles, which are titanium oxide particles having at least a portion of their surface covered with alumina and silica, and has a dynamic surface tension γ at a life time of 10 milliseconds measured by a maximum bubble pressure method. 10 , and the dynamic surface tension γ at a lifetime of 5,000 milliseconds 5,000 But, γ 5,000 / γ 10 ≧0.80.

Citation Information

Patent Citations

  • Inkjet recording method

    JP2019119115A

  • Ink jet recording method

    WO2017138439A1