Polishing pad
The polishing pad with a curable resin composition for the end point detection window addresses slicing defects and scratches by using a specific polyol and polyester polyol blend, ensuring consistent hardness and transparency for accurate optical detection.
Patent Information
- Application Number
- JP2023053211
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
The occurrence of slicing defects and scratches during the polishing process due to deformation or breakage of the end point detection window, and the difference in material properties between the pad body and window component leading to scratches during polishing.
A polishing pad with an end point detection window made from a curable resin composition containing a polyisocyanate compound and a curing agent, including a low molecular weight polyol and a trifunctional or higher functional polyester polyol, with a specific hardness ratio and molecular weight range to ensure compatibility and durability.
The solution effectively suppresses slicing defects and scratches by maintaining consistent hardness and transparency, ensuring accurate optical detection and reducing material degradation.
Smart Images

Figure 2024141513000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polishing pad. In particular, the present invention relates to a polishing pad that can be suitably used for polishing optical materials, semiconductor wafers, semiconductor devices, hard disk substrates, and the like. [Background technology]
[0002] Chemical mechanical polishing (CMP) is commonly used as a polishing method for planarizing the surfaces of optical materials, semiconductor wafers, semiconductor devices, and hard disk substrates.
[0003] The CMP method will be described with reference to FIG. 1. As shown in FIG. 1, a polishing apparatus 1 for carrying out the CMP method is provided with a polishing pad 3, which contacts an object 8 to be polished held on a holding platen 16 and includes a polishing layer 4, which is a layer for polishing, and a cushion layer 6 for supporting the polishing layer 4. The polishing pad 3 is rotated while the object 8 to be polished is pressed against it, and polishes the object 8 to be polished. At that time, a slurry 9 is supplied between the polishing pad 3 and the object 8 to be polished. The slurry 9 is a mixture (dispersion liquid) of water, various chemical components, and hard fine abrasive grains, and the chemical components and abrasive grains in the slurry are flowed and move relative to the object 8 to increase the polishing effect. The slurry 9 is supplied to the polishing surface through grooves or holes and discharged.
[0004] In the CMP method, it is possible to confirm by an optical method whether the workpiece 8 has been polished to a desired position. For example, the polishing apparatus 1 shown in Fig. 1 is equipped with an optical sensor 14 for confirming the end point. Specifically, a light-transmitting end point detection window 5 is provided in a part of the polishing layer 4, and further, a light source 13 and an optical sensor 14 are provided below the polishing platen 10.
[0005] The principle of detecting the end point by an optical method will be described with reference to Fig. 2. When light 2 irradiated by a light source 13 is incident on a thin film (e.g., an insulating film) 12 formed on a substrate 11, which is an object to be polished 8, a part of the light 2a is reflected by the surface of the thin film 12, while another part of the light 2b passes through the thin film 12 and is reflected by the surface of the object to be polished 8. The reflected lights 2a and 2b pass through an end point detection window 5 and are detected by an optical sensor 14, and the phase difference and intensity of the reflected lights vary depending on the thickness of the thin film 12, and by detecting the phase difference and the change in reflection intensity, the polishing status of the thin film 12 can be confirmed.
[0006] An example of a polishing pad used in such a chemical mechanical polishing method using optical end point detection is Patent Document 1. Patent Document 1 discloses that, for the purpose of providing a polishing pad that can increase the detection accuracy of the polishing rate by suppressing accumulation of slurry in a groove formed by joining a window member and a pad body when the window member is fitted into an opening in the pad body, a polishing pad having a pad body and a transparent window member formed integrally with a part of the pad body is provided, in which the material of the window member has higher abrasiveness than the material of the pad body, and the surface of the window member is recessed from the surface of the pad body so that the window member does not protrude from the surface of the pad body. However, because the material of this window member is different from that of the pad body, when the pad body and the window member are heated and sliced, the physical properties (especially hardness) of the pad body and the window member differ, which may cause deformation or damage to the window member and lead to poor slicing. Also, the pad body and the window member come into contact during polishing, but because the materials of the pad body and the window member are different, scratches may occur due to the polishing characteristics of the window member, which may ultimately have an adverse effect. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2002-001647 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention aims to provide a polishing pad that suppresses the occurrence of slicing defects due to deformation or damage of the end point detection window during slicing, and suppresses the occurrence of scratches due to the end point detection window during polishing. [Means for solving the problem]
[0009] The present inventors have found that the above problems can be solved by using a curing agent containing at least a low-molecular-weight polyol and a polyester polyol having three or more functional groups as a curing agent contained in the curable resin composition that constitutes the endpoint detection window, and have thus completed the present invention. That is, the present invention includes the following. [1] A polishing pad having a polishing layer and an endpoint detection window integrally formed in a portion of the polishing layer, the end point detection window is a cured product of a curable resin composition containing a polyisocyanate compound and a curing agent, The curing agent comprises a low molecular weight polyol and a polyester polyol having three or more functional groups; A polishing pad, wherein the value obtained from the following formula (1) is 0.65 or more. (D hardness of the end point detection window at 80°C) / (D hardness of the end point detection window at 20°C) Equation (1) [2] The polishing pad according to [1], wherein the polyester polyol has a number average molecular weight of 1,000 to 2,000. [3] The polishing pad according to [1], wherein the polyester polyol has a functionality of 3. [4] The polishing pad according to [1], wherein the weight ratio of the polyester polyol to the low molecular weight polyol (polyester polyol:low molecular weight polyol) is 80:20 to 98:2. [5] The polishing pad according to [1], wherein the molecular weight of the low molecular weight polyol is 80 to 150. [6] The polishing pad described in [1], wherein the curing agent comprises a polyether polyol. [7] The polishing pad according to [6], wherein the polyether polyol has a number average molecular weight of 500 to 2,000. Effect of the Invention
[0010] The polishing pad can suppress the occurrence of poor slicing due to deformation or damage of the end point detection window during slicing, and can suppress the occurrence of scratches due to the end point detection window during polishing. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a perspective view of a polishing apparatus 1. As shown in FIG. [Diagram 2] FIG. 2 is a schematic diagram showing the paths of incident and reflected light. [Diagram 3] FIG. 3 is a perspective view of a polishing pad 3 of the present invention. [Figure 4] FIG. 4 is a cross-sectional view (cross-sectional view taken along the line AA') of the polishing pad 3 of the present invention. [Diagram 5] FIG. 5 is a diagram showing one embodiment of forming the polishing layer 4. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, a mode for carrying out the invention will be described, however, the present invention is not limited to the mode for carrying out the invention. The number average molecular weight described in this specification can be measured by gel permeation chromatography (GPC). When measuring the number average molecular weight of a polyol compound from a polyurethane resin, each component can be decomposed by a conventional method such as amine decomposition, and then the number average molecular weight can be estimated by GPC.
[0013] <<Polishing pad>> The polishing pad 3 has a polishing layer 4 and an end point detection window 5 formed integrally with a part of the polishing layer 4, the end point detection window 5 being a cured product of a curable resin composition containing a polyisocyanate compound and a curing agent, the curing agent containing a low molecular weight polyol and a polyester polyol having three or more functionalities, and the ratio of the D hardness of the end point detection window 5 at 80°C to the D hardness of the end point detection window 5 at 20°C is 0.65 or more. This suppresses the occurrence of poor slicing due to deformation or damage of the end point detection window 5 during slicing, and also suppresses the occurrence of scratches due to the end point detection window 5 during polishing. The end point detection window 5 formed integrally with a part of the polishing layer 4 means an end point detection window 5 formed seamlessly with the polishing layer 4 by placing a hardened material for the end point detection window in mold 17 before casting the material for the polishing layer 4, casting the material for the polishing layer 4 therein, and forming a hardened material. In general, the end point detection window 5 is provided in an exposed state on the polishing surface of the polishing layer 4 and is also in contact with the workpiece 8 to be polished.
[0014] The structure of the polishing pad 3 will be described with reference to Fig. 3. The polishing pad 3 provided in the polishing apparatus 1 includes a polishing layer 4 having at least one end point detection window 5 (two end point detection windows 5 are provided in Fig. 3) and a cushion layer 6 having a hole 18 leading to the end point detection window 5, as shown in Fig. 3. Since the polishing pad 3 has the end point detection window 5, the polishing status of the workpiece 8 can be optically confirmed using a light source 13 and an optical sensor 14. The shape of the polishing pad 3 is preferably disk-shaped, but is not particularly limited thereto, and the size (diameter) can be appropriately determined depending on the size of the polishing apparatus 1 in which the polishing pad 3 is installed, and can be, for example, about 10 cm to 2 m in diameter. In the polishing pad 3 of the present invention, the polishing layer 4 is preferably bonded to the cushion layer 6 via an adhesive layer 7, but it may be composed of only the polishing layer 4. The polishing pad 3 is attached to a polishing platen 10 of a polishing device by double-sided tape or the like arranged on the cushion layer 6. The polishing pad 3 is rotated by the polishing device 1 while being pressed against an object 8 to be polished, thereby polishing the object 8 to be polished.
[0015] A method for manufacturing a polishing pad 3 having a polishing layer 4 with an end point detection window 5 will be described with reference to FIG. 5. The material for the end point detection window 5 is filled into a mold and cured to obtain a cured product. The cured product for the end point detection window 5 is placed in a mold 17 for the polishing layer 4 (FIG. 5(a)). The material for the polishing layer 4 is filled into the mold 17 and cured (FIG. 5(b)), to obtain a cured product for the polishing layer 4 with the end point detection window 5 (FIG. 5(c)). The cured product for the polishing layer 4 with the end point detection window 5 is cut in a direction perpendicular to the thickness direction of the polishing layer 4 and the end point detection window 5 (for example, a thickness of about 0.5 mm to 5.0 mm) (FIG. 5(d)), to obtain the polishing layer 4. The cushion layer 6 is bonded to the polishing layer 4. At this time, since the cushion layer 6 is in a state where the window is blocked, a hole 18 is made in the part of the end point detection window 5 so as not to block the end point detection window 5. Finally, it is cut into a circle so that it can be used as the polishing pad 3. Furthermore, in the polishing pad 3 of the present invention, the front and / or back surfaces of the polishing layer 4 and the end point detection window 5 may be ground, and the surface may be grooved or embossed, if necessary.
[0016] When using the polishing pad 3 of the present invention, the polishing pad 3 is attached to the polishing platen 10 of the polishing device 1 so that the polishing surface of the polishing layer 4 faces the workpiece 8. Then, the polishing platen 10 is rotated while supplying slurry, to polish the processed surface of the workpiece 8.
[0017] <End point detection window> The end point detection window 5 is translucent since it is used to confirm the end point of polishing by optical means, and since it may be required to have the same function as the polishing layer 4, i.e., to polish the workpiece 8, it is preferable that the main component be the same as that of the polishing layer 4. The end point detection window 5 is a cured product of a curable resin composition containing a polyisocyanate compound and a curing agent. The curable resin composition containing a polyisocyanate compound and a curing agent is not particularly limited as long as it is a curable resin composition containing a polyisocyanate compound and a curing agent, but a polyurethane resin composition, a polyurea resin composition, and a polyurethane polyurea resin composition can be suitably used. In this specification, polyurethane resin, polyurea resin, and polyurethane polyurea resin are referred to as "polyurethane resin".
[0018] (Polyisocyanate compounds) In this specification, the polyisocyanate compound means a compound having two or more isocyanate groups in the molecule. Examples of the polyisocyanate compound include alicyclic isocyanate compounds, aliphatic isocyanate compounds, and aromatic isocyanate compounds. Among these, it is preferable to include an alicyclic isocyanate compound and / or an aliphatic isocyanate compound. This tends to improve transparency and improve the yellowing resistance of the window. The polyisocyanate compound is not particularly limited as long as it has two or more isocyanate groups in the molecule. Specific examples of diisocyanate compounds having two isocyanate groups in the molecule include m-phenylene diisocyanate, p-phenylene diisocyanate, 2,6-tolylene diisocyanate (2,6-TDI), 2,4-tolylene diisocyanate (2,4-TDI), naphthalene-1,4-diisocyanate, diphenylmethane-4,4'-diisocyanate (MDI), 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), isophorone diisocyanate (IPDI), 3,3'-dimethoxy-4,4'-biphenyl diisocyanate, and the like. Examples of the polyisocyanate include 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, xylylene-1,4-diisocyanate, 4,4'-diphenylpropane diisocyanate, trimethylene diisocyanate, hexamethylene diisocyanate, propylene-1,2-diisocyanate, butylene-1,2-diisocyanate, cyclohexylene-1,2-diisocyanate, cyclohexylene-1,4-diisocyanate, p-phenylene diisothiocyanate, xylylene-1,4-diisothiocyanate, and ethylidine diisothiocyanate. These polyisocyanate compounds may be used alone or in combination with a plurality of polyisocyanate compounds. Among them, 4,4'-methylene-bis(cyclohexyl isocyanate) is preferred from the viewpoints of ease of adjusting the D hardness and transparency. Also preferred is isophorone diisocyanate (IPDI).
[0019] (Polyisocyanate compound containing urethane bonds) As the polyisocyanate compound, a urethane bond-containing polyisocyanate compound (urethane prepolymer) can be used. The urethane bond-containing polyisocyanate compound may be a commercially available product, or may be a compound obtained by reacting the above polyisocyanate compound with a polyol compound under commonly used conditions. The urethane bond-containing polyisocyanate compound is one that contains a urethane bond and an isocyanate group in the molecule. Furthermore, within the range not impairing the effects of the present invention, a mixture containing a trace amount of other components together with the urethane bond-containing polyisocyanate compound may be used as the urethane bond-containing polyisocyanate compound.
[0020] The urethane bond-containing polyisocyanate compound may be synthesized by reacting a polyisocyanate compound with a polyol compound. There is no particular limitation on the reaction, and the addition polymerization reaction may be carried out using a method and conditions known in the production of polyurethane resins. For example, the polyisocyanate compound heated to 50°C is added to a polyol compound heated to 40°C while stirring in a nitrogen atmosphere, and the temperature is raised to 80°C after 30 minutes, and the reaction is continued at 80°C for 60 minutes.
[0021] (hardening agent) The curing agent includes a low molecular weight polyol and a polyester polyol having three or more functional groups. The term "tri- or higher functional polyester polyol" refers to a polyester polyol having three or more functional groups, and by using this, it is possible to suppress a decrease in hardness even at high temperatures, so that the hardness of the end point detection window 5 does not decrease too much during slicing, and slicing defects can be suppressed. In addition, by using a low molecular weight polyol, it is possible to easily adjust the D hardness at 20°C, so that the physical properties (D hardness) of the end point detection window 5 during polishing can be adjusted to the same level as those of the polishing layer 4, and the occurrence of scratches caused by the end point detection window 5 can be suppressed.
[0022] In this specification, the term "polyol" refers to a compound having two or more hydroxyl groups (OH) in the molecule, and the term "low molecular weight polyol" refers to a polyol having a molecular weight of less than 300. The polyester polyol is not particularly limited as long as it is a polyol having an ester bond, and examples thereof include aliphatic polyester polyols and aromatic polyester polyols. The polyester polyol can be produced, for example, by polycondensing a dibasic acid and a polyhydric alcohol and adding a hydroxyl group to the end. Examples of the dibasic acid include succinic acid, adipic acid, sebacic acid, azelaic acid, phthalic acid, and dimer acid, and examples of the polyhydric alcohol include ethylene glycol, 1,4-butylene glycol, propylene glycol, neopentyl glycol, 3-methyl-1,5-pentanediol, diethylene glycol, and 1,6-hexanediol. Other examples of polyester polyols include polyester polyols synthesized by condensation polymerization of hydroxycarboxylic acids, polyester polyols synthesized by ring-opening polymerization of lactones (reaction of a lactone compound with a low molecular weight polyol), and polyester polyols synthesized by condensation polymerization of glycols and dicarboxylic acids, with polyester polyols synthesized by ring-opening polymerization of lactones being preferred due to their excellent heat resistance.
[0023] Specific examples of this lactone include β-propiolactone, β-butyrolactone, γ-butyrolactone, γ-valerolactone, γ-caprolactone, γ-heptalactone, γ-octalactone, γ-nonalactone, γ-decanolactone, δ-valerolactone, β-methyl-δ-valerolactone, δ-hexanolactone, δ-octanolactone, δ-decanolactone, δ-nonalactone, and ε-caprolactone, of which ε-caprolactone is preferred because it has excellent heat resistance and suppresses a decrease in the D hardness of the endpoint detection window 5 due to an increase in temperature.
[0024] A known polymerization method can be applied to produce a polyester polyol by ring-opening polymerization of lactone, but a divalent to hexavalent polyhydroxy compound is usually added to convert the terminal functional group into a hydroxyl group.
[0025] Specific examples of polyhydroxy compounds (low molecular weight polyols) include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 1,8-octanediol, 2-methyl-1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, diethylene glycol, triethylene glycol, and tetraethylene glycol. Examples of the polyol include glycols such as glycol, polyethylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, and 1,4-cyclohexanedimethanol, and polyols such as trimethylolpropane, trimethylolethane, glycerin, pentaerythritol, ditrimethylolpropane, dipentaerythritol, sorbitol, and tris(2-hydroxyethyl) isocyanurate, of which trimethylolpropane is preferred because it is easy to adjust the D hardness of the end point detection window 5. The amount of these polyhydroxy compounds added is usually 0.01 to 50 mol %, preferably 0.1 to 20 mol %, based on the lactone. As the polyester polyol, commercially available products may be used, or products synthesized by ring-opening polymerization of lactone may be used.
[0026] The number of functional groups of the polyester polyol is 3 or more, and preferably 3. When the number of functional groups of the polyester polyol is 3, a three-dimensional network structure is formed by a crosslinking reaction, and it becomes easy to adjust the ratio of the D hardness at 80° C. to the D hardness at 20° C. The functional group refers to an atomic group that determines the chemical properties of an organic compound, and in the polyester polyol of this specification, a hydroxyl group is preferred. The number average molecular weight of the polyester polyol is preferably 1000 to 2000. When the number average molecular weight is 1000 to 2000, it becomes easy to adjust the D hardness to a desired range. The content of the polyester polyol is preferably 50.0 to 250.0 parts, more preferably 60.0 to 220.0 parts, based on 100 parts of the polyisocyanate compound. When the content of the polyester polyol is within the above range, a decrease in D hardness accompanying an increase in temperature can be suppressed.
[0027] The low molecular weight polyol is not particularly limited, but examples thereof include low molecular weight polyols having two hydroxyl groups such as ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 2,3-butylene glycol, 1,4-butylene glycol, 1,5-pentanediol, neopentyl glycol, 1,6-hexane glycol, 2,5-hexanediol, dipropylene glycol, 2,2,4-trimethyl-1,3-pentanediol, tricyclodecane dimethanol, and 1,4-cyclohexane dimethanol; and low molecular weight polyols having three or more hydroxyl groups such as glycerin, hexanetriol, trimethylolpropane (TMP), isocyanuric acid, and erythritol. The low molecular weight polyols may be used alone or in combination of two or more. Among these, a low molecular weight polyol having three or more hydroxyl groups is preferred, and glycerin is more preferred. By using such a low molecular weight polyol, the transparency is further improved, and the yellowing resistance of the window tends to be further improved. The molecular weight of the low-molecular-weight polyol is preferably 80 to 150. When the molecular weight is 80 to 150, it becomes easy to adjust the D hardness. The content of the low molecular weight polyol is preferably 5.0 to 19.0 parts, more preferably 7.0 to 17.0 parts, based on 100 parts of the polyisocyanate compound. When the content of the low molecular weight polyol is within the above range, it becomes easy to adjust the ratio of the D hardness at 80°C to the D hardness at 20°C.
[0028] The weight ratio of the polyester polyol to the low molecular weight polyol (polyester polyol: low molecular weight polyol) is preferably 80:20 to 98:2, more preferably 90:10 to 98:2. When the weight ratio of the polyester polyol to the low molecular weight polyol (polyester polyol: low molecular weight polyol) is 80:20 to 98:2, it becomes easy to adjust the ratio of the D hardness at 80°C to the D hardness at 20°C, and there is a tendency that the occurrence of scratches and slicing defects are easily suppressed.
[0029] The curing agent may include a curing agent other than polyester polyol and low molecular weight polyol. Examples of the curing agent other than polyester polyol and low molecular weight polyol include compounds having a hydroxyl group that reacts with the isocyanate group of the polyisocyanate compound, such as polyether polyol, polycarbonate polyol, polyether polycarbonate polyol, polyurethane polyol, epoxy polyol, vegetable oil polyol, polyolefin polyol, acrylic polyol, and vinyl monomer modified polyol. Among them, it is preferable that polyether polyol represented by polytetramethylene ether glycol (PTMG) is contained. When polyether polyol is contained, it becomes easy to adjust the D hardness at 20°C. The number average molecular weight of the polyether polyol is preferably 500 to 2000. When the number average molecular weight of the polyether polyol is 500 to 2000, brittleness can be eliminated and appropriate elasticity can be imparted.
[0030] The content of the polyether polyol is preferably 50.0 to 100.0 parts, more preferably 65.0 to 90.0 parts, based on 100 parts of the polyisocyanate compound. When the content of the polyether polyol is within the above range, appropriate elasticity is imparted, making it easy to adjust the D hardness.
[0031] (Additives) The curable resin composition that is the material of the end point detection window 5 may contain additives. For example, a catalyst such as a tin-containing catalyst or an amine catalyst, a chain extender, or the like can be used.
[0032] (D hardness) In this specification, D hardness refers to a value measured in accordance with Japanese Industrial Standards (JIS K6253). The ratio of the D hardness of the endpoint detection window 5 at 80° C. to the D hardness of the endpoint detection window 5 at 20° C. (D hardness of the endpoint detection window 5 at 80° C. / (D hardness of the endpoint detection window 5 at 20° C.)·Equation (1)) is 0.65 or more, preferably 0.70 or more, and more preferably 0.75 or more. When the ratio of the D hardness of the endpoint detection window 5 at 80° C. to the D hardness of the endpoint detection window 5 at 20° C. is 0.65 or more, the hardness of the endpoint detection window is less likely to decrease even if the temperature increases. The ratio of the D hardness of the end point detection window 5 at 80°C to the D hardness at 20°C (Equation (1)) indicates the degree of decrease in the hardness of the end point detection window 5 at high temperatures. A high value of this ratio indicates that the hardness at high temperatures is less likely to decrease. Since the slicing of the cured material for the polishing layer 4 having the end point detection window 5 is performed while the cured material is warm, if the hardness of the end point detection window 5 decreases too much at high temperatures, slicing failure occurs due to deformation or breakage of the end point detection window 5. Therefore, it is preferable that the hardness of the end point detection window 5 does not decrease too much at high temperatures. The D hardness of the endpoint detection window 5 at 20° C. is preferably 20 to 50, and more preferably 30 to 40. When the D hardness of the endpoint detection window 5 at 20° C. is 20 to 50, the occurrence of scratches during polishing tends to be suppressed. The D hardness at 20° C. means the initial hardness during polishing, and is preferably adjusted to have the same physical properties (hardness) as the polishing layer 4 in order to suppress the occurrence of scratches caused by the endpoint detection window 5.
[0033] (transmittance) Since the end point detection window 5 transmits light, it is preferable that the transmittance is high in the frequently used wavelength range of 300 to 800 nm. For example, the transmittance of light at 660 nm is preferably 50% or more, more preferably 60% or more, even more preferably 70% or more, and even more preferably 80% or more. If the transmittance is high, errors are less likely to occur and measurements can be made with high accuracy. The transmittance can be measured using a spectrophotometer (U-3210 Spectro Photometer, manufactured by Hitachi, Ltd.) and the sample thickness is 10 mm.
[0034] Usually, one or more endpoint detection windows 5 are required. The diameter of the endpoint detection window 5 is preferably about 1 cm to 15 cm, and the thickness is the same as that of the polishing layer 4, usually about 0.8 to 5 mm. Furthermore, as shown in FIG. 4 (a cross-sectional view taken along the line AA' in FIG. 3), the surface 4a of the polishing layer 4 and the surface 5a of the end point detection window 5 are adjusted so that they are at the same height. The endpoint detection window 5 generally has a cylindrical shape that penetrates the upper and lower surfaces of the polishing layer 4, but is not particularly limited as long as it penetrates the upper and lower surfaces of the polishing layer 4, and can be appropriately selected from shapes such as an elliptical cylinder or a polygonal cylinder. stomach.
[0035] <Polishing layer> The polishing pad 3 includes a polishing layer 4 that is a layer for polishing an object to be polished 8. Polyurethane resin, polyurea resin, and polyurethane polyurea resin can be suitably used as materials constituting the polishing layer 4. In this specification, polyurethane resin, polyurea resin, and polyurethane polyurea resin are referred to as "polyurethane resin". The size (diameter) of the polishing layer 4 is the same as that of the polishing pad 3, and may be about 10 cm to 2 mm in diameter, and the thickness of the polishing layer 4 may be about 0.8 to 5 mm. The polishing layer 4 is rotated together with the polishing platen 10 of the polishing device 1, and while slurry 9 is flowed onto it, the chemical components and abrasive grains contained in the slurry are moved relative to the workpiece 8, thereby polishing the workpiece 8. By providing the surface of the polishing layer 4 with grooves in a concentric, lattice, radial, or other pattern, it is possible to adjust the retention and discharge of the slurry 9 and change the polishing characteristics. Before casting the material for the polishing layer 4, a hardened material for the end point detection window is placed in the mold 17, and the material for the polishing layer 4 is cast therein to form a hardened material, so that the end point detection window 5 is integrally formed in a part of it.
[0036] The polishing layer 4 is preferably made of a polyurethane resin foam having cells. The cells of the polyurethane resin foam are classified into closed cells, in which a plurality of cells exist independently, and open cells, in which a plurality of cells are connected by communicating holes, depending on the form of the cells. Among these, the polyurethane resin foam used in the present invention preferably has closed cells, and more preferably is a polyurethane resin foam containing a polyurethane resin and hollow microspheres dispersed in the polyurethane resin.
[0037] The polyurethane resin foam having closed cells can be produced by using hollow microspheres that have an outer shell and are hollow inside. The hollow microspheres may be either already expanded (pre-expanded) or unexpanded, but when unexpanded microspheres are used, they can expand at the curing temperature.
[0038] The hollow microspheres may be commercially available or may be synthesized by a conventional method. The material of the shell of the hollow microspheres is not particularly limited, but may be, for example, polyvinyl alcohol, polyvinylpyrrolidone, poly(meth)acrylic acid, polyacrylamide, polyethylene glycol, polyhydroxyether acrylate, maleic acid copolymer, polyethylene oxide, polyurethane, poly(meth)acrylonitrile, polyvinylidene chloride, polyvinyl chloride and organic silicone resins, and copolymers of two or more monomers constituting these resins. In addition, the commercially available hollow microspheres may be, but are not limited to, Expancel series (trade name manufactured by Akzo Nobel), Matsumoto Microsphere (trade name manufactured by Matsumoto Oil Co., Ltd.), etc.
[0039] The shape of the hollow microspheres in the polyurethane resin foam is not particularly limited, and may be, for example, spherical or nearly spherical. The average particle size of the hollow microspheres is not particularly limited, but is preferably 5 to 200 μm, more preferably 5 to 80 μm, further preferably 5 to 50 μm, and particularly preferably 5 to 35 μm. The average particle size can be measured by a laser diffraction particle size distribution analyzer (e.g., Mastersizer 2000, manufactured by Spectris Co., Ltd.).
[0040] The expansion start temperature of the hollow microspheres is preferably 85° C. to 150° C., more preferably 90° C. to 140° C. When the expansion start temperature of the hollow microspheres is within the above range, the difference between the temperature of the hollow microspheres and that of the material of the polishing layer is small, and the degree of expansion of the hollow microspheres can be uniformly controlled.
[0041] The hollow microspheres are added in an amount of preferably 0.1 to 10 parts by weight, more preferably 1 to 5 parts by weight, and even more preferably 1 to 4 parts by weight, based on 100 parts by weight of the urethane prepolymer. Although this is merely an example, the difference in aperture ratio between the region around the end point detection window 5 and the region other than the region around the end point detection window 5 is preferably 15 or less, and more preferably 10 or less. Here, the area around the endpoint detection window 5 on the polishing surface of the polishing layer 4 refers to a range 10 mm away from the edge of the endpoint detection window 5. In addition, the area other than the periphery of the endpoint detection window 5 on the polishing surface of the polishing layer 4 refers to a range 10 mm outside from the edge of the endpoint detection window 5.
[0042] In addition to the above components, a conventionally used blowing agent may be used in combination with the hollow microspheres, provided that the effect of the present invention is not impaired.
[0043] The D hardness of the polishing layer 4 is not particularly limited, but is, for example, 20 to 100, preferably 30 to 80, and more preferably 30 to 70. If the D hardness is low, it becomes difficult to flatten fine irregularities by low-pressure polishing. If the D hardness is too high, the polishing layer 4 may be rubbed strongly against the polished object 8, causing scratches on the processed surface of the polished object 8.
[0044] <Cushion layer> Since the cushion layer 6 is made of a resin-impregnated nonwoven fabric, a flexible material such as a synthetic resin, or a foam having a cellular structure, the polishing layer 4 can be more uniformly brought into contact with the workpiece 8. In the present invention, the polishing pad 3 may be made of only the polishing layer 4, but it is preferable that the cushion layer 6 is bonded to the polishing pad 3. In addition, in the cushion layer 6, it is necessary to form holes 18 in the same number as the endpoint detection windows 5 in the portions corresponding to the installation positions of the endpoint detection windows 5 so as to allow light for optical detection to pass through.
[0045] <Adhesive layer> The adhesive layer 7 is a layer for adhering the cushion layer 6 and the polishing layer 4, and is usually made of a double-sided tape or an adhesive. Any double-sided tape or adhesive known in the art can be used.
[0046] <Polishing equipment> As already explained, the polishing apparatus 1 equipped with the polishing pad 3 of the present invention can confirm the polishing state by optical means. For example, as shown in FIG. 1, the polishing table 10 having the polishing apparatus 1 is equipped with a light source 13 and an optical sensor 14. Light emitted from the light source 13 passes from the bottom to the top of the polishing table 10, passes through the hole 18 in the cushion layer 6 and further through the end point detection window 5 in the polishing layer 4, reaches the workpiece 8 to be polished, and is reflected by the workpiece 8 and returned, and is detected by the optical sensor 14. In this way, the light source 13 and the optical sensor 14 rotate together with the polishing table 10, so that the polishing state can be confirmed while polishing. EXAMPLES
[0047] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0048] In each of the examples and comparative examples, unless otherwise specified, "parts" means "parts by weight." Also, "R value" means the equivalent ratio of active hydrogen groups present in a curing agent to isocyanate groups of a polyisocyanate compound or a urethane bond-containing polyisocyanate compound.
[0049] <Example 1> (Manufacture of End Point Detection Window 5) Each of the raw materials, 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), a trifunctional polyester polyol having a number average molecular weight of 1257 obtained by the reaction of ε-caprolactone with trimethylolpropane, and glycerin, was preliminarily kept at 80°C. Next, 100 parts of 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), 178.5 parts of the above trifunctional polyester polyol, and 9.2 parts of glycerin were mixed by vacuum stirring and degassing at room temperature for 4 minutes to obtain a reaction mixture. Thereafter, the reaction mixture was poured into a preheated mold, the mold was clamped, and the mixture was heated at 120°C for 30 minutes, after which the cured reaction mixture (curable resin composition A) was removed from the mold. This was post-cured at 120°C for 6 hours, and then cooled at 25°C for 24 hours. Next, the curable resin composition A was heated at 120°C for 1 hour before being used in the polishing layer manufacturing process, and the curable resin composition A was used in the polishing layer manufacturing process. The raw material of the curing agent (polyester polyol: low molecular weight polyol) was 95.1:4.9. The R value was 0.95.
[0050] (Manufacture of abrasive layer 4) A urethane prepolymer having an NCO equivalent of 560 obtained by reacting 2,4-tolylene diisocyanate (2,4-TDI), polypropylene glycol (PPG) having a number average molecular weight of 1000, and diethylene glycol (DEG) was mixed with a urethane prepolymer having an NCO equivalent of 600 obtained by reacting 2,4-tolylene diisocyanate (2,4-TDI), polyester diol having a number average molecular weight of 2000 obtained by reacting adipic acid and butanediol, and diethylene glycol (DEG) in a weight ratio of 1:1. 100 parts of the urethane prepolymer were mixed with 3.5 parts of unexpanded hollow microspheres (average particle size: 8.5 μm) whose shell portion is made of acrylonitrile-vinylidene chloride copolymer to obtain a urethane prepolymer mixture. The obtained urethane prepolymer mixture was charged into a first liquid tank and kept at 60°C. In addition to the first liquid tank, 20.2 parts of 3,3'-dichloro-4,4'-diaminodiphenylmethane (methylene bis-o-chloroaniline) (MOCA) was placed in a second liquid tank as a hardener, melted and mixed at 120°C, and further degassed under reduced pressure to obtain a hardener molten liquid.
[0051] Next, the liquids in the first liquid tank and the second liquid tank were poured from the respective inlets of a mixer equipped with two inlets, and mixed and stirred to obtain a mixed liquid. The temperature of the mixed liquid poured into the mixer was 90°C. At this time, the curable resin composition A, which had been preheated to 120°C, was placed in a mold. The mixed liquid was poured into a mold for a polishing layer preheated to 80°C while being mixed and stirred, and then the mold was clamped and heated at 80°C for 30 minutes to perform primary curing. After the primary cured molded product was demolded, it was secondary cured in an oven at 120°C for 4 hours to obtain a resin molded product. The obtained resin molded product was allowed to cool to 25°C, and then heated again in an oven at 120°C for 5 hours, and then sliced to a thickness of 1.3 mm to obtain a polishing layer A integrally formed with an end point detection window. A double-sided tape was attached to the back surface of the obtained polishing layer, a cushion layer was attached, and a double-sided tape was further attached to the surface of the cushion layer to obtain a polishing pad.
[0052] <Example 2> Using 100 parts of 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), 168.6 parts of the same trifunctional polyester polyol as in Example 1, and 9.9 parts of glycerin, a curable resin composition B was produced under the same conditions as in Example 1. A polishing layer B and a polishing pad were obtained in the same manner as in Example 1, except that the curable resin composition B was used. The ratio of the raw materials for the curing agent (polyester polyol: low molecular weight polyol) was 94.5:5.5. The R value was 0.95.
[0053] <Example 3> Using 100 parts of 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), 112.4 parts of the same trifunctional polyester polyol as in Example 1, 5.8 parts of glycerin, and 87.2 parts of poly(oxytetramethylene) glycol (PTMG) having a number average molecular weight of 650, a curable resin composition C was produced under the same conditions as in Example 1. In addition, a polishing layer C and a polishing pad were obtained in the same manner as in Example 1, except that the curable resin composition C was used. The ratio of the raw material of the curing agent (polyester polyol: low molecular weight polyol) was 95.1:4.9. The R value was 0.95.
[0054] <Example 4> Using 100 parts of 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), 108.4 parts of the same trifunctional polyester polyol as in Example 1, 6.4 parts of glycerin, and 84.1 parts of poly(oxytetramethylene) glycol (PTMG) having a number average molecular weight of 650, a curable resin composition D was produced under the same conditions as in Example 1. A polishing layer D and a polishing pad were obtained in the same manner as in Example 1 except that the curable resin composition D was used. The ratio of the raw material of the curing agent (polyester polyol: low molecular weight polyol) was 94.5:5.5. The R value was 0.95.
[0055] <Example 5> Using 100 parts of 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), 104.6 parts of the same trifunctional polyester polyol as in Example 1, 6.9 parts of glycerin, and 81.2 parts of poly(oxytetramethylene) glycol (PTMG) having a number average molecular weight of 650, a curable resin composition E was produced under the same conditions as in Example 1. A polishing layer E and a polishing pad were obtained in the same manner as in Example 1 except that the curable resin composition E was used. The ratio of the raw material of the curing agent (polyester polyol: low molecular weight polyol) was 93.8:6.2. The R value was 0.95.
[0056] <Example 6> Using 100 parts of 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), 173.4 parts of the same trifunctional polyester polyol as in Example 1, and 13.9 parts of trimethylolpropane (TMP), a curable resin composition F was produced under the same conditions as in Example 1. A polishing layer F and a polishing pad were obtained in the same manner as in Example 1, except that the curable resin composition F was used. The ratio of the raw material of the curing agent (polyester polyol: low molecular weight polyol) was 92.6:7.4. The R value was 0.95.
[0057] <Example 7> Using 100 parts of 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), 151.7 parts of the same trifunctional polyester polyol as in Example 1, and 16.2 parts of trimethylolpropane (TMP), a curable resin composition G was produced under the same conditions as in Example 1. A polishing layer G and a polishing pad were obtained in the same manner as in Example 1 except that the curable resin composition G was used. The ratio of the raw material of the curing agent (polyester polyol: low molecular weight polyol) was 90.4:9.6. The R value was 0.95.
[0058] <Example 8> Using 100 parts of 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), 86.7 parts of the same trifunctional polyester polyol as in Example 1, 13.9 parts of trimethylolpropane (TMP), and 67.2 parts of poly(oxytetramethylene) glycol (PTMG) having a number average molecular weight of 650, a curable resin composition H was produced under the same conditions as in Example 1. A polishing layer H and a polishing pad were obtained in the same manner as in Example 1 except that the curable resin composition H was used. The ratio of the raw material of the curing agent (polyester polyol: low molecular weight polyol) was 86.2:13.8. The R value was 0.95.
[0059] <Example 9> Using 100 parts of 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), 75.9 parts of the same trifunctional polyester polyol as in Example 1, 16.2 parts of trimethylolpropane (TMP), and 58.8 parts of poly(oxytetramethylene) glycol (PTMG) having a number average molecular weight of 650, a curable resin composition I was produced under the same conditions as in Example 1. A polishing layer I and a polishing pad were obtained in the same manner as in Example 1 except that the curable resin composition I was used. The ratio of the raw material of the curing agent (polyester polyol: low molecular weight polyol) was 82.4:17.6. The R value was 0.95.
[0060] <Comparative Example 1> Using 100 parts of 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI) and 303.4 parts of the same trifunctional polyester polyol as in Example 1, a curable resin composition J was produced under the same conditions as in Example 1. A polishing layer J and a polishing pad were obtained in the same manner as in Example 1, except that the curable resin composition J was used. The R value was 0.95.
[0061] <Comparative Example 2> A curable resin composition K was obtained by producing under the same conditions as in Example 1 using 100 parts of 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), 9.9 parts of glycerin, and 201.2 parts of poly(oxytetramethylene) glycol (PTMG) having a number average molecular weight of 1000. A polishing pad was obtained by the same method as in Example 1 except that the curable resin composition K was used. In addition, the R value was 0.95.
[0062] <Comparative Example 3> A curable resin composition L was obtained by producing under the same conditions as in Example 1 using 100 parts of 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), 8.6 parts of glycerin, and 222.8 parts of poly(oxytetramethylene) glycol (PTMG) having a number average molecular weight of 1000. A polishing layer L and a polishing pad were obtained in the same manner as in Example 1 except that the curable resin composition L was used. In addition, the R value was 0.95.
[0063] <Comparative Example 4> Using 100 parts of 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), 121.4 parts of the same trifunctional polyester polyol as in Example 1, and 19.4 parts of trimethylolpropane (TMP), a curable resin composition M was produced under the same conditions as in Example 1. A polishing layer M and a polishing pad were obtained in the same manner as in Example 1, except that the curable resin composition M was used. The R value was 0.95.
[0064] (Measurement of D hardness of polishing layer 4 and end point detection window 5) The D hardness of the polishing layer 4 and the end point detection window 5 was measured using a Shore D hardness tester in accordance with the Japanese Industrial Standards (JIS-K-6253). Here, the measurement sample was obtained by stacking a plurality of polishing layers 4 and end point detection windows 5 as necessary so that the total thickness was at least 4.5 mm. The measurement results of the D hardness of the polishing layer 4 and the end point detection window 5 are shown in Tables 1 and 2.
[0065] (Evaluation of deformation and damage of the end point detection window 5 during slicing) The endpoint detection windows of each polishing layer obtained as described above were visually inspected for deformation or damage such as distortion, cracks, breaks, and chips. Those without deformation or damage were marked with an O, and those with deformation and / or damage were marked with an X. The evaluation results are shown in Tables 1 and 2.
[0066] (Defect performance evaluation) A nonwoven fabric impregnated with urethane was attached to the back surface of the polishing layer 4 having the end point detection window 5 of Examples 1-9 and Comparative Examples 1-4 to form a cushion layer 6, thereby producing a polishing pad 3. Using the obtained polishing pad 3, a polishing test was carried out under the following polishing conditions, and the defect performance was evaluated. (polishing conditions) Polishing equipment used: F-REX300X (manufactured by Ebara Corporation) Disk: A188 (3M) Abrasive temperature: 20℃ Polishing platen rotation speed: 85 rpm Polishing head rotation speed: 86 rpm Grinding pressure: 3.5psi Polishing slurry (metal film): CSL-9044C (CSL-9044C stock solution: pure water = mixed solution of 1:9 by weight) (manufactured by Fujimi Corporation) Polishing slurry flow rate: 200ml / min Polishing time: 60 seconds Object to be polished (metal film): Cu film substrate Pad break: 35N 10 minutes Conditioning: Ex-situ, 35N, 4 scans
[0067] The 16th, 26th, and 51st polished substrates were inspected for surface defects with a size of 155 nm or more using the high sensitivity measurement mode of a surface inspection device (KLA Tencor, Surfscan SP2XP). The SEM images of the detected surface defects were analyzed using a review SEM, and the number of scratches was counted. The number of scratches of 10 or less, which is considered to be required in practice, was marked as ○, and the number of scratches of more than 10 was marked as ×, and the evaluation results are shown in Tables 1 and 2.
[0068] [Table 1]
[0069] [Table 2]
[0070] The materials used in the examples and comparative examples and their molecular weights are as follows. Isocyanate: Hydrogenated MDI (molecular weight 262.35, equivalent weight: 131.2) Trifunctional polyester polyol: obtained by reacting trimethylolpropane and ε-caprolactone (number average molecular weight 1257, equivalent weight: 419) Glycerin: Molecular weight 92.09 (equivalent weight: 30.7) TMP: Trimethylolpropane (molecular weight 134.17, equivalent weight: 44.7) Poly(oxytetramethylene) glycol (number average molecular weight 1000, equivalent weight: 500) Poly(oxytetramethylene) glycol (number average molecular weight 6500, equivalent weight: 325) [Industrial Applicability]
[0071] The present invention contributes to the manufacture and sale of polishing pads and has industrial applicability.
[0072] Explanation of symbols 1 Polishing equipment 2 Incident light 2a,2b Reflected light 3 Polishing Pads 4 Polishing layer 4a Surface of the polishing layer 5 End point detection window 5a Surface of end point detection window 6 Cushioning Layer 7 Adhesive layer 8 Object to be polished 9. Slurry 10 Polishing plate 11 Substrate 12 Thin Films 13 Light source 14 Optical Sensor 16 Holding Plate 17 Polishing layer type 18 Cushion layer holes
Claims
1. A polishing pad having a polishing layer and an end point detection window integrally formed in a portion of the polishing layer, the end point detection window is a cured product of a curable resin composition containing a polyisocyanate compound and a curing agent, The curing agent comprises a low molecular weight polyol and a polyester polyol having three or more functional groups; A polishing pad, wherein the value obtained from the following formula (1) is 0.65 or more. (D hardness at 80° C. in the end point detection window) / (D hardness at 20° C. in the end point detection window) (Equation 1)
2. 2. The polishing pad according to claim 1, wherein the polyester polyol has a number average molecular weight of 1,000 to 2,000.
3. 2. The polishing pad of claim 1, wherein the functionality of the polyester polyol is 3.
4. 2. The polishing pad according to claim 1, wherein the weight ratio of the polyester polyol to the low molecular weight polyol (polyester polyol:low molecular weight polyol) is 80:20 to 98:
2.
5. 2. The polishing pad of claim 1, wherein the low molecular weight polyol has a molecular weight of 80 to 150.
6. The polishing pad of claim 1 , wherein the curing agent comprises a polyether polyol.
7. 7. The polishing pad according to claim 6, wherein the polyether polyol has a number average molecular weight of 500 to 2,000.
Citation Information
Patent Citations
Polishing pad and manufacturing method of semiconductor device
JP2004228101A
Abrasive pad and polished product manufacturing method
JP2022155532A
Polishing pad and method for manufacturing semiconductor device using the same
US20230059394A1
Method for manufacturing polishing pad
WO2022202059A1
Polishing pad
JP2002001647A