Granular carrier, granular pharmaceutical composition, absorbent article, and method for producing granular carrier
The production of granular carriers using crosslinked carboxyalkyl cellulose salts addresses the environmental and aesthetic challenges of polyacrylic SAPs by creating biodegradable, spherical, and uniform particles for efficient drug support in gel preparations.
Patent Information
- Application Number
- JP2023053731
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Existing superabsorbent polymers, particularly polyacrylic acid-based SAPs, face issues with high production costs, environmental impact, and non-biodegradability, leading to soil contamination and energy-intensive disposal. There is a need for biodegradable alternatives that maintain high water absorption, strength, and aesthetic appeal, especially in granular gel preparations for containers.
A method involving the production of granular carriers using crosslinked carboxyalkyl cellulose salts through reverse-phase suspension polymerization, followed by washing with ethanol-containing solvents, to achieve spherical, uniform particles with balanced water absorption and strength, suitable for supporting drugs in gel preparations.
The method produces granular carriers that are biodegradable, spherical, and uniform in size, ensuring efficient drug function, air flow, and aesthetic appeal, while maintaining high water absorption and strength, suitable for use in absorbent articles and drug carriers.
Smart Images

Figure 2024141875000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a granular carrier, a granular pharmaceutical composition and an absorbent article, as well as a method for producing the granular carrier. [Background technology]
[0002] Superabsorbent polymers (SAP) absorb water upon contact with water and instantly become a transparent hydrated gel. This gel is one of the functional polymers that does not release water even when pressure is applied and retains water. Superabsorbent polymers have a wide range of uses, for example, in the field of sanitary products, they are used as highly absorbent substances in absorbent articles such as paper diapers and sanitary napkins for women. In addition, superabsorbent polymers are also used as carriers in gel preparations that absorb and support aqueous liquid compositions containing pharmaceuticals such as fragrances and deodorants. Gel preparations containing carriers made of such superabsorbent polymers are widely used in stationary air fresheners and deodorants because there is no risk of liquid spilling from the container and they have excellent design.
[0003] Currently, polyacrylic acid-based SAP is the mainstream of superabsorbent polymers (SAP) from the viewpoints of ease of synthesis and cost. However, since polyacrylic acid-based SAP is made from petroleum, there is a problem that the production cost is affected by fluctuations and increases in crude oil prices, and there is also a large amount of CO2 emissions during production and disposal. In particular, when used for diapers, SAP is disposed of in a water-absorbed state, so a large amount of energy is required for incineration of acrylic acid-based SAP, resulting in particularly large amounts of CO2 emissions. In addition, when acrylic acid-based SAP is disposed of in landfills, there are problems such as soil pollution due to its lack of biodegradability.
[0004] The fact that polyacrylic acid-based SAPs are the mainstream of superabsorbent polymers (SAPs) may be a cause of environmental problems. As the demand for disposable diapers is expected to rapidly increase in emerging countries in the future, it is desirable to use biodegradable natural polymers as superabsorbent polymers. In this situation, superabsorbent polymers using plant-derived raw materials such as polysaccharides have been proposed.
[0005] For example, Patent Documents 1 to 3 propose a cellulose-based SAP consisting of a cross-linked polymer of carboxymethyl cellulose (CMC) or CMC salt as a biodegradable, highly water-absorbent polymer to replace polyacrylic acid-based SAP. This CMC is a water-soluble cellulose derivative, and is synthesized by etherifying the hydroxyl groups of cellulose with chloroacetic acid or the like. Its aqueous solution exhibits anionic properties and has high viscosity and excellent dispersibility, and is therefore widely used as a thickener, dispersant, and stabilizer.
[0006] CMC is neither toxic nor allergenic, and is also used as a food additive and a pharmaceutical binder. Its physical properties depend strongly on the degree of substitution (DS), which is the average number of carboxymethyl groups substituted per glucose residue, and in one example, it is said to be water-soluble when DS>0.55. For example, Patent Document 1 uses CMC and CMC salts with a degree of substitution of 1.1 or more (see Claim 1, etc.), and Patent Document 2 uses CMC salts with a degree of substitution of 0.65 to 1.4 (see Claim 1, etc.). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2011-140534 A [Patent Document 2] International Publication No. 2012 / 147255 [Patent Document 3] JP 2008-285611 A Summary of the Invention [Problem to be solved by the invention]
[0008] Stationary products in which gel preparations such as fragrance compositions and deodorant compositions are filled in containers are on the market. Many of these products use granular gel preparations in which liquid compositions containing various chemicals are supported on gel carriers made of highly water-absorbent polymers. Many of these products are designed to have the surface of the granular gel preparation exposed to air to exert the functions of the various chemicals supported on the gel carriers. That is, when the chemical supported on the gel carrier is a volatile chemical such as a fragrance, the surface of the granular gel preparation is exposed to air to volatilize the volatile chemical. Also, when the chemical supported on the gel carrier is a non-volatile chemical, for example, a deodorant that uses a chemical reaction to deodorize, the surface of the granular gel preparation is exposed to air to bring the malodorous molecules into contact with the non-volatile deodorant, and the malodorous molecules are decomposed by a chemical reaction to deodorize.
[0009] Therefore, in order to efficiently function the drug carried by the gel carrier in the granular gel preparation, it is desirable that air flow easily occurs when the granular gel preparation is filled in the container. In order to facilitate air flow, it is preferable that the gaps between the granular gel preparations are uniform and have a certain size. Therefore, it is desirable that the granular gel preparations are uniform in size and nearly spherical in shape. Many stationary products are filled with granular gel preparations in transparent or translucent containers and are visible from the outside. The uniform size and nearly spherical shape of the granular gel preparations are preferable from the viewpoint of aesthetics, in addition to enabling the above-mentioned drug to function efficiently.
[0010] In addition, the higher the water absorption rate of the gel carrier, the more the drug-containing composition can be supported, which is preferable, but the higher the water absorption amount, the lower the strength tends to be. If the gel carrier does not have a certain strength compared to its water absorption rate, the shape of the granular gel is likely to collapse during the manufacturing process. For this reason, a good balance between water absorption rate and strength is required for the gel carrier.
[0011] From the viewpoint of aesthetics, it is also important that the granular gel preparation has excellent transparency.
[0012] On the other hand, as a conventional method for producing cellulose-based SAP, a method of polymerizing CMC and / or a CMC salt in an aqueous solution using a crosslinking agent (hereinafter referred to as "aqueous solution polymerization") is known. For example, a crosslinking agent is added to a CMC salt aqueous solution in which CMC or a CMC salt is dissolved in a sodium hydroxide aqueous solution, and a crosslinking reaction is carried out to obtain a hydrogel in which the aqueous solution is uniformly gelled. The hydrogel is pulverized and undergoes a sorting process such as classification to form a cellulose-based SAP (for example, see paragraph 0035 of Patent Document 1, paragraph 0024 of Patent Document 2, and paragraph 0044 of Patent Document 3).
[0013] Crushed gel particles (crushed gel) finely granulated by crushing are typically fragmented with sharp edges, and most of them are irregularly shaped particles that are difficult to call spherical. When such cellulose-based SAP consisting of a collection of small, non-spherical, non-uniform gel fragments is filled in a container, the gel particles are in close contact with each other, making it difficult for air to flow. In addition, cellulose-based SAP consisting of a collection of such non-uniform small gel fragments is not preferable from the viewpoint of aesthetics.
[0014] The present invention aims to provide a technology for producing a granular carrier that combines high water absorption and biodegradability, has a roughly spherical shape, a uniform particle size, and excellent water absorption, strength, and transparency. [Means for solving the problem]
[0015] According to one aspect of the present invention, there is provided a method for producing a granular carrier comprising gel particles containing a crosslinked product of a carboxyalkyl cellulose salt, comprising the steps of: preparing a carboxyalkyl cellulose salt aqueous solution by dissolving a carboxyalkyl cellulose and / or a salt thereof having a viscosity of 5 mPa·s or more and 300 mPa·s or less in a 1 mass% aqueous solution at 25°C in an alkaline aqueous solution; preparing a mixture of the aqueous carboxyalkyl cellulose salt and a crosslinking agent; dispersing the mixture in a low-polarity organic solvent to form a suspension, and proceeding with crosslinking polymerization of the carboxyalkyl cellulose salt in the suspension to form dispersed particles consisting of gel particles containing a crosslinked body of the carboxyalkyl cellulose salt; filtering the gel particles from the suspension; and The gel particles are washed with a washing solvent having an ethanol content of more than 60% by mass. Including, The low-polarity organic solvent has a relative dielectric constant of 10 or less at 25°C and a kinetic viscosity of 10mm at 37.8°C. 2 / s or more.
[0016] According to another aspect of the present invention, there is provided the production method according to the above aspect, wherein the content of the ethanol in the washing solvent is in the range of more than 60 mass % and not more than 100 mass %.
[0017] According to yet another aspect of the present invention, there is provided the production method according to the above aspect, wherein the washing solvent is a mixed solvent of the above ethanol and water.
[0018] According to yet another aspect of the present invention, there is provided the production method according to the above aspect, wherein the content of the ethanol in the washing solvent is in the range of more than 60% by mass and not more than 85% by mass.
[0019] According to yet another aspect of the present invention, there is provided the method according to any one of the above aspects, wherein the gel particles washed with the washing solvent have a solvent absorption rate of the washing solvent, represented by the following formula (1), of 25 or less. Solvent absorption rate=(M1-M2) / M2 (1) In formula (1), M1 represents the mass of the gel particles carrying a saturated amount of the washing solvent after the washing, and M2 represents the mass of the gel particles after drying after the washing.
[0020] According to yet another aspect of the present invention, there is provided the production method according to any one of the above aspects, wherein the low-polarity organic solvent is liquid paraffin or silicone oil.
[0021] According to yet another aspect of the present invention, the low-polarity organic solvent has a kinetic viscosity of 10 mm at 37.8° C. 2 / s or more 100mm 2 / s or less.
[0022] According to yet another aspect of the present invention, there is provided the method according to any one of the above aspects, wherein the viscosity of the carboxyalkyl cellulose and / or salt thereof is 5 mPa·s or more and 100 mPa·s or less.
[0023] According to yet another aspect of the present invention, there is provided the method according to any one of the above aspects, wherein the mass ratio (X / Y) of the carboxyalkyl cellulose and / or salt thereof (X) to the crosslinking agent (Y) in the mixture is in the range of 10 / 2 to 10 / 5.
[0024] According to yet another aspect of the present invention, there is provided the method according to any one of the above aspects, wherein the crosslinking agent is a compound having two or more epoxy groups in the molecule.
[0025] According to yet another aspect of the present invention, there is provided a method according to any of the above aspects, wherein the granular carrier is used for carrying a drug.
[0026] According to yet another aspect of the present invention, there is provided a dry granular carrier produced by the production method according to any one of the above aspects.
[0027] According to yet another aspect of the present invention, there is provided a granular carrier according to the above aspect, which is used for carrying a drug.
[0028] According to yet another aspect of the present invention, there is provided a granular drug composition comprising a granular carrier according to any of the above aspects and a liquid composition supported on the granular carrier and containing at least one drug selected from drugs having aromatic, deodorizing, odor eliminating, insect repellent, insecticidal or antifungal properties.
[0029] According to yet another aspect of the present invention, there is provided a granular pharmaceutical composition according to the above aspect, which is an air freshener composition or a deodorant composition.
[0030] According to yet another aspect of the present invention, there is provided an absorbent article comprising a granular carrier according to any of the above aspects. Effect of the Invention
[0031] According to the present invention, a technology is provided for producing a granular carrier that combines high water absorption and biodegradability, has an approximately spherical shape, a uniform particle size, and has excellent water absorption, strength, and transparency. [Brief description of the drawings]
[0032] [Figure 1] FIG. 1 is a flow diagram showing an example of a method for producing a granular carrier according to an embodiment of the present invention. [Diagram 2] 2 is a photograph of the granular carrier 12 produced in Example 3-4 of the [Examples]. (a) shows the dry gel particles, and (b) shows the water-absorbed gel particles. [Figure 3A] 3A is a photograph comparing the particle shape of the granular carrier according to the embodiment of the present invention with the particle shape of crushed gel particles for comparison. (a) is the crushed gel particles (dry state) produced in Example 4-1 of [Example], and (b) is the granular carrier 2 (dry state) produced in Example 1-2 of [Example]. [Figure 3B] 3B is a photograph comparing the particle shape of the granular carrier according to the embodiment of the present invention with the particle shape of crushed gel particles for comparison, where (a) is the crushed gel particles (water-absorbed state) produced in Example 4-1 of [Examples], and (b) is the granular carrier 2 (water-absorbed state) produced in Example 1-2 of [Examples]. [Figure 4]FIG. 4 is a particle size distribution showing the relationship between the particle diameter D (mm) and the frequency (mass %) of the granular carrier 2 produced in Example 1-2 of [Example]. [Diagram 5] FIG. 5 is a photograph of a granular carrier (in a water-absorbed state) produced using an ethanol-containing washing solvent having a different blending ratio of ethanol and water. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. The preferred embodiments described below are embodiments in which any of the above aspects are more specifically embodied.
[0034] The granular carrier obtained by the manufacturing method according to the embodiment of the present invention is a gel particle containing a crosslinked body of a carboxyalkyl cellulose salt, and is a gel particle derived from a dispersed particle formed by suspension polymerization (i.e., reversed-phase suspension polymerization) in a suspension using a low-polarity organic solvent as a dispersion medium, as described below. The granular carrier derived from the dispersed particle obtained by forming a crosslinked body of a carboxyalkyl cellulose salt by this reversed-phase suspension polymerization and washing the filtrate with a specific washing solvent has a substantially spherical shape and a uniform particle size, and is excellent in balance between water absorption and strength, as well as transparency. According to the manufacturing method according to the embodiment of the present invention, a granular carrier having such characteristics can be easily obtained without going through the steps of crushing the gel body and classifying in the above-mentioned conventional manufacturing method.
[0035] In an embodiment of the present invention, the carboxyalkyl cellulose or its salt as the raw material is preferably a carboxyalkyl cellulose or its salt having an alkyl group having 1 to 3 carbon atoms, for example, from the viewpoint of production costs, etc., and specific examples thereof include carboxymethyl cellulose, carboxyethyl cellulose, carboxybutyl cellulose, or salts thereof. The carboxyalkyl cellulose and / or its salt may be used alone or in combination of two or more.
[0036] In an embodiment of the present invention, it is important to select carboxyalkyl cellulose and / or its salt as the raw material, which has a viscosity of 1% by mass aqueous solution within a predetermined range. The longer the polymer chain of carboxyalkyl cellulose, the higher the viscosity when dissolved, and the worse the handling property when injected into the low-polarity organic solvent, which is the dispersion medium. As a result, there is a possibility that the uniformity of the particle shape and particle size of the obtained granular carrier may be adversely affected. On the other hand, the longer the polymer chain of carboxyalkyl cellulose, the higher the water absorption amount, which means that when the granular carrier according to this embodiment is used as a drug carrier, it can carry a large amount of drug. However, if the water absorption amount becomes too large, problems such as a decrease in gel strength and an increase in water separation may occur. From these points of view, in an embodiment of the present invention, carboxyalkyl cellulose and / or its salt is used, which has a viscosity of 5 mPa·s to 300 mPa·s in a 1% by mass aqueous solution.
[0037] Here, the viscosity of a 1% by mass aqueous solution of carboxyalkyl cellulose and / or a salt thereof is the viscosity value measured by a B-type viscometer after preparing a 200 mL aqueous solution of carboxyalkyl cellulose so that the solid content is 1% by mass. Hereinafter, the viscosity of a 1% by mass aqueous solution of carboxyalkyl cellulose and / or a salt thereof measured under these conditions will be simply referred to as the "viscosity of carboxyalkyl cellulose." The viscosity of carboxyalkyl cellulose is preferably 10 mPa·s or more and 100 mPa·s or less, more preferably 20 mPa·s or more and 50 mPa·s or less.
[0038] In an embodiment of the present invention, the average degree of etherification (average degree of substitution, DS) of the raw carboxyalkyl cellulose may be, for example, 0.5 to 1.5. By using a carboxyalkyl cellulose having an average degree of etherification in this range, the water absorption and strength of the gel can be easily improved. The average degree of etherification (average degree of substitution) is the average of the degrees of substitution of hydroxyl groups at the 2-, 3-, and 6-positions of the glucose units constituting the cellulose.
[0039] Fig. 1 is a flow diagram showing an example of a method for producing a granular carrier according to an embodiment of the present invention. The production method shown in Fig. 1 includes the steps of dissolving carboxyalkyl cellulose and / or its salt in an alkaline aqueous solution to prepare a carboxyalkyl cellulose salt aqueous solution S1, preparing a mixture of the carboxyalkyl cellulose salt aqueous solution obtained in step S1 and a crosslinking agent in step S2, dispersing the mixture obtained in step S2 in a low-polarity organic solvent to form a suspension (reverse phase suspension), proceeding with crosslinking polymerization of the carboxyalkyl cellulose salt in this suspension to form dispersed particles containing a crosslinked body of the carboxyalkyl cellulose salt in step S3, and filtering, washing, and drying the dispersed particles formed in step S3 from the suspension in step S4.
[0040] 1 is an example, as described above. In other examples, the manufacturing method according to the embodiment of the present invention may further include other steps not shown in FIG.
[0041] In step S1, carboxyalkyl cellulose and / or its salt are added (injected) into the aqueous alkali solution and completely dissolved under stirring at room temperature to prepare an aqueous carboxyalkyl cellulose salt solution. In step S1, the time required to prepare the aqueous carboxyalkyl cellulose salt solution can be appropriately set, but according to one example, it can be 1 to 5 hours. After adding the carboxyalkyl cellulose to the aqueous alkali solution, a defoaming treatment can be performed by reducing pressure or by leaving it at normal pressure for a predetermined time, as necessary.
[0042] The carboxyalkyl cellulose and / or salt thereof used in step S1 may be one obtained by using cellulose such as pulp as a starting material and carboxyalkylating it in a conventional manner, or a commercially available carboxyalkyl cellulose and / or salt thereof may be used.
[0043] The carboxyalkylcellulose salt contained in the carboxyalkylcellulose salt aqueous solution obtained in step S1 may be, for example, an alkali metal salt or an alkaline earth metal salt of carboxyalkylcellulose, and in this case, an alkali aqueous solution containing an alkali metal or an alkaline earth metal is used as the alkali aqueous solution to which carboxyalkylcellulose and / or its salt is added. Examples of carboxyalkylcellulose salt include sodium salt, potassium salt, or calcium salt. In this case, an aqueous solution of sodium hydroxide, potassium hydroxide, or calcium hydroxide is used as the alkali aqueous solution to which carboxyalkylcellulose is added. According to one example, sodium carboxymethylcellulose (CMC-Na) is used as the carboxyalkylcellulose and / or its salt, and sodium hydroxide is used as the alkali aqueous solution to prepare a CMC-Na aqueous solution in step S1.
[0044] In step S2, the carboxyalkyl cellulose salt aqueous solution obtained in step S1 is mixed with a crosslinking agent to prepare a mixture of the carboxyalkyl cellulose salt aqueous solution and the crosslinking agent. Hereinafter, when the term "mixture" is used simply, this refers to the mixture of the carboxyalkyl cellulose salt aqueous solution and the crosslinking agent prepared in step S2.
[0045] The mixing of the aqueous carboxyalkyl cellulose salt solution and the crosslinking agent is preferably carried out at 10°C to 80°C, more preferably 20°C to 50°C, using, for example, a static mixer. If the temperature is higher than 80°C, the crosslinking reaction proceeds quickly, and it tends to be difficult to obtain uniform spherical gel particles in the next step S3. If the temperature is lower than 10°C, the viscosity of the mixture increases, and the handling properties when the mixture is added to the low-polarity organic solvent in the next step S3 tend to deteriorate. Immediately after the crosslinking agent is added to the aqueous carboxyalkyl cellulose salt solution in step S2, the crosslinking reaction of the carboxyalkyl cellulose salt starts, and the viscosity begins to increase. Therefore, from the viewpoint of handling properties when the mixture is added to the low-polarity organic solvent in the next step S3, the time from adding the crosslinking agent to the aqueous carboxyalkyl cellulose salt solution to adding the mixture to the low-polarity organic solvent can be appropriately set. According to one example, the reaction temperature can be adjusted within the above range and within 30 minutes as a guideline. After stirring, a degassing operation under reduced pressure may be performed as necessary.
[0046] The crosslinking agent used in the production method according to the embodiment of the present invention is not particularly limited, and known compounds such as polyepoxy compounds, polyglycidyl compounds, polyaldehyde compounds, polycarboxylic acids, vinyl ether compounds, methylol compounds, polyisocyanates, polyoxazoline compounds, polyvinyl compounds, polyacrylate compounds, polymethacrylate compounds, polyhalogen compounds, methylene bisacrylamide, epichlorohydrin, polyacid anhydrides, citric acid, methylene bisacrylamide, and glycidyl methacrylate can be used.
[0047] Preferred specific examples of the crosslinking agent include (a) a compound having two or more hydroxyl groups in the molecule, (b) a compound having two or more polymerizable double bonds, and (c) a compound having two or more epoxy groups.
[0048] (a) Examples of compounds having two or more hydroxyl groups in the molecule include ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, glycerin, polyglycerin, propylene glycol, diethanolamine, polyoxypropylene, sorbitan fatty acid esters, trimethylolpropane, pentaerythritol, 1,3-propanediol, and sorbitol.
[0049] (b) Examples of compounds having two or more polymerizable double bonds in the molecule include bis(meth)acrylamide, allyl(meth)acrylamide, diethylene glycol diacrylate, trimethylolpropane triacrylate, polyethylene glycol diacrylate, and ethoxylated trimethylolpropane triacrylate.
[0050] (c) Examples of compounds having two or more epoxy groups in the molecule include polyglycidyl ethers such as ethylene glycol diglycidyl ether (EGDE), polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, glycerin triglycidyl ether, glycerol polyglycidyl ether, polyglycerol polyglycidyl ether, trimethylolpropane polyglycidyl ether, sorbitol polyglycidyl ether, pentaerythritol polyglycidyl ether, resorcinol diglycidyl ether, neopentyl glycol diglycidyl ether, and hydrogenated bisphenol A diglycidyl ether.
[0051] Among these, from the viewpoints of reactivity and the water absorption performance of the resulting granular carrier, (b) a compound having two or more polymerizable double bonds in its molecule, and (c) a compound having two or more epoxy groups in its molecule are preferred, (c) a compound having two or more epoxy groups in its molecule is more preferred, polyglycidyl ether is even more preferred, and ethylene glycol diglycidyl ether (EGDE) is particularly preferred.
[0052] The blending mass ratio of the carboxyalkyl cellulose and / or its salt to the crosslinking agent can be appropriately set. From the viewpoint of the shape, transparency and strength of the granular carrier, the blending mass ratio (X / Y) of the carboxyalkyl cellulose and / or its salt (X) to the crosslinking agent (Y) is preferably in the range of 10 / 2≧X / Y≧10 / 5, more preferably in the range of 10 / 2>X / Y≧10 / 4.
[0053] In step S3, the mixture obtained in step S2 is added (injected) into a low-polarity organic solvent and dispersed to form a suspension (reverse phase suspension), and dispersed particles containing crosslinked bodies of carboxyalkyl cellulose salt are formed by crosslinking polymerization in this suspension.
[0054] The low-polarity organic solvent used as the dispersion medium in step S3 is a low-polarity organic solvent having a relative dielectric constant of 10 or less at 25°C, and is less polar than the above mixture of dispersoids. Therefore, the suspension prepared in step S3 is a reversed-phase suspension, and the cross-linking polymerization of the carboxyalkyl cellulose salt is a reversed-phase suspension polymerization. Here, the relative dielectric constant is the relative dielectric constant at 25°C measured by a capacitance meter. According to one example, it is more preferable that the low-polarity organic solvent used as the dispersion medium has a relative dielectric constant of 3 or more and 6 or less.
[0055] Examples of low-polarity organic solvents having a relative dielectric constant of 10 or less include aliphatic hydrocarbons, alicyclic hydrocarbons, aromatic hydrocarbons, liquid paraffin, silicone oil, etc., and these can be used alone or in combination of two or more.
[0056] The low polarity organic solvent used in step S3 has a kinetic viscosity of 10 mm at 37.8° C. 2 When the dispersion medium is a viscous fluid, the aggregation of the generated spherical gel particles can be suppressed, and the adhesion between the spherical gel particles can be suppressed, thereby suppressing the formation of clumps of the spherical gel particles. 2 / s or more is important in order to obtain high quality granular carriers which are spherical in shape and have a uniform particle size.
[0057] Here, the kinematic viscosity is the kinematic viscosity at 37.8° C. measured by a vibration viscometer. According to one example, the low polarity organic solvent used as the dispersion medium has a kinematic viscosity of 10 mm 2 / s or more 100mm 2 / s or less, and according to other examples, 15 mm 2 / s or more 80mm 2 / s or less, and according to another example, 20 mm 2 / s or more 50mm 2 / s or less.
[0058] Among the above-mentioned specific examples of low-polarity organic solvents having a relative dielectric constant of 10 or less, liquid paraffin and silicone oil are particularly preferable as the low-polarity organic solvent used in step S3 because they are viscous fluids.
[0059] The liquid paraffin is not particularly limited as long as it is a paraffin that is liquid at room temperature, and examples thereof include liquid saturated hydrocarbons having 12 to 50 carbon atoms, and may be any of n-paraffin, isoparaffin, and naphthene. In addition, examples of commercially available products that can be used include Moresco White, Moresco Bioless, and Smoil (registered trademark) (all trade names, manufactured by Matsumura Oil Research Institute), Stanol, Krystoll, Esso White Oil, and Purelex (all trade names, manufactured by Esso Oil Co., Ltd.). These may be used alone, or two or more of them may be used in combination.
[0060] The silicone oil is not particularly limited as long as it has a siloxane structure that is liquid at room temperature, and examples thereof include polysiloxane oils such as dimethyl silicone oil, and modified silicone oils having functional groups such as hydroxyl groups, carboxyl groups, amino groups, epoxy groups, cyano groups, mercapto groups, trifluoropropyl groups, chlorophenyl groups, long-chain alkyl groups, and the like, or modified with polyethers, alcohols, etc. These may be used alone or in combination of two or more kinds.
[0061] In step S3, the above-mentioned crosslinking agent may be further added to the low-polarity organic solvent to perform surface crosslinking (secondary crosslinking) to provide a portion with high crosslink density on the surface layer of the gel particles. By performing surface crosslinking (secondary crosslinking), it is possible to improve the gel strength while maintaining the water absorption amount.
[0062] In step S3, the low polarity organic solvent to which the mixture obtained in step S2 is added is stirred. Examples of the stirring device include a mechanical stirrer, and examples of the stirring blade include an anchor type, a propeller type, a paddle type, and the like, and can be appropriately selected and used. In one example, in step S3, the low polarity organic solvent is stirred at a rotation speed of 50 to 500 rpm, in another example, at a rotation speed of 200 to 500 rpm, and in yet another example, at a rotation speed of 250 to 400 rpm.
[0063] In step S3, the mixture obtained in step S2 is added (injected) into the low-polarity organic solvent, for example, by dripping the mixture drop by drop from the liquid surface of the low-polarity organic solvent using a pipette (hereinafter, sometimes referred to as the "drop injection method"). Another example is by continuously injecting the mixture while immersing a pipette in the low-polarity organic solvent (hereinafter, sometimes referred to as the "continuous injection method"). The drop injection method is preferred because it makes it easier to obtain uniform particle sizes for the dispersed particles. The continuous injection method is preferred because it can be easily performed in a short time.
[0064] In step S3, the time required for the cross-linking polymerization reaction of the carboxyalkyl cellulose salt can be appropriately set. According to one example, it can be set to 1 hour to 6 hours.
[0065] In step S3, the low-polarity organic solvent is at room temperature or in a heated state immediately before the mixture obtained in step S2 is added. According to one example, in step S3, the cross-linking polymerization is carried out by carrying out a first step of stirring the suspension under a first condition and a second step of stirring the suspension under a second condition in this order.
[0066] First, in the first step, the low polarity organic solvent is adjusted to a moderately low temperature (T1) immediately before the mixture is added, and after the mixture is added, the mixture is stirred at the temperature T1 for a predetermined time (t1). Specifically, the temperature T1 is preferably in the range of 15°C to 43°C, more preferably in the range of 15°C to 40°C. The stirring time t1 at the temperature T1 is preferably in the range of 10 minutes to 120 minutes, more preferably in the range of 20 minutes to 60 minutes. In the first step, stirring is continued for a sufficiently long time under temperature conditions in which cross-linking polymerization does not proceed rapidly. Therefore, in the first step, the particle size is uniformized by the coalescence and division of the dispersed particles. In addition, in the first step, since the cross-linking polymerization proceeds slowly, further coalescence and division of the dispersed particles are unlikely to occur as the particle size is uniformized. Therefore, the particle size of the dispersed particles is uniform at the time when the first step is completed.
[0067] In the second step, the low polarity organic solvent is heated to a higher temperature T2 and stirred for a predetermined time (t2). Specifically, the temperature T2 is preferably in the range of 46°C to 80°C, more preferably in the range of 46°C to 60°C. The stirring time t2 at the temperature T2 is preferably in the range of 120 minutes to 360 minutes, more preferably in the range of 240 minutes to 300 minutes. By carrying out the stirring at a higher temperature in the second step, the crosslinking polymerization proceeds sufficiently. Therefore, the step S3 can be completed in a sufficiently short time.
[0068] Thereafter, step S4 is carried out as shown in Fig. 1. That is, the dispersed particles containing the crosslinked body of the carboxyalkyl cellulose salt formed in the suspension in step S3 are taken out from the suspension by filtration, washed, and further dried as necessary.
[0069] The washing after filtration usually involves washing the gel particles with an aqueous detergent solution containing a surfactant, etc., and then washing with a washing solvent containing ethanol. The above step of washing with an aqueous detergent solution is preferred because it can effectively remove low-polarity organic solvents attached to the surfaces of the gel particles. For example, this is done by rinsing the surfaces of the filtered gel particles with an appropriate amount of an aqueous detergent solution. However, this step can be omitted.
[0070] The above-mentioned washing step using a washing solvent containing ethanol is carried out for dehydrating and de-alkalizing the gel particles. The ethanol-containing washing solvent used here (hereinafter also simply referred to as "washing solvent") has an ethanol content of more than 60% by mass. The washing solvent may be a solvent with an ethanol content of 100% by mass, or may be a mixed solvent of ethanol and water.
[0071] It is preferable that the washing solvent is a mixed solvent of ethanol and water in order to obtain a granular carrier with excellent water absorption. By adding water to ethanol as a washing solvent, the shrinkage speed of the gel particles during washing can be reduced, and therefore it becomes possible to wash the gel to the center. As a result, the water absorption rate of the granular carrier is improved. On the other hand, the strength of the gel particles tends to decrease as the amount of liquid absorption increases. If the granular carrier does not have a predetermined strength compared to its water absorption rate, the shape of the granular gel is easily destroyed by shearing due to stirring during the manufacturing process. Thus, the balance between the water absorption rate and the strength of the granular carrier is important. From the viewpoint of the balance between the water absorption rate and the strength, the ethanol content of the washing solvent is more than 60% by mass. As described above, the washing solvent may be a solvent with an ethanol content of 100% by mass, or a mixed solvent of ethanol and water, as long as the ethanol content is more than 60% by mass. When the washing solvent is a mixed solvent of ethanol and water, the ethanol content is more preferably in the range of more than 60 mass% to not more than 85 mass%, even more preferably in the range of more than 60 mass% to not more than 78 mass%, and most preferably in the range of more than 60 mass% to not more than 73 mass%.
[0072] In the manufacturing process of this embodiment, a granular carrier having an excellent balance between water absorption and strength has a solvent absorption rate of the cleaning solution represented by the following formula (1) immediately after washing with the above-mentioned ethanol-containing cleaning solvent of preferably 25 or less, more preferably in the range of 0.8 or more and 25 or less, even more preferably in the range of 1 or more and 25 or less, and most preferably in the range of 2 or more and 25 or less. Solvent absorption rate=(M1-M2) / M2 (1) In formula (1), M1 represents the mass of the gel particles carrying a saturated amount of the washing solvent after the above washing, and M2 represents the mass of the gel particles after drying after the above washing.
[0073] The washing with the ethanol-containing washing solvent is carried out, for example, by immersing the filtered gel particles in the washing solvent, which is preferably stirred at this time.
[0074] In step S4, the washed gel particles are dried. Drying can be performed by, for example, air drying or drying under reduced pressure.
[0075] The particle diameter of the granular carrier according to the present embodiment is not particularly limited, but there is a preferred particle diameter depending on the purpose of use.For example, when the granular carrier according to the present embodiment is used for carrying medicine, the average particle diameter of the gel particles in the water-absorbed state may be 2 mm or more and 30 mm or less in one example, and 2 mm or more and 20 mm or less in another example.Here, the average particle diameter means the one measured by measuring the major axis of 30 randomly selected particles using a caliper and averaging them.
[0076] In addition, when the granular carrier according to the present embodiment is used for carrying drugs, the average particle size of the gel particles in a dry state may be, for example, 0.2 mm to 6 mm, and in another example, 0.5 mm to 4 mm. Here, the average particle size refers to the value measured by measuring the major axis of 30 randomly selected particles using a vernier caliper and averaging the measurements.
[0077] According to one example, the granular carrier of this embodiment can be used in a dry state as a highly absorbent material in absorbent articles such as disposable diapers, sanitary products (napkins, tampons, etc.), pads (sweat pads, breast milk pads, incontinence pads, etc.), and pet toilets.
[0078] In another example, the granular carrier according to the present embodiment is used as a drug carrier. That is, a liquid composition containing at least one drug selected from drugs having, for example, aromatic, deodorant, deodorizing, insect repellent, insecticidal, or antifungal properties is absorbed and carried by the granular carrier made of the dry gel particles according to the present embodiment. This makes it possible to provide gel formulations such as granular drug compositions, such as granular aromatic composition, granular deodorant composition, granular deodorant composition, granular insect repellent composition, granular insecticide composition, and granular antifungal composition.
[0079] In a gel preparation consisting of such a granular pharmaceutical composition, various commonly used drugs can be used as the pharmaceutical component contained in the liquid composition that is absorbed and carried by the granular carrier, depending on the purpose. Specific examples of aromatic drugs include animal fragrances such as musk, spirit cat fragrance, and dragon jasmine fragrance, and vegetable fragrances such as abies oil, acorn oil, almond oil, angelica root oil, page oil, bergamot oil, perch oil, boa bur rose oil, kayabuchi oil, gananga oil, capsicum oil, caraway oil, cardamom oil, cassia oil, celery oil, cinnamon oil, citronella oil, cognac oil, coriander oil, cumin oil, camphor oil, basil oil, estugoran oil, eucalyptus oil, fennel oil, garlic oil, ginger oil, grapefruit oil, hop oil, lemon oil, lemongrass oil, nutmeg oil, mandarin oil, peppermint oil, orange oil, sage oil, star anise oil, turpentine oil, rosemary oil, eucalyptus oil, anise oil, lavender oil, cumin oil, cinnamon oil, and hiba oil. In addition, artificial fragrances such as synthetic fragrances or extracted fragrances can also be used. Specific examples include hydrocarbon fragrances such as pinene and limonene, alcohol fragrances such as linalool, geraniol, citronellol, menthol, borneol, benzyl alcohol, anise alcohol, and β-phenethyl alcohol, phenol fragrances such as anethole and eugenol, aldehyde fragrances such as n-butyl aldehyde, isobutyraldehyde, hexyl aldehyde, citral, citronellal, benzaldehyde, and cinnamic aldehyde, ketone fragrances such as carvone, menthone, camphor, acetophenone, and ionone, lactone fragrances such as γ-butyrolactone, coumarin, and cineol, and ester fragrances such as octyl acetate, benzyl acetate, cinnamyl acetate, butyl propionate, and methyl benzoate. These may be used alone or in any combination of two or more.
[0080] The deodorizing agent may be either a volatile agent or a non-volatile agent, and specific examples include metal oxides such as titanium oxide and zinc oxide, flavonoid compounds, plant extracts such as catechin and polyphenol or derivatives thereof, cyclodextrin or derivatives thereof, amine compounds, etc. These may be used alone or in any combination of two or more.
[0081] Specific examples of deodorizing agents include activated carbon such as coconut shell activated carbon, charcoal such as binchotan charcoal, and other carbon-based adsorbents, as well as silica-based adsorbents such as zeolite, silica gel, and layered zinc aluminosilicate, etc. These may be used alone or in any combination of two or more.
[0082] Specific examples of agents having insect repellent or insecticidal properties include pyrethroid insecticidal components such as empenthrin, transfluthrin, allethrin, fenothrin, eminence, and profluthrin, and volatile insect repellent and insecticidal components such as paradichlorobenzene, naphthalene, camphor, 2-phenoxyethanol, hinokitiol, and allyl isothiocyanate. These can be used alone or in any combination of two or more.
[0083] In addition to the above-mentioned drugs, various additives can be used in the liquid composition, such as surfactants, colorants, preservatives, and pH adjusters.
[0084] The granular pharmaceutical composition according to this embodiment can be produced, for example, by impregnating dry gel particles into a liquid pharmaceutical composition.
[0085] As described above, the granular carrier according to the present embodiment, which is a gel particle derived from a dispersed particle formed by reversed-phase suspension polymerization using a low-polarity organic solvent as a dispersion medium, has a substantially spherical shape and a uniform particle size. Therefore, the granular drug composition obtained by carrying a liquid drug composition on the granular carrier according to the present embodiment is likely to cause air flow when filled in a container, and the drug carried on the granular carrier can function efficiently. In addition, the granular drug composition according to the present embodiment is also excellent in strength, transparency, and ability to suppress water separation. Therefore, the granular carrier according to the present embodiment is suitably used for carrying a drug in a granular gel preparation filled in a container in stationary products such as air fresheners and deodorants. EXAMPLES
[0086] Tests carried out in relation to the present invention are described below. ≪Example 1≫ CMC-Na viscosity <Example 1-1: Production of Granular Carrier 1> The raw material used was sodium carboxymethylcellulose (CMC-Na) (Daicel 1110, manufactured by Daicel Miraize Co., Ltd.) with a viscosity in the range of 10 to 20 mPa s. The viscosity here is the viscosity of a 1% by mass aqueous solution of CMC-Na at 25°C measured by the method described above.
[0087] 10.0 g of the above CMC-Na (Daicel 1110) was dissolved in 100 mL of 0.5 mol / L aqueous sodium hydroxide solution. 4.0 g of ethylene glycol diglycidyl ether (EGDE) (Denacol EX-810, Nagase Chemtex Corporation) was added dropwise to this aqueous solution as a crosslinking agent, and the solution was stirred for 20 minutes, after which a degassing operation was performed for 5 minutes under reduced pressure. This resulted in a mixture of an aqueous CMC-Na solution and EGDE. In this example, the blending mass ratio of CMC-Na to the crosslinking agent EGDE (CMC-Na / EGDE) was 10 / 4.
[0088] Next, the obtained mixture was added to liquid paraffin (Moresco White P-100, manufactured by MORESCO Corporation; kinematic viscosity 20.5 mm) heated to 60° C. and stirred at a stirring speed of 250 rpm. 2 The mixture was injected into a liquid paraffin (100 ml / s). A high-viscosity pipette was used to inject the mixture, and the tip of the pipette was immersed in the liquid paraffin while it was being injected. The mixture was allowed to react in the liquid paraffin for 4 hours. After the reaction, the gel particles that had formed were filtered off, and the liquid paraffin adhering to the gel particle surface was washed off with an appropriate amount of aqueous surfactant solution. The gel particles were then immersed in ethanol to dehydrate and dealkalinize, and then air-dried to obtain a white to pale yellow solid (granular carrier 1).
[0089] <Examples 1-2 to 1-6: Production of Granular Carriers 2 to 6> Granular carriers 2 to 6 were produced in the same manner as in Example 1-1, except that the CMC-Na (Daicel 1110, viscosity 10-20 mPa·s) in Example 1-1 was changed to the CMC-Na shown in Table 1 below.
[0090] <Evaluation> [Handling when pouring into liquid paraffin (ease of pouring)] In the manufacturing process of each granular carrier, the handling property when injecting the mixture of CMC sodium salt and EGDE into the liquid paraffin was evaluated based on the following criteria from the viewpoint of ease of drawing into the pipette and ease of injection from the pipette into the liquid paraffin. The evaluation results are shown in Table 1. A: It can be easily aspirated and injected. B: Aspiration and injection take some time, but are not difficult. C: Difficult to suction and inject.
[0091] [Shape of granular carrier (dried gel)] The shape of each of the resulting granular carriers (dried gels) was visually evaluated according to the following criteria. The evaluation results are shown in Table 1. A: Spherical dry gels make up the majority of the gel, and dry gels of other shapes are hardly found. B: Spherical dry gels make up the majority of the gel. Flat or thread-like dry gels are mixed in, but not noticeable. C: Most of the gel is thread-like, with few spherical gels.
[0092] [Transparency] Each of the obtained granular carriers (dried gels) was immersed in ion-exchanged water to absorb the maximum amount of water that it could absorb, and the transparency of the water-absorbed gel particles was evaluated visually according to the following criteria. The evaluation results are shown in Table 1. A: There is no cloudiness and the overall transparency is high. B: Some parts are cloudy, but more than 80% is transparent, and the overall appearance is transparent. C: Many parts are cloudy or the whole is cloudy, with low transparency overall.
[0093] [Strength] 1 g of each of the obtained granular carriers (dried gel particles) was filled into a 200 mL beaker, 150 mL of ion-exchanged water was added, and the mixture was left to stand overnight to obtain water-absorbed gel particles carrying the maximum amount of water that they could absorb. After filtering the water-absorbed gel particles to remove excess water, the water-absorbed gel particles were filled into the 200 mL beaker again. At this time, the inside of the container was piled up with approximately six layers of particles from the bottom to the top. These were used as evaluation samples, and their strength was evaluated according to the following criteria. The evaluation results are shown in Table 1. A: The strength at which a particle located at the bottom of a container and bearing a weight approximately six times its own weight maintains its spherical shape and uniformly sized gaps form between particles throughout the packed structure. B: A strength at which at least some of the particles located at the bottom of the container and subjected to a weight approximately six times its own weight are unable to maintain their spherical shape, resulting in some areas where no gaps exist between the particles at the bottom. C: A strength at which the particles are unable to maintain their spherical shape even under their own weight.
[0094] [Table 1]
[0095] From Table 1, it can be seen that granular carriers 1 to 5 of Examples 1-1 to 1-5 according to the embodiment of the present invention are excellent in particle shape, transparency, and strength. Moreover, Examples 1-1 to 1-5 are also excellent in handleability when injecting the mixture into liquid paraffin, and it can be seen that granular carriers (gel particles) excellent in particle shape, transparency, and strength can be easily obtained by reversed-phase suspension polymerization. On the other hand, it can be seen that it is difficult to produce spherical gel particles by reversed-phase suspension polymerization in Example 1-6 (Comparative Example), which uses CMC with high viscosity.
[0096] Example 2: CMC-Na / crosslinking agent (mass ratio) <Examples 2-1 and 2-2: Production of Granular Carriers 7 and 8> Granular carriers 7 and 8 were produced in the same manner as in Example 1-2 above, in which Daicel 1120 (viscosity 20 to 50 mPa s) was used as the raw material (CMC-Na), except that the blending mass ratio of CMC-Na and EGDE was changed as shown in Table 2. The dried gel shape, transparency, and strength of each granular carrier were evaluated in the same manner as in Example 1-1. The evaluation results are shown in Table 2.
[0097] [Table 2]
[0098] In addition, in Example 2-1, the strength evaluation was B, but the portion where no gaps occurred between the particles was only a part of the bottom part of the packed particles, and the fluidity of the air was ensured.
[0099] <Example 3> Dynamic viscosity of liquid paraffin and stirring speed <Examples 3-1 to 3-5: Production of Granular Carriers 9 to 13> Granular carriers were produced in the same manner as in Example 1-2 (granular carrier 2) above, which used Daicel 1120 (viscosity 20 to 50 mPa s) as the raw material (CMC-Na), except that the liquid paraffin and stirring speed were changed as shown in Table 3. The dried gel shape of each granular carrier was evaluated in the same manner as in Example 1-1. The evaluation results are shown in Table 3.
[0100] However, low viscosity (kinetic viscosity 4.51 mm 2 In Examples 3-1 and 3-2, in which liquid paraffin (100 g / s) was used, the mixture accumulated at the bottom and coalesced, and granular gel particles could not be obtained.
[0101] [Table 3]
[0102] In addition, in Example 3-3, the strength evaluation was B, but the portion where no gaps occurred between the particles was only a part of the bottommost part of the packed particles, and the fluidity of the air was ensured.
[0103] Example 4 Comparison of particle shapes between granular carrier according to the embodiment and crushed gel particles <Example 4-1: Production of crushed gel> 10.0 g of CMC-Na (Daicel 1120, Daicel Miraize Co., Ltd.) was dissolved in 100 mL of 0.5 mol / L aqueous sodium hydroxide solution. 4.0 g of EGDE (Denacol EX-810, Nagase ChemteX Co., Ltd.) was added dropwise and stirred for 20 minutes. After degassing for 5 minutes under reduced pressure, the mixture was reacted for 4 hours in a thermostatic bath at 60°C. After the reaction, the gel-like material formed was removed from the beaker and roughly crushed using a mixer. The crushed gel obtained was immersed in ethanol to be dehydrated and dealkalized, and then air-dried to obtain a white to pale yellow solid.
[0104] <Evaluation> Fig. 3A(a) is a photograph of the dried pulverized gel particles produced in Example 4-1, and Fig. 3B(a) is a photograph of the water-absorbed state of the particles. Fig. 3A(b) is a photograph of the granular carrier 2 (dried gel particles) produced in Example 1-2, and Fig. 3B(b) is a photograph of the water-absorbed state of the particles. Comparing (a) and (b) of Figure 3A and (a) and (b) of Figure 3B, it is clear that the particle shape of the granular carrier in this embodiment is completely different from the particle shape of the crushed gel particles. That is, from (a) of Figure 3A and (a) of Figure 3B, it can be seen that the crushed gel particles obtained by the conventional method of crushing the hydrogel formed by aqueous solution polymerization are in the form of fragments with sharp edges, and most of the particles have a distorted shape that cannot be said to be spherical. On the other hand, from (b) of Figure 3A and (b) of Figure 3B, the gel particles according to this embodiment derived from the dispersed particles formed by reverse suspension polymerization are spherical in shape and have a uniform particle size. It can be seen that the manufacturing method according to the embodiment of the present invention makes it possible to easily obtain high-quality gel particles.
[0105] Example 5: Uniformity of particle size The granular carrier 2 (dried gel particles) obtained in Example 1-2 was classified into particles having a particle size of D>4 mm, 4 mm≧D>2 mm, 2 mm≧D>1 mm, 1 mm≧D>0.25 mm, and 0.25 mm≧D using sieves with openings of 4 mm, 2 mm, 1 mm, and 0.25 mm. Figure 4 shows the results and is a graph showing the particle size distribution of the granular carrier 1-2. From FIG. 4, it can be seen that 90% by mass or more of the frequency (mass%) of the granular carrier 2 has a particle diameter D in the range of 2 mm or more and less than 4 mm, and thus the uniformity of the particle size is excellent.
[0106] Example 6: Uniformity of particle shape and size Figure 2 is a photograph of the granular carrier 12 obtained in Example 3-4. (a) is a dry gel particle, and (b) is a water-absorbed gel particle. From the photograph in Figure 2, it can be seen that the granular carrier 12 is dominated by roughly spherical particles and has excellent uniformity in particle size.
[0107] Example 7: Evaluation of the balance between water absorption and strength in granular carriers <Examples 7-1 to 7-4: Production of Granular Carriers 14 to 17> 6 g of sodium hydroxide was added to 300 mL of ion-exchanged water in a resin beaker to obtain an aqueous sodium hydroxide solution. 30 g of CMC-Na (Daicel 1120, Daicel Miraize Co., Ltd.) was added to this aqueous sodium hydroxide solution and completely dissolved while stirring. The obtained aqueous CMC-Na solution was left to stand overnight to defoam. Next, 12 g of EGDE (Denacol EX-810, Nagase ChemteX Co., Ltd.) was dropped into this aqueous CMC-Na solution as a crosslinking agent, and the mixture was stirred at a rotation speed of 250 rpm for 30 minutes to obtain a mixture of the aqueous CMC-Na solution and EGDE. In this example, the blending mass ratio of CMC-Na to the crosslinking agent EGDE (CMC-Na / EGDE) was 10 / 4.
[0108] Next, the obtained mixture was added to liquid paraffin (Sumoil P100, manufactured by Matsumura Oil Co., Ltd.; kinematic viscosity 20.45 mm) at room temperature of 23°C, which was being stirred at a stirring speed of 250 rpm. 2The mixture was injected into a liquid paraffin tube (900 g) at 100°C (100 / s). A high-viscosity pipette was used to inject the mixture, and the tip of the pipette was immersed in the liquid paraffin while it was being injected. With stirring continued, the liquid temperature was kept at room temperature for 10 minutes after the injection of the mixture was completed, and then heating was started. After the liquid temperature exceeded 50°C, the reaction was allowed to proceed for 4 hours while stirring. During this time, the liquid temperature was kept within the range of 50 to 65°C.
[0109] After the reaction, the gel particles formed were filtered, and the liquid paraffin adhering to the surface of the gel particles was washed off with an appropriate amount of surfactant aqueous solution. The gel particles were washed with the surfactant aqueous solution and each was taken in an amount of 70 g to obtain six samples.
[0110] Six types of ethanol-containing cleaning solvents (700 mL) were prepared, with ethanol (EtOH):deionized water (DIW) ratios of 100:0, 90:10, 80:20, 75:25, 70:30, and 60:40 (mass ratio). Each of the six samples obtained above was immersed in the six types of ethanol-containing cleaning solvents and stirred overnight at a rotation speed of 200 rpm. Next, each sample was filtered, and the mass M1 (g) of the gel particles carrying the saturated amount of ethanol-containing cleaning solvent immediately after filtration was measured. Thereafter, the gel particles were immersed in a single solvent of ethanol to be dehydrated and dealkalized again. After 4 hours, the gel particles were filtered, air-dried at ambient temperature overnight, and then dried under reduced pressure for 4 hours to obtain granular carriers (granular carriers 14 to 19) that were completely dry solids. The mass M2 (g) of the granular carriers 14 to 19 in the dry state was measured.
[0111] <Evaluation> Solvent absorption rate (R1) Using the mass M1 of the gel particles carrying a saturated amount of the ethanol-containing washing solvent and the mass M2 of the dried gel particles (granular carrier), the solvent absorption rate (R1) of the gel particles after washing with the ethanol-containing washing solvent was calculated according to the following formula (1). The results are shown in Table 4. Solvent absorption rate (R1)=(M1-M2) / M2 (1)
[0112] ·Water absorption rate (R2) The amount of water absorption (M3) (g) of each of the granular carriers 14 to 17 in a dry state obtained above was measured using 0.2 g of each of the granular carriers by the tea bag method described below. The water absorption rate (R2) of each of the granular carriers was calculated using the amount of water absorption M3 and the mass of the granular carrier according to the following formula (2). The results are shown in Table 4. Water absorption rate (R2)=M3 / 0.2 (2)
[0113] The water absorption was measured according to the tea bag method described in JIS K7223 Super Absorbent Resin Water Absorption Test Method. Nylon fabric with 57 μm mesh was cut into a 10 x 40 cm rectangle, folded lengthwise, and both ends were heat sealed to form a bag to make a tea bag. The bottom 150 mm of the tea bag containing 0.2 g of sample was immersed in 1 L of deionized water. After 24 hours, the tea bag was removed from the deionized water and the mass of the tea bag was measured. The same procedure was performed on a tea bag without a sample, and the amount of liquid absorbed by the sample was measured from the difference.
[0114] The water absorption amount (M3) of the granular carriers 14 to 19 was measured by the above-mentioned tea bag method, and then the gel particles were taken out of the tea bags to obtain each gel particle in a water-absorbed state. Each of these gel particles was divided into water-absorbed gel particles in which the granular gel shape was broken (hereinafter referred to as "crushed") and water-absorbed gel particles in which the granular gel shape was not broken (hereinafter referred to as "not crushed"). The mass Mx (g) of the crashed water-absorbed gel particles and the mass My (g) of the not-crushed water-absorbed gel particles were measured, and the crush rate (R3) (%) was calculated by the following formula (3). The results are shown in Table 4. In addition, photographs of the gel particles of Examples 7-1, 7-3, 7-4, and 7-6 among the above gel particles in a water-absorbed state taken out of the tea bags are shown in FIG. 5. Crash rate (R3)(%)=[Mx / (Mx+My)]×100 (3)
[0115] [Table 4]
[0116] Comparing Examples 7-1 to 7-6, it can be seen that as the water content in the ethanol-containing washing solvent increases, the solvent absorption rate (R1) of the gel particles immediately after washing increases. Furthermore, in Comparative Example 7-6, which uses a washing solvent with an ethanol content of 60 mass%, the water absorption rate (R2) is high, but the crush rate R3 is also high, and it can be seen that the granular carrier 19 has a poor balance between water absorption rate and strength. On the other hand, in Examples 7-1 to 7-5, the water absorption rate (R2) is high and the crush rate is low, and it can be seen that the balance between water absorption rate and strength is excellent.
[0117] The present invention is not limited to the above-mentioned embodiment, and can be modified in various ways without departing from the gist of the present invention. The embodiments may be combined as appropriate, and in that case, the combined effect can be obtained. Furthermore, the above-mentioned embodiment includes various inventions, and various inventions can be extracted by combinations selected from the multiple components disclosed. For example, if the problem can be solved and the effect can be obtained even if some components are deleted from all the components shown in the embodiment, the configuration from which the components are deleted can be extracted as an invention. [Explanation of symbols]
[0118] S1...process, S2...process, S3...process, S4...process.
Claims
1. A method for producing a granular carrier comprising gel particles containing a crosslinked body of a carboxyalkyl cellulose salt, comprising the steps of: A carboxyalkyl cellulose and / or a salt thereof having a viscosity of 5 mPa·s or more and 300 mPa·s or less in a 1% by mass aqueous solution at 25°C is dissolved in an alkaline aqueous solution to prepare a carboxyalkyl cellulose salt aqueous solution; preparing a mixture of the aqueous carboxyalkyl cellulose salt and a crosslinking agent; dispersing the mixture in a low-polarity organic solvent to form a suspension, and proceeding with crosslinking polymerization of the carboxyalkyl cellulose salt in the suspension to form dispersed particles consisting of gel particles containing a crosslinked body of the carboxyalkyl cellulose salt; filtering the gel particles from the suspension; and Washing the gel particles with a washing solvent having an ethanol content of more than 60% by mass. Including, The low-polarity organic solvent has a relative dielectric constant of 10 or less at 25° C. and a kinetic viscosity of 10 mm at 37.8° C. 2 / s or more.
2. 2. The method according to claim 1, wherein the washing solvent is a mixed solvent of ethanol and water.
3. The method according to claim 2 , wherein the content of the ethanol in the washing solvent is in the range of more than 60% by mass and not more than 85% by mass.
4. 3. The method according to claim 1, wherein the gel particles washed with the washing solvent have a solvent absorption rate of the washing solvent represented by the following formula (1) of 25 or less. Solvent absorption rate = (M1-M2) / M2 (1) In formula (1), M1 represents the mass of the gel particles carrying a saturated amount of the washing solvent after the washing, and M2 represents the mass of the gel particles after drying after the washing.
5. 3. The method according to claim 1, wherein the low-polarity organic solvent is liquid paraffin or silicone oil.
6. The kinetic viscosity of the low polarity organic solvent at 37.8° C. is 10 mm 2 / s or more 100mm 2 The method according to claim 1 or 2, wherein the solubility is 1 / s or less.
7. The method according to claim 1 or 2, wherein the viscosity of the carboxyalkyl cellulose and / or salt thereof is 5 mPa·s or more and 100 mPa·s or less.
8. The method according to claim 1 or 2, wherein the mass ratio (X / Y) of the carboxyalkyl cellulose and / or its salt (X) to the crosslinking agent (Y) in the mixture is in the range of 10 / 2 to 10 / 5.
9. 3. The method according to claim 1, wherein the crosslinking agent is a compound having two or more epoxy groups in the molecule.
10. The method according to claim 1 or 2, wherein the granular carrier is used for carrying a drug.
11. A dry granular carrier produced by the method according to claim 1 or 2.
12. The granular carrier according to claim 11, which is used for carrying a drug.
13. A granular drug composition comprising the granular carrier described in claim 11 and a liquid composition supported on the granular carrier and containing at least one drug selected from drugs having aromatic, deodorizing, odor eliminating, insect repellent, insecticidal or antifungal properties.
14. The granular pharmaceutical composition according to claim 13, which is an air freshener composition or a deodorant composition.
15. An absorbent article comprising the granular carrier according to claim 11.
Citation Information
Patent Citations
Composite polymer presenting gel form by water absorption
JP2014227519A
Absorbent and manufacturing method thereof
JP2023176772A
Granular carrier, granular pharmaceutical composition and absorbent article containing the same, and method for producing the granular carrier
JP7792227B2
Process for producing crosslinked gel and its crosslinked gel
JP2008285611A
High water-absorbing polymer
JP2011140534A