Perovskite composite oxide powder
A perovskite-type composite oxide powder with controlled composition and manufacturing improves conductivity and reduces resistance in SOFC air electrodes, addressing the challenges of high conductivity and stability at reduced temperatures.
Patent Information
- Application Number
- JP2023054605
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing solid oxide fuel cell (SOFC) air electrode materials face challenges in achieving high conductivity and stability at reduced operating temperatures, with a need for improved conductivity and reduced resistance.
A perovskite-type composite oxide powder containing La, Sr, Ca, Co, Ni, Mn, and Fe, with specific BET surface area, residue ratio, and particle size distributions, is developed to enhance conductivity and reduce agglomeration, using a controlled manufacturing process involving wet methods and precise firing and pulverization techniques.
The composite oxide powder achieves higher conductivity and improved conductivity in fuel cells, reducing resistance and enhancing the performance of SOFC air electrodes.
Smart Images

Figure 2024142461000002 
Figure 2024142461000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite oxide powder having a perovskite structure, and more particularly to a composite oxide powder suitable for use as an air electrode material for solid oxide fuel cells (SOFCs: Solid Oxide Fuel Cells, hereinafter sometimes simply referred to as "SOFCs"). [Background technology]
[0002] Among various types of fuel cells, SOFCs have high power generation efficiency and can use a variety of fuels, and therefore are being developed as a next-generation power generation device with less environmental impact. A single SOFC cell has a structure in which a porous air electrode (cathode), a dense solid electrolyte containing an oxide ion conductor, and a porous fuel electrode (anode) are stacked in this order (see Figure 1). When an SOFC is in operation, an O2 (oxygen)-containing gas such as air is supplied to the air electrode, and a fuel gas such as H2 (hydrogen) is supplied to the fuel electrode. When a current is applied to the SOFC in this state, O2 is reduced at the air electrode to produce O 2- It becomes an anion (oxygen ion). And this O 2- The anions pass through the solid electrolyte to the anode, where they oxidize H2 and release electrons, thereby generating electrical energy (i.e. electricity).
[0003] The operating temperature of such SOFCs was previously around 800°C to 1000°C, but in recent years efforts have been made to lower the operating temperature of SOFCs. However, the minimum temperature of SOFCs in practical use remains high at 600°C or higher.
[0004] Due to this cell structure and high operating temperatures, the material for the air electrode of an SOFC is required to have the following basic properties: high oxygen ion conductivity, high electronic conductivity, thermal expansion equal to or similar to that of the electrolyte, high chemical stability, good compatibility with other constituent materials, a porous sintered body, and a certain level of strength.
[0005] As a material for the air electrode of such a solid oxide fuel cell, the applicant disclosed in Patent Document 1 a compound represented by the general formula ABO 3-δ (δ represents the amount of oxygen vacancy and is 0≦δ<1. The element contained in the A site is La, and the elements contained in the B site are Co and Ni) and a perovskite-type composite oxide powder with a crystallite diameter of 20 nm or more and 100 nm or less as determined by the Williamson-Hall method has been proposed (Patent Document 1).
[0006] In addition, in Patent Document 2, La is used as the material for the electrode layer and lead layer of the electrode of the gas sensor element. a M b Ni c O x A conductive oxide having a perovskite-type oxide crystal structure represented by a composition formula expressed as (M is at least one of Co and Fe, a+b+c=1, 1.25≦x≦1.75) has been proposed.
[0007] Furthermore, Patent Document 3 proposes a cathode raw material powder which is a perovskite composite oxide powder represented by the general formula ABO3, in which A consists of one or more elements selected from the group of La and rare earth elements, and one or more elements selected from the group of Sr, Ca and Ba, and B consists of one or more elements selected from the group of Mn, Co, Fe, Ni and Cu, and which has an average particle size of 1 μm or less and a width of the particle size distribution limited within a prescribed range. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] International Publication No. 2022 / 013903 [Patent Document 2] JP 2018-112490 A [Patent Document 3] JP 2006-32132 A Summary of the Invention [Problem to be solved by the invention]
[0009] The material used for the air electrode of a solid oxide fuel cell should have as low resistance and as high conductivity as possible, and in recent years, there has been a demand for further improvements in performance.
[0010] Therefore, an object of the present invention is to obtain higher electrical conductivity in a perovskite type composite oxide powder having a specific composition. [Means for solving the problem]
[0011] The perovskite complex oxide powder according to an embodiment of the present invention that achieves the above object is a perovskite complex oxide powder that contains La and further contains at least one element selected from the group consisting of Sr, Ca, Co, Ni, Mn, and Fe, and has a BET specific surface area of 6.0 m 2 / g or less, and the residue ratio measured by the following procedure is 5% or less. (Measurement of Residue Ratio) The upper part is fixed and the mass (referred to as Ma) of a 15 cm square nylon mesh bag (mesh opening 10 μm, opening rate 4%) folded into a bag shape is measured. Next, the mass (referred to as Mb) of the composite oxide powder placed inside the nylon mesh bag is measured. Hold the nylon mesh bag containing the composite oxide powder by the fixed part with your hand and immerse it in 300 mL of 500 ppm sodium hexametaphosphate aqueous solution (dissolved in ion-exchanged water, liquid temperature 20°C) for 2 minutes while shaking it up and down (amplitude 3 cm, 3 times per second). This measurement is considered as one set, and perform 10 sets of measurements while exchanging the sodium hexametaphosphate aqueous solution. The nylon mesh bag with the top fixed is then dried at 120°C for 5 minutes. After drying, the mass of the nylon mesh bag (referred to as Mc) is measured with the top fixed. The difference between Ma and Mc (Mc-Ma) is taken as the residual mass (Md) of the composite oxide powder in the nylon mesh bag, and the residual ratio (%) is calculated using the following formula: Residue ratio (%) = Md / Mb × 100
[0012] In the perovskite complex oxide powder of the above embodiment, the proportion of particles having a particle size of 100 nm or more, calculated by filtration through a 100 nm mesh membrane filter, is preferably 98% or more.
[0013] Furthermore, according to the present invention, there is provided an air electrode for a solid oxide fuel cell which is formed by containing any one of the perovskite-type composite oxide powders described above.
[0014] The present invention also provides a solid oxide fuel cell comprising a fuel electrode, a solid electrolyte, and an air electrode, the solid oxide fuel cell using the air electrode described above as the air electrode.
[0015] In this specification, the BET specific surface area is measured by the method described in the Examples section below. In addition, unless otherwise specified, the range "to" in this specification includes the values before and after the range as the lower and upper limits. Effect of the Invention
[0016] According to the present invention, it is possible to realize a perovskite complex oxide powder having a higher electrical conductivity. By using such a perovskite complex oxide powder, it is possible to realize a highly electrically conductive air electrode of a fuel cell and a fuel cell. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a solid oxide fuel cell. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The perovskite-type composite oxide powder according to the present invention (hereinafter, sometimes simply referred to as "composite oxide powder") is a perovskite-type composite oxide powder containing La (lanthanum) and further containing at least one element selected from the group consisting of Sr (strontium), Ca (calcium), Co (cobalt), Ni (nickel), Mn (manganese), and Fe (iron).
[0019] In other words, the composite oxide powder according to the present invention has the general formula ABO 3―x The A site contains La and may contain at least one of Sr and Ca, and the B site contains at least one element selected from the group consisting of Co, Ni, Mn, and Fe. x represents the amount of oxygen vacancy including 0, and the value of x is in the range of 0≦x<1.
[0020] Among these compositions, the general formula ABO 3―x In the formula, it is preferable that La and Sr are contained in the A site and Mn is contained in the B site. The amount of Sr contained in the A site and Mn contained in the B site can be adjusted as desired. The general formula is LaSr y Mn 1-y O 3―x In the formula, y is preferably 0.1≦y≦0.9, and more preferably 0.3≦y≦0.85. The value of x is in the range of 0≦x<1.
[0021] In another embodiment, the composite oxide powder according to the present invention is represented by the general formula ABO 3―x and La on the A site. 1-(a+b) Sr a Ca b and at least one element selected from the group consisting of Co, Ni, Mn, and Fe is contained in the B site. x indicates the amount of oxygen vacancy including 0, and the value of x is in the range of 0≦x<1. The range of a and b is 0 <a<1、0≦b<1である。
[0022] The composite oxide powder of the present embodiment has a perovskite-type structure crystalline phase, which is identified by the analysis software attached to the X-ray diffraction (XRD) device based on the X-ray diffraction pattern obtained by X-ray diffraction (XRD) measurement using a Cu tube. The crystalline phase is preferably a single phase of the perovskite-type structure. In addition, the ratio of the peak height due to the components not incorporated in the perovskite-type structure to the peak height of the maximum diffraction line of the perovskite-type composite oxide powder (peak height of the components not incorporated in the perovskite-type structure / peak height of the maximum diffraction line of the perovskite-type composite oxide powder) is preferably 10% or less, more preferably 5% or less, and even more preferably 1% or less.
[0023] One of the major features of the composite oxide powder of the present invention is that the BET specific surface area measured by the BET single point method is 6.0 m 2 The BET specific surface area of the composite oxide powder is 6.0 m 2 When the composite oxide powder has a BET specific surface area of 4.5 m / g or less, the increase in viscosity is suppressed when the composite oxide powder is made into a slurry or paint to be used as an air electrode material, and the applicability of the slurry or paint is improved, which contributes to electrical conductivity. 2 / g or less. On the other hand, the BET specific surface area of the composite oxide powder is 0.1 m 2 / g or more, and 1.0m 2 / g or more, and 2.0m 2 It is more preferable that the BET specific surface area of the composite oxide powder is 0.1 m / g or more. 2 When the composite oxide powder has a molecular weight of 1000 or more, when the composite oxide powder is used to form an air electrode of a fuel cell, an appropriate number of pores can be formed on the surface of the air electrode, and the contact area with gas can be increased, thereby improving the exchange efficiency when constructing the fuel cell.
[0024] Another major feature of the complex oxide powder according to the present invention is that the residue ratio measured by the following procedure is 5% or less. With the aim of increasing the conductivity of the air electrode of a fuel cell, the inventors conducted various studies and discovered a new finding that the conductivity of the air electrode improves when the content ratio of agglomerated powder in the complex oxide powder, which is the material of the air electrode, is reduced. The inventors then decided to use the residue ratio measured by the following procedure as an index of the content ratio of agglomerated powder in the complex oxide powder. It is determined that the lower the residue ratio of the complex oxide powder, the less agglomerated powder there is in the complex oxide powder.
[0025] The residue ratio of the complex oxide powder according to the present invention is a ratio calculated from the mass change when the complex oxide placed in a nylon mesh bag is repeatedly immersed in a specified aqueous solution while being shaken a specified number of times. In detail, the mass (hereinafter referred to as Ma) of a 15 cm square nylon mesh bag (mesh opening 10 μm, opening ratio 4%) folded into a bag shape with the upper part fixed by clipping or the like is measured. Next, the mass (hereinafter referred to as Mb) of the complex oxide powder placed inside the nylon mesh bag is measured. In this example, the mass of the complex oxide powder placed is 0.5 g. Next, 0.5 g of the complex oxide powder is placed inside the nylon mesh bag, and the upper part is fixed by clipping again. The fixed part (clipped part) of the nylon mesh bag containing the composite oxide powder was held by hand and immersed in 300 mL of 500 ppm sodium hexametaphosphate aqueous solution (dissolved in ion-exchanged water, liquid temperature 20°C) for 2 minutes while shaking up and down (amplitude width 3 cm, 3 reciprocations per second). The immersion work of the nylon mesh bag containing the composite oxide powder in the sodium hexametaphosphate aqueous solution for 2 minutes while shaking was counted as one set, and 10 sets were performed while changing the sodium hexametaphosphate aqueous solution for each set. Then, with the top of the nylon mesh bag fixed with a clip, the nylon mesh bag is dried for 5 minutes at 120° C. After drying, the mass (referred to as Mc) of the nylon mesh bag is measured with the top of the bag fixed with a clip. The difference between Ma and Mc (Mc-Ma) is taken as the residual mass (Md) of the composite oxide powder in the nylon mesh bag, and the residual ratio (%) is calculated using the following formula. Residue ratio (%) = Md / Mb × 100
[0026] In the present invention, the residual ratio of the composite oxide powder is set to 5% or less. If the residual ratio is more than 5%, that is, if the content of agglomerated powder in the composite oxide powder is high, it is not possible to improve the conductivity of the air electrode of the fuel cell produced using the composite oxide powder. The preferred upper limit of the residual ratio is 2.5%.
[0027] In addition, the composite oxide powder according to this embodiment preferably has a ratio of particles having a size of 100 nm or more, calculated by filtration through a membrane filter with a 100 nm mesh, of 98% or more. The ratio of particles having a size of 100 nm or more is measured by the following procedure. Measure the mass (W1) of the composite oxide powder. Also, measure the mass (W2) of the tray with the membrane filter placed in it before use. The sum of mass (W1) and mass (W2) is the mass before filtration (Wb). The mass of the composite oxide powder is measured and dispersed in 100 g of water to prepare a slurry. The slurry is filtered while being suctioned through a filter equipped with the membrane filter. After filtration, remove the membrane filter from the filter and place it in a tray and dry it at 100℃ for 2 hours. After drying, measure the mass of the tray with the membrane filter still placed on it (mass after filtration (Wa)). The difference between Wa and Wb (Wb-Wa) is taken as the mass of particles of 100 nm or more, and the percentage (%) of particles of 100 nm or more in the composite oxide powder is calculated using the following formula. Ratio of particles of 100 nm or more in composite oxide powder = (Wb-Wa) / Wb x 100
[0028] On the other hand, the particle size D at the cumulative 50% calculated on a volume basis using a particle size distribution measuring device using the laser diffraction / scattering method of the composite oxide powder is 50It is preferable that the distribution be in the range of 0.4 μm or more and 2.0 μm or less, and more preferably in the range of 0.6 μm or more and 1.5 μm or less.
[0029] (Manufacturing method) The method for producing the composite oxide powder according to the present invention is not particularly limited, but an example of the production method will be described below. The method for producing the composite oxide powder includes a wet method in which a precursor is formed in a liquid and then heat-treated to form a composite oxide, and a dry method in which the raw materials are weighed, mixed as is, and fired to form a composite oxide, but it is preferable to produce the composite oxide by the wet method in order to achieve the object of the present invention. Below, an example of a method for producing a composite oxide powder by the wet method is given, but it is possible to appropriately adjust the method as long as it does not deviate from the spirit of the method exemplified here.
[0030] (Preparation of precursor) As a method for producing the composite oxide powder according to the present embodiment, a method can be adopted in which a raw material solution in which a raw material containing an element such as La is dissolved in water or acid is added to an alkaline solution such as ammonia water in advance to carry out a neutralization reaction, thereby producing a slurry containing a neutralized product of the composite oxide. It is preferable that the raw material is one that does not remain in the form of impurities at the firing stage, but escapes as a gas.
[0031] When generating the neutralized product, it is preferable to include carbon dioxide. By doing so, when the neutralized product (sometimes referred to as "precursor" in this specification) is separated and collected, it is prevented from reacting with carbon dioxide in the air to locally carbonatize and crystallize. As a result, it is preferable because it prevents the precipitation of impurity phases when perovskite is formed in the subsequent process. Carbon dioxide may be added to the system as a carbonate salt. The neutralized product obtained in this way is an amorphous nanoparticle in which each element is uniformly mixed, so that the diffusion of elements during firing is facilitated, and the effect of promoting single-phase formation and crystallite growth is obtained.
[0032] The temperature at which the neutralization product is formed is preferably 60° C. or less, more preferably 50° C. or less, and even more preferably 40° C. or less. By setting the temperature in this manner, substances that are likely to become gas, such as carbon dioxide and ammonia, contained in the liquid are dispersed from the liquid, so that the neutralization product can be suitably obtained. The neutralization product of the complex oxide obtained in this embodiment is an amorphous nanoparticle in which each element is uniformly mixed, so that the diffusion of elements during firing is facilitated, and the effect of promoting the formation of a single phase and the growth of crystallites is obtained.
[0033] (filtration and drying) The obtained neutralized product is separated from the slurry as necessary, washed, and then dried to obtain a precursor by drying the neutralized product. As a method for separating from the slurry, for example, any of filtration separation, separation and recovery by a filter press, and direct drying by spray drying or freeze drying can be adopted. For filtration separation and filter press, any known method can be adopted. In addition, when directly drying, the pH may be adjusted to adjust the obtained precursor to a desired size. When adjusting the pH, in order to avoid impurities such as alkali metals and alkaline earth metals remaining in the dried aggregates, it is preferable to adjust with ammonia, which is less likely to volatilize and remain during drying, rather than using an adjuster containing an alkali metal such as sodium hydroxide or potassium hydroxide. The drying temperature when drying the neutralized product is preferably 150°C or higher and 350°C or lower, more preferably 200°C or higher and 300°C or lower. Drying at a temperature extremely outside this drying temperature range is not preferable because there is a risk that a part of it will become a perovskite, or that it will not be completely dried and moisture will remain in the precursor.
[0034] (Precursor grinding) The dried precursor can be pulverized to a fine particle size by pulverization. The pulverization may be performed after the firing process described below. In the case where the drying process is performed using a spray dryer, pulverization may not be required. Examples of the apparatus used for pulverization include a mortar, a sample mill, a Henschel mixer, a hammer mill, a jet mill, a pulverizer, an impeller mill, and an impact mill when dry pulverization is used. For example, the rotation speed of an impact mill is preferably in the range of 9000 rpm to 16000 rpm. The rotation speed and pulverization time of the impact mill are related to the firing temperature and firing time in the firing process, and it is desirable to increase the rotation speed of the impact mill and increase the pulverization time as the firing temperature and firing time are increased.
[0035] (Firing) The prepared precursor powder is calcined in a calcination furnace to obtain a composite oxide. The calcination furnace may be a conventionally known furnace such as an electric or gas-powered shuttle kiln, roller hearth kiln, or rotary kiln. The calcination temperature is preferably higher than 1000°C in order to increase the crystallite size of the particles constituting the perovskite-type composite oxide powder. A calcination temperature of 1500°C or lower is also preferred because it facilitates deagglomeration of the calcined product after calcination.
[0036] The temperature rise rate during firing is 10°C / min or less, and the firing atmosphere may be air or nitrogen containing 1 ppm to 20% oxygen. By slowing the firing, the crystallite size can be adjusted. The firing furnace or firing vessel is an open system, and the temperature is raised while removing gas components generated from the raw material salt of the component raw materials. In the present invention, an open system refers to a reaction system in which the firing furnace or firing vessel is not sealed and the gas atmosphere can flow in and out.
[0037] (Crushing) Next, the granulated product (calcined product) after calcination is pulverized. The pulverization may be either wet pulverization or dry pulverization, or both may be used. When dry pulverization is performed, any of the devices exemplified when pulverizing the precursor may be used. When wet pulverization is performed, a wet ball mill, a sand grinder, an attritor, a pearl mill, an ultrasonic homogenizer, a pressure homogenizer, an ultimaizer, etc. may be used. By performing wet pulverization using these, a perovskite-type composite oxide that meets the above-mentioned conditions can be constructed. In particular, it is preferable to use a pearl mill. When selecting a pearl mill for wet pulverization, any of the existing wet pulverizers such as the known vertical flow tube bead mill, horizontal flow tube bead mill, and strong pulverization type rush flow viscomill can be used, but preferably a horizontal flow tube bead mill is used. The horizontal flow tube bead mill is preferable because it is more uniformly pulverized while the material is retained in the vessel than the vertical flow tube bead mill, and more uniform pulverization is possible at the same flow rate. In addition, the horizontal flow tube type bead mill is economically preferable because it has a larger processing flow rate than the strong grinding type rush flow type viscomill. As the grinding media, balls made of hard raw materials such as glass, ceramic, alumina, zirconia, etc. are preferably used. The particle size of the balls to obtain a perovskite type composite oxide having a desired particle size is preferably about 0.1 mm to 5.0 mm, more preferably 0.5 mm to 2.0 mm. As the dispersion medium used in the case of wet grinding, water or an organic solvent such as ethanol, which has a relatively low boiling point and is easily removed, can be used. From the viewpoint of production costs, it is preferable to use water as the dispersion medium.
[0038] The pulverized material after wet pulverization is dried to obtain a pulverized and dried material. The preferred drying method is spray drying. A spray dryer is preferably used as the spray drying device. Among them, a disk-type spray dryer is more preferred from the viewpoint of drying efficiency and mass productivity. The drying temperature is preferably 60°C or higher and 350°C or lower, preferably 75°C or higher and 325°C or lower, and more preferably 100°C or higher and 300°C or lower. If the powder is dried at a temperature far outside this range, there is a risk that some of the powder will turn into perovskite, or the powder may not be completely dried and moisture may remain in the powder.
[0039] The crushed product after dry crushing or the crushed and dried product after wet crushing is subjected to a crushing process. The term "crushing" refers to breaking up the aggregated powder. The crushing device can be the same as that used for dry crushing, and the dried product can be crushed without being crushed by making the processing conditions such as the rotation speed looser than those for crushing, i.e., by making the rotation speed lower than that for crushing. The crushing device is preferably a device capable of mechanically crushing, such as a sample mill, a Henschel mixer, a hammer mill, a jet mill, a pulverizer, an impeller mill, or an impact mill. By carrying out such a crushing process, the content of aggregates in the composite oxide powder is further reduced. For example, when a sample mill is used as the crushing device, the rotation speed is preferably set to a range of 1000 to 4000 rpm.
[0040] (Sieving) The crushed product after wet crushing is dried and then sieved to remove coarse particles (agglomerated powder) to obtain a composite oxide powder. The mesh size of the sieve used for sieving may be appropriately determined taking into consideration the average primary particle size of the composite oxide powder (after ultrasonic dispersion), etc. When the average primary particle size of the composite oxide powder is about several tens of μm, the mesh size of the sieve is preferably 250 μm or less (60 mesh or more), and more preferably 150 μm or less (100 mesh or more). The particle size distribution of the fired product (perovskite-type composite oxide powder) after sieving is determined based on the cumulative 50% particle size D calculated from the volume-based particle size distribution using a Microtrack particle size distribution measuring device before ultrasonic dispersion. 50BThe cumulative 50% particle diameter D calculated from the volume-based particle size distribution by a Microtrac particle size distribution measuring device after ultrasonic dispersion is preferably 0.5 μm or more and 3.0 μm or less. 50A It is preferable that the thickness is 0.5 μm or more and 3.0 μm or less.
[0041] (Solid oxide fuel cell, SOFC) A solid oxide fuel cell will now be described. Fig. 1 is a cross-sectional view showing a schematic configuration of an example of a solid oxide fuel cell. The fuel cell has a laminated structure including a thin plate or sheet-like fuel electrode 1 serving as a support, a solid electrolyte membrane 2 formed on the surface of the fuel electrode 1, and a thin plate or sheet-like air electrode 3 formed on the surface of the solid electrolyte membrane 2.
[0042] When a fuel gas (typically hydrogen (H2), but can also be a hydrocarbon (methane (CH4))) is supplied to the fuel electrode 1, a gas (air) containing oxygen (O2) is passed through the air electrode 3, and a current is applied to the fuel cell, the oxygen in the air becomes oxide ions at the air electrode 3. The oxide ions are supplied from the air electrode 3 through the solid electrolyte 2 to the fuel electrode 1. The oxide ions then react with the fuel gas at the fuel electrode 1 to produce water (H2O), which releases electrons and generates electricity.
[0043] In SOFCs, although it depends on the configuration and manufacturing process of the fuel cell to be applied, a laminate including an anode, a solid electrolyte membrane, etc. is prepared in advance, and a layer containing the cathode material is formed on the laminate by a printing method, deposition, etc., and then sintered to form the cathode, thereby producing a fuel cell.
[0044] The thickness of the air electrode is not particularly limited and may be appropriately determined depending on the cell structure, etc., but is preferably, for example, 20 μm to 50 μm. The material for the air electrode may be only the composite oxide powder of this embodiment, or may be a mixture of the composite oxide powder of this embodiment and a perovskite composite oxide powder having a different composition or one or more perovskite composite oxide powders having different particle sizes.
[0045] As the solid electrolyte layer, the electrolyte materials used in the air electrode material can be used, for example, rare earth element-doped ceria-based solid oxide electrolytes and rare earth element-doped zirconia-based solid oxide electrolytes.
[0046] The thickness of the solid electrolyte layer is set by balancing between being thick enough to maintain the denseness of the solid electrolyte layer and being thin enough to provide oxygen ion or hydrogen ion conductivity suitable for a fuel cell, and is preferably 0.1 μm or more and 50 μm or less, and more preferably 1 μm or more and 20 μm or less.
[0047] The fuel electrode may be made of any material that has a porous structure and is capable of contacting the supplied fuel gas, and may be made of any material that has been used in solid oxide fuel cells. For example, metal oxides made of one or more of metals and / or elements such as nickel (Ni), copper (Cu), gold (Au), platinum (Pt), palladium (Pd), ruthenium (Ru) and other platinum group elements, cobalt (Co), lanthanum (La), strontium (Sr), titanium (Ti), etc. may be used alone or in combination.
[0048] The thickness of the fuel electrode is preferably 20 μm or more and 1 mm or less, and more preferably 20 μm or more and 250 μm or less, in view of durability, thermal expansion coefficient, and the like.
[0049] The structure of the SOFC may be a conventionally known flat, polygonal, or cylindrical (Tubular) type, or a flat tubular type (Flat Tubular) type in which the peripheral side of a cylinder is vertically crushed, and the shape and size are not particularly limited. In addition to the anode-supported cell (ASC), the flat SOFC may be, for example, an electrolyte-supported cell (ESC) with a thick electrolyte, or a cathode-supported cell (CSC) with a thick cathode. In addition, a metal-supported cell (MSC) in which a porous metal sheet is placed under the anode may also be used. EXAMPLES
[0050] Example 1 (1) Precursor preparation A solution of lanthanum oxide dissolved in nitric acid (La concentration: 15.04 mass%, NO3 - A mixed solution of nitrates obtained by mixing 290 g of nitrate solution (270 g / L) with 17.1 g of strontium nitrate (Sr(NO3)2) powder and 144.3 g of manganese nitrate (Mn(NO3)2) aqueous solution with a manganese metallic concentration of 50.4 mass% was dissolved in 549.1 g of ion-exchanged water to prepare a mixed solution.
[0051] Furthermore, 2670 g of ion-exchanged water and 330 g of ammonium carbonate were placed in a reaction tank, and the water temperature was adjusted to 25° C. while stirring. The mixed solution was gradually added to this ammonium carbonate solution to carry out a neutralization reaction at a water temperature of 25° C. After precipitating a neutralized product of perovskite-type composite oxide, the neutralized product was aged for 30 minutes to complete the reaction.
[0052] (2) Filtration and drying The neutralized product was filtered, washed with water, and then molded into elongated cylindrical pellets with a diameter of 5 mm. The pellets were then immediately dried at 250°C for 2 hours while blowing air through them, to obtain a black precursor.
[0053] (3) Firing 50 g of the obtained precursor was placed in a round crucible (a container with a diameter of 90 mm and a height of 75 mm) and set in an electric muffle furnace (KM-160 manufactured by Toyo Seisakusho Co., Ltd.). The temperature was increased from room temperature to 800°C at a rate of 3.1°C / min, and then from 800°C to 1100°C at a rate of 2.6°C / min. The material was held at 1100°C (firing temperature) for 2 hours for firing, and then naturally cooled to room temperature.
[0054] (4) Dry grinding The obtained fired product was ground twice for 30 seconds at a rotation speed of 16,000 rpm using a sample mill grinding device (manufactured by Kyoritsu Riko Co., Ltd., model name: SK-M10) with a charge of 20 g / batch to obtain a composite oxide powder.
[0055] (5) Wet grinding 50 g of the obtained composite oxide powder was placed in the pot of an Imex four-cylinder sand grinder (TSG-4U type, volume capacity: 350 mL) together with 200 g of ZrO2 beads with a diameter of 1.0 mm and 93 g of ion-exchanged water. Then, while cooling the pot with cooling water at 20°C, it was rotated at a rotation speed of 1500 rpm for 40 minutes to perform wet grinding. After that, the slurry containing the crushed composite oxide as the solid content was granulated and dried at a drying temperature of 200°C using a spray dryer (Okawahara Kakoki Co., Ltd., model: FL-12) while spraying with an atomizer rotation speed of 20000 rpm and a slurry supply rate of 160 g / min.
[0056] (6) Crushing The wet-grinding process was repeated several times to obtain 200 g of dry powder. The obtained dry powder was subjected to a crushing treatment at a rotation speed of 3600 rpm using a sample mill crushing device (Dalton, model: KIIWR-1, screen: dot diameter 1 mm).
[0057] (7) Screening The obtained dry powder was sieved using a vibrating sieve (Verder Scientific KK, model number: AS200) with a mesh size of 500 μm (30 mesh) to obtain the composite oxide powder of Example 1. The physical properties of the obtained composite oxide powder were measured by the following measuring methods. The measurement results are shown in Table 1.
[0058] Comparative Example 1 A composite oxide powder according to Comparative Example 1 was obtained in the same manner as in Example 1, except that the crushing step after the wet grinding was not carried out. The physical properties of the obtained composite oxide powder were measured by the following measuring methods. The measurement results are shown in Table 1.
[0059] (composition analysis) The composition of the composite oxide powder was analyzed using an inductively coupled plasma (ICP) emission spectrometer (Agilent Technologies 720ES).
[0060] (BET specific surface area) The BET specific surface area of the obtained composite oxide powder was determined by the BET single point method using a BET specific surface area measuring device (4Sorb US manufactured by Yuasa Ionics Corporation).
[0061] (Conductivity measurement) 2 g of the composite oxide powder was placed in a unit with a radius of 10 mm and compressed at a pressure of 20 kN (Newtons) using a powder resistivity measurement system (MCP-PD51, manufactured by Mitsubishi Chemical Analytech Co., Ltd.), and the electrical conductivity was measured by the four-point probe method using a resistivity meter (MCP-T610, manufactured by Mitsubishi Chemical Analytech Co., Ltd.).
[0062] (X-ray diffraction measurement) XRD measurements of the obtained composite oxide powder were performed using an UltimaIV manufactured by Rigaku Corporation. The measurement conditions were as follows: a Cu tube, a tube voltage of 40 kV, a tube current of 40 mA, a divergence slit of 1 / 2°, a scattering slit of 8 mm, a receiving slit set to open, a step width of 0.02°, and a measurement time of 4° / min. Based on the obtained X-ray diffraction pattern, the crystal phase of the obtained composite oxide powder was identified using the analysis software (Rigaku Corporation's integrated powder X-ray analysis software PDXL2 ICDS (Inorganic Crystal Structure Database)) attached to the above X-ray diffraction (XRD) device.
[0063] (Measurement of Residue Ratio) The mass (referred to as Ma) of a 15 cm square nylon mesh bag (mesh opening 10 μm, opening ratio 4%, manufactured by Kureha Co., Ltd., model number: PA8) folded into a bag shape with the top clipped was measured. Next, 0.5 g of the composite oxide powder was placed inside the nylon mesh bag, and the top was clipped again. The mass of the composite oxide powder placed in the nylon mesh bag was designated as Mb. The nylon mesh bag containing the composite oxide powder was held by the clip with a hand and immersed in 300 mL of a 500 ppm aqueous solution of sodium hexametaphosphate (dissolved in ion-exchanged water, liquid temperature 20°C) for 2 minutes while shaking up and down (amplitude 3 cm, 3 back and forth per second). The above measurement procedure was counted as one set, and 10 sets of measurements were performed while changing the sodium hexametaphosphate aqueous solution. Thereafter, the nylon mesh bag in the clipped state was dried for 5 minutes at 120° C. After drying, the mass (referred to as Mc) of the nylon mesh bag in the clipped state was measured. The difference between Ma and Mc (Mc-Ma) was taken as the residual mass (Md) of the composite oxide powder in the nylon mesh bag, and the residual ratio (%) was calculated using the following formula. Residue ratio (%) = Md / Mb × 100
[0064] [Table 1]
[0065] From the results of the composition analysis of the composite oxide powder by an ICP emission spectrometer, the composite oxide powders of Example 1 and Comparative Example 1 were found to have the composition formula La 0.8 Sr 0.2 Mn 1.0 O3, and X-ray diffraction measurements confirmed that it was a single-phase perovskite-type composite oxide powder.
[0066] The composite oxide powder of Example 1, in which the residue ratio was 2.0%, had a conductivity of 9610 μS / cm, whereas the composite oxide powder of Comparative Example 1, in which the residue ratio was 5.9%, which was higher than the range specified in the present invention, had a conductivity of 7074 μS / cm, which was significantly lower than that of the composite oxide powder of Example 1. [Industrial Applicability]
[0067] According to the present invention, it is possible to realize a perovskite complex oxide powder having higher electrical conductivity. By using such a perovskite complex oxide powder, it is possible to realize a highly electrically conductive air electrode of a fuel cell and a fuel cell. [Explanation of symbols]
[0068] 1 Fuel electrode 2 Solid electrolyte membrane 3 Air electrode
Claims
1. A perovskite-type composite oxide powder containing La and further containing at least one element selected from the group consisting of Sr, Ca, Co, Ni, Mn, and Fe, BET specific surface area is 6.0m 2 / g or less, The residue rate measured by the following procedure is 5% or less.
1. A perovskite-type composite oxide powder comprising: (Measurement of Residue Ratio) The upper part is fixed and the mass (referred to as Ma) of a 15 cm square nylon mesh bag (mesh opening: 10 μm, opening ratio: 4%) folded into a bag shape is measured. Next, the mass (referred to as Mb) of the composite oxide powder placed inside the nylon mesh bag is measured. The nylon mesh bag containing the composite oxide powder was held by the fixed part with a hand and immersed in 300 mL of a 500 ppm aqueous solution of sodium hexametaphosphate (dissolved in ion-exchanged water, liquid temperature 20° C.) for 2 minutes while shaking up and down (amplitude 3 cm, 3 reciprocations per second). This measurement operation was counted as one set, and 10 sets of measurements were performed while exchanging the aqueous solution of sodium hexametaphosphate. The nylon mesh bag with its upper part fixed is then dried at 120° C. for 5 minutes. After drying, the mass (referred to as Mc) of the nylon mesh bag with its upper part fixed is measured. The difference between Ma and Mc (Mc-Ma) is taken as the residual mass (Md) of the composite oxide powder in the nylon mesh bag, and the residual ratio (%) is calculated using the following formula: Residue ratio (%) = Md / Mb x 100
2. 2. The perovskite complex oxide powder according to claim 1, wherein the proportion of particles having a particle size of 100 nm or more calculated by filtration through a 100 nm mesh membrane filter is 98% or more.
3. 3. An air electrode for a solid oxide fuel cell, comprising the perovskite complex oxide powder according to claim 1 or 2.
4. A solid oxide fuel cell comprising a fuel electrode, a solid electrolyte, and an air electrode, A solid oxide fuel cell using the air electrode according to claim 3 as the air electrode.
Citation Information
Patent Citations
Method for manufacturing ceramics
JP2003095749A
Air electrode material powder of solid oxide fuel cell, air electrode and solid oxide fuel cell
JP2006032132A
Aeroelectrode materials, interconnector materials, and solid oxide fuel cell cells
JP5140787B1
Perovskite-type composite oxide powder
WO2022013903A1
Gas sensor element and gas sensor
JP2018112490A