The polyester film addresses color unevenness issues in screen display devices by controlling transmittance and phase difference, ensuring high-quality image capture and sensor performance without a depolarizing member.

JP2024142556APending Publication Date: 2024-10-11TORAY INDUSTRIES INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023054733
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Plastic films used as back plates in screen display devices cause rainbow-like color unevenness in images captured by cameras installed on the image display side, affecting image quality and other sensors like fingerprint authentication and light sensors.

Method used

A polyester film for screen display devices is developed with specific optical properties, including controlled differences in transmittance and phase difference between S and P waves, and a laminated structure to minimize color unevenness without using a depolarizing member.

Benefits of technology

The polyester film effectively suppresses color unevenness in images and enhances the quality of information captured by cameras and other sensors, maintaining high transmittance and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000028_0000
    Figure 00000028_0000
  • Figure 00000028_0001
    Figure 00000028_0001
  • Figure 00000028_0002
    Figure 00000028_0002
Patent Text Reader

Abstract

To provide a polyester film for screen display apparatuses which can suppress the occurrence of color haze in an image viewed with naked eyes or observed from an imaging apparatus in a screen display apparatus, and a screen display apparatus using the polyester film for screen display apparatus, and a device having the screen display apparatus.SOLUTION: A polyester film for screen display apparatus that satisfies a relationship of formulas (1) to (3) below, when it is assumed that a difference in average transmittance in wavelengths of 400 nm to 800 nm of S and P waves at an incidence angle 60° is T60 [%] with a vertical axis taken as reference 0°, a phase difference value determined by entering a beam in a wavelength of 590 nm at an incidence angle 50°with the vertical axis taken as reference 0°along a plane including a fast axis of the film and a vertical axis with respect to the film surface is R50 [nm], and a value of ΔT60 and R50 multiplied together and divided by 100 is a parameter X, the following formulae are satisfied. Formula (1): X≤700; formula (2): 5.0≤ΔT60≤30; and formula (3): 100≤R50≤5000, where X=ΔT60 / 100×R50.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyester film for use in a screen display device, a screen display device using said film, and a device having a screen display device. [Background technology]

[0002] 2. Description of the Related Art With the development of display terminals, there is a demand for image display devices to be small, thin, lightweight, and the like.

[0003] Electroluminescent display devices, typified by organic light-emitting display devices, are self-emitting display devices that, unlike liquid crystal display devices, do not require a separate light source, are easy to make thin and lightweight, and are also excellent in color realization, response speed, viewing angle, and contrast ratio, and are therefore used in display devices.

[0004] On the other hand, as display devices become smaller, there is a demand for display devices with larger screens (wider display areas), and there is also a demand to reduce the area of ​​display devices other than the display area, so full-screen display on display terminals is attracting attention.

[0005] On the other hand, cameras are often installed in smartphones and tablet devices to meet the needs of taking photos to record them, share them with friends, etc. In such devices, cameras are sometimes installed not only on the back side but also on the image display side.

[0006] In most cases where a camera is placed on the image display surface side, a slot or aperture method is used. That is, a hole or slot is provided on the image display surface side to allow light from the outside to enter the camera lens. When taking a picture, light from the outside passes through the slot or aperture and enters the camera placed below the image display surface. Since the area where such a slot or aperture exists is a non-display area, development of an image display device without a slot or aperture is underway (for example, Patent Document 1).

[0007] In addition, the realization of large-screen display and miniaturization and weight reduction of terminals are being considered by reducing the bezel area corresponding to the non-display area that is the outer periphery of the display area, and the development of a foldable display device that is configured so that multiple image display devices can be opened and closed in a folding manner. In these developments, a thin and flexible image display device that can maintain display performance even when warped has been proposed, but such an image display device is too thin, so it may not be restored when folded or the fold may become fixed. Therefore, a backplate is placed under the flexible substrate to support it and maintain the curvature when folded within an appropriate range. As such a backplate, those made of metal such as stainless steel and those made of plastic such as polymethyl methacrylate, polycarbonate, polyvinyl alcohol, and polyethylene terephthalate are known (for example, Patent Document 2). In addition, it is known that color unevenness or rainbow unevenness occurs in plastic films when combined with specific members (polarizing plates, etc.), and various measures have been taken (for example, Patent Documents 3 to 5). [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Special Publication No. 2021-511649 [Patent Document 2] JP 2021-110936 A [Patent Document 3] JP 2022-133016 A [Patent Document 4] JP 2010-204630 A [Patent Document 5] Patent No. 6617561 Summary of the Invention [Problem to be solved by the invention]

[0009] It has been revealed that when a specific plastic film is used as a back plate film, a problem occurs in that an image captured by a camera installed on the image display surface side without providing a slot or an aperture has a rainbow-like color unevenness. The occurrence of such color unevenness leads to a decrease in image quality, and also causes problems such as a decrease in the quality of the information obtained when other imaging elements such as a fingerprint authentication sensor, a light sensor, or a distance sensor are used instead of a camera. To improve such color unevenness, a depolarizing member is inserted between the camera and the plastic film as in the technology of Patent Document 3, but the transmittance decreases, causing problems such as a decrease in the quality of the information obtained. In addition, the technology of Patent Document 4, which aims to eliminate color unevenness by setting the reflectance at Brewster's angle within a specific range and reducing the reflectance difference between the S wave and P wave, which are the polarized components of light, and the technology of Patent Document 5, which reduces the film phase difference, do not sufficiently eliminate the color unevenness at the edge of the captured image, and there is room for improvement in terms of color unevenness.

[0010] Therefore, the object of the present invention is to provide a film for screen display devices that does not use a depolarizing member and yet can fully eliminate the above-mentioned color unevenness, and to provide a film for use in screen display devices in which no color unevenness is observed even at the very edge of the captured image. [Means for solving the problem]

[0011] In order to solve the above problems, a preferred embodiment of the present invention is as follows. [1] A polyester film for screen display devices that satisfies the relationships of the following formulas (1) to (3), where ΔT60 [%] is the difference in average transmittance between S waves and P waves at wavelengths of 400 nm to 800 nm at an incident angle of 60° with the vertical axis as the reference 0°, R50 [nm] is the phase difference value obtained by irradiating a light beam with a wavelength of 590 nm at an incident angle of 50° with the vertical axis as the reference 0° along a plane including the fast axis of the film and the axis perpendicular to the film surface, and X is the parameter obtained by multiplying ΔT60 and R50 and dividing the result by 100. X≦700 Formula (1) 5.0≦ΔT60≦30 Formula (2) 100≦R50≦5000 Formula (3) where X = ΔT60 / 100 × R50. [2] The polyester film for screen display devices according to [1], in which the difference between the maximum and minimum chromaticity a* and b* values ​​at a viewing angle of 50° and an azimuth angle of 0° to 360° is each 15 or less, as measured from the side of the polyester film for screen display devices using a viewing angle characteristic measuring and evaluation device (EZcontrast X88RC, manufactured by ELDIM). [3] The polyester film for a screen display device according to [1] or [2], which has polyethylene terephthalate as a main component. [4] The polyester film for a screen display device according to any one of [1] to [3], wherein ΔHg / ΔCp, calculated by dividing the endothermic peak ΔHg [J / g] observed in an irreversible curve of a temperature modulated DSC (30 to 150°C) by the baseline shift ΔCp [J / (g°C)] observed in a reversible curve, is 1.0 or more. [5] The polyester film for a screen display device according to any one of [1] to [4], which is used in an image display device having a polarizing plate, a light-emitting element array for image display, a polyester film for a screen display device, and an imaging element mounted in this order, as viewed from a viewer. [6] The polyester film for a screen display device according to [5], wherein the light-receiving angle range of the imaging element is 60° or more and 140° or less. [7] The polyester film for a screen display device according to any one of [1] to [6], in which two different types of thermoplastic resins are alternately laminated in five or more layers. [8] The polyester film for a screen display device according to any one of [1] to [7], wherein the average transmittance of S waves and P waves at wavelengths of 400 nm to 800 nm at an incident angle of 60° with the vertical axis as the reference 0° is 70% or more for both S waves and P waves. [9] The polyester film for a screen display device according to any one of [1] to [8], which has a layer including an antireflection layer on at least one surface thereof.

[10] The polyester film for a screen display device according to any one of [1] to [9], wherein n / n' is 1.08 or more, where n is an average value of the refractive index in the longitudinal direction and the width direction of the outermost layer of the base film, and n' is a refractive index of a low refractive index layer formed on the surface layer of the base film.

[11] The polyester film for a screen display device according to any one of [1] to

[10] , comprising 10 mol % or more of naphthalene dicarboxylic acid, polyetherimide, a fluorene derivative, paraxylene glycol, bisphenol A, isosorbide, cyclohexane dicarboxylic acid, or cyclohexane dimethanol.

[12] A screen display device comprising the polyester film for a screen display device according to any one of [1] to

[11] .

[13] A foldable display comprising the polyester film for a screen display device according to any one of [1] to

[11] .

[14] A device having, as one of its components, an image display device equipped with the polyester film for a screen display device according to any one of [1] to

[11] . Effect of the Invention

[0012] According to the present invention, it is possible to provide a polyester film for a screen display device that is capable of suppressing the occurrence of color unevenness in an image viewed with the naked eye or observed through an imaging device in a screen display device, as well as a screen display device using the polyester film for a screen display device and a device having the screen display device. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic front view of an example of an image display device of the present invention. [Diagram 2] Reference diagram for R50 measurement test. [Diagram 3] FIG. 2 is a diagram for explaining the configuration of an apparatus used in a visibility test. [Figure 4] Reference diagram for recovery angle measurement test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The polyester film for a screen display device according to the present invention will be described in detail below together with embodiments.

[0015] The screen display device in the present invention refers to devices in general that display images, such as liquid crystal display devices, organic electroluminescence display devices, inorganic electroluminescence display devices, μLED display devices, etc. The polyester film for screen display devices of the present invention can be suitably used for protective films, touch sensor substrate films, polarizer protective films, back plates, etc., used in these screen display devices. Among screen display devices, the polyester film is particularly preferably used in organic electroluminescence display devices or inorganic electroluminescence display devices that have a small layer structure, and is more preferably used in organic electroluminescence display devices in that it can form clear images with a wide color gamut.

[0016] The organic electroluminescence display device includes an organic electroluminescence element array, and may further include a circular polarizing plate, a touch panel module, a surface protection film, a back plate, an image pickup element, etc. as necessary, and may further include other components. For example, a pressure-sensitive adhesive layer may be provided between the image display light-emitting element array and the back plate, an abrasion-resistant layer may be provided on the viewer side as viewed from the polarizing plate, and a color filter, a lens film, a diffusion sheet, an anti-reflection film, etc. may be provided as necessary.

[0017] An example of an organic electroluminescence element array includes a substrate, a thin film transistor, an organic electroluminescence element, and a sealing layer, and the organic electroluminescence element includes an anode, a light-emitting layer, and a cathode. For example, the organic electroluminescence element may have the layer structure of the following (i) to (vi). In addition, the light-emitting layer may be composed of a blue light-emitting layer, a green light-emitting layer, and a red light-emitting layer.

[0018] Representative examples of the configuration of the organic electroluminescent device are shown below. (i) Anode / hole injection transport layer / light emitting layer / electron injection transport layer / cathode (ii) anode / hole injecting and transporting layer / light emitting layer / hole blocking layer / electron injecting and transporting layer / cathode (iii) Anode / hole injection transport layer / electron blocking layer / light emitting layer / hole blocking layer / electron injection transport layer / cathode (iv) Anode / hole injection layer / hole transport layer / light emitting layer / electron transport layer / electron injection layer / cathode (v) anode / hole injection layer / hole transport layer / light emitting layer / hole blocking layer / electron transport layer / electron injection layer / cathode (vi) anode / hole injection layer / hole transport layer / electron blocking layer / light emitting layer / hole blocking layer / electron transport layer / electron injection layer / cathode.

[0019] The substrate is a base material for supporting various elements of the light emitting element array for displaying an image, and may be made of an insulating material. For example, the substrate may be a glass substrate or a plastic substrate. For example, the plastic substrate may be selected from polyester, polyimide, polyethersulfone, polyimide, olefin, and polycarbonate, but is not limited thereto.

[0020] A rear plate is placed on the rear side of the substrate to support the substrate. Flexible glass or plastic substrates are thin and have low rigidity, and sagging may occur when various elements are arranged on the substrate. The rear plate film supports the light emitting element array for image display so that it does not sag, and protects the light emitting element array for image display from moisture, heat, impact, etc. An adhesive layer can be placed between the light emitting element array for image display and the rear plate film to bond the light emitting element array for image display and the rear plate film. The polyester film for a screen display device of the present invention can be suitably used as a rear plate film.

[0021] As a polarizing plate, by applying it to an organic electroluminescent display device or the like as a circular polarizing plate used together with an optical film (λ / 4 phase difference film), it exerts an effect of blocking reflected light from metal electrodes of the organic electroluminescent device or the like in all wavelengths of visible light, and can prevent reflections during observation and improve the expression of black. A circular polarizing plate is composed of a polarizer that converts incident light into linearly polarized light, and a phase difference plate that converts linearly polarized light into circularly polarized light.

[0022] The polarizing plate may be any polarizing plate or coated polarizing film used in fields related to screen display devices. A representative polarizing plate may be a polyvinyl alcohol film or the like dyed with a dichroic material such as iodine, but is not limited thereto, and any known or future developed polarizing plate may be appropriately selected and used.

[0023] The retardation plate can be selected from any retardation plate used in fields related to screen display devices. The retardation plate can be a plastic film stretched in a specific direction, and examples of the retardation plate include polycarbonate, polyester, polysulfone, polystyrene, and polymethyl methacrylate. The retardation plate can be formed of a single birefringent film, but it may also be formed by laminating multiple birefringent films so that the wavelength dependency of the retardation value is reduced and the plate functions over the entire visible light wavelength range.

[0024] The polarizer and the retardation plate can be attached to each other using an acrylic transparent pressure sensitive adhesive or bonding agent having no optical anisotropy.

[0025] The imaging element is installed for the purpose of capturing an image of the viewer's side (the side where an image is displayed; hereinafter, this may also be referred to as "front"). When the imaging element is installed, the polarizing plate, the light-emitting element array for screen display, the back plate, and the imaging element are arranged in this order as viewed from the viewer's side. In this way, by arranging the imaging element on the back of the light-emitting element array for screen display, an image can also be captured at the location where the camera is arranged, and the screen display surface can be made large. The polyester film for screen display device of the present invention can be particularly suitably used as this back plate. FIG. 1 is a schematic diagram for explaining an example of an image display device in the case where an imaging element is included. As shown in FIG. 1, the image display device 101 includes a light-emitting element array for image display having a screen region 102 in which an imaging element 104 for capturing the screen display side is arranged on the back side of the light-emitting element array, a screen region 103 in which the imaging element is not arranged on the back side, and a bezel portion 105 in which the light-emitting element array is not arranged. In the portion corresponding to the screen area 102 where the imaging element 104 is arranged on the back side of the image display surface, the image display light-emitting element array has a highly transparent image display light-emitting element that employs a transparent material for the cathode, anode, and light-emitting element substrate, and in the other portion corresponding to the screen area 103, it may have a low-transparency image display light-emitting element or a highly transparent image display light-emitting element.

[0026] Since the screen region 102 has high transparency, the image sensor 104 can collect information outside the screen that is incident through the screen region 102, and the image display device can realize full-screen display. In this example, an example in which the image sensor 104 is arranged has been described, but in the region corresponding to the screen region 102, an image sensor having a different viewing angle from the image sensor 104, or another image sensor such as a fingerprint authentication sensor may be arranged.

[0027] The image pickup device used in the present invention preferably has a diagonal angle of view, which is the maximum angle at which the external light irradiated to the image display device can be collected and identified, of 60 to 140°, and the lower limit is more preferably 70° or more, and even more preferably 75° or more. If the diagonal angle of view is too high, the productivity may decrease, so the upper limit is preferably 140° or less, and more preferably 130° or less. Due to the mechanism for suppressing the occurrence of color unevenness described below, an image pickup device with a particularly large diagonal angle of view can be used in the image display device, and image information of a wider range can be accurately collected and identified. In addition, when a camera is used as the image pickup device, the number of pixels is preferably 7 million pixels or more in order to capture a clear image, and more preferably 12 million pixels or more. Although there is no restriction on the upper limit, the upper limit is preferably 48 million pixels or less from the viewpoint of productivity.

[0028] The polyester film in the present invention refers to a film whose main component is polyester, and the polyester in the present invention is composed of a dicarboxylic acid component and a diol component. The film whose main component is polyester is one that contains 60% by mass or more of polyester with respect to the total mass of the film. In the present invention, the component refers to the smallest unit that can be obtained by hydrolyzing polyester.

[0029] Examples of dicarboxylic acid components constituting the polyester used in the present invention include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 5-sodiumsulfoisophthalic acid, phenylendanedicarboxylic acid, anthracenedicarboxylic acid, phenanthrenedicarboxylic acid, and 9,9'-bis(4-carboxyphenyl)fluorene acid; aliphatic dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, sebacic acid, dodecanedioic acid, dimer acid, eicosanedioic acid, pimelic acid, azelaic acid, methylmalonic acid, and ethylmalonic acid; alicyclic dicarboxylic acids such as adamantanedicarboxylic acid, norbornenedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, and decalindicarboxylic acid, and ester derivatives thereof. Among them, it is preferable to use an aromatic dicarboxylic acid component as the main dicarboxylic acid component. These dicarboxylic acid components may be used alone or in combination of two or more, and further, oxyacids such as hydroxybenzoic acid may be partially copolymerized.

[0030] Examples of diol components constituting the polyester used in the present invention include ethylene glycol, paraxylene glycol, 1,3-butanediol, 1,4-butanediol, tetramethylene glycol, 1,6-hexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, diethylene glycol, triethylene glycol, polyalkylene glycol, isosorbate, 1,2-propanediol, 1,3-propanediol, neopentyl glycol, 1,5-pentanediol, 1,7-heptanediol, 2,2-bis(4-hydroxyethoxyphenyl)propane, spiroglycol, etc. These diol components may be used alone or in combination of two or more.

[0031] From the viewpoints of productivity, film formation stability, and production costs, the polyester film of the present invention preferably contains polyethylene terephthalate as a main component. "Containing polyethylene terephthalate as a main component" means that the polyester contains 60 mol % or more of an ethylene glycol component as a diol component and 60 mol % or more of a terephthalic acid component as a dicarboxylic acid component.

[0032] The polyester film for screen display devices of the present invention satisfies the relationships of the following formulas (1) to (3), where ΔT60 is the difference in average transmittance between S waves and P waves at wavelengths of 400 nm to 800 nm at an incident angle of 60° with the vertical axis as the reference 0°, R50 is the phase difference value determined by illuminating a light beam with a wavelength of 590 nm at an incident angle of 50° along a plane including the fast axis of the film and the axis vertical to the film surface with the vertical axis as the reference 0°, and X is the value obtained by multiplying ΔT60 and R50 and dividing the result by 100. X≦700 Formula (1) 5.0≦ΔT60≦30 Formula (2) 100≦R50≦5000 Formula (3) Where, X = ΔT60 / 100 × R50 The inventors have discovered that by satisfying formula (1), it is possible to suppress color unevenness seen from an oblique direction when used as a screen protection film for an organic electroluminescent display device, for example, and color unevenness in an image depicted by an imaging element placed behind the film when used as a back plate.

[0033] Most of the color unevenness observed in screen display devices is observed when a birefringent film is sandwiched between two optical elements (such as polarizers, hereinafter referred to as "polarizing optical elements") that have different transmittances of polarized light depending on the in-plane direction. It is known that this color unevenness becomes less visible by controlling the phase difference of the birefringent film to a low value. On the other hand, as described above, an organic electroluminescence display device includes only one polarizing optical element in its configuration, so it is thought that color unevenness is not observed. However, when light is obliquely incident on the interface of materials with different refractive indexes, such as the interface between air and a film, the transmittance of the S wave and P wave may differ. In other words, when light is obliquely incident on the interface of the film, it is thought that the film interface acts as a pseudo polarizing optical element. As a result, it is thought that the organic electroluminescence display device is sandwiched between two pseudo polarizing optical elements, together with the polarizing optical element mounted thereon. Therefore, it is possible to make color unevenness less visible by reducing the difference in transmittance between the S wave and the P wave.

[0034] The reason why color unevenness is less visible by reducing the phase difference of the film is that when the wavelength dependency of the transmittance is measured with the film sandwiched between two polarizing plates, the amount of change in the transmittance due to the change in wavelength becomes gentle, and it is possible to prevent the transmittance in a specific wavelength range from decreasing. In addition, even when the difference in the transmittance of the S wave and the P wave described above is reduced, there is an effect of reducing the wavelength dependency of the amount of transmitted light. Since the effect of reducing the wavelength dependency of these transmitted light works synergistically with the phase difference of the film and the difference in the transmittance when viewed from an oblique direction, it is effective to control the parameter X, which is the product of the phase difference Re50 of the film when viewed from an oblique 50° direction and the difference ΔT60 in the transmittance at an oblique 60° direction, to a low value. The parameter X needs to be 700 or less, and from the viewpoint of effectively suppressing color unevenness, it is more preferable that it is 500 or less, and most preferable that it is 300 or less.

[0035] From the same viewpoint as above, it is more preferable that any one of the following (i) to (iV) is satisfied, and it is particularly preferable that (i) is satisfied. (i) 5.0≦ΔT60≦23 and 100≦R50≦1300 (ii) 5.0≦ΔT60≦25 and 100≦R50≦1700 (iii) 5.0≦ΔT60≦15 and 1700≦R50≦3200 (iV) 5.0≦ΔT60≦10 and 3200≦R50≦4600 In reducing the parameter X, the method of reducing R50 and ΔT60 is not limited. For example, the method of reducing R50 includes using an unstretched film, adding a copolymer component to increase the amorphousness and control the refractive index in the thickness direction to be high, and stretching the film and then subjecting it to heat treatment at a high temperature to relax the molecular orientation and control the refractive index in the thickness direction to be high. However, when R50 is controlled to less than 100 nm by the above-mentioned methods, the orientation of the polyester film is reduced, and the mechanical strength is reduced. Therefore, the R50 of the polyester film for a screen display device of the present invention is 100 nm or more, more preferably 300 nm or more. By setting it in this range, the Young's modulus in both the longitudinal direction and the transverse direction of the film can be 2.1 MPa or more, and for example, in the process of processing the polyester film for a screen display device in the manufacturing process of the screen display device, the film can be prevented from being torn. The Young's modulus is preferably 2.1 MPa or more, more preferably 2.5 MPa or more. In order to reduce R50, a method of reducing the film thickness is often used, but since reducing the film thickness leads to loss of support when used as a back plate, the film thickness is preferably 20 μm or more. The upper limit is preferably 70 μm or less, more preferably 60 μm or less, from the viewpoint of controlling R50 low and increasing the bending resistance described later.

[0036] As a method for controlling ΔT60 to be low, for example, a method for controlling the surface structure, such as a method for forming a low refractive index layer on the surface layer having a refractive index lower than that of the substrate by applying an anti-reflection treatment to the film surface, thereby suppressing the reflectance at the film interface and improving the transmittance, and a method for forming fine protrusions on the film surface to suppress the reflectance at the film interface and thereby increasing the transmittance and reducing ΔT60, are preferably used. The anti-reflection treatment here refers to laminating a layer having a different refractive index on the formed film by a method such as off-coating or vacuum deposition, and a method such as depositing magnesium fluoride on the surface layer is preferably used. In other words, it is preferable that the film of the present invention has a layer including an anti-reflection layer on at least one surface. When a low refractive index layer is formed on the film surface, when the average value of the refractive index in the longitudinal direction and the width direction of the outermost layer of the substrate film is n, and the refractive index of the low refractive index layer formed on the surface layer of the substrate film is n', it is preferable that n / n' is 1.08 or more from the viewpoint of controlling ΔT60 within the above range, and more preferably 1.10 or more. The refractive index of the low refractive index layer is preferably 1.35 to 1.58 from the viewpoint of increasing the transmittance, and more preferably 1.35 to 1.45. The thickness of the low refractive index layer is preferably 1 nm to 1 μm from the viewpoint of not imparting any other performance than optical performance, and is preferably 30 nm to 500 nm, and more preferably 60 nm to 200 nm from the viewpoint of increasing the transmittance by interfering with visible light. The low refractive index layer can be made to have the above refractive index range by using, for example, an acrylic resin as an easy-adhesion resin layer. In addition, silica fine particles having voids inside (hereinafter, sometimes also referred to as hollow silica particles) are preferably used as particles added to the low refractive index layer as a lubricant, since the refractive index can be controlled to be low. The preferred range of the average particle size is 40 nm to 100 nm, and more preferably 40 nm to 60 nm. If the average particle size is less than 40 nm, the reduction in the refractive index is insufficient, and if it is more than 100 nm, the film may become white or the surface unevenness may become large.

[0037] In addition to the design of the surface layer, a method of controlling only the reflectance of P waves to be high and controlling ΔT60 to be low by controlling the thickness and refractive index of each layer as a multi-layer laminate film in which layers A and B made of two different types of thermoplastic resins are alternately laminated in five or more layers can also be preferably used. When a film is laminated, the reflectance increases as the refractive index difference increases. Therefore, by designing the refractive index difference between layers A and B in the in-plane direction to be large and the refractive index difference in the direction perpendicular to the plane to be small, it is possible to control the reflectance of light incident from an oblique direction to be high and the reflectance of light incident from the front direction to be low, and it is possible to control only the reflectance of P waves to be high. From the viewpoint of making it easy to control the reflectance to be high, the total number of layers is preferably 50 or more, and more preferably 400 or more.

[0038] However, in order to control ΔT60 to a low range such as less than 5%, precise control is required whether using surface structure control technology or a multilayer laminate film, which is inferior in productivity. From this perspective, ΔT60 must be 5% or more. In particular, it is more preferable that it is 10% or more.

[0039] Furthermore, in order to increase the transmittance of light incident from an oblique direction and clarify the edges of the image captured by the imaging element, it is preferable that the average transmittance for S waves and P waves at wavelengths of 400 nm to 800 nm at an incident angle of 60°, with the vertical axis as the reference 0°, is 70% or more for both S waves and P waves.

[0040] By controlling R50 and ΔT60 in the above-mentioned method to satisfy formula (3), it is possible to suppress color unevenness, but when R50 is greater than 5000 nm or ΔT60 is greater than 30%, even if the other parameter is controlled to a low value, the influence of the other parameter on color unevenness is so great that it is difficult to suppress color unevenness, so R50 must be 5000 nm or less, and preferably 3000 nm or less. ΔT60 must be 30% or less, and more preferably 25% or less.

[0041] Only by satisfying all of the above formulas (1), (2), and (3) can a film be produced that suppresses color unevenness in the image sensor when used as a back plate and that also has excellent mechanical properties and productivity.

[0042] In an image taken from the polyester film for screen display devices of the present invention, arranged in this order, a polarizing plate, and a light source, using a viewing angle characteristic measuring and evaluating device (EZcontrast X88RC, manufactured by ELDIM) from the polyester film for screen display devices side, the difference between the maximum and minimum values ​​of chromaticity a* and b* at a viewing angle of 50° and an azimuth angle of 0° to 360° is preferably 15 or less, more preferably 12 or less, and most preferably 10 or less. Note that chromaticity a* and b* are determined by the method described in the Examples.

[0043] By setting the chromaticity a* and b* within the above range, it is possible to suppress unevenness in color, particularly at the edge of an image captured by an image sensor. In order to set the chromaticity a* and b* within the above range, the parameter X is set to 700 or less, and the unevenness in film thickness is controlled to 10% or less. It is more preferable that the unevenness in film thickness is 8% or less. In order to control the unevenness in thickness to a low level, the stretching ratio in the width direction is set to 2 times or more, and the stretching temperature in the width direction is set to the glass transition temperature Tg+50°C or less of the resin type.

[0044] The polyester film for a screen display device in the present invention preferably has a ΔHg / ΔCp value, calculated by dividing the specific heat difference ΔCp (unit: J / (g°C)) at the glass transition temperature observed in the reversible curve of temperature-modulated differential scanning calorimetry (temperature-modulated DSC) between 30°C and 150°C by the endothermic heat amount ΔHg (unit: J / g) observed in the irreversible curve between 30°C and 150°C, of ​​1.0 or more.

[0045] By controlling it within this range, the polyester film has good static bending properties, and a suitable polyester film can be obtained even when used in a bendable screen display device. A preferred range is that ΔHg / ΔCp is more than 1.0 and less than 10.0, with the lower limit being more preferably more than 2.0, particularly preferably more than 2.5, and the upper limit being more preferably less than 5.0.

[0046] Since polyester films are composed of polymer chains, they consist of crystalline components with relatively high rigidity, rigid amorphous components, and mobile amorphous components. The mobile amorphous components are classified into aggregated amorphous components with relatively high rigidity due to their heterogeneity, and relaxed amorphous components with dispersed polymer chains. The amount of relaxed amorphous components in polyester films can be calculated by subtracting the amount of aggregated amorphous components from the amount of mobile amorphous components based on the above relationship. The amount of mobile amorphous components and the amount of aggregated amorphous components can be analyzed by temperature modulated DSC. The specific heat difference ΔCp at the glass transition temperature observed between 30°C and 150°C in the reversible curve obtained by temperature modulated DSC is proportional to the amount of mobile amorphous components. In addition, the endothermic amount ΔHg observed between 30°C and 150°C in the irreversible curve is the amount of heat required for the aggregated amorphous components to relax and transition to the relaxed amorphous components, and therefore depends on the amount of aggregated amorphous components. The values ​​of ΔCp and ΔHg are calculated as the average values ​​of three measurements.

[0047] The method for controlling ΔHg / ΔCp within the above range is as described in the following steps (1) to (3), and in particular, it can be controlled by the temperature in the third stage of the heat treatment step and the relaxation rates in the machine direction and cross direction. Step (1) Stretching the film in the longitudinal direction by a factor of 2.9 to 3.3. Step (2) Stretching the film 3.7 times or more and 4.5 times or less in the transverse stretching direction Step (3) Heat treatment and relaxation at 210°C to 245°C Further details of each step are given below.

[0048] Step (1): Regarding the step of stretching the film 2.9 to 3.3 times in the longitudinal stretching direction, in order to obtain a more significant effect of the present invention, it is important to perform the stretching in three stages. Furthermore, it is preferable that the stretching ratios in the first, second, and third stages satisfy the following condition. 1st stage:≦1.3 times 2nd stage:≦1.5 times 3rd stage: 2.0 times or more and 2.3 times or less.

[0049] Step (2): In order to obtain the effects of the present invention in the step of stretching 3.7 times or more and 4.5 times or less in the transverse stretching direction, it is important to perform stretching in three stages. Furthermore, it is preferable that the stretching ratios in the first, second and third stages satisfy the following conditions. 1st stage: 2.0 times or more and 2.5 times or less 2nd stage:≦1.5 times 3rd row:≦1.5x.

[0050] Regarding step (3): the step of performing heat treatment relaxation at 220° C. or more and 245° C. or less, in order to obtain a more significant effect of the present invention, it is important to perform the heat treatment relaxation in three stages. Furthermore, it is preferable that the heat treatment temperatures in the first, second, and third stages and the relaxation rates in the longitudinal and transverse directions satisfy the following conditions. 1st stage: 150℃ or higher and 245℃ or lower 2nd stage: 220℃ or higher and 245℃ or lower 3rd tier: 100℃ or more and 180℃ or less Longitudinal relaxation rate: 1% to 8% Transverse relaxation rate: 1% or more and 8% or less.

[0051] The reason why the bending resistance is improved by increasing the value of ΔHg / ΔCp is considered to be as follows. Since polyester films are composed of polymer chains, they are composed of crystalline components with relatively high rigidity, rigid amorphous components, and mobile amorphous components. The mobile amorphous components are classified into aggregated amorphous components with relatively high rigidity due to their heterogeneity, and relaxed amorphous components with dispersed polymer chains. When a polyester film is bent, the polymer chains are subjected to elongation and compression forces at the bent portion, and the relaxed amorphous components with relatively low rigidity are considered to be plastically deformed. When a polyester film is plastically deformed by bending, it is plastically deformed when left standing in a folded state for a certain period of time, causing wrinkles, lifting, cracks, etc. in the polyester film. In addition, when repeatedly bent, the base point of the polyester film's breakage occurs due to plastic deformation, leading to breakage. From the above, it is considered that in order to improve static bending resistance and dynamic bending resistance, it is preferable to increase the amount of aggregated amorphous components and reduce the amount of relaxed amorphous components. That is, it was found that the flex resistance can be improved by increasing ΔHg, which indicates the amount of aggregated amorphous components, and decreasing ΔCp, which indicates the amount of mobile amorphous components, i.e., by increasing the value of ΔHg / ΔCp.

[0052] The polyester film for a screen display device in the present invention preferably contains a copolymerized polyester containing 10 mol % or more of any one of the following components among the constituent components (dicarboxylic acid component, diol component, the maximum value of each being 100 mol %): naphthalene dicarboxylic acid, polyetherimide, fluorene derivative, paraxylene glycol, bisphenol A, isosorbate, cyclohexane dicarboxylic acid, and cyclohexane dimethanol. Examples of fluorene derivatives include, but are not limited to, 9,9-bis(t-butoxycarbonylmethyl)fluorene, 9,9-bis[2-(t-butoxycarbonyl)ethyl]fluorene, 9,9-bis[1-(t-butoxycarbonyl)ethyl]fluorene, 9,9-bis[2-(t-butoxycarbonyl)-1-cyclohexylethyl]fluorene, 9,9-bis[2-(t-butoxycarbonyl)-1-phenylethyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-methylphenyl]fluorene, and 9,9-bis[4-(2-hydroxyethoxy)-3,5-dimethylphenyl]fluorene. In addition, the polyester film for a screen display device in the present invention more preferably contains a copolymerized polyester containing 15 mol% or more of any of the following components among the constituents (dicarboxylic acid component, diol component, each maximum value being 100 mol%): naphthalene dicarboxylic acid, polyetherimide, fluorene derivative, paraxylene glycol, bisphenol A, isosorbate, cyclohexane dicarboxylic acid, and cyclohexane dimethanol. By using this composition, the amorphousness of the polyester is improved, and the value of R50 can be controlled to be low. In addition, the amount of the above-mentioned aggregated amorphous components can be increased by increasing the proportion of the amorphous structure, and the value of ΔHg, which indicates the amount of aggregated amorphous, can be easily controlled to be high. In addition, the glass transition temperature Tg can be increased, and even at the processing temperature when incorporated into a screen display device, an increase in haze can be suppressed, and a film with excellent transparency can be obtained. From the same viewpoint as above, the film of the present invention preferably contains 50 mass% or more of the copolymerized polyester.

[0053] Next, examples of the polyester film for a screen display device and a specific method for producing the polyester film for a screen display device of the present invention will be described. Here, polyethylene terephthalate is used as a resin constituting the film, but the present invention is not limited to such examples.

[0054] First, polyethylene terephthalate resin is dried and pre-crystallized as a resin used for the film, and then fed to a single-screw extruder and melt-extruded. At this time, it is preferable to control the resin temperature to 265 to 295°C. Next, foreign matter is removed and the extrusion amount is balanced through a filter or a gear pump, and the resin is discharged in a sheet form onto a cooling drum from a T-die. At this time, the sheet-shaped polymer is adhered to the casting drum by using an electrostatic application method in which a high-voltage electrode is used to make the resin adhere to the cooling drum with static electricity, a casting method in which a water film is provided between the casting drum and the extruded polymer sheet, a method in which the casting drum temperature is set to the glass transition temperature of the polyester resin to (glass transition temperature -20°C) to make the extruded polymer adhere, or a method in which a combination of these methods is used, and the sheet-shaped polymer is cooled and solidified to obtain an unstretched film. Among these casting methods, when polyester is used, the electrostatic application method is preferably used from the viewpoints of productivity and flatness.

[0055] The unstretched film obtained in the casting process can be stretched in the longitudinal direction and then in the width direction, or in the width direction and then in the longitudinal direction (sequential biaxial stretching method), or in the simultaneous biaxial stretching method in which the film is stretched in the longitudinal and width directions almost simultaneously.

[0056] In the present invention, it is preferable to obtain the above-mentioned composition by carrying out at least the following steps (1) to (3) in this order. Step (1) Stretching the film in the longitudinal direction by a factor of 2.9 to 3.3. Step (2) Stretching the film 3.7 times or more and 4.5 times or less in the transverse stretching direction Step (3) Heat treatment and relaxation at 220°C to 245°C Further details of each step are given below.

[0057] Step (1): Regarding the step of stretching the film 2.9 to 3.3 times in the longitudinal stretching direction, in order to obtain a more significant effect of the present invention, it is important to perform the stretching in three stages. Furthermore, it is preferable that the stretching ratios in the first, second, and third stages satisfy the following condition. 1st stage:≦1.3 times 2nd stage:≦1.5 times 3rd stage: 2.0 times or more and 2.3 times or less.

[0058] Step (2): In order to obtain the effects of the present invention in the step of stretching 3.7 times or more and 4.5 times or less in the transverse stretching direction, it is important to perform stretching in three stages. Furthermore, it is preferable that the stretching ratios in the first, second and third stages satisfy the following conditions. 1st stage: 2.0 times or more and 2.5 times or less 2nd stage:≦1.5 times 3rd row:≦1.5x.

[0059] Regarding step (3): the step of performing heat treatment relaxation at 220° C. or more and 245° C. or less, in order to obtain a more significant effect of the present invention, it is important to perform the heat treatment relaxation in three stages. Furthermore, it is preferable that the heat treatment temperatures in the first, second, and third stages and the relaxation rates in the longitudinal and transverse directions satisfy the following conditions. 1st stage: 150℃ or higher and 245℃ or lower 2nd stage: 220℃ or higher and 245℃ or lower 3rd tier: 100℃ or more and 180℃ or less Longitudinal relaxation rate: 1% to 8% Transverse relaxation rate: 1% or more and 8% or less.

[0060] In addition, the stretching temperature in the longitudinal stretching step is preferably set to a temperature at which stretching unevenness does not occur, and for example, when a sequential biaxial stretching method is adopted in which stretching is performed in the longitudinal direction and then in the width direction, the preheating temperature in the longitudinal direction is preferably not less than the glass transition temperature of the resin -20°C and not more than the glass transition temperature, the stretching temperature is preferably not less than the glass transition temperature of the resin and not more than the glass transition temperature +20°C, the preheating temperature in the width direction is preferably not less than the glass transition temperature of the resin and not more than the glass transition temperature +20°C, and the stretching temperature is preferably not less than the glass transition temperature of the resin and not more than the glass transition temperature +10°C and not more than the glass transition temperature +50°C. Stretching may be performed multiple times in each direction.

[0061] In order to obtain the effects of the present invention, the heat treatment step after stretching in the width direction can be performed by any conventionally known method, such as in an oven or on a heated roll. It is important that the heat treatment is performed in a plurality of zones, with the temperature being increased and decreased stepwise, and the temperature and relaxation rate are as described above. In addition, a method of slightly stretching the film to about 1.01 to 1.20 times in the width direction in the heat treatment step can also be used. The heat treatment time can be any time within a range that does not deteriorate the properties, and is preferably performed for 1 to 60 seconds, more preferably 5 to 30 seconds.

[0062] In addition, from the viewpoint of adhesion with a layer containing a curable resin, the polyester film for a screen display device of the present invention is preferably laminated with an easy-adhesion resin layer having a thickness of 10 nm to 500 nm and a surface free energy of 38 mN / m or more on at least one side, and the easy-adhesion resin layer can be formed by coating the surface of the polyester film with an easy-adhesion resin (composite melt extrusion method, hot melt coating method, in-line coating method from a solvent other than water, water-soluble and / or water-dispersible resin, etc.), or a surface lamination method of a similar composition or a blend thereof. Among them, the in-line coating method in which a coating agent is applied to one side of a polyester film before the orientation crystallization is completed, stretched in at least one direction, and heat-treated to complete the orientation crystallization is industrially preferable for forming a uniform coating. In addition, when the easy-adhesion resin layer is provided by coating, the resin to which the easy-adhesion resin layer is applied is not particularly limited, but for example, acrylic resins, urethane resins, polyester resins, olefin resins, fluorine resins, vinyl resins, chlorine resins, styrene resins, various graft resins, epoxy resins, silicone resins, etc. can be used, and a mixture of these resins can also be used. From the viewpoint of adhesion, it is preferable to use polyester resins, acrylic resins, or urethane resins. In addition, from the viewpoint of suppressing the reflectance at the interface between the film and the air, the lower the refractive index of the easy-adhesion resin is compared with the refractive index of the film, the more the reflectance at the interface can be suppressed, which is preferable. When the polyester resin is used as a water-based coating liquid, a water-soluble or water-dispersible polyester resin is used, but for such water-solubilization or water-dispersion, it is preferable to copolymerize a compound containing a sulfonate group or a compound containing a carboxylate group. In addition, when the acrylic resin is used as a water-based coating liquid, it is necessary to make it dissolved or dispersed in water, and a surfactant (for example, polyether compounds, etc., but not limited thereto) may be used as an emulsifier.

[0063] In addition, in order to further improve the adhesiveness of the easy-adhesion resin layer used in the present invention, various crosslinking agents can be used in combination with the resin. As the crosslinking agent resin, melamine-based, epoxy-based, and oxazoline-based resins are generally used. As the particles contained in the resin layer of the present invention, inorganic particles and organic particles can be mentioned, but inorganic particles are more preferred because they improve the slipperiness and blocking resistance. As the inorganic particles, silica, alumina, kaolin, talc, mica, calcium carbonate, titanium, hollow silica, etc. can be used.

[0064] The image display device using the polyester film for screen display device of the present invention can also be suitably used as a foldable image display device that can be folded with a bending diameter of 1 to 10 mm. A more preferable range of the bending diameter is 8 mm or less as an upper limit, more preferably 6 mm or less, and even more preferably 5 mm or less. If the bending diameter is 10 mm or less, it can be made thin in the folded state. It can be said that the smaller the bending diameter, the better, but the smaller the bending diameter, the more likely it is to leave a crease. The bending diameter is preferably 0.1 mm or more, but may be 1 mm or more. Even if the bending diameter is 1 mm, it is possible to achieve a practically sufficient thinness when carrying it. In addition, the foldable image display device may be folded in three or four, or may be a rollable type, all of which are considered to be within the scope of the foldable image display device of the present invention.

[0065] When the polyester film for screen display device of the present invention is used for a screen display device that is bent, such as a foldable image display device, the angle between the bending direction and the main orientation axis in the polyester film plane is preferably 1° or more and 89° or less. By having the main orientation axis of the polyester film and the bending direction of the image display device in the above range, the static bending resistance and dynamic bending resistance of the foldable image display device can be maintained at high performance, and it is preferable in that mass productivity and economic efficiency can be improved. The angle between the bending direction and the main orientation axis in the polyester film plane is more preferably 20° or more, more preferably 30° or more, even more preferably 40° or more, and particularly preferably 50° or more as the lower limit, and more preferably 80° or less, even more preferably 75° or less, and even more preferably 70° or less as the upper limit.

[0066] Similarly, when producing a laminated film, a laminated polyester film can be obtained by co-extrusion using two or more extruders. The laminated structure can be set as necessary, for example, an A / B laminated structure in which one layer A and one layer B are laminated, a B / A / B laminated structure in which a layer B is further laminated, a multi-layered laminated structure in which layers A and B are alternately laminated, or a laminated structure in which three or more types of layers are laminated. When making a laminated polyester with 51 or more layers, a static mixer or a feed block is applied to allow layer A made of the polyester composition of the present invention and layer B made of another polyester composition to be alternately laminated, so that both surface layers become layer B.

[0067] Examples of the imaging element used in the image display device using the polyester film for screen display device of the present invention include image sensors such as cameras that obtain information on light having a wavelength of about 300 nm to 1500 nm from near ultraviolet to visible light and near infrared. A plurality of imaging elements may be disposed in one screen display device. EXAMPLES

[0068] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Measurement methods and evaluation methods in these examples are described below.

[0069] (1) Polyester composition The film was hydrolyzed with an alkali, and each component was analyzed by gas chromatography or high performance liquid chromatography, and the composition ratio was determined from the peak area of ​​each component. The dicarboxylic acid components were measured by high performance liquid chromatography. The measurement conditions can be analyzed by known methods, and the measurement conditions for the dicarboxylic acid components are shown below. Note that the measurement was performed after filtering and separating the inorganic particles. Equipment: Shimadzu LC-10A Column: YMC-Pack ODS-A 150×4.6mm S-5μm 120A Column temperature: 40℃ Flow rate: 1.2ml / min Detector: UV 240nm The diol components can be quantitatively determined by a known method using gas chromatography. The measurement conditions are as follows: Equipment: Shimadzu 9A (manufactured by Shimadzu Corporation) Column: SUPELCOWAX-10 capillary column 30m Column temperature: 140℃~250℃ (heating rate 5℃ / min) Flow rate: Nitrogen 25ml / min Detector: FID.

[0070] (2) Intrinsic viscosity The measurement sample was dissolved in 10 mL of orthochlorophenol at 100°C (solution concentration C (measurement sample mass / solution volume) = 0.08 g / mL), and the viscosity of the solution at 25°C was measured using a viscometer (VMR-052UPC·F10, manufactured by Rigo Co., Ltd.). The viscosity of the solvent was also measured in the same manner. Using the obtained solution viscosity and solvent viscosity, [η] was calculated according to the following formula (α), and the obtained value was taken as the intrinsic viscosity. ηsp / C=[η]+K[η]2·C (α) (Here, ηsp = (solution viscosity / solvent viscosity)-1, and K is the Huggins constant (assumed to be 0.343).) When the solution in which the measurement sample was dissolved contained insoluble matter such as inorganic particles, the measurement was performed using the following methods (i) to (iv). (i) Dissolve the measurement sample in 10 mL of orthochlorophenol to prepare a solution with a concentration of more than 0.08 g / mL. The mass of the measurement sample provided to orthochlorophenol is defined as the measurement sample mass. (ii) Next, the solution containing the insoluble matter is filtered, and the mass of the insoluble matter and the volume of the filtrate after filtration are measured. (iii) Add orthochlorophenol to the filtrate after filtration to adjust the mass of the sample (g) - mass of insoluble matter (g) / (volume of the filtrate after filtration (mL) + volume of added orthochlorophenol (mL)) to 0.08 g / mL. (For example, when a concentrated solution with a measurement sample mass of 1.00 g / solution volume of 10 mL is prepared, if the mass of insoluble matter when the solution is filtered is 0.02 g and the volume of the filtrate after filtration is 9.9 mL, an adjustment is made by adding 5.1 mL of orthochlorophenol. ((1.00 g-0.20 g) / (9.9 mL+0.1 mL)=0.08 g / mL)) The viscosity of the solution obtained in (iv) and (iii) at 25°C is measured using a viscometer, and the thus obtained solution viscosity and solvent viscosity are used to calculate [η] according to the above formula (α), and the obtained value is regarded as the intrinsic viscosity.

[0071] (3) Film thickness The film thickness was measured at five random locations on the film using a dial gauge (Mitutoyo Corporation, standard dial gauge 2109S-10) in accordance with JIS K7130 (1992) A-2 method, and the average value was taken as the film thickness.

[0072] (4) Uneven film thickness A sample with a width of 5 cm was cut out from the center of the entire width of the polyester film so that it was parallel to the film width direction and had a measurement length of 20 cm or more in order to evaluate thickness unevenness. Next, the sample was used to run the film at a running speed of 0.15 m / min using a film thickness tester KG601A manufactured by Anritsu Corporation. The thickness change was detected using a wide-range electronic micrometer K306C manufactured by Anritsu Corporation, and the thickness change over time was stored using a high-precision temperature and voltage measurement unit NT-TH08 manufactured by Keyence Corporation. The sampling period at this time was 100 ms, and the AD integration time was 2 ms. The thickness data was read out using Keyence Corporation's analysis software wave logger, and the thickness unevenness was calculated using the following formula (4).

[0073] Thickness unevenness (%) = (maximum thickness - minimum thickness) / average thickness × 100... Formula (4) (5) Identification of the longitudinal direction, width direction, slow axis direction, and fast axis direction of the film In the present invention, the flow direction during film production is the longitudinal direction, and the direction perpendicular to the longitudinal direction is the width direction. The slow axis direction and the fast axis direction are measured at 0° increments of 15° from an arbitrary direction, and the refractive index is measured from 0 to 360°. The direction with the highest refractive index is the slow axis direction, and the direction perpendicular to the slow axis direction is the fast axis direction. When the longitudinal direction and the width direction are unknown, the longitudinal direction and the slow axis direction, and the width direction and the fast axis direction are assumed to be consistent with each other. The refractive index was measured in accordance with JIS K7142 (2014) A method using an Abbe refractometer 4T (manufactured by Atago Co., Ltd.) at 25°C using sodium D line (wavelength 589 nm) as a light source and methylene iodide as a mounting liquid. The test piece used had a refractive index of 1.74.

[0074] (6) Glass transition temperature of resin and film Measurements and analysis were performed using a Rigaku Corporation Thermo plus ECO2 series DSC vesta and a Thermo plus ECO2 system manufactured by the same company in accordance with JIS K7121 (1987). Specifically, the temperature of 5 mg of sample was raised from 25°C to 300°C at 20°C / min, and the stepwise change in the glass transition of the differential scanning calorimetry chart obtained from the DSC curve was determined from the point where the curve of the stepwise change in the glass transition intersected with a straight line equidistant in the vertical direction from the extended straight line of each baseline.

[0075] (7) Front phase difference Re, R50 The measurement was performed using a retardation measurement device ("KOBRA" (registered trademark)-WPR) manufactured by Oji Scientific Instruments Co., Ltd. A sample was cut out to 3.5 cm x 3.5 cm from the center in the width direction of the film, and placed in the device so that the angle of the film width direction was 0° as defined by this measurement device, and the front retardation Re was measured at a wavelength of 590 nm.

[0076] The procedure for measuring R50 will be described with reference to Fig. 2. A light ray 205 having a wavelength of 590 nm was incident along a plane including a fast axis 202 of the film of a film sample 201 and a perpendicular axis 203 to the film surface at an incident angle 204 of 50° when the perpendicular axis is set as a reference 0°, and the retardation value determined was defined as R50.

[0077] (8)ΔT60 This was determined by the following steps (b1) to (b3). (b1) A spectrophotometer (U-4100 Spectrophotometer) manufactured by Hitachi High-Tech Corporation (formerly Hitachi High-Technologies Corporation) was fitted with an angle variable transmission accessory for the U-4100 spectrophotometer, a light source mask of 8 mm (H) x 5 mm (W), and a polarizer manufactured by Glan-Taylor. A polarized light that becomes p-polarized light was incident at an incident angle of 60° with respect to the incident surface when the film surface, which is the measurement sample, was used as the reflection surface, and the transmission spectrum in the wavelength range of 400 to 800 nm was measured. At this time, the slow axis direction of the film was aligned with the p-polarized direction. The measurement conditions were a slit of 2 nm, a gain of 2, a scanning speed of 600 nm / min, a sampling pitch of 1 nm, and a polarizer was attached just before the detector to allow only the p-polarized component of the transmitted light to enter the detector. From the obtained transmission spectrum, the average value of the transmittance in the wavelength range of 400 to 800 nm was calculated, and this was taken as the amount of p-polarized component in the transmitted light, Tpp [%]. (b2) An experiment similar to that in (c1) above was carried out, except that the light incident on the detector was changed to an s-polarized component, and the amount of s-polarized component Tps [%] in the transmitted light was determined. (b3) ΔT60 [%] was calculated using the following formula (5). ΔT60[%]=Tps-Tpp Equation (5) (9)Young’s modulus A rectangular sample of 150 mm in length and 10 mm in width was cut out in the longitudinal and transverse directions of the film. Young's modulus and breaking elongation were measured using a tensile tester according to the method specified in JIS K7127 (1999). The measurements were performed under the following conditions, with 10 samples, and the average values ​​were calculated. Measuring device: Orientec Co., Ltd.'s automatic film strength and elongation measuring device "Tensilon" (registered trademark) AMF / RTA-100 Sample size: width 10mm x length 50mm Pulling speed: 300mm / min Measurement environment: temperature 23℃, humidity 65%RH (10) Chromaticity difference Δa*, Δb* The film sample and polarizing plate (Kenis Co., Ltd., polarizing film thin size S, transmittance 0.43, polarization rate 0.9999, product code 1-115-0820) were stacked with the slow axis direction of the film sample aligned with the absorption axis direction of the polarizing plate, and the film sample, polarizing plate, and surface light source (Treviewer A4-100, Tritec Co., Ltd.) were placed horizontally in this order. The image was measured from the film sample side using a viewing angle characteristic measurement evaluation device (ELDIM Co., Ltd., EZcontrast X88RC). The chromaticity a* and b* at a viewing angle of 50° were calculated at azimuth angles of 1° each, and the difference between the maximum and minimum values ​​was calculated as the chromaticity difference Δa* and Δb*, respectively. When calculating the chromaticity a* and b*, analysis was performed using the attached software EZCom V6.10.

[0078] (11) ΔCp of film Using a TA Instruments temperature modulated differential scanning calorimeter, 5 mg of sample was measured in a nitrogen atmosphere from 0°C to 200°C at a heating rate of 2°C / min, a temperature modulation amplitude of ±1°C, and a temperature modulation period of 60 seconds. The specific heat difference ΔCp (unit: J / (g°C)) at the glass transition temperature was calculated in the reversible curve obtained by the measurement in the range of 30°C to 150°C. Specifically, the glass transition temperature of the reversible curve was determined, and the specific heat difference ΔCp was calculated from the distance between two straight lines extending each baseline at the glass transition temperature.

[0079] (12) ΔHg of film Using a TA Instruments temperature-modulated differential scanning calorimeter, 5 mg of sample was measured in a nitrogen atmosphere from 0°C to 200°C at a heating rate of 2°C / min, with a temperature modulation amplitude of ±1°C and a temperature modulation period of 60 seconds. The endothermic heat ΔHg (unit: J / g) was calculated in the irreversible curve obtained by the measurement in the range from 30°C to 150°C.

[0080] (13) Refractive index of film Using sodium D line (wavelength 589 nm) as a light source and methylene iodide as a mounting liquid, the refractive indexes in the longitudinal, width and thickness directions of the film were measured at 25°C using an Abbe refractometer 4T (manufactured by Atago Co., Ltd.) in accordance with JIS K7142 (2014) A method, and the refractive index in the longitudinal direction of the film was calculated as nx, the refractive index in the width direction as ny, and the refractive index in the thickness direction as nz. The refractive index of the test piece placed on the film during measurement was 1.74. When evaluating a laminated film, each layer was peeled off and the measurement was performed.

[0081] (14) Measurement of coating layer thickness The cross section of the sample was cut into ultra-thin sections and observed with a transmission electron microscope (Hitachi H-7100FA type) at an accelerating voltage of 100 kV (100,000 times magnification), and the thickness of the thin film layer was measured from the cross-sectional photograph. The layer thickness was measured at a total of 10 points, and the average value was determined as the film thickness.

[0082] (15) Refractive index of coating layer The number of layers in the surface layer of the film and the thickness of each layer were measured using the above-mentioned transmission electron microscope (Hitachi H-7100FA type). Based on this information, the refractive index of each layer was determined by measuring the absolute reflectance of the surface layer of the laminate in the range of 300 to 800 nm using a reflection spectroscopic film thickness meter (Otsuka Electronics Co., Ltd. FE-3000), and using the software FE-Analysis attached to the device, according to the method described in the film thickness measurement device general catalogue page 6 (nonlinear least square method) manufactured by Otsuka Electronics Co., Ltd., to determine the refractive index at 550 nm.

[0083] The optical constants (C1, C2, C3) were calculated by the least squares method (curve fitting method) using the Cauchy dispersion formula (Formula 1) as an approximation formula for the wavelength dispersion of the refractive index, and the refractive index at 550 nm was measured.

[0084]

number

[0085] (16) Camera visibility FIG. 3 shows a schematic diagram of a visibility test in a model device configuration of an image display device in which an imaging element is placed below the image display surface.

[0086] A film 201 cut to 50 mm x 50 mm was layered on a polarizing plate 301 (Kenis Co., Ltd., polarizing film thin size S, transmittance 0.43, polarization rate 0.9999, product code 1-115-0820) to prepare a measurement sample. The sample was supported so that the polarizing plate 301 side was facing down and placed horizontally on a surface light source 305 (Treviewer A4-100, Tritec Co., Ltd.), and photographed using an ultra-wide-angle lens 303 (diagonal angle of view 122°) of a camera-built-in device 302 (Samsung "Galaxy" (registered trademark) S10) so that the optical axis of the camera lens was perpendicular to the film 201. At this time, the photograph was taken so that the entire photographing angle of view 304 was within the range where the surface light source 305 was shining. The photographed image was observed, and the presence of color unevenness was observed, especially at the end positions, and judged as follows. Note that A, B, and C were determined to be acceptable levels that could be used sufficiently in an image display device. A: Almost no interference color is observed overall. B: Although some interference color can be seen in the corners of the image, this does not affect practical use. C: Interference colors are visible throughout, but it is usable. D: Not suitable for practical use as interference colors are clearly visible.

[0087] (17) Color uniformity The measurement sample prepared in (16) was placed on a surface light source (Treviewer A4-100, manufactured by Tritec Corporation). The laminate was observed from a position 50 to 100 cm away at angles of about 50°, about 60°, and about 70° to see if there was any color change. The observation results were evaluated into the following four stages. A: No color change was observed at any angle. B: The color change was only visible from one angle. C: The color change was only visible from two angles. D: The color change was visible from all angles.

[0088] (18) Handling A film 300 mm wide and 200 m long (wound on a 6-inch, 350 mm long core) was prepared and rewound onto a 3-inch, 350 mm long core under the conditions below. The conveying speed and tension were changed and evaluated according to the following criteria. A and B were determined to be at a level that could be handled adequately during processing. A: No tears or chips occurred even when rewinding at a speed of 15 m / min and a conveying tension of 70 N / m. B: No tears or chips occurred when rewinding at a speed of 10 m / min and a conveying tension of 70 N / m, but when the speed was increased to 15 m / min, tears and chips sometimes occurred. C: When rewinding at a speed of 10 m / min and a conveying tension of 70 N / m, tears and chips occurred.

[0089] (19) Bending resistance (rise angle) The measurement was carried out using a U-shaped stretch tester (Yuasa System Co., Ltd. DLDMLH-FS). With reference to FIG. 4, a film sample 201 cut to a length of 60 mm and a width of 25 mm was fixed to a tilt clamp with the clamp surface horizontal so that the direction parallel to the long side was the bending direction 401, and the film was left to stand for 24 hours in a state in which the center part 402 of the film was bent with a face-to-face distance of 3 mm. After 24 hours, the film was released from the bent state, taken out of the device, and left to stand with the bent outer side facing down, and the angle 403 formed by the film sample was measured. This measurement was repeated five times for each of the film sample cut with the longitudinal direction of the film as the long side and the film sample cut with the width direction as the long side, and the arithmetic average value was calculated to be the rise angle. The angle 403 was read with 0° as the completely folded state and 180° as the state in which the film recovered to its original unfolded state before folding. The bending resistance was evaluated according to the following criteria using the measurement result with the larger recovery angle from the measurement results in the longitudinal direction and the width direction. Note that bending resistance A and B are levels suitable for use as a foldable screen display device. A: The rise angle was 160° or more, and when mounted on a foldable screen display device, no wrinkles or lifting due to bending occurred. B: The rise angle is 150° or more and less than 160°, and slight wrinkles are observed, but there is no problem in practical use as a foldable screen display device. C: The rising angle is 140° or more and less than 150°, and slight wrinkles and rising phenomenon are observed, but there is no problem in practical use as a foldable screen display device. D: The rising angle is less than 140°, and although it is practically usable as an image display device, it is not suitable for practical use as a foldable screen display device.

[0090] (Production of polyester) The polyester resin used for film formation was prepared as follows.

[0091] (Polyester A) A polyester resin with 100 mol% terephthalic acid as the dicarboxylic acid component and 100 mol% ethylene glycol as the diol component. (Intrinsic viscosity: 0.65) (Polyester B) A copolymer polyester resin with 90 mol% terephthalic acid and 10 mol% isophthalic acid as dicarboxylic acid components, 90 mol% ethylene glycol as diol components, and 10 mol% isosorbate as diol components. (Intrinsic viscosity: 0.80) (Polyester C) A copolymer polyester resin with 100 mol% terephthalic acid as the dicarboxylic acid component, 80 mol% ethylene glycol as the diol component, 10 mol% 1,4-cyclohexanedimethanol as the diol component, and 10 mol% isosorbate as the diol component. (Intrinsic viscosity: 0.80) (Polyester D) A copolymer polyester resin with 92 mol% terephthalic acid and 8 mol% isophthalic acid as dicarboxylic acid components, and 80 mol% ethylene glycol, 10 mol% 1,4-cyclohexanedimethanol, and 10 mol% isosorbate as diol components. (Intrinsic viscosity: 0.80) (Polyester E) A copolymer polyester resin with 80 mol% of 2,6-naphthalenedicarboxylic acid as dicarboxylic acid components, 20 mol% of isophthalic acid as isophthalic acid components, 95 mol% of ethylene glycol as diol components, and 5 mol% of polyethylene glycol with a molecular weight of 400. (Intrinsic viscosity: 0.65) (Easy-adhesion coating layer) The easy-adhesion coating layer to be laminated on the surface of the film was prepared as follows.

[0092] <Coating Layer A> Resin solution (a): An acrylic resin solution copolymerized with 64 mass% methyl methacrylate, 30 mass% ethyl acrylate, 5 mass% acrylic acid, and 1 mass% acrylonitrile. Crosslinker (b): Methylol group-type melamine crosslinker Particles (c): Water dispersion of colloidal silica particles with a particle diameter of 60 nm. Fluorosurfactant (d): "Megafac" (registered trademark) F-444 manufactured by DIC Corporation These were mixed in a solid content mass ratio of (a) / (b) / (c) / (d) = 30 parts by mass / 8 parts by mass / 2 parts by mass / 0.6 parts by mass. The refractive index after drying was 1.50.

[0093] <Coating layer B> Resin solution (e): A solution obtained by mixing 70 parts by mass of a water-soluble coating liquid of a polyester resin consisting of acid components and diol components, namely, terephthalic acid (88 mol%), 5-sodium sulfoisophthalic acid (12 mol%), and ethylene glycol (100 mol%), which are acid components, with 30 parts by mass of an aqueous dispersion of a polyester resin consisting of acid components and diol components, namely, terephthalic acid (50 mol%), isophthalic acid (49 mol%), 5-sodium sulfoisophthalic acid (1 mol%), and diol components, namely, ethylene glycol (55 mol%), neopentyl glycol (44 mol%), and polyethylene glycol (molecular weight: 4000) (1 mol%). Crosslinker (b): Methylol group-type melamine crosslinker Crosslinking agent (f): Oxazoline group-containing crosslinking agent Particles (g): Water dispersion of colloidal silica particles with a particle diameter of approximately 150 nm Particles (h): Water dispersion of colloidal silica particles with a particle diameter of approximately 300 nm Fluorosurfactant (d): "Megafac" (registered trademark) F-444 manufactured by DIC Corporation These were mixed in a solid content mass ratio of (e) / (b) / (f) / (g) / (h) / (d) = 47 parts by mass / 19 parts by mass / 20 parts by mass / 4.9 parts by mass / 0.7 parts by mass / 0.1 parts by mass. The refractive index after drying was 1.57.

[0094] (Surface processing layer) <Off-coat layer> 219 parts by mass of methyltrimethoxysilane (KBM-7103 manufactured by Shin-Etsu Silicones) was hydrolyzed with 89 parts by mass of 0.5N formic acid while stirring at 20° C.±5° C. After 60 minutes, 412 parts by mass of isopropyl alcohol was mixed in to prepare a treatment liquid (X1).

[0095] Similarly, 158 parts by mass of 3,3,3-trifluoropropyltrimethoxysilane (KBM-7103 manufactured by Shin-Etsu Silicones) was hydrolyzed with 41 parts by mass of 1N formic acid while stirring at 30° C.±10° C. After 460 minutes, 521 parts by mass of isopropyl alcohol was mixed in to prepare a treatment liquid (X2).

[0096] Next, a silica slurry (X3) was prepared, which consisted of 144 parts by mass of hollow silica particles ("Suluria" (registered trademark) manufactured by Catalysts and Chemical Industries Co., Ltd.) having a porosity of 30% and an outer shell with an average primary particle diameter of 50 nm, and 560 parts by mass of isopropyl alcohol.

[0097] 720 parts by mass of treatment liquid (X1), 720 parts by mass of treatment liquid (X2), 704 parts by mass of silica slurry (X3), 356 parts by mass of methanol, 4272 parts by mass of isopropyl alcohol, and 713 parts by mass of polypropylene glycol monoethyl ether were stirred and mixed, and then 15 parts by mass of acetoacetoxyaluminum was added as a curing catalyst and stirred and mixed again to prepare a coating material with a refractive index of 1.45.

[0098] The prepared coating material was applied by a microgravure coater, dried at 80°C, and then heat-treated at 130°C to harden the coating layer, forming an off-coat layer with a thickness of about 0.1 μm. The refractive index of this off-coat layer was 1.45.

[0099] <Formation of deposition layer> Magnesium fluoride was evaporated onto the outermost layer of the long film using a winding vacuum evaporation device equipped with an electron beam evaporation source. After the film was set in the vacuum evaporation device, 5 × 10 -3 The chamber was evacuated to a vacuum of less than 1 Pa. The film was conveyed at a speed of 1.0 m / min while applying a tension of 130 N / m. The evaporation rate of magnesium fluoride was monitored using a quartz crystal film thickness gauge. The electron beam current of the electron beam evaporation source was adjusted to control the evaporation rate of magnesium fluoride so that the thickness of the evaporated thin magnesium fluoride layer obtained on the outermost surface of the film would be 100 nm, thereby obtaining the desired evaporated layer. The refractive index of the evaporated layer was 1.38.

[0100] (Examples 1 to 8, Comparative Examples 1 to 4) As shown in the table, the resin type was the polyester shown in the table, and the resin was vacuum dried at 160°C for 3 hours and then put into an extruder, melted at the extruder temperature shown in the table, and discharged from a T-die into a sheet on a cooling drum controlled at the temperature shown in the table. At that time, electrostatic was applied using a wire-shaped electrode with a diameter of 0.1 mm, and the sheet was attached to the cooling drum to obtain an unstretched sheet. Then, the sheet was quenched with a cooling roll controlled at a temperature of 25°C, and then stretched in the longitudinal direction at the stretching temperature and stretching ratio shown in the table, and then cooled once. Next, corona discharge treatment was performed on both sides of this uniaxially stretched film to set the wet tension of the film to 55 mN / m, and the coating layer shown in the table was applied to both sides of the film, and then the film was stretched in the width direction at the stretching temperature and stretching ratio shown in the table, and the film was heat-treated in a tenter at the heat treatment temperature shown in the table and relaxed in the longitudinal direction and / or width direction to obtain a film. The thickness of the coating layer after drying was 80 nm in each case. Furthermore, an off-coat layer was laminated according to the table. The physical properties of the obtained film are shown in the table.

[0101] In Examples 1 to 8, the parameters were within the range of the present invention, the camera visibility was excellent, and the handling was also excellent.

[0102] (Examples 9 to 15, Comparative Example 5) The resin types prepared by vacuum drying at 160 ° C for 3 hours using polyester of the resin types listed in the table were charged into two single-screw extruders, respectively, and melted at the temperature listed in the table. Then, each was charged into two short-screw extruders, melted at the temperature listed in the table, and kneaded. Next, after passing through five FSS-type leaf disk filters, the A layer was laminated in the inner layer part and the B layer was laminated on both surface layers in a three-layer merging block equipped with a rectangular lamination part while measuring with a gear pump so that the discharge ratio was polyester A / polyester B = 1 / 6, and extruded into a sheet shape from a T-die, and then wrapped around a casting drum at 25 ° C by preparing an electrostatic casting method, cooled and solidified, and an unstretched film was produced. Then, it was quenched with a cooling roll controlled at a temperature of 25 ° C, and then stretched in the longitudinal direction at the stretching temperature and stretching ratio listed in the table, and then cooled once. Next, both sides of the uniaxially stretched film were subjected to corona discharge treatment to set the wet tension of the film to 55 mN / m, and the coating layers shown in the table were applied to both sides of the film, which was then stretched in the width direction at the stretching temperature and stretching ratio shown in the table, and heat-treated in a tenter at the heat treatment temperature shown in the table and relaxed in the longitudinal direction and / or width direction to obtain a film. A surface processing layer was laminated according to the table.

[0103] In Examples 9 to 15, the parameters were within the range of the present invention, the camera visibility was excellent, and the handling was also excellent. In particular, in Example 13, all the evaluation results were good.

[0104] (Examples 17 to 20, Comparative Example 6) As shown in the table, the resin type was prepared by vacuum drying at 160 ° C for 3 hours using the polyester in the table, and the resin type was charged into two single-screw extruders and melted at the temperature shown in the table. Next, for each raw material, five FSS type leaf disk filters were passed through each, and then the raw materials were merged in a lamination device in which the number of slits matched the number of layers listed in the table so that the mass ratio of the resin type of layer A to the resin type of layer B was 1 while being metered with a gear pump, and a molten resin laminate was obtained in which the resin type of layer B was alternately laminated in the thickness direction so that it was located on the outermost layer on both sides. Then, the molten resin laminate was discharged from the die, cooled and solidified on a casting drum at a temperature of 25 ° C. to obtain a cast film. Then, it was quenched with a cooling roll controlled at a temperature of 25 ° C., and then stretched in the longitudinal direction at the stretching temperature and stretching ratio listed in the table, and then cooled once. Next, both sides of this uniaxially stretched film were subjected to a corona discharge treatment to set the wet tension of the film to 55 mN / m, and the coating layer shown in the table was applied to both sides of the film. The film was then stretched in the width direction at the stretching temperature and stretch ratio shown in the table, and heat-treated in a tenter at the heat treatment temperature shown in the table and relaxed in the longitudinal and / or width directions to obtain a film.

[0105] The reflectance of P waves changes by changing the number of layers, and in Examples 17 to 20, the parameter X was controlled low due to low ΔT, and the evaluation results of camera visibility were good. On the other hand, in Comparative Example 6, ΔT was large, and the evaluation results of camera visibility were poor.

[0106] [Table 1]

[0107] [Table 2]

[0108] [Table 3]

[0109] [Table 4]

[0110] [Table 5] [Industrial Applicability]

[0111] The polyester film for a screen display device of the present invention, when used in a screen display device, allows normal image information to be collected and recognized by an imaging element disposed below the image display surface, and has extremely high industrial applicability. The polyester film for a screen display device of the present invention can also be suitably used as a screen protection film used in screen display devices in general, a polarizer protection film used in liquid crystal displays and organic EL displays, and a touch panel substrate film for forming a transparent conductive layer. [Explanation of symbols]

[0112] 101: Image display device 102: Screen area where the image sensor is located behind the image display surface 103: Screen area where the image sensor is not located behind the screen display surface 104: Image sensor 105: Bezel part 201: Film (back plate) 202: Fast axis 203: Vertical axis 204: Angle of incidence 205: Ray of light 301: Polarizing plate 302: Camera-equipped device 303: Ultra-wide-angle lens 304: Shooting angle 305: Area light source 401: Bending direction 402: Center of the film 403: Angle of film sample

Claims

1. A polyester film for a screen display device, which satisfies the relationships of the following formulas (1) to (3), where ΔT60 [%] is the difference in average transmittance between S waves and P waves at wavelengths of 400 nm to 800 nm at an incident angle of 60° with the vertical axis as the reference 0°, R50 [nm] is the phase difference value obtained by irradiating a light beam with a wavelength of 590 nm at an incident angle of 50° with the vertical axis as the reference 0° along a plane including the fast axis of the film and the axis perpendicular to the film surface, and X is the value obtained by multiplying ΔT60 and R50 and dividing the result by 100. X≦700 Formula (1) 5.0≦ΔT60≦30 Formula (2) 100≦R50≦5000 Formula (3) where X = ΔT60 / 100 × R50

2. The polyester film for screen display devices according to claim 1, wherein the difference between the maximum and minimum values ​​of chromaticity a* and b* at a viewing angle of 50° and an azimuth angle of 0° to 360° is 15 or less when the polyester film for screen display devices, a polarizing plate, and a light source are arranged in this order and measured from the polyester film for screen display devices side using a viewing angle characteristic measuring and evaluating device (EZcontrast X88RC, manufactured by ELDIM).

3. 3. The polyester film for a screen display device according to claim 1, which comprises polyethylene terephthalate as a main component.

4. 3. The polyester film for a screen display device according to claim 1 or 2, wherein ΔHg / ΔCp, calculated by dividing the endothermic peak ΔHg [J / g] observed in an irreversible curve of a temperature-modulated DSC (30 to 150°C) by the baseline shift ΔCp [J / (g°C)] observed in a reversible curve, is 1.0 or more.

5. 3. The polyester film for a screen display device according to claim 1 or 2, which is used in an image display device in which, as viewed from the viewer's side, a polarizing plate, an array of light-emitting elements for image display, a polyester film for a screen display device, and an imaging element are mounted in this order.

6. 6. The polyester film for a screen display device according to claim 5, wherein the light-receiving angle range of the imaging element is 60° or more and 140° or less.

7. 3. The polyester film for a screen display device according to claim 1, wherein the average transmittance of S waves and P waves at wavelengths of 400 nm to 800 nm at an incident angle of 60° with respect to the vertical axis as the reference 0° is 70% or more for both S waves and P waves.

8. 3. The polyester film for a screen display device according to claim 1, wherein five or more layers of two different thermoplastic resins are laminated alternately.

9. 3. The polyester film for a screen display device according to claim 1, which has a layer including an antireflection layer on at least one surface thereof.

10. 3. The polyester film for a screen display device according to claim 1, wherein n / n' is 1.08 or more, where n is an average value of the refractive index in the longitudinal direction and the width direction of the outermost layer of the base film, and n' is a refractive index of the low refractive index layer formed on the surface layer of the base film.

11. 3. The polyester film for a screen display device according to claim 1, which contains 10 mol % or more of naphthalenedicarboxylic acid, polyetherimide, a fluorene derivative, paraxylene glycol, bisphenol A, isosorbide, cyclohexanedicarboxylic acid, or cyclohexanedimethanol.

12. A screen display device comprising the polyester film for a screen display device according to claim 1 or 2.

13. A foldable display comprising the polyester film for a screen display device according to claim 1 or 2.

14. A device having, as one of its components, an image display device on which the polyester film for a screen display device according to claim 1 or 2 is mounted.

Citation Information

Patent Citations

  • Polarizing plate protection film, polarizing plate and liquid crystal display apparatus

    JP2010204630A

  • Organic light-emitting display device

    JP2021110936A

  • Display panel, display and display terminal

    JP2021511649A

  • Display device with under-display camera

    JP2022133016A

  • Laminated polyester film and polarizing plate using the same

    JP6617561B2