Active material and manufacturing method thereof, and electrode mixture, electrode, and battery including the same

By applying a metal sulfate coating to the surface of core particles in solid-state batteries, the initial resistance is reduced through aligned electrochemical potential, enhancing lithium ion transfer and overall battery performance.

JP2024143695APending Publication Date: 2024-10-11MITSUI MINING & SMELTING CO LTD

Patent Information

Application Number
JP2023056485
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing solid-state batteries face high initial resistance due to the high resistance between the positive electrode active material and the solid electrolyte, which is not adequately addressed by current coating materials.

Method used

A coating comprising metal sulfate, such as lithium sulfate, is applied to the surface of core particles, forming a layer that reduces the initial resistance by aligning the electrochemical potential of lithium ions with the solid electrolyte, thereby minimizing the formation of a space charge layer.

Benefits of technology

The proposed coating significantly reduces the initial resistance of solid-state batteries by facilitating lithium ion transfer, improving the battery's performance and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143695000001
    Figure 2024143695000001
  • Figure 2024143695000002
    Figure 2024143695000002
Patent Text Reader

Abstract

To provide an active material capable of suppressing the initial resistance of a solid-state battery, which is a battery that is prone to having a high initial resistance.SOLUTION: An active material according to the present invention includes a core particle and a coating portion. The coating portion contains a metal sulfate. The active material has a peak in the range of 55.7±0.4 eV in the Li1s spectrum measured by X-ray photoelectron spectroscopy. When peak separation is performed on the Li1s orbital in the Li1s spectrum measured by X-ray photoelectron spectroscopy, the active material preferably has an area ratio of 0.5 or more of the peak observed in the range of 55.7±0.4 eV to the peak observed in the range of 54.0±0.5 eV.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an active material and a method for producing the same, and also to an electrode mixture, an electrode, and a battery each containing the active material. [Background technology]

[0002] In recent years, secondary batteries have been attracting attention as an effort to prevent global warming by reducing CO2 emissions. Among them, solid-state batteries are expected to be put to practical use as batteries that combine safety and high energy density. In solid-state batteries, the resistance between the active material and solid electrolyte in the positive electrode layer is high, so the surface of the positive electrode active material is coated with an ion-conductive inorganic material to reduce the resistance between the active material and solid electrolyte. For example, Patent Document 1 describes an all-solid-state lithium secondary battery including an oxide-based positive electrode active material coated with a Li-containing sulfate in which a Li-containing sulfate is formed on the surface of the oxide-based positive electrode active material. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2010-080168 A Summary of the Invention [Problem to be solved by the invention]

[0004] The selection of the coating material for the positive electrode active material has a large effect on the resistance of a solid-state battery, and the Li-containing sulfate-coated oxide-based positive electrode active material described in Patent Document 1 could not sufficiently reduce the resistance of the solid-state battery. Therefore, there is a demand for an active material that is more suitable for use in solid-state batteries and can further reduce the initial resistance of solid-state batteries, which tend to have high initial resistance.

[0005] Therefore, an object of the present invention is to provide an active material having a coating portion that can suppress the initial resistance of a solid-state battery, which is a battery that is prone to having high initial resistance. [Means for solving the problem]

[0006] The present invention provides an active material having a core particle and a coating portion disposed on a surface of the core particle, the coating portion contains a metal sulfate, The present invention provides an active material having a peak in the range of 55.7±0.4 eV in the Li1s spectrum measured by X-ray photoelectron spectroscopy.

[0007] The present invention also provides an active material having a core particle and a coating portion disposed on a surface of the core particle, the coating portion contains a metal sulfate, The metal sulfate is lithium sulfate.

[0008] The present invention also provides a method for producing an active material having core particles and a coating portion arranged on the surface of the core particles, the method comprising a step of dry-mixing the core particles with a compound containing lithium (Li), sulfur (S) and oxygen (O) while cooling. Effect of the Invention

[0009] According to the present invention, there is provided an active material capable of suppressing the initial resistance of a solid-state battery, which is a battery that tends to have a high initial resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will now be described based on its preferred embodiments. The present invention relates to an active material for a battery, for example, an active material for a lithium ion battery, and a manufacturing method thereof. The active material of the present invention has a core particle and a coating portion disposed on the surface of the core particle. The core particle is a portion that occupies the majority of the active material and is composed of an active material base material. The coating portion contains a metal sulfate as described later. The details of the metal sulfate will be described later. By disposing a coating portion containing a metal sulfate on the surface of the core particle and using an active material having a peak of binding energy in a specific range as described later, the initial resistance of a solid-state battery, which is a battery that tends to have a high initial resistance, can be suppressed. The following mechanism, for example, is considered as the reason why such an effect is obtained. In the case of a lithium ion battery, when a solid electrolyte and an active material come into contact with each other, lithium ions move from the solid electrolyte to the active material. This is because the electrochemical potential of the lithium ion is different between the solid electrolyte and the active material. The formation of a space charge layer between the solid electrolyte and the active material due to the movement of the lithium ions is one of the causes of an increase in the resistance of a solid-state battery. Therefore, in order to suppress the formation of the space charge layer, it is preferable to use a compound having an electrochemical potential of lithium ions close to that of the core particles as the coating portion of the active material. Furthermore, it is preferable that the compound contained in the coating portion has ion conductivity. This makes it easier to insert and remove lithium ions into and from the active material, thereby reducing the initial resistance of the solid-state battery.

[0011] [Metal sulfates] In the active material of the present invention, the coating portion preferably contains a metal sulfate. This makes it possible to provide an active material capable of effectively suppressing the initial resistance of a solid-state battery, which is a battery that is prone to high initial resistance. The metal in the metal sulfate is preferably one belonging to a typical element. Examples of such elements include Group 1 elements, Group 2 elements, and Group 13 elements. Specifically, Group 1 elements include lithium and sodium. Examples of Group 2 elements include magnesium and calcium. Examples of Group 13 elements include aluminum. These metals can be used alone or in combination of two or more.

[0012] An example of the composition of a metal sulfate is the formula (1): x (SO4) y In the formula (1), M preferably contains at least one metal selected from the above-mentioned Group 1 elements, Group 2 elements, and Group 13 elements. "x" and "y" are represented by the formula (1): x (SO4) y It is preferable that the range be such that electrical neutrality is maintained. For example, when M is a metal element (Group 1 element) that can become a monovalent cation, in formula (1), "x" is, for example, preferably 1.0 or more, more preferably 1.8 or more. Also, "x" is, for example, preferably 5.0 or less, more preferably 3.0 or less, and even more preferably 2.2 or less. When "x" is in this range, it is possible to effectively reduce the initial resistance of the solid-state battery. Also, in formula (1), "y" is, for example, preferably 0.5 or more, more preferably 0.8 or more. Also, "y" is, for example, preferably 2.5 or less, more preferably 1.5 or less, and even more preferably 1.2 or less. When "y" is in this range, it is possible to effectively reduce the initial resistance of the solid-state battery. Also, for example, when M is a metal element (group 2 element) that can become a divalent cation, "x" is, for example, preferably 0.5 or more, more preferably 0.8 or more. Also, "x" is, for example, preferably 4.0 or less, more preferably 2.0 or less, and even more preferably 1.2 or less. When "x" is in this range, it is possible to effectively reduce the initial resistance of the solid-state battery. Also, in formula (1), "y" is, for example, preferably 0.5 or more, more preferably 0.8 or more. Also, "y" is, for example, preferably 2.5 or less, more preferably 1.5 or less, and even more preferably 1.2 or less. When "y" is in this range, it is possible to effectively reduce the initial resistance of the solid-state battery. Also, for example, when M is a metal element (group 13 element) that can become a trivalent cation, "x" is preferably, for example, 1.0 or more, and more preferably 1.8 or more. Also, "x" is preferably, for example, 5.0 or less, more preferably 3.0 or less, and even more preferably 2.2 or less. When "x" is in this range, it is possible to effectively reduce the initial resistance of the solid-state battery. Also, in formula (1), "y" is preferably, for example, 1.5 or more, and more preferably 2.8 or more. Also, "y" is preferably, for example, 4.5 or less, more preferably 3.5 or less, and even more preferably 3.2 or less. When "y" is in this range, it is possible to effectively reduce the initial resistance of the solid-state battery.

[0013] Examples of the metal sulfate represented by formula (1) include lithium sulfate, sodium sulfate, magnesium sulfate, aluminum sulfate, and calcium sulfate. From the viewpoint of effectively lowering the initial resistance of a solid-state battery, which is a battery that is prone to having a high initial resistance, among these metal sulfates, it is preferable that M in formula (1) is a Group 1 element, and specifically, it is particularly preferable that the coating portion contains lithium sulfate. The metal sulfates can be used alone or in combination of two or more.

[0014] The metal sulfate is preferably contained in an amount of, for example, 0.1 mass % or more relative to the active material, more preferably 1.0 mass % or more, and even more preferably 3.0 mass % or more. The metal sulfate is preferably contained in an amount of, for example, 10.0% by mass or less, more preferably 8.0% by mass or less, and even more preferably 7.0% by mass or less, relative to the active material. By setting the content of the metal sulfate in the core particles within the above range, it is possible to effectively reduce the initial resistance of a solid-state battery, which is a battery that tends to have a high initial resistance.

[0015] [Covering part] The metal sulfate is present on the surface of the core particle as (I) particles, (II) aggregate particles formed by aggregation of particles, or (III) a layer. The term "layer" refers to a state in which the compound is present with a certain thickness. In this specification, any of the above embodiments (I) to (III) is included in the "coating portion containing a metal sulfate is formed."

[0016] The proportion of the metal sulfate contained in the coating portion is, for example, preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 95% by mass or more. When the proportion of the metal sulfate contained in the coating portion is within this lower limit, it becomes possible to effectively reduce the initial resistance of a solid-state battery, which is a battery that tends to have high initial resistance. The closer the proportion of the metal sulfate contained in the coating portion is to 100% by mass, the more it contributes to reducing the initial resistance of the solid-state battery.

[0017] The coating portion may contain compounds containing other elements in addition to the above-mentioned metal sulfates. Examples of other elements include phosphorus (P), carbon (C), silicon (Si), etc. These elements can be used alone or in combination of two or more. Examples of compounds containing these elements include lithium phosphate, lithium carbonate, silicon dioxide, etc.

[0018] The thickness of the coating portion is preferably, for example, 1 nm or more, more preferably 2 nm or more, and even more preferably 5 nm or more. When the thickness of the coating portion is within this lower limit, the formation of a space charge layer between the active material and the solid electrolyte can be effectively suppressed. The thickness of the coating portion is preferably, for example, 100 nm or less, more preferably 50 nm or less, even more preferably 30 nm or less, and particularly preferably 15 nm or less. When the thickness of the coating portion has this upper limit, resistance caused by the movement of ions from the solid electrolyte to the coating layer can be effectively suppressed. Considering the above, by having the thickness of the covering portion within the above range, it is possible to effectively reduce the initial resistance of a solid-state battery, which is a battery that tends to have high initial resistance. The thickness of the coating layer can be measured, for example, by X-ray photoelectron spectroscopy (XPS). If necessary, it can also be observed and measured in combination with a scanning transmission electron microscope (STEM) or Auger electron spectroscopy (AES).

[0019] The surface of the core particle may have a portion where the coating portion is not present. In this case, it is preferable that the coating portion covers, for example, 10% or more of the total surface area of ​​the core particle, more preferably 20% or more, and even more preferably 25% or more (this value is also called the "coverage ratio"). The fact that the surface of the core particle is covered by the coating portion can be confirmed, for example, by observing the surface of the core particle using X-ray photoelectron spectroscopy (XPS) in combination with a scanning transmission electron microscope (STEM) or energy dispersive X-ray analysis (EDS) as necessary, as well as Auger electron spectroscopy (AES), as described above. Furthermore, the thickness of the coating portion that coats the surface of the core particle does not need to be uniform.

[0020] [Core particles] The core particles are not particularly limited as long as they function as an active material. The core particles may contain, for example, a lithium metal composite oxide. As the lithium metal composite oxide, a known lithium metal composite oxide can be used. For example, it is preferable to include at least one selected from a lithium-containing composite oxide having a layered rock salt structure represented by the general formula LiMO2 (M represents a metal element), a lithium-excess layered rock salt type lithium-containing composite oxide, a lithium-containing composite oxide having a spinel structure represented by the general formula LiM2O4 (M represents a metal element), and a phosphate compound having an olivine structure represented by the general formula LiMPO4 (M represents a metal element). Alternatively, it may be a combination of two or more of these. However, it is not limited to these.

[0021] [Core particle A] The core particles are preferably particles made of a lithium transition metal composite oxide having a spinel structure containing Li, Mn, and O and one or more other elements (hereinafter, the core particles are also referred to as "core particles A"). When the active material of the present invention containing the core particles A is used as a positive electrode active material, it has an operating potential of 4.5 V or more based on a metal Li reference potential. "Having an operating potential of 4.5 V or more based on a metal Li reference potential" does not necessarily have to have only an operating potential of 4.5 V or more as a plateau region, but also includes a case where the operating potential is partially 4.5 V or more. Therefore, the present invention is not limited to a positive electrode active material consisting only of a 5 V class positive electrode active material having an operating potential of 4.5 V or more as a plateau region. For example, the active material of the present invention may contain a positive electrode active material having an operating potential of less than 4.5 V as a plateau region. Specifically, it is preferable that the 5V class positive electrode active material occupies, for example, 30 mass% or more, preferably 50 mass% or more, and particularly preferably 80 mass% or more (including 100 mass%) of the positive electrode active material.

[0022] As described above, the core particle A is preferably a particle made of a spinel-type composite oxide containing Li, Mn, and O and two or more other elements. At least one of the "two or more other elements" is preferably a metal element M1 selected from the group consisting of Ni, Co, and Fe, and the other element is preferably a metal element M2 consisting of one or a combination of two or more selected from the group consisting of Na, Mg, Al, K, Ca, Ti, V, Cr, Fe, Co, Cu, Ga, Y, Zr, Nb, Mo, In, Ta, W, Re, and Ce.

[0023] A preferred composition example of the core particle A is LiMnO 4-δ Examples of the lithium-manganese-containing spinel-type composite oxide include those having a crystal structure in which a part of the Mn sites in the above formula is substituted with Li, a metal element M1, and another metal element M2.

[0024] The metal element M1 is a substitution element that mainly contributes to realizing an operating potential of 4.5 V or more based on the metallic Li reference potential, and examples of such elements include Ni, Co, and Fe. The active material A may contain at least one of these elements, and it is particularly preferable that the active material A contains at least one of Ni and Co.

[0025] The metal element M2 is a substitution element that mainly contributes to stabilizing the crystal structure and improving the characteristics. For example, examples of substitution elements that contribute to improving the capacity retention rate include Na, Mg, Al, K, Ca, Ti, V, Cr, Fe, Co, Cu, Ga, Y, Zr, Nb, Mo, In, Ta, W, Re, and Ce, and among them, Na, Mg, Al, K, Ca, Ti, Cr, Fe, Co, Cu, Ga, Y, Zr, Nb, Mo, Ta, and W are preferably used. The metal element M2 may be one or a combination of two or more of the above-mentioned elements. The metal element M2 preferably contains at least one of the above-mentioned elements, and may contain a metal element other than the above-mentioned elements. The metal element M2 contained in the structure is an element type different from the metal element M1.

[0026] An example of the composition of the core particle A is represented by the formula (2): Li x (M1 y M2 z Mn 2-x-y-z )O 4-δ Examples include a spinel-type lithium manganese-containing composite oxide represented by the following formula (2): The metal element M1 and the metal element M2 in the formula (2) are as described above.

[0027] In the formula (2), "x" is preferably 1.00 or more, more preferably 1.01 or more, and even more preferably 1.02 or more. In the formula (2), "x" is preferably 1.20 or less, more preferably 1.10 or less, and even more preferably 1.08 or less. "y" indicating the content of the metal element M1 is preferably 0.20 or more, more preferably 0.30 or more, and even more preferably 0.35 or more. In addition, "y" indicating the content of the metal element M1 is preferably 1.20 or less, more preferably 1.10 or less, and even more preferably 1.05 or less. "z" indicating the content of the metal element M2 is preferably 0.001 or more, more preferably 0.002 or more, more preferably 0.005 or more, and even more preferably 0.100 or more. In particular, by making it 0.100 or more, the cycle characteristics can be improved more effectively. Moreover, "z" indicating the content of the metal element M2 is, for example, preferably 0.400 or less, and more preferably 0.300 or less.

[0028] Another example of the composition of the core particle A is a compound represented by the formula (3): Li x (Ni y M3 z Mn 3-x-y-z )O 4-δ Examples of the spinel-type lithium manganese-containing composite oxide include those represented by the formula (3). In formula (3), "x" is preferably 1.00 or more, more preferably 1.01 or more, and even more preferably 1.02 or more. In formula (3), "x" is preferably 1.20 or less, more preferably 1.10 or less, and even more preferably 1.08 or less. In formula (3), "y" is preferably 0.20 or more, more preferably 0.30 or more, and even more preferably 0.35 or more. In formula (3), "y" is preferably 0.70 or less, more preferably 0.60 or less, and even more preferably 0.55 or less.

[0029] In the formula (3), examples of the metal element M3 include Na, Mg, Al, K, Ca, Ti, V, Cr, Fe, Co, Cu, Ga, Y, Zr, Nb, Mo, In, Ta, W, Re, and Ce, and among these, Na, Mg, Al, K, Ca, Ti, Cr, Fe, Co, Cu, Ga, Y, Zr, Nb, Mo, Ta, and W are preferred. The metal element M3 may be one or a combination of two or more of the above-mentioned elements. "z" indicating the molar ratio of the metal element M3 is preferably, for example, greater than 0, and more preferably greater than 0.01, and even more preferably 0.05 or more, and even more preferably 0.10 or more. By setting "z" to this lower limit or more, the cycle characteristics can be improved more effectively. In addition, "z" indicating the molar ratio of the metal element M3 is preferably, for example, 0.50 or less, and even more preferably 0.45 or less, and even more preferably 0.40 or less, and even more preferably 0.35 or less.

[0030] In addition, "4-δ" in the above formulas (2) and (3) indicates that oxygen vacancies may be included. In addition, a part of oxygen may be substituted with fluorine or other elements. In this case, δ is preferably 0 or more. In addition, δ is preferably, for example, 0.20 or less, more preferably 0.10 or less, and even more preferably 0.05 or less.

[0031] The core particle A may contain B (boron). The state of existence of B may include a composite oxide phase containing Ni, Mn, and B in addition to a spinel crystal phase. An example of the composite oxide phase containing Ni, Mn, and B is a Ni5MnO4(BO3)2 crystal phase. The presence of the Ni5MnO4(BO3)2 crystal phase can be confirmed by comparing a diffraction pattern obtained by X-ray diffraction (XRD) with PDF (Powder Diffraction File) number "01-079-1029".

[0032] Regarding the content of the complex oxide phase containing Ni, Mn and B, it is preferable to contain the complex oxide phase so that the content of the B element in the core particle A is 0.02 mass% or more, and more preferably, the complex oxide phase is contained so that the content is 0.05 mass% or more. If the content of the B element is 0.02 mass% or more, it is preferable because the discharge capacity at high temperatures can be maintained. In addition, it is preferable to contain the complex oxide phase so that the content of the B element in the core particle A is 0.80 mass% or less, and more preferably, the complex oxide phase is contained so that the content is 0.60 mass% or less, more preferably, 0.30 mass% or less, and particularly preferably, 0.25 mass% or less. If the content of the B element is 0.80 mass% or less, it is preferable because the rate characteristic can be maintained.

[0033] The core particle A may contain components other than the above-mentioned Li, Mn, metal element M1, metal element M2, metal element M3, O, and B. In particular, the other elements may each be contained in an amount of 0.5 mass% or less, because such amounts are considered to have little effect on the performance of the core particle.

[0034] In addition, when the core particle A is fitted to a cubic crystal structure model of the space group Fd-3m (Origin Choice 2), for example, it can be confirmed that the core particle A has a spinel structure when the ranges of Rwp and S, which indicate the degree of agreement between the observed intensity and the calculated intensity, are Rwp<10 or S<2.5.

[0035] The primary particles of the core particles A are preferably polycrystalline rather than monocrystalline. A monocrystalline refers to a particle in which the primary particle is composed of one crystallite, and a polycrystalline refers to a particle in which multiple crystallites exist within the primary particle. Whether the core particles are polycrystalline or not can be confirmed by observing the cross section of the primary particle using electron backscatter diffraction (EBSD). In the case of a polycrystalline, it can be confirmed that crystals with multiple orientations exist within the primary particle.

[0036] [Core particle B] The core particles are also preferably particles made of a lithium transition metal composite oxide having a layered rock-salt structure containing Li, M element (M includes at least one or a combination of two or more elements selected from the group consisting of Ni, Co, Mn, and Al), and O (hereinafter, the core particles are also referred to as "core particles B"). The active material of the present invention may contain other components in addition to core particles B. However, from the viewpoint of effectively obtaining the characteristics of core particles B, it is preferable that core particles B account for, for example, 80% by mass or more, preferably 90% by mass or more, and more preferably 95% by mass or more (including 100% by mass).

[0037] The core particle B is represented by the formula (4): Li 1+x M 1-x O2 (wherein M is a combination of one or more elements selected from the group consisting of Ni, Co, Mn, and Al, or includes a combination of one or more elements selected from the group consisting of Ni, Co, Mn, and Al and a combination of one or more elements selected from the group consisting of transition metal elements present between Groups 3 and 11 of the periodic table, and typical metal elements from Periods 1 to 3 of the periodic table).

[0038] Formula (4): Li 1+x M 1-x In O2, "1+x" is, for example, preferably 0.95 or more, more preferably 0.97 or more, and even more preferably 0.98 or more. 1+x M 1-x In O2, "1+x" is, for example, preferably 1.09 or less, more preferably 1.07 or less, and even more preferably 1.05 or less.

[0039] "M" in the formula (4) may contain the three elements Mn, Co, and Ni. For example, it may be composed of only the three elements Mn, Co, and Ni, or may contain one or more of the other elements in addition to the three elements, or may have another composition.

[0040] Examples of transition metal elements present among the elements of Groups 3 to 11 of the periodic table, and typical metal elements from Period 1 to Period 3 of the periodic table include Al, V, Fe, Ti, Mg, Cr, Ga, In, Cu, Zn, Nb, Zr, Mo, W, Ta, and Re, and among these, V, Fe, Ti, Mg, Cr, Ga, Cu, Zn, Nb, Zr, Mo, W, and Ta are preferred.

[0041] When "M" in the above formula (4) contains the three elements Mn, Co, and Ni, the molar ratios of Mn, Co, and Ni are preferably Mn:Co:Ni=more than 0.00 and not more than 0.45:more than 0.00 and not more than 0.40:0.30 to 1.00, and more preferably Mn:Co:Ni=0.01 to 0.45:0.01 to 0.40:0.30 to 0.95, and more preferably Mn:Co:Ni=0.05 to 0.40:0.03 to 0.40:0.30 to 0.85, and even more preferably Mn:Co:Ni=0.05 to 0.40:0.03 to 0.40:0.30 to 0.75.

[0042] In the above formula (4), the atomic ratio of the oxygen amount is described as "2" for convenience, but may have some non-stoichiometry. That is, the atomic ratio of the oxygen amount may be "2-δ", where "-δ" indicates oxygen deficiency. In this case, δ is preferably 0 or more. In addition, δ is preferably, for example, 0.20 or less, more preferably 0.10 or less, and even more preferably 0.05 or less.

[0043] The core particles B may contain impurities. For example, the impurity elements may each be contained in an amount of 0.17 mass % or less. This is because it is believed that such amounts have almost no effect on the properties of the core particles B.

[0044] In addition, when the core particle B is fitted to a hexagonal crystal structure model of space group R-3m, for example, the ranges of Rwp and S, which indicate the degree of agreement between the observed intensity and the calculated intensity, are Rwp<10 or S<2.5, and thus it can be confirmed that the core particle B has a layered structure.

[0045] The primary particles of the core particles B are preferably polycrystalline rather than single crystal, like the core particles A. The definitions of single crystal and polycrystalline are the same as those for the core particles A.

[0046] [Core particle C] The core particles are preferably particles made of a lithium-excess layered lithium metal composite oxide containing Li, Ma (Ma necessarily contains Mn and contains at least one selected from Ni and Co), Mb (Mb contains at least one selected from Al, Mg, Ti, Fe and Nb) and O (hereinafter, the core particles are also referred to as "core particles C"). The active material of the present invention may contain other components in addition to the core particles C. However, from the viewpoint of effectively obtaining the characteristics of the core particles C, it is preferable that the core particles C occupy, for example, 50% by mass or more, particularly 70% by mass or more, of which 90% by mass or more, and of which 95% by mass or more (including 100% by mass) is included.

[0047] The core particle C is represented by the formula (5): Li 1+x Ma 1-x-y Mb y O2 (wherein Ma necessarily contains Mn and contains at least one selected from Ni and Co. Mb contains at least one selected from Al, Mg, Ti, Fe and Nb).

[0048] In the above formula (5), "x" is, for example, preferably 0.10 or more, more preferably 0.11 or more, and even more preferably 0.12 or more. Also, in the above formula (5), "x" is, for example, preferably 0.33 or less, more preferably 0.32 or less, and even more preferably 0.31 or less. In the above formula (5), "y" is, for example, preferably 0.000 or more, more preferably 0.005 or more, and even more preferably 0.010 or more. Also, in the above formula (5), "y" is, for example, preferably 0.300 or less, more preferably 0.295 or less, and even more preferably 0.290 or less.

[0049] Regarding the content of Ma in the core particles, the content of Mn in Ma is, for example, preferably 30% by mass or more, more preferably 31% by mass or more, and even more preferably 32% by mass or more. Also, the content of Mn in Ma is, for example, preferably 80% by mass or less, more preferably 79% by mass or less, and even more preferably 78% by mass or less.

[0050] In the above formula (5), the atomic ratio of the oxygen amount is described as "2" for convenience, but may have some non-stoichiometry. That is, the atomic ratio of the oxygen amount may be "2-δ", where "-δ" indicates oxygen deficiency. In this case, δ is preferably 0 or more. In addition, δ is preferably, for example, 0.20 or less, more preferably 0.10 or less, and even more preferably 0.05 or less.

[0051] The core particles C may contain impurities. For example, when the impurity is SO4, the impurity may be 1.0 mass% or less. Alternatively, when the impurity is an element other than SO4, the impurity may be 0.5 mass% or less. This is because such an amount is considered to have almost no effect on the properties of the core particles C.

[0052] [Active material] The active material of the present invention preferably has a peak in a specific range in the spectrum of Li1s measured by X-ray photoelectron spectroscopy (XPS). XPS is a measurement method that can analyze the constituent elements of the sample surface and their electronic state by measuring the photoelectron energy generated from the sample surface by irradiating the sample with X-rays. Therefore, by measuring the active material of the present invention by XPS, the chemical state of the metal sulfate forming the coating portion arranged on the surface of the core particle can be observed. As a result of the study by the present inventor, it was found that by observing a specific binding energy in the metal sulfate by XPS measurement, it is possible to reduce the initial resistance of a solid-state battery, which is a battery that is prone to high initial resistance. From this viewpoint, the active material of the present invention preferably has a peak in the range of 55.7±0.4 eV in the spectrum of Li1s measured by XPS, more preferably has a peak in the range of 55.7±0.3 eV, even more preferably has a peak in the range of 55.7±0.2 eV, and even more preferably has a peak in the range of 55.7±0.1 eV. In this specification, "having a peak in the range of 55.7±0.4 eV" means that the position of the peak top is in the range of 55.7±0.4 eV.

[0053] The active material is required to reduce the resistance of a solid-state battery, but the active material described in the above-mentioned Patent Document 1 could not solve this problem. In detail, the active material described in the same document is treated to cover its surface with a Li-containing sulfate, but the Li-containing sulfate is heat-treated after the treatment. Therefore, it is considered that the chemical structure of the Li-containing sulfate has changed, and as a result, the surface of the active material is covered with a compound different from the Li-containing sulfate. The different compound generated by the heat treatment of the Li-containing sulfate does not have a binding energy peak observed in a specific range in the spectrum of Li1s measured by XPS. In other words, unlike the active material of the present invention, the active material described in the same document does not have a binding energy peak observed in a specific range in the spectrum of Li1s measured by XPS. This is also clear from the results of Comparative Examples 1 and 2 described later. As a result, the active material described in the same document cannot sufficiently reduce the resistance of a solid-state battery. In contrast, the active material of the present invention, whose surface is covered with a specific coating portion, can further reduce the initial resistance of the above-mentioned solid-state battery compared to the active material described in Patent Document 1.

[0054] In order to make the active material have a peak in the range of 55.7±0.4 eV in the Li1s spectrum measured by XPS, it is preferable to dry mix the core particles and the compound that forms the coating portion while cooling in the manufacturing method described below, to include a metal sulfate in the coating portion, or to control the moisture content as described below.

[0055] As described above, the active material of the present invention has peak A in the range of 55.7±0.4 eV in the spectrum of Li1s, and may have peak B in the range of 54.0±0.5 eV. This peak is a peak derived from a compound contained in the core particle in the active material. This peak is observed, for example, when the thickness of the coating portion is extremely thin, or when there is a portion of the surface of the core particle where the coating portion does not exist. When the active material of the present invention has peak B in addition to peak A, it is also preferable that the value of R1 / R2 (hereinafter referred to as "area ratio R"), which is the ratio of the peak area R1 of peak A to the peak area R2 of peak B, is a predetermined value or more. By having the area ratio R be a predetermined value or more, it is possible to reduce the initial resistance of a solid battery, which is a battery that is prone to high initial resistance. For this reason, the area ratio R is preferably 0.5 or more, more preferably 0.8 or more, and even more preferably 1.0 or more. The larger the area ratio R, the more preferable it is, but if it is about 20.0, the above-mentioned effect is fully manifested. In this specification, "a peak observed in the range of 54.0±0.5 eV" means that the peak top position is in the range of 54.0±0.5 eV. The area ratio R can be determined by the method described in the Examples below.

[0056] In order to set the area ratio R in the active material within the above range, it is preferable to dry mix the core particles and the compound that forms the coating portion while cooling in the manufacturing method described below, to include a metal sulfate in the coating portion, or to control the moisture content as described below.

[0057] The active material of the present invention is generally in the form of particles, 50 That is, the volume cumulative particle size at 50% cumulative volume measured by a volume particle size distribution measurement method obtained by a laser diffraction scattering type particle size distribution measurement method is, for example, preferably 0.5 μm or more, more preferably 1.0 μm or more, and even more preferably 2.0 μm or more. 50 is preferably, for example, 15.0 μm or less, more preferably 10.0 μm or less, and even more preferably 8.0 μm or less.50 By setting the range above, it is possible to reduce the resistance when Li ions diffuse into the particles of the active material, and as a result, it is possible to improve the end-of-discharge characteristics.

[0058] The active material of the present invention may have a moisture content (mass ppm) up to 250°C measured by the Karl Fischer method of, for example, 1500 ppm or less, 1000 ppm or less, 800 ppm or less, or 700 ppm or less. The moisture content may be, for example, 1 ppm or more, 5 ppm or more, 10 ppm or more, 100 ppm or more, 200 ppm or more, or 300 ppm or more. The amount of moisture contained in the active material is preferably as small as possible from the viewpoint of suppressing structural deterioration of the active material and suppressing the reaction between the active material and the solid electrolyte during battery operation. In order to minimize the amount of moisture contained in the active material, for example, the active material may be dried at a temperature of 250°C or the like, under vacuum, or in an inert atmosphere. The procedure for measuring the moisture content by the Karl Fischer method is as follows: using a Karl Fischer moisture meter capable of coulometric titration, the measurement sample is heated to 110°C, the released moisture content (ppm by mass) is measured, and then the measurement sample is heated to 250°C, the released moisture content (ppm by mass) is measured, and the sum of these values ​​is taken as the moisture content. The measurement is performed in an argon atmosphere, and for example, an 860 KF Thermoprep (manufactured by Metrohm) and an 899 Coulometer (manufactured by Metrohm) are used as the measurement device.

[0059] The active material of the present invention can be used in a battery having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer. Specifically, the active material of the present invention can be used in the positive electrode layer or the negative electrode layer, and it is particularly preferable that the positive electrode layer contains the active material of the present invention. The active material of the present invention is preferably used in a solid battery containing a solid electrolyte. In a solid battery, the effect of the present invention can be enjoyed by the presence of a contact portion between the active material of the present invention and the solid electrolyte. The "solid-state battery" includes not only a solid-state battery that does not contain any liquid substance or gel substance as an electrolyte, but also, for example, a mode that contains a liquid substance or gel substance of 50% by mass or less, 30% by mass or less, 10% by mass or less as an electrolyte.

[0060] The active material of the present invention can obtain an electrode binder by mixing it with a solid electrolyte and a conductive material. As the solid electrolyte, it can be the same as the solid electrolyte used in general solid-state batteries. For example, sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, halide solid electrolytes, etc. can be mentioned. Among them, it is preferable to use a sulfide solid electrolyte containing the sulfur (S) element. The sulfide solid electrolyte may, for example, contain the Li element and the S element and have lithium ion conductivity, or may contain the Li element, the P element and the S element and have lithium ion conductivity. The sulfide solid electrolyte may be any of a crystalline material, glass ceramics, and glass. The sulfide solid electrolyte may have a crystalline phase of an argyrodite-type structure. Examples of such sulfide solid electrolytes include Li2S-P2S5, Li2S-P2S5-LiX (where "X" represents one or more halogen elements), Li2S-P2S5-P2O5, Li2S-Li3PO4-P2S5, Li3PS4, Li4P2S6, Li 10 GeP2S 12 、Li 3.25 Ge 0.25 P 0.75 S4、Li7P3S 11 、Li 3.25 P 0.95 S4、Li 7-x PS 6-x X x (a solid electrolyte having a crystalline phase of an argyrodite-type structure, "X" represents one or more halogen elements, and 0.2 < x < 2.0 or 0.2 < x < 1.8). As the conductive material, for example, electronically conductive carbonaceous materials such as carbon black and acetylene black can be used.

[0061] The electrode mixture is mixed with a solvent and a binder to prepare a paste, and the paste is applied to a current collector such as aluminum foil and dried to prepare an electrode (positive electrode layer and / or negative electrode layer). The electrode thus prepared contains the electrode mixture and the binder.

[0062] [Method for producing active material] Methods for producing active materials are roughly divided into methods for producing core particles and methods for forming coating portions on the surfaces of core particles. An example of the method for producing the core particles includes a manufacturing method including a raw material mixing step, a wet grinding step, a granulation step, a firing step, a heat treatment step, a washing / drying step and a grinding step, although this manufacturing method is merely a preferred example and is not limited to this manufacturing method.

[0063] The method for forming the coating portion is appropriately selected depending on the type of compound that constitutes the coating portion. For example, when the coating portion contains lithium sulfate as a metal sulfate, it is preferable to dry-mix the core particles with a compound containing lithium (Li), sulfur (S) and oxygen (O) elements, and to arrange the coating portion containing the compound on the surface of the core particles. In particular, when the dry mixing is performed while cooling, the compound is less likely to be altered. As a result, the obtained active material is preferable because it is possible to reduce the initial resistance of a solid-state battery, which is a battery that is prone to having a high initial resistance. When the dry mixing is performed with cooling, for example, a dry mixer equipped with a water-cooling jacket can be used. The temperature of the mixture during the dry mixing is preferably maintained at 10°C or higher and 50°C or lower.

[0064] For example, when the coating portion includes a compound containing other elements in addition to the compound containing the above-mentioned elements, a mixture containing the core particles, the above-mentioned compound, and a compound containing other elements may be dry-mixed to arrange the coating portion containing these compounds on the surface of the core particles. Alternatively, a mixture containing the core particles and the above-mentioned compound may be dry-mixed, and a compound containing other elements may be dry-mixed to arrange the coating portion containing these compounds on the surface of the core particles. Alternatively, one compound may be arranged on the surface of the core particles by a wet method, and then the core particles on which the compound is arranged and the other compound may be dry-mixed to arrange the coating portion containing these compounds on the surface of the core particles.

[0065] When a coating portion containing a compound is arranged on a core particle, it has been common to contact the core particle with a solution containing the compound. This method aims to uniformly coat the surface of the core particle with the compound. However, the conventional method has a problem that a drying process and a heat treatment process may be required after the coating portion is arranged. In addition, there is a problem that the chemical structure of the compound changes, especially due to the heat treatment process. As a result of intensive research into these problems, the present inventor has found that when a coating portion containing a compound is arranged on a core particle, these problems can be solved by performing dry mixing while cooling as described above.

[0066] Although the present invention has been described based on the preferred embodiment, the present invention is not limited to the above embodiment.

[0067] In relation to the above-described embodiment, the following active material and its manufacturing method, as well as an electrode mixture, an electrode, and a battery each containing the same are further disclosed. [1] An active material having a core particle and a coating portion disposed on the surface of the core particle, the coating portion contains a metal sulfate, The active material has a peak in the range of 55.7±0.4 eV in the Li1s spectrum measured by X-ray photoelectron spectroscopy.

[0068] [2] The active material according to [1], wherein, in the Li1s spectrum measured by the X-ray photoelectron spectroscopy, when peak separation is performed on the Li1s orbital, the ratio of the peak area of ​​a peak observed in the range of 55.7±0.4 eV to the peak area of ​​a peak observed in the range of 54.0±0.5 eV is 0.5 or more. [3] The active material according to [1] or [2], wherein the coating portion contains lithium sulfate. [4] An active material having a core particle and a coating portion disposed on the surface of the core particle, the coating portion contains a metal sulfate, The active material wherein the metal sulfate is lithium sulfate. [5] The active material according to any one of [1] to [4], wherein the proportion of the metal sulfate contained in the coating portion is 50 mass % or more. [6] The active material according to any one of [1] to [5], wherein the coating portion has a thickness of 1 nm or more and 100 nm or less.

[0069] [7] The active material according to any one of [1] to [6], wherein the core particles contain a lithium metal composite oxide, and the lithium metal composite oxide contains at least one selected from a compound having a layered rock salt structure, a compound having a spinel structure, and a compound having an olivine structure. [8] The active material according to any one of [1] to [7], which has a moisture content of 1,500 ppm or less at up to 250° C. as measured by the Karl Fischer method. [9] An electrode mixture comprising the active material according to any one of [1] to [8], a solid electrolyte, and a conductive material.

[10] An electrode comprising the electrode mixture according to [9] and a binder.

[11] A battery having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer, A battery, wherein the positive electrode layer contains the active material according to any one of [1] to [8].

[12] A method for producing an active material having core particles and a coating portion disposed on the surface of the core particles, the method comprising a step of dry-mixing, while cooling, a compound containing lithium (Li), sulfur (S) and oxygen (O) with the core particles. EXAMPLES

[0070] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. Unless otherwise specified, "%" means "% by mass".

[0071] Example 1 (1) Preparation of core particles As the core particles, a spinel-type lithium transition metal composite oxide (hereinafter also referred to as "LNMO") having a composition of Li: 4.1%, Mn: 41.3%, Ni: 13.3%, and Ti: 5.4% was prepared.

[0072] (2) Formation of the coating The core particles and lithium sulfate were mixed using a dry particle composite device NOB-MINI manufactured by Hosokawa Micron Corporation, and lithium sulfate was attached to the surface of the core particles to form a coating portion containing lithium sulfate. The amount of the core particles and lithium sulfate was adjusted so that the ratio of lithium sulfate to the active material was 5.0%. During mixing, the device was cooled and maintained at 30°C. In this manner, active material particles were obtained.

[0073] Example 2 In step (1) of Example 1, a lithium transition metal composite oxide (hereinafter also referred to as "NCM") having a composition of Ni: 60%, Co: 20%, Mn: 20% was prepared as the core material particles. Except for this, the active material particles were obtained in the same manner as in Example 1.

[0074] Comparative Example 1 This comparative example corresponds to an example of Patent Document 1. Instead of the step (2) in Example 1, the following step was added. First, an aqueous solution of lithium sulfate was prepared. The concentration of lithium sulfate in the aqueous solution was 0.64 mmol / L. The concentration was set so that the ratio of lithium sulfate to the active material was 1.2%. The core particles were added to the obtained aqueous solution, and the two were mixed at 10,000 rpm for 30 minutes using a homogenizer (IKA, T-25). After that, the solvent was removed using an evaporator while irradiating ultrasonic waves in a thermostatic chamber at 55°C. Furthermore, after drying at 120°C for 1 hour, the dried material was heat-treated in air at 500°C for 10 hours to obtain active material particles. As a result of XPS measurement, no Li1S peak was observed in the range of 55.7±0.4 eV. Therefore, the area ratio R could not be calculated.

[0075] Comparative Example 2 In the step (2) of Comparative Example 1, the concentration of lithium sulfate in the aqueous solution was adjusted to 2.65 mmol / L so that the ratio of lithium sulfate to the active material was 5.0%. The concentration was adjusted so that the ratio of lithium sulfate to the active material was 5.0%. Except for this, active material particles were obtained in the same manner as in Comparative Example 1. As a result of XPS measurement, no Li1S peak was observed in the range of 55.7±0.4 eV. Therefore, the area ratio R could not be calculated.

[0076] Comparative Example 3 Instead of step (2) of Example 1, the following step was added. First, 29.5 g of LiOH·H2O was dissolved in 214 g of water to obtain a lithium hydroxide aqueous solution. After this aqueous solution was heated to 100°C, 2 mL of 30% hydrogen peroxide and 0.862 g of niobium hydroxide were dissolved in the aqueous solution. The concentration of the aqueous solution was adjusted so that the ratio of lithium niobate to the active material was 1.3%. After stirring the aqueous solution for 30 minutes while keeping it at 100°C, 50 g of core particles were added to the aqueous solution and stirred for another 20 minutes. Next, the heating and stirring were stopped and the solution was left to stand, and the active material was allowed to settle in the aqueous solution. The aqueous solution was decanted, and the active material was washed twice with 200 mL of a 0.14 mol / L lithium sulfate aqueous solution. Then, the active material was dried at 80°C to obtain active material particles with lithium niobate present on the surface.

[0077] Comparative Example 4 In the step (1) of Example 1, NCM was prepared as the core material particles. In addition, the following step was provided instead of the step (2). First, 0.027 g of ethoxylithium was dissolved in 10 g of anhydrous ethanol to obtain an ethoxylithium solution. 0.167 g of pentaethoxyniobium was dissolved in 10 g of anhydrous ethanol to obtain a pentaethoxyniobium solution. The concentration of the solution was adjusted so that the ratio of lithium niobate to the active material was 0.8%. 10 g of NCM was added to 140 g of anhydrous ethanol, and dispersed using a homogenizer at 10,000 rpm for 30 minutes to obtain an ethanol solution in which NCM was dispersed. Next, the ethoxylithium solution was added to the ethanol solution in which NCM was dispersed, and the mixture was stirred at 10,000 rpm for 2 minutes. The pentaethoxyniobium solution was further added to this solution, and the mixture was stirred at 10,000 rpm for 8 minutes. The solution was ultrasonically treated at 55°C to evaporate the ethanol, and active material particles with lithium niobate on the surface were obtained. As a result of XPS measurement, no Li1S peak was observed in the range of 55.7±0.4 eV. Therefore, the area ratio R could not be calculated.

[0078] [Rating 1] The active materials obtained in the examples were subjected to XPS measurement by the following method to determine the Li1s peak position. The area ratio R was also determined by the following method. The coverage and thickness of the coating portion were also measured by the following method. Furthermore, the moisture content was measured by the above-mentioned method. The results obtained for Example 1 and Comparative Examples 1 to 3 are shown in Table 1 below. The results obtained for Example 2 and Comparative Example 4 are shown in Table 2 below.

[0079] [Li1s peak position] The particle surfaces of the active materials obtained in the examples and comparative examples were analyzed using a PHI Quantes XPS device manufactured by ULVAC-PHI, Inc. The conditions used for the measurements are as follows. Excitation X-ray: Monochromatic Al line (1486.7 eV) Output: 50W Acceleration voltage: 15 kV X-ray irradiation diameter: 200μmφ Measurement area: 1000μm x 300μm Take Angle: 45° Pass energy: 26.0 eV Energy step: 0.1 eV

[0080] The XPS data was analyzed using data analysis software (ULVAC-PHI XPS analysis software "MultiPakVer9.9"). The background mode was Iterated Shirley. Li1s was selected as the orbital used for calculation. Energy correction was performed using the C1s hydrocarbon peak (correction position: 284.8 eV).

[0081] [Covering rate of the coated part] The coverage of the coating was measured using PHI Quantes, an XPS device used to measure the Li1s peak position. Specifically, the ratio of the quantitative value of the element present only in the coating to the sum of the quantitative value of the element present only in the coating and the quantitative value of the element present only in the core particle was calculated. For example, when LNMO was used as the core particle and lithium sulfate was used as the coating, the coverage was calculated by S / (Ni+Mn+Ti+S)×100. Similarly, when NCM was used as the core particle and lithium sulfate was used as the coating, the coverage was calculated by S / (Co+Ni+Mn+S)×100. The conditions used for the measurement were the same as those used for the measurement of the Li1s peak position.

[0082] [Area ratio R] The active material was measured by XPS, and the spectrum of Li1s was subjected to background removal and peak fitting with a Gaussian function. Peaks observed in the range of 55.7 ± 0.4 eV were fitted with a full width at half maximum of 1.8 ± 0.2 eV. Peaks observed in the range of 54.0 ± 0.5 eV were fitted with a full width at half maximum of 1.3 ± 0.4 eV. Peak separation was performed for Li1s on these fitted peaks. The area of ​​the separated peak was taken as the peak area, and the ratio of the peak area of ​​the peak observed in the range of 55.7 ± 0.4 eV to the peak area of ​​the peak observed in the range of 54.0 ± 0.5 eV was taken as the area ratio R.

[0083] [Thickness of Covering Part] The thickness of the coating was measured using PHI Quantes, the XPS device used to measure the Li1s peak position. Specifically, Ar ion sputtering was performed and XPS measurement was performed to obtain a depth profile. The SiO2-equivalent sputtering depth at which the area of ​​the Li1s peak was halved compared to before sputtering was taken as the thickness of the coating. The conditions used for the measurement were the same as those used for measuring the Li1s peak position.

[0084] [Evaluation 2] Using the active materials obtained in the Examples and Comparative Examples, solid state batteries were manufactured by the following method, and the initial resistance of the solid state batteries was measured. The results obtained for Example 1 and Comparative Examples 1 to 3 are shown in Table 1 below. The results obtained for Example 2 and Comparative Example 4 are shown in Table 2 below. "-" in Tables 1 and 2 indicates that no Li1S peak was observed in the range of 55.7±0.4 eV, and therefore the area ratio R could not be calculated.

[0085] [Manufacturing of solid-state batteries] The active materials obtained in the examples and comparative examples were used as the positive electrode active material, and graphite (Gr) powder was used as the negative electrode active material. A sulfide solid electrolyte having an argyrodite structure was used as the solid electrolyte powder. The positive electrode composite powder was prepared by mixing the positive electrode active material, the solid electrolyte powder, and a carbon-based material serving as a conductive assistant in a mass ratio of 70:27:3 in a mortar. The negative electrode composite powder was prepared by mixing the negative electrode active material and the solid electrolyte powder in a mass ratio of 1:1 in a mortar. The lower opening of a polypropylene cylinder (opening diameter 10.5 mm, height 18 mm) with openings at the top and bottom was blocked with a positive electrode (made of SUS), solid electrolyte powder was placed on top of it, and it was blocked with a negative electrode (made of SUS), and then uniaxially pressed at 10 MPa to form a solid electrolyte layer. Next, the negative electrode was temporarily removed, and a negative electrode composite powder was placed on the solid electrolyte layer and blocked again with the negative electrode. Then, the cylinder was turned upside down, the positive electrode was temporarily removed, and a positive electrode composite powder was placed on the solid electrolyte layer and blocked again with the positive electrode, and then uniaxially pressed at 60 MPa to produce a solid battery consisting of a three-layer structure of a positive electrode composite, a solid electrolyte layer, and a negative electrode composite.

[0086] [Initial resistance of solid-state batteries] A charge / discharge test was carried out using the solid-state batteries produced in the examples and comparative examples as follows. In detail, the batteries were placed in an environmental tester set so that the environmental temperature for charging and discharging the batteries was 25° C., and the batteries were prepared for charging and discharging, and were left to stand until the battery temperature reached the environmental temperature. In Example 1 and Comparative Examples 1 to 3 in which the core particles were LNMO, the batteries were charged at a constant current and constant potential at 0.1 C to 5.0 V, and then discharged at a constant current of 0.1 C to 3.0 V, and this cycle was repeated for three cycles. Thereafter, the batteries were charged until the state of charge (SOC) reached 50%, and the initial resistance of the solid-state batteries was measured by impedance measurement. In Example 2 and Comparative Example 4 in which the core material particles were NCM, constant current constant potential charging was performed at 4.5 V, and constant current discharging was performed at 2.5 V. Other than these, the initial resistance value of the solid state battery was measured under the same conditions as when the core material particles were spinel-type lithium transition metal composite oxide.

[0087] [Table 1]

[0088] [Table 2]

[0089] As is clear from the results shown in Table 1, the solid state battery obtained using the active material of Example 1 has a lower initial resistance than the solid state batteries obtained using the active materials of Comparative Examples 1 to 3. Furthermore, as is clear from the results shown in Table 2, the solid-state battery obtained using the active material of Example 2 has a lower initial resistance than the solid-state battery obtained using the active material of Comparative Example 4.

Claims

1. An active material having a core particle and a coating portion disposed on the surface of the core particle, the coating portion contains a metal sulfate, An active material having a peak in the range of 55.7±0.4 eV in the Li1s spectrum measured by X-ray photoelectron spectroscopy.

2. 2. The active material according to claim 1, wherein, when peak separation is performed on the Li1s orbital in the Li1s spectrum measured by the X-ray photoelectron spectroscopy, the ratio of the peak area of ​​a peak observed in the range of 55.7±0.4 eV to the peak area of ​​a peak observed in the range of 54.0±0.5 eV is 0.5 or more.

3. The active material according to claim 1 , wherein the coating contains lithium sulfate.

4. An active material having a core particle and a coating portion disposed on the surface of the core particle, the coating portion contains a metal sulfate, The active material wherein the metal sulfate is lithium sulfate.

5. The active material according to claim 1 or 4, wherein the proportion of the metal sulfate contained in the coating portion is 50 mass % or more.

6. The active material according to claim 1 or 4, wherein the coating portion has a thickness of 1 nm or more and 100 nm or less.

7. 5. The active material according to claim 1, wherein the core particles contain a lithium metal composite oxide, and the lithium metal composite oxide contains at least one compound selected from the group consisting of a compound with a layered rock salt structure, a compound with a spinel structure, and a compound with an olivine structure.

8. 5. The active material according to claim 1, wherein the moisture content at temperatures up to 250°C as measured by the Karl Fischer method is 1500 ppm or less.

9. An electrode mixture comprising the active material according to claim 1 or 4, a solid electrolyte, and a conductive material.

10. An electrode comprising the electrode mixture according to claim 9 and a binder.

11. A battery having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer, A battery, wherein the positive electrode layer comprises the active material according to claim 1 or 4.

12. A method for producing an active material having core particles and a coating portion arranged on the surface of the core particles, the method comprising a step of dry-mixing the core particles with a compound containing lithium (Li), sulfur (S), and oxygen (O) while cooling.

Citation Information

Patent Citations

  • Cathode material coating method, coating system, cathode composite material and application

    CN115394996A

  • Positive electrode material for nonaqueous electrolyte lithium ion secondary battery and its manufacturing method

    JP2006073482A

  • All-solid lithium secondary battery

    JP2010080168A

Cited By

  • Lithium ion battery positive electrode material, preparation method thereof and lithium ion battery

    CN120033234A