Active material and manufacturing method for the same, and electrode mixture, electrode, and battery including the same
A coated active material with specific oxide compounds addresses high initial resistance and storage issues in solid-state batteries, enhancing their performance and stability.
Patent Information
- Application Number
- JP2023056488
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Solid-state batteries exhibit high initial resistance and are susceptible to storage characteristics influenced by environmental conditions.
An active material is developed with a core particle coated by a first and second oxide compound, where the first compound contains elements from specific periods of the periodic table and the second compound includes phosphorus, enhancing the coating's effectiveness.
The active material suppresses the increase in initial resistance and improves storage characteristics of solid-state batteries, ensuring better performance and stability.
Smart Images

Figure 2024143698000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an active material and a method for producing the same, and also to an electrode mixture, an electrode, and a battery each containing the active material. [Background technology]
[0002] In recent years, secondary batteries have been attracting attention as an effort to prevent global warming by reducing CO2 emissions. Among them, solid-state batteries are expected to be put to practical use as batteries that combine safety and high energy density. Various techniques are known for forming a coating on the surface of an active material in order to improve various performances of solid-state batteries. For example, Patent Document 1 proposes coating the surface of an active material with lithium niobate. This coating prevents a resistance layer from being formed between the active material and the solid electrolyte, thereby preventing an increase in interface resistance, and ultimately allowing lithium ions to move smoothly.
[0003] Patent Document 2 describes coating the surface of an active material with lithium metaphosphate. In this document, the active material is mixed with an aqueous solution of lithium metaphosphate, and then the active material is dried at 400° C. to form a coating on the surface of the active material. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2012-74240 A [Patent Document 2] International Publication No. 2017 / 094416 Brochure Summary of the Invention [Problem to be solved by the invention]
[0005] The present inventors have focused on the problems that solid-state batteries tend to have high initial resistance and that their storage characteristics are easily affected by the storage environment, and as a result of extensive research, have found that solving these problems simultaneously is important for improving the performance of solid-state batteries. Therefore, an object of the present invention is to provide an active material that can suppress an increase in the initial resistance of a solid-state battery, which is a battery that tends to have a high initial resistance, and can further improve the storage characteristics of the solid-state battery. [Means for solving the problem]
[0006] The present invention provides an active material having a core particle and a coating portion disposed on a surface of the core particle, the coating portion includes a first compound and a second compound, The first compound is M a It is an oxide containing the element, The second compound is M b It is an oxide containing the element, M b The element contains phosphorus (P), The above-mentioned problems are solved by providing an active material in which the first compound and the second compound are different compounds.
[0007] The present invention also provides a method for producing an active material having a core particle and a coating portion disposed on a surface of the core particle, comprising the steps of: the coating portion includes a first compound and a second compound, dry-mixing the core particles with at least one of a first compound and a second compound while cooling; The first compound is M a It is an oxide containing the element, The second compound is M b It is an oxide containing the element, M b The element contains phosphorus (P), The present invention provides a method for producing an active material, in which the first compound and the second compound are different compounds. Effect of the Invention
[0008] According to the present invention, there are provided an active material and a manufacturing method thereof that can suppress an increase in the initial resistance of a solid-state battery, which is a battery that tends to have a high initial resistance, and further improve the storage characteristics of the solid-state battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will now be described based on its preferred embodiments. The present invention relates to an active material for a battery, for example an active material for a lithium ion battery, and a method for producing the same. The active material of the present invention has a core particle and a coating portion disposed on the surface of the core particle. The core particle is a portion that occupies the majority of the active material and is composed of an active material base material. The coating portion includes a first compound and a second compound. The first compound and the second compound will be described later. By disposing a coating portion made of a specific compound on the surface of the core particle, it is possible to suppress an increase in the initial resistance of a solid-state battery, which is a battery that is prone to having high initial resistance, and further improve storage characteristics.
[0010] [First compound] In the active material of the present invention, the first compound forming the coating portion is an oxide. The oxide as the first compound may be used alone or in combination of two or more. The oxide is preferably M a Contains the element M a The elements may be selected from a wide range of different elements. For example, M a The element may be at least one of the elements belonging to the third to sixth periods of the periodic table of the second group of the periodic table. Of these elements, it is particularly preferable to use at least one of magnesium (Mg), strontium (Sr), and barium (Ba).
[0011] M aAs the element, at least one of the elements belonging to Groups 3 to 12 of the 4th period of the periodic table can be used. Among these elements, it is particularly preferable to use at least one of titanium (Ti), vanadium (V), manganese (Mn), iron (Fe), cobalt (Co), copper (Cu) and zinc (Zn), and it is particularly preferable to use Ti.
[0012] M a As the element, at least one of the elements belonging to Groups 3 to 8 of the 5th period of the periodic table can be used. Among these elements, it is particularly preferable to use at least one of yttrium (Y), zirconium (Zr), niobium (Nb), and ruthenium (Ru), and it is particularly preferable to use at least one of Zr and Nb.
[0013] M a The element may be at least one of the elements belonging to Groups 5 to 6 of the sixth period of the periodic table. Of these elements, it is particularly preferable to use tantalum (Ta).
[0014] M a As the element, at least one of the elements belonging to Periods 2 to 4 of Group 13 of the Periodic Table can be used. Among these elements, it is particularly preferable to use at least one of boron (B) and aluminum (Al).
[0015] M a As the element, at least one of elements belonging to Periods 3 to 6 of Group 14 of the periodic table can be used. Among these elements, it is particularly preferable to use at least one of silicon (Si) and tin (Sn), and it is particularly preferable to use Si.
[0016] M aThe element may be at least one of the elements belonging to Periods 2 to 6 of Group 15 of the Periodic Table. Of these elements, it is particularly preferable to use bismuth (Bi).
[0017] M a The element may be at least one of the elements belonging to Periods 2 to 6 of Group 16 of the periodic table. Of these elements, it is particularly preferable to use sulfur (S).
[0018] Furthermore, M a The element may be at least one of the lanthanoids in the periodic table having atomic numbers 57 and 58. Of these elements, it is particularly preferable to use the lanthanum (La) element.
[0019] Furthermore, M a As the element, lithium (Li) element can also be used.
[0020] The above various M a Among the elements, the oxide that is the first compound preferably contains Li element. By including Li element in the oxide, it is possible to suppress an increase in the initial resistance of a solid-state battery, which is a battery that tends to have a high initial resistance, and further to effectively improve storage characteristics.
[0021] In order to make the above-mentioned advantages more remarkable, the oxide which is the first compound is M a As an element, it is preferable to include an A element in addition to Li element. The A element is at least one element selected from Ti element, Zr element, Nb element, Ta element, B element, Al element, Si element, S element and La element. Particularly preferable A element is at least one element selected from Nb element, Ti element, S element and Zr element. Hereinafter, an oxide containing Li element and A element is also referred to as "LiA oxide" for convenience.
[0022] An example of LiA oxide is Li, where the A element is Nb. x NbO yIn the formula, x and y can take any value within the range according to the valence of the Nb element. Specifically, Li3NbO4, LiNbO3, LiNb3O8, and Li8Nb6O 19 etc. When the A element is Ta, an example of the LiA oxide is lithium tantalate (LiTaO3). When the A element is an S element, examples of LiA oxide include lithium sulfate (Li2SO4) and lithium sulfite (Li2SO3). When the A element is Zr, an example of the LiA oxide is lithium zirconate (Li2ZrO3). The above-mentioned various LiA oxides can be used alone or in combination of two or more.
[0023] The first compound is preferably contained in the active material of the present invention in an amount of, for example, 0.05% by mass or more, from the viewpoint of suppressing an increase in the initial resistance of a solid-state battery, which is a battery that is prone to having a high initial resistance, and further effectively improving storage characteristics. In order to make this advantage more prominent, the first compound is preferably contained in the active material of the present invention in an amount of, for example, 0.50% by mass or more, and even more preferably 1.50% by mass or more. In addition, from the viewpoint of ensuring the battery capacity and the ionic conductivity inside the battery, the first compound is preferably contained in an amount of, for example, 10.00 mass % or less, more preferably 7.00 mass % or less, and even more preferably 5.00 mass % or less, relative to the active material of the present invention.
[0024] [Second Compound] In the active material of the present invention, the second compound forming the coating portion is M b It is an oxide containing the element M bThe element preferably contains phosphorus (P). In other words, the second compound is preferably a compound containing P and oxygen (O). However, the oxide of the first compound and the oxide of the second compound are different compounds. By having the second compound exist in the coating portion together with the first compound, it is possible to suppress an increase in the initial resistance of a solid-state battery, which is a battery that is prone to high initial resistance, and further to effectively improve storage characteristics.
[0025] The oxide of the second compound is preferably orthophosphoric acid, and its condensates such as pyrophosphoric acid, metaphosphoric acid, and polyphosphoric acid, or a salt thereof, in order to suppress an increase in the initial resistance of a solid-state battery, which is a battery that is prone to have a high initial resistance, and to effectively improve storage characteristics. In order to make this advantage even more pronounced, it is preferable to use orthophosphoric acid, metaphosphoric acid, and salts thereof as the oxide of the second compound. The second compound may be used alone or in combination of two or more.
[0026] The oxide, which is the second compound, may further contain other elements in addition to the P element and the O element in order to make the effect of the present invention more remarkable. Examples of such elements include at least one element selected from the group consisting of lithium (Li), aluminum (Al), titanium (Ti), germanium (Ge), iron (Fe), cobalt (Co), bismuth (Bi), boron (B), yttrium (Y) and zirconium (Zr). By including these elements in the second compound, it is possible to suppress an increase in the initial resistance of a solid-state battery, which is a battery that is prone to high initial resistance, and further to effectively improve storage characteristics. In order to make the above advantages even more pronounced, it is more preferable to use at least one element selected from the group consisting of Li, Al, Ti and Ge as the element.
[0027] When the phosphate compound contains other elements in addition to the P and O elements, the elements are preferably present in the form of a salt of the above-mentioned phosphate compound, specifically, lithium phosphate, aluminum phosphate, iron phosphate, lithium iron phosphate, cobalt phosphate, lithium cobalt phosphate, bismuth phosphate, yttrium phosphate, etc. When the phosphate compound is an orthophosphate, the element is preferably present in the form of, for example, lithium orthophosphate, aluminum orthophosphate, iron orthophosphate, cobalt orthophosphate, bismuth orthophosphate, yttrium orthophosphate, etc. For example, lithium orthophosphate may be Li3PO4, aluminum orthophosphate may be AlPO4, iron orthophosphate may be FePO4, cobalt orthophosphate may be Co3(PO4)2, bismuth orthophosphate may be BiPO4, and yttrium orthophosphate may be YPO4. Other examples include LiFePO4, LiCoPO4, Li 0.1 B 0.967 PO4, Li 1.4 Al 0.4 Ti 1.6 It may exist in the form of (PO4)3, etc. When the phosphate compound is a metaphosphate, the metal element is preferably present in the form of, for example, lithium metaphosphate, aluminum metaphosphate, etc. For example, lithium metaphosphate may be LiPO3, and aluminum metaphosphate may be Al(PO3)3.
[0028] The second compound is preferably contained in an amount of 0.05% by mass or more relative to the active material of the present invention, from the viewpoint of suppressing an increase in the initial resistance of a solid-state battery, which is a battery that is prone to have a high initial resistance, and further effectively improving storage characteristics. In order to make this advantage more prominent, the second compound is preferably contained in an amount of, for example, 0.50% by mass or more, and even more preferably 1.50% by mass or more relative to the active material of the present invention. In addition, from the viewpoint of ensuring the battery capacity and the ionic conductivity inside the battery, the second compound is preferably contained in an amount of, for example, 10.00 mass % or less, more preferably 7.00 mass % or less, and even more preferably 5.00 mass % or less, relative to the active material of the present invention. Taking the above into consideration, the second compound is preferably contained in the active material of the present invention in an amount of, for example, 0.05 mass% or more and 10.00 mass% or less, more preferably 0.50 mass% or more and 7.00 mass% or less, and even more preferably 1.50 mass% or more and 5.00 mass% or less.
[0029] There is no particular limitation on the combination of the first compound and the second compound, and the above-mentioned first compound and second compound can be appropriately selected and used in combination. For example, if the first compound is M a The second compound is an oxide containing phosphorus as an element, and the second compound is M b It may be an oxide containing phosphorus (P) as an element. Alternatively, the first compound is M a The oxide does not contain phosphorus as an element, and the second compound is M b The first compound may be an oxide containing phosphorus (P) as an element. a When phosphorus (P) is not included as an element, it is preferable to use, for example, lithium sulfate or lithium niobate as the first compound, and it is particularly preferable to use lithium sulfate. In that case, for example, lithium metaphosphate, aluminum metaphosphate, Li 1.4 Al 0.4 Ti 1.6 It is preferable to use (PO4)3, and particularly preferable to use lithium metaphosphate. Selecting a combination of these compounds is preferable from the viewpoint of suppressing an increase in the initial resistance of a solid-state battery, which is a battery that is prone to having a high initial resistance, and further effectively improving storage characteristics.
[0030] [Covering part] The first compound and the second compound are present on the surface of the core particle as (I) particles, (II) aggregated particles, or (III) a layer. The term "a layer" refers to a state in which the first compound and the second compound are present with a certain thickness. In this specification, any of the above embodiments (I) to (III) is encompassed by "a coating portion containing a first compound and a second compound is formed."
[0031] The state in which the first compound and the second compound are present in the coating portion depends on the method for forming the coating portion. Depending on the method for forming the coating portion, the first compound and the second compound may be present in the coating portion in a mixed state. Alternatively, depending on the method for forming the coating portion, a layer mainly containing the first compound and a layer mainly containing the second compound may be laminated to form the coating portion. In this case, a layer mainly containing the first compound may be present on the surface of the core particle, and a layer mainly containing the second compound may be present thereon. Conversely, a layer mainly containing the second compound may be present on the surface of the core particle, and a layer mainly containing the first compound may be present thereon.
[0032] Regardless of the state of the first compound and the second compound in the coating portion, the ratio of the first compound to the second compound is preferably, for example, 0.050 or more, expressed as the mass ratio of the second compound to the first compound, from the viewpoint of suppressing an increase in the initial resistance of a solid-state battery, which is a battery that is prone to have a high initial resistance, and further effectively improving storage characteristics. From the viewpoint of making this advantage more prominent, the mass ratio of the second compound to the first compound is, for example, more preferably 0.100 or more, even more preferably 0.125 or more, and even more preferably 0.250 or more. In addition, from the viewpoint of being able to suppress an increase in the initial resistance of a solid-state battery, which is a battery that is prone to having high initial resistance, and further being able to effectively improve storage characteristics, the mass ratio of the second compound to the first compound is preferably 20,000 or less, more preferably 10,000 or less, even more preferably 8,000 or less, and even more preferably 4,000 or less.
[0033] The ratio of the first compound and the second compound in the coating portion and the ratio of the first compound and the second compound to the active material can be measured by elemental analysis using ICP emission spectroscopy. If necessary, measurements using X-ray absorption fine structure (XAFS), Fourier transform infrared spectroscopy (FT-IR), and X-ray photoelectron spectroscopy (XPS) can also be combined.
[0034] The thickness of the covering portion is preferably, for example, 1 nm or more, more preferably 10 nm or more, and even more preferably 20 nm or more. The thickness of the covering portion is preferably, for example, 100 nm or less, more preferably 50 nm or less, and even more preferably 35 nm or less. By setting the thickness of the covering portion within this range, the interface resistance caused by the formation of the covering portion is prevented from becoming excessively large, and the covering portion can function as a good lithium ion conductive layer. The thickness of the layer can be measured, for example, by X-ray photoelectron spectroscopy (XPS). In addition, it can also be observed and measured in combination with a scanning transmission electron microscope (STEM) and Auger electron spectroscopy (AES) as necessary.
[0035] The surface of the core particle may have a portion where the coating portion is not present. In this case, it is preferable that the coating portion covers 10% or more of the total surface area of the core particle, more preferably 20% or more, and even more preferably 30% or more (this value is also called "coverage rate"). The fact that the surface of the core particle is covered by the coating portion can be confirmed, for example, by observing the surface of the core particle using X-ray photoelectron spectroscopy (XPS) in combination with a scanning transmission electron microscope (STEM) or energy dispersive X-ray analysis (EDS) as necessary, as well as Auger electron spectroscopy (AES), as described above. Furthermore, the thickness of the coating portion that coats the surface of the core particle does not need to be uniform.
[0036] [Core particles] The core particles are not particularly limited as long as they function as an active material. The core particles may contain, for example, a lithium metal composite oxide. As the lithium metal composite oxide, a known lithium metal composite oxide can be used. For example, the lithium metal composite oxide may be any one or a combination of two or more of a layered rock salt type lithium-containing composite oxide represented by the general formula LiMO2 (M represents a metal element), a lithium-excess layered rock salt type lithium-containing composite oxide, a spinel structure lithium-containing composite oxide represented by the general formula LiM2O4 (M represents a metal element), and an olivine structure lithium-containing composite oxide represented by the general formula LiMPO4 (M represents a metal element). However, the lithium metal composite oxide is not limited to these.
[0037] [Core particle A] The core particles are preferably particles made of a lithium transition metal composite oxide having a spinel structure containing Li, Mn, and O and one or more other elements (hereinafter, the core particles are also referred to as "core particles A"). When the active material of the present invention containing the core particles A is used as a positive electrode active material, it has an operating potential of 4.5 V or more based on a metal Li reference potential. "Having an operating potential of 4.5 V or more based on a metal Li reference potential" does not necessarily have to have only an operating potential of 4.5 V or more as a plateau region, but also includes a case where the operating potential is partially 4.5 V or more. Therefore, the present invention is not limited to a positive electrode active material consisting only of a 5 V class positive electrode active material having an operating potential of 4.5 V or more as a plateau region. For example, the active material of the present invention may contain a positive electrode active material having an operating potential of less than 4.5 V as a plateau region. Specifically, it is preferable that the 5V class positive electrode active material occupies, for example, 30 mass% or more, preferably 50 mass% or more, and particularly preferably 80 mass% or more (including 100 mass%) of the positive electrode active material.
[0038] As described above, the core particle A is preferably a particle made of a spinel-type composite oxide containing Li, Mn, and O and two or more other elements. At least one of the "two or more other elements" is preferably a metal element M1 selected from the group consisting of Ni, Co, and Fe, and the other element is preferably a metal element M2 consisting of one or a combination of two or more selected from the group consisting of Na, Mg, Al, K, Ca, Ti, V, Cr, Fe, Co, Cu, Ga, Y, Zr, Nb, Mo, In, Ta, W, Re, and Ce.
[0039] A preferred composition example of the core particle A is LiMnO 4-δ Examples of the lithium-manganese-containing spinel-type composite oxide include those having a crystal structure in which a part of the Mn sites in the above formula is substituted with Li, a metal element M1, and another metal element M2.
[0040] The metal element M1 is a substitution element that mainly contributes to realizing an operating potential of 4.5 V or more based on the metallic Li reference potential, and examples of such elements include Ni, Co, and Fe. The active material A may contain at least one of these elements, and it is particularly preferable that the active material A contains at least one of Ni and Co.
[0041] The metal element M2 is a substitution element that mainly contributes to stabilizing the crystal structure and improving the characteristics. For example, examples of substitution elements that contribute to improving the capacity retention rate include Na, Mg, Al, K, Ca, Ti, V, Cr, Fe, Co, Cu, Ga, Y, Zr, Nb, Mo, In, Ta, W, Re, and Ce, and among them, Na, Mg, Al, K, Ca, Ti, Cr, Fe, Co, Cu, Ga, Y, Zr, Nb, Mo, Ta, and W are preferably used. The metal element M2 may be one or a combination of two or more of the above-mentioned elements. The metal element M2 preferably contains at least one of the above-mentioned elements, and may contain a metal element other than the above-mentioned elements. The metal element M2 contained in the structure is an element type different from the metal element M1.
[0042] An example of the composition of the core particle A is represented by the formula (1): Li x (M1 y M2 z Mn 2-x-y-z )O 4-δ Examples include a spinel-type lithium manganese-containing composite oxide represented by the following formula (1): The metal element M1 and the metal element M2 in the formula (1) are as described above.
[0043] In the formula (1), "x" is preferably 1.00 or more, more preferably 1.01 or more, and even more preferably 1.02 or more. In the formula (1), "x" is preferably 1.20 or less, more preferably 1.10 or less, and even more preferably 1.08 or less. "y" indicating the content of the metal element M1 is preferably 0.20 or more, more preferably 0.30 or more, and even more preferably 0.35 or more. In addition, "y" indicating the content of the metal element M1 is preferably 1.20 or less, more preferably 1.10 or less, and even more preferably 1.05 or less. "z" indicating the content of the metal element M2 is preferably 0.001 or more, more preferably 0.002 or more, more preferably 0.005 or more, and even more preferably 0.100 or more. In particular, by making it 0.100 or more, the cycle characteristics can be improved more effectively. Moreover, "z" indicating the content of the metal element M2 is, for example, preferably 0.400 or less, and more preferably 0.300 or less.
[0044] Another example of the composition of the core particle A is a compound represented by the formula (2): Li x (Ni y M3 z Mn 3-x-y-z )O 4-δ Examples of the spinel-type lithium manganese-containing composite oxide include those represented by the formula (2). In formula (2), "x" is preferably 1.00 or more, more preferably 1.01 or more, and even more preferably 1.02 or more. In formula (2), "x" is preferably 1.20 or less, more preferably 1.10 or less, and even more preferably 1.08 or less. In formula (2), "y" is preferably 0.20 or more, more preferably 0.30 or more, and even more preferably 0.35 or more. In formula (2), "y" is preferably 0.70 or less, more preferably 0.60 or less, and even more preferably 0.55 or less.
[0045] In the formula (2), examples of the metal element M3 include Na, Mg, Al, K, Ca, Ti, V, Cr, Fe, Co, Cu, Ga, Y, Zr, Nb, Mo, In, Ta, W, Re, and Ce, among which Na, Mg, Al, K, Ca, Ti, Cr, Fe, Co, Cu, Ga, Y, Zr, Nb, Mo, Ta, and W are preferred. The metal element M3 may be one or a combination of two or more of the above-mentioned elements. "z" indicating the molar ratio of the metal element M3 is preferably, for example, greater than 0, and more preferably greater than 0.01, and even more preferably 0.05 or more, and even more preferably 0.10 or more. By setting "z" to this lower limit or more, the cycle characteristics can be improved more effectively. In addition, "z" indicating the molar ratio of the metal element M3 is preferably, for example, 0.50 or less, and even more preferably 0.45 or less, and even more preferably 0.40 or less, and even more preferably 0.35 or less.
[0046] In addition, "4-δ" in the above formulas (1) and (2) indicates that oxygen vacancies may be included. In addition, a part of oxygen may be substituted with fluorine or other elements. In this case, δ is preferably 0 or more. In addition, δ is preferably, for example, 0.20 or less, more preferably 0.10 or less, and even more preferably 0.05 or less.
[0047] The core particle A may contain B (boron). In addition to being present in a spinel crystal phase, B may be present as a composite oxide phase containing Ni, Mn, and B. An example of the composite oxide phase containing Ni, Mn, and B is a crystal phase of Ni5MnO4(BO3)2. The presence of the Ni5MnO4(BO3)2 crystal phase can be confirmed by comparing a diffraction pattern obtained by X-ray diffraction (XRD) with PDF (Powder Diffraction File) number "01-079-1029".
[0048] Regarding the content of the complex oxide phase containing Ni, Mn and B, it is preferable to contain the complex oxide phase so that the content of the B element in the core particle A is 0.02 mass% or more, and more preferably, the complex oxide phase is contained so that the content is 0.05 mass% or more. If the content of the B element is 0.02 mass% or more, it is preferable because the discharge capacity at high temperatures can be maintained. In addition, it is preferable to contain the complex oxide phase so that the content of the B element in the core particle A is 0.80 mass% or less, and more preferably, the complex oxide phase is contained so that the content is 0.60 mass% or less, more preferably, 0.30 mass% or less, and particularly preferably, 0.25 mass% or less. If the content of the B element is 0.80 mass% or less, it is preferable because the rate characteristics can be maintained.
[0049] The core particle A may contain components other than the above-mentioned Li, Mn, metal element M1, metal element M2, metal element M3, O, and B. In particular, the other elements may each be contained in an amount of 0.5 mass% or less, because such amounts are considered to have little effect on the performance of the core particle.
[0050] In addition, when the core particle A is fitted to a cubic crystal structure model of the space group Fd-3m (Origin Choice 2), for example, the range of Rwp and S, which indicate the degree of agreement between the observed intensity and the calculated intensity, is Rwp<10 or S<2.5, and thus it can be confirmed that the core particle A has a spinel structure.
[0051] The primary particles of the core particles A are preferably polycrystalline rather than monocrystalline. A monocrystalline refers to a particle in which the primary particle is composed of one crystallite, and a polycrystalline refers to a particle in which multiple crystallites exist within the primary particle. Whether the core particles are polycrystalline or not can be confirmed by observing the cross section of the primary particle using electron backscatter diffraction (EBSD). In the case of a polycrystalline, it can be confirmed that crystals with multiple orientations exist within the primary particle.
[0052] [Core particle B] The core particles are also preferably particles made of a lithium transition metal composite oxide having a layered rock-salt structure containing Li, M element (M includes at least one or a combination of two or more elements selected from the group consisting of Ni, Co, Mn, and Al), and O (hereinafter, the core particles are also referred to as "core particles B"). The active material of the present invention may contain other components as the core particles in addition to the core particles B. However, from the viewpoint of effectively obtaining the characteristics of the core particles B, it is preferable that the core particles B account for, for example, 80% by mass or more, preferably 90% by mass or more, and more preferably 95% by mass or more (including 100% by mass).
[0053] The core particle B is represented by the formula (3): Li 1+x M 1-x O2 (wherein M is a combination of one or more elements selected from the group consisting of Ni, Co, Mn, and Al, or includes a combination of one or more elements selected from the group consisting of Ni, Co, Mn, and Al and a combination of one or more elements selected from the group consisting of transition metal elements present between Groups 3 and 11 of the periodic table, and typical metal elements from Periods 1 to 3 of the periodic table).
[0054] Formula (3): Li 1+x M 1-x In O2, "1+x" is, for example, 0.95 or more, preferably 0.97 or more, and more preferably 0.98 or more. 1+x M 1-x In O2, "1+x" is, for example, preferably 1.09 or less, more preferably 1.07 or less, and even more preferably 1.05 or less.
[0055] "M" in the formula (3) may contain the three elements Mn, Co, and Ni. For example, it may be composed of only the three elements Mn, Co, and Ni, or may contain one or more of the other elements in addition to the three elements, or may have another composition.
[0056] Examples of transition metal elements present among the elements of Groups 3 to 11 of the periodic table, and typical metal elements from Period 1 to Period 3 of the periodic table include Al, V, Fe, Ti, Mg, Cr, Ga, In, Cu, Zn, Nb, Zr, Mo, W, Ta, and Re, and among these, V, Fe, Ti, Mg, Cr, Ga, Cu, Zn, Nb, Zr, Mo, W, and Ta are preferred.
[0057] When "M" in the above formula (3) contains the three elements Mn, Co, and Ni, the molar ratios of Mn, Co, and Ni are preferably Mn:Co:Ni=more than 0.00 and not more than 0.45:more than 0.00 and not more than 0.40:0.30 to 1.00, and more preferably Mn:Co:Ni=0.01 to 0.45:0.01 to 0.40:0.30 to 0.95, and more preferably Mn:Co:Ni=0.05 to 0.40:0.03 to 0.40:0.30 to 0.85, and even more preferably Mn:Co:Ni=0.05 to 0.40:0.03 to 0.40:0.30 to 0.75.
[0058] In the above formula (3), the atomic ratio of the oxygen amount is described as "2" for convenience, but may have some non-stoichiometry. That is, the atomic ratio of the oxygen amount may be "2-δ". "-δ" indicates oxygen deficiency. In this case, δ is preferably 0 or more. In addition, δ is preferably, for example, 0.20 or less, more preferably 0.10 or less, and even more preferably 0.05 or less.
[0059] The core particles B may contain impurities. For example, the impurity elements may be contained in an amount of 0.17% by mass or less. This is because it is believed that such amounts have almost no effect on the properties of the core particles B.
[0060] In addition, when the core particle B is fitted to a hexagonal crystal structure model of space group R-3m, for example, the ranges of Rwp and S, which indicate the degree of agreement between the observed intensity and the calculated intensity, are Rwp<10 or S<2.5, and thus it can be confirmed that the core particle B has a layered structure.
[0061] The primary particles of the core particles B are preferably polycrystalline rather than single crystal, like the core particles A. The definitions of single crystal and polycrystalline are the same as those for the core particles A.
[0062] [Active material] The active material of the present invention is generally in the form of particles, 50 That is, the volume cumulative particle size at 50% by volume of cumulative volume measured by a volume particle size distribution measurement method obtained by a laser diffraction scattering type particle size distribution measurement method is, for example, preferably 0.5 μm or more, more preferably 1.0 μm or more, even more preferably 2.0 μm or more, and even more preferably 2.5 μm or more. 50 For example, it is preferable that the thickness is 15.0 μm or less, more preferably 10.0 μm or less, and particularly preferably 8.0 μm or less. 50 By setting the range above, it is possible to reduce the resistance when Li ions diffuse into the particles of the active material, and as a result, it is possible to improve the end-of-discharge characteristics.
[0063] The active material of the present invention may have a moisture content (mass ppm) up to 250°C measured by the Karl Fischer method of, for example, 3000 ppm or less, 1500 ppm or less, 1000 ppm or less, or 800 ppm or less. The moisture content may be 1 ppm or more, 5 ppm or more, 10 ppm or more, or 20 ppm or more. The amount of moisture contained in the active material is preferably as small as possible from the viewpoint of reducing structural deterioration of the active material due to reaction with lithium and reducing reaction with the electrolyte during battery operation. In order to reduce the amount of moisture contained in the active material as much as possible, the active material may be dried at a temperature of, for example, 300°C, under vacuum, or in an inert atmosphere. The procedure for measuring the moisture content by the Karl Fischer method is as follows. That is, using a Karl Fischer moisture meter capable of coulometric titration, the measurement sample is heated to 110°C, the released moisture content (ppm by mass) is measured, and then the measurement sample is heated to 250°C, the released moisture content (ppm by mass) is measured, and the sum of these values is taken as the moisture content. The measurement is performed in an argon atmosphere. For example, an 860 KF Thermoprep (manufactured by Metrohm) and an 899 Coulometer (manufactured by Metrohm) are used as the measurement device.
[0064] The active material of the present invention can be used in a battery having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer. Specifically, the active material of the present invention can be used in the positive electrode layer or the negative electrode layer, and it is particularly preferable that the positive electrode layer contains the active material of the present invention. The active material of the present invention is preferably used in a solid battery containing a solid electrolyte. In a solid battery, the effect of the present invention can be enjoyed by the presence of a contact portion between the active material of the present invention and the solid electrolyte. The term "solid-state battery" refers not only to solid-state batteries that do not contain any liquid or gel substance as an electrolyte, but also to batteries that contain, for example, 50% by mass or less, 30% by mass or less, or 10% by mass or less of a liquid or gel substance as an electrolyte.
[0065] The active material of the present invention can be used to obtain an electrode binder by mixing it with a solid electrolyte and a conductive material. As the solid electrolyte, it can be the same as the solid electrolytes used in general solid-state batteries. For example, sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, halide solid electrolytes, etc. can be mentioned. Among them, it is preferable to use a sulfide solid electrolyte containing sulfur (S) element. The sulfide solid electrolyte may, for example, contain Li element and S element and have lithium ion conductivity, or may contain Li element, P element and S element and have lithium ion conductivity. The sulfide solid electrolyte may be any of a crystalline material, glass ceramics, and glass. The sulfide solid electrolyte may have a crystal phase of an argyrodite-type structure. Examples of such sulfide solid electrolytes include Li2S-P2S5, Li2S-P2S5-LiX (where "X" represents one or more halogen elements), Li2S-P2S5-P2O5, Li2S-Li3PO4-P2S5, Li3PS4, Li4P2S6, Li 10 GeP2S 12 、Li 3.25 Ge 0.25 P 0.75 S4、Li7P3S 11 、Li 3.25 P 0.95 S4、Li 7-x PS 6-x X x (a solid electrolyte having a crystal phase of an argyrodite-type structure, "X" represents one or more halogen elements, and 0.2 < x < 2.0 or 0.2 < x < 1.8). etc. can be mentioned. As the conductive material, for example, electronically conductive carbonaceous materials such as carbon black and acetylene black can be used.
[0066] The electrode binder can be used to produce an electrode (positive electrode layer and / or negative electrode layer) by mixing it with a solvent and a binder to prepare a paste, and applying and drying the paste on a current collector such as an aluminum foil. The electrode thus produced contains the electrode binder and the binder.
[0067] [Method for producing active material] Methods for producing active materials are roughly divided into methods for producing core particles and methods for forming coating portions on the surfaces of core particles. An example of the method for producing the core particles includes a manufacturing method including a raw material mixing step, a wet grinding step, a granulation step, a firing step, a heat treatment step, a washing / drying step and a grinding step, although this manufacturing method is merely a preferred example and is not limited to this manufacturing method.
[0068] The method for forming the coating portion is appropriately selected depending on the types of the first compound and the second compound that constitute the coating portion. For example, when the coating portion contains lithium sulfate as the first compound and metaphosphate or orthophosphate as the second compound, it is preferable to dry-mix a mixed powder containing the core particles (which may be in the form of a powder or other forms), the powder of the first compound, and the powder of the second compound, and to arrange the coating portion containing the compounds on the surface of the core particles. Alternatively, the core particles (which may be in the form of a powder or other forms), the powder of the first compound, and the powder of the second compound may be dry-mixed simultaneously. In either case, it is preferable to perform the dry mixing while cooling, since this can suppress an increase in the initial resistance of a solid-state battery, which is a battery that is prone to high initial resistance, and further effectively improve storage characteristics. When the dry mixing is performed with cooling, for example, a dry mixer equipped with a water-cooling jacket can be used. The temperature of the mixed powder during dry mixing is preferably maintained at 10°C or higher and 50°C or lower.
[0069] The coating portion contains, for example, Li as the first compound. x NbO y In the case where the second compound contains a metaphosphate or an orthophosphate, Li is added to the surface of the powder of the core material particle by a wet method. x NbO y Then Li x NbO yThe core particles on which the Li is arranged can be dry-mixed with a metaphosphate or an orthophosphate. Conversely, the core particles can be dry-mixed with a metaphosphate or an orthophosphate, and then Li is applied to the surface of the core particles on which the Li is arranged by a wet method. x NbO y In any case, it is preferable to perform the dry mixing while cooling as described above, from the viewpoint of suppressing an increase in the initial resistance of the solid-state battery, which is a battery that is prone to have a high initial resistance, and further effectively improving the storage characteristics.
[0070] As described above, when forming the coating portion, it is preferable to dry mix the core particles with at least one of the first compound and the second compound which are compounds constituting the coating portion while cooling, and it is particularly preferable to dry mix the second compound while cooling. In either case of dry mixing the core particles with one of the first compound and the second compound, or dry mixing the core particles with both the first compound and the second compound, the ratio of the second compound to the first compound is preferably 0.050 or more, more preferably 0.100 or more, even more preferably 0.125 or more, and even more preferably 0.250 or more, expressed as the mass ratio of the second compound to the first compound. Also, it is preferably 20.000 or less, more preferably 10.000 or less, even more preferably 8.000 or less, and even more preferably 4.000 or less.
[0071] Li as the first compound x NbO yWhen the core particles or the core particles having the metaphosphate or orthophosphate disposed thereon are placed in a mixed solution in which the lithium raw material and the Nb element raw material are dissolved in a solvent, the core particles or the core particles having the metaphosphate or orthophosphate disposed thereon may be added and dried under a predetermined condition. For example, the water-soluble Nb element salt and the lithium raw material are dissolved in water to prepare a surface treatment liquid, and the core particles or the core particles having the metaphosphate or orthophosphate disposed thereon are put into the surface treatment liquid, kneaded to form a slurry, and then dried to produce the surface treatment liquid. In this case, the surface treatment liquid is heated to promote dissolution of the water-soluble Nb element salt and the lithium raw material and to prevent Li x NbO y The heating temperature is preferably, for example, 80° C. or higher and 100° C. or lower.
[0072] In relation to the above-mentioned embodiments, the present invention further discloses the following active material, electrode mixture, electrode and battery, and method for producing the active material. [1] An active material having a core particle and a coating portion disposed on a surface of the core particle, the coating portion includes a first compound and a second compound, The first compound is M a It is an oxide containing the element, The second compound is M b It is an oxide containing the element, M b The element contains phosphorus (P), The active material, wherein the first compound and the second compound are different compounds. [2] M a The elements of the periodic table Elements in group 2, period 3 to period 6 Elements belonging to groups 3 to 12 of the 4th period, Elements belonging to groups 3 to 8 of the fifth period, Elements belonging to groups 5 to 6 of the 6th period, Elements belonging to the second to fourth periods of group 13, Elements in group 14, period 3 to period 6 Elements belonging to the 2nd to 6th periods of group 15, Elements belonging to the 2nd to 6th periods of Group 16, Lanthanides, elements with atomic numbers 57 and 58, and Lithium (Li) element, The active material according to [1], which contains at least one element selected from the group consisting of [3] M b The active material according to [1] or [2], further comprising at least one element selected from the group consisting of lithium (Li), aluminum (Al), titanium (Ti), germanium (Ge), iron (Fe), cobalt (Co), bismuth (Bi), boron (B), yttrium (Y) and zirconium (Zr). [4] The active material according to any one of [1] to [3], wherein the second compound is contained in an amount of 0.05% by mass or more based on the active material. [5] The active material according to any one of [1] to [4], wherein the core particles contain at least one selected from the group consisting of a lithium transition metal composite oxide having a spinel structure, a lithium transition metal composite oxide having a layered rock salt structure, and a lithium-containing composite oxide having an olivine structure. [6] The active material according to any one of [1] to [5], wherein the coating portion has a thickness of 1 nm or more and 100 nm or less. [7] The active material according to any one of [1] to [6], which has a moisture content of 3000 ppm or less up to 250° C. as measured by the Karl Fischer method. [8] An electrode mixture comprising the active material according to any one of [1] to [7], a solid electrolyte, and a conductive material. [9] An electrode comprising the electrode mixture according to [8] and a binder.
[10] A battery having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer, A battery, wherein the positive electrode layer contains the active material according to any one of [1] to [7].
[11] A method for producing an active material having a core particle and a coating portion disposed on a surface of the core particle, comprising the steps of: the coating portion includes a first compound and a second compound, dry-mixing the core particles with at least one of a first compound and a second compound while cooling; The first compound is M a It is an oxide containing the element, The second compound is M b It is an oxide containing the element, M b The element contains phosphorus (P), A method for producing an active material, wherein the first compound and the second compound are different compounds.
[12] The method according to
[11] , wherein the ratio of the second compound to the first compound is 0.050 or more and 20,000 or less. EXAMPLES
[0073] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. Unless otherwise specified, "%" means "% by mass".
[0074] Example 1 (1) Preparation of core particles As the core particles, a spinel-type lithium transition metal composite oxide (hereinafter also referred to as "LNMO") having a composition of Li: 4.1%, Mn: 41.3%, Ni: 13.3%, and Ti: 5.4% was prepared.
[0075] (2) Formation of the Covering Part 1 29.5g of LiOH·H2O was dissolved in 214g of water to obtain a lithium hydroxide aqueous solution. After this aqueous solution was heated to 100°C, 2mL of 30% hydrogen peroxide and 0.862g of niobium hydroxide were dissolved in the aqueous solution. The concentration of the solution was adjusted so that the lithium niobate in the coating portion was 1.3% relative to the active material. After stirring the aqueous solution for 30 minutes while keeping it at 100°C, 50g of core material particles were added to the aqueous solution and stirred for another 20 minutes. Next, the heating and stirring were stopped and the solution was left to stand, and the active material was allowed to settle in the aqueous solution. The aqueous solution was decanted, and the product was washed twice with 200mL of 0.14mol / L lithium sulfate solution. The product was then dried at 80°C. In this way, an oxide containing lithium and niobium (Li8Nb6O 19 ) was produced.
[0076] (3) Formation of the coating 2 Li8Nb6O on the surface 19 The core particles on which the above-mentioned was formed and lithium metaphosphate were mixed using a dry particle composite device NOB-MINI manufactured by Hosokawa Micron Corporation, and the lithium metaphosphate was attached to the surface of the core particles to form Li8Nb6O 19 and a coating portion containing lithium metaphosphate was formed. The amount of the core particles and lithium metaphosphate was adjusted so that the amount of lithium metaphosphate relative to the active material was 2.5%. During mixing, the device was cooled and maintained at 30°C. In this manner, active material particles were obtained.
[0077] Example 2 In Example 1, step (2) was not performed. In step (3), the core particles, lithium sulfate, and lithium metaphosphate were mixed to form a coating portion containing lithium sulfate and lithium metaphosphate on the surface of the core particles. The amounts of the core particles, lithium sulfate, and lithium metaphosphate were adjusted so that the lithium sulfate was 5.0% and the lithium metaphosphate was 2.5% relative to the active material. During mixing, the device was cooled and maintained at 30°C. Except for this, the active material particles were obtained in the same manner as in Example 1.
[0078] Example 3 In Example 1, step (2) was not performed. In step (3), core particles, lithium sulfate, and aluminum orthophosphate were mixed to form a coating containing lithium sulfate and aluminum orthophosphate on the surface of the core particles. The amounts of core particles, lithium sulfate, and aluminum orthophosphate were adjusted so that lithium sulfate was 5.0% and aluminum orthophosphate was 2.5% relative to the active material. During mixing, the device was cooled and maintained at 30°C. Other than this, active material particles were obtained in the same manner as in Example 1.
[0079] Example 4 In Example 1, step (2) was not performed. In step (3), the core particles, lithium sulfate, and Li 1.4 Al 0.4 Ti 1.6 (PO4)3, and lithium sulfate and Li 1.4 Al 0.4 Ti 1.6 A coating containing (PO4)3 was formed. Core particles, lithium sulfate, Li 1.4 Al 0.4 Ti 1.6 The amount of (PO4)3 is 5.0% lithium sulfate and 5.0% Li 1.4 Al 0.4 Ti 1.6 The content of (PO4)3 was adjusted to 2.5%. During mixing, the device was cooled and maintained at 30° C. Except for this, the same procedure as in Example 1 was carried out to obtain active material particles.
[0080] [Examples 5 to 9] The amounts of lithium sulfate and lithium metaphosphate mixed with the core particles were changed in Example 2. Except for this, active material particles were obtained in the same manner as in Example 2. The ratios of lithium sulfate and lithium metaphosphate to the core particles were as shown in Table 1 below.
[0081] Comparative Example 1 Step (3) was not carried out in Example 1. Except for this, the same procedure as in Example 1 was carried out to obtain active material particles.
[0082] Comparative Example 2 Step (2) was not carried out in Example 1. Except for this, the same procedure as in Example 1 was carried out to obtain active material particles.
[0083] Comparative Example 3 In step (3) of Example 2, the core particles and lithium sulfate were mixed to form a coating portion containing lithium sulfate on the surface of the core particles, but the other procedures were the same as in Example 2 to obtain active material particles.
[0084] [Rating 1] For the active materials obtained in the examples, the thickness and coverage of the coating portion were measured by the following method. Furthermore, the moisture content was measured by the above-mentioned method. The results are shown in Table 1 below. In the table, blanks indicate that no measurement was performed.
[0085] [Thickness of Covering Part] The thickness of the coating was measured using PHI Quantes, an XPS device manufactured by ULVAC-PHI Inc. Specifically, Ar ion sputtering was performed and XPS measurement was performed to obtain a depth profile of the active material. The sputtering depth at which the area of the peak derived from the elements specific to the coating, not the main elements constituting the core particles, was halved compared to before sputtering was converted into the sputtering depth of SiO2, and the converted value was taken as the thickness of the coating. The conditions used for the measurement are as follows. Excitation X-ray: Monochromatic Al line (1486.7 eV) Output: 50W Acceleration voltage: 15 kV X-ray irradiation diameter: 200μmφ Measurement area: 1000μm x 300μm Take Angle: 45° Pass energy: 26.0 eV Energy step: 0.1 eV The XPS data was analyzed using data analysis software (ULVAC-PHI XPS analysis software "MultiPakVer9.9"). The background mode used was Iterated Shirley.
[0086] [Covering rate of the coated part] The coverage rate was measured by quantitative analysis using XPS. It was calculated from the ratio of the quantitative value of the element present only in the coating to the sum of the quantitative values of the elements present only in the coating and the elements present only in the core particle. For example, when the core particle is LNMO and the coating uses lithium sulfate as the first compound and lithium metaphosphate as the second compound, the coverage rate can be calculated by (P+S) / (Ni+Mn+Ti+P+S)×100. The measurement conditions were the same as when the thickness of the coating was measured.
[0087] [Evaluation 2] Using the active materials obtained in the Examples and Comparative Examples, solid-state batteries were manufactured by the following method, and the initial resistance and the resistance increase rate after storage at 60° C., which is an index of storage characteristics, were measured. The results are shown in Table 1 below.
[0088] [Initial resistance and resistance after storage at 60℃] The active materials obtained in the examples and comparative examples were used as the positive electrode active material, and graphite (Gr) powder was used as the negative electrode active material. A sulfide solid electrolyte having an argyrodite structure was used as the solid electrolyte powder. The positive electrode active material, the solid electrolyte powder, and a carbon-based material serving as a conductive assistant were mixed in a mortar at a mass ratio of 70:27:3 to prepare a positive electrode mixture powder. In addition, the negative electrode active material and the solid electrolyte powder were mixed in a mortar at a mass ratio of 1:1 to prepare a negative electrode mixture powder. The lower opening of a polypropylene cylinder (opening diameter 10.5 mm, height 18 mm) with open top and bottom was blocked with a positive electrode (made of SUS), solid electrolyte powder was placed on top of it, and it was blocked with a negative electrode (made of SUS), and then uniaxially pressed at 10 MPa to form a solid electrolyte layer. Next, the negative electrode was temporarily removed, and a negative electrode mixture powder was placed on the solid electrolyte layer and blocked again with the negative electrode. Then, the cylinder was turned upside down, the positive electrode was temporarily removed, and a positive electrode mixture powder was placed on the solid electrolyte layer and blocked again with the positive electrode, and then uniaxially pressed at 60 MPa to produce a solid battery consisting of a three-layer structure of a positive electrode mixture, a solid electrolyte layer, and a negative electrode mixture.
[0089] [Resistance increase rate after storage at 60℃] A charge / discharge test was carried out using the produced solid-state battery as follows: In detail, the solid-state battery was placed in an environmental tester in which the environmental temperature for charging and discharging the battery was set to 25° C., and prepared for charging and discharging, and was left to stand until the temperature of the solid-state battery reached the environmental temperature. Next, the battery was charged at a constant current and constant potential to 5.0 V at 0.1 C, and then discharged at a constant current to 3.0 V at 0.1 C, and this cycle was repeated for three cycles. After that, the battery was charged until the state of charge (SOC) reached 50%, and the resistance value before the storage test was measured by impedance measurement. The resistance value before the storage test was taken as the initial resistance value. The battery was then charged at a constant current and constant potential to 4.9 V at 0.1 C, discharged at a constant current to 3.0 V at 0.1 C, and then charged at a constant current and constant potential to 4.9 V at 0.1 C again. The battery was charged at a constant current and constant potential to 4.9 V at 0.1 C, and placed in a thermostatic chamber set at 60 ° C. and stored for 168 hours. After 168 hours, the solid battery was removed, and the battery was returned to room temperature, and then placed in an environmental tester set to 25 ° C., and discharged at a constant current to 3.0 V at 0.1 C. Thereafter, the battery was charged at a constant current and constant potential to 4.9 V at 0.1 C, and discharged at a constant current to 3.0 V at 0.1 C. After charging until the SOC was 50%, the resistance value after the storage test was measured by impedance measurement. The resistance value after the storage test was calculated relative to the resistance value before the storage test, and this value was taken as the resistance increase rate after storage at 60°C.
[0090] [Table 1]
[0091] As is clear from the results shown in Table 1, the solid-state batteries obtained using the active materials obtained in each Example exhibited low initial resistance values, and the increase in the resistance increase rate after storage at 60°C was suppressed.
Claims
1. An active material having a core particle and a coating portion disposed on a surface of the core particle, the coating portion includes a first compound and a second compound, The first compound is M a It is an oxide containing the element, The second compound is M b It is an oxide containing the element, M b The element includes phosphorus (P), The active material, wherein the first compound and the second compound are different compounds.
2. M a The elements of the periodic table Elements belonging to the 3rd to 6th periods of Group 2, Elements belonging to groups 3 to 12 of the 4th period, Elements belonging to groups 3 to 8 of the fifth period, Elements belonging to groups 5 to 6 of the 6th period, Elements belonging to the second to fourth periods of Group 13, Elements belonging to the 3rd to 6th periods of Group 14, Elements belonging to the second to sixth periods of Group 15, Elements belonging to the second to sixth periods of Group 16, Lanthanides, elements with atomic numbers 57 and 58, and Lithium (Li) element, The active material according to claim 1 , comprising at least one element selected from the group consisting of:
3. M b 2. The active material of claim 1, wherein the elements further comprise at least one of the following elements: lithium (Li), aluminum (Al), titanium (Ti), germanium (Ge), iron (Fe), cobalt (Co), bismuth (Bi), boron (B), yttrium (Y), and zirconium (Zr).
4. The active material according to claim 1 , wherein the second compound is contained in an amount of 0.05% by mass or more based on the active material.
5. 2. The active material according to claim 1, wherein the core particles contain at least one selected from the group consisting of a lithium transition metal composite oxide having a spinel structure, a lithium transition metal composite oxide having a layered rock salt structure, and a lithium-containing composite oxide having an olivine structure.
6. The active material according to claim 1 , wherein the coating portion has a thickness of 1 nm or more and 100 nm or less.
7. 2. The active material according to claim 1, which has a moisture content of 3000 ppm or less at up to 250° C. as measured by the Karl Fischer method.
8. An electrode mixture comprising the active material according to claim 1 , a solid electrolyte, and a conductive material.
9. An electrode comprising the electrode mixture according to claim 8 and a binder.
10. A battery having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer, A battery, wherein the positive electrode layer comprises the active material according to claim 1 .
11. A method for producing an active material having a core particle and a coating portion disposed on a surface of the core particle, comprising the steps of: the coating portion includes a first compound and a second compound, dry-mixing the core particles with at least one of a first compound and a second compound while cooling; The first compound is M a It is an oxide containing the element, The second compound is M b It is an oxide containing the element, M b The element includes phosphorus (P), A method for producing an active material, wherein the first compound and the second compound are different compounds.
12. The method according to claim 11, wherein the ratio of the second compound to the first compound is 0.050 or more and 20,000 or less.
Citation Information
Patent Citations
Positive pole material and battery
WO2022019099A1
Lithium-transition metal oxide powder and manufacturing method thereof, cathode active material for lithium ion battery, and lithium ion secondary battery
JP2012074240A
Positive electrode active material for lithium secondary batteries, positive electrode for lithium secondary batteries, lithium secondary battery, method for producing positive electrode active material for lithium secondary batteries, and method for manufacturing lithium secondary battery
WO2017094416A1
Cited By
Positive electrode active material for non-aqueous electrolyte secondary battery, method of producing said positive electrode active material, and non-aqueous electrolyte secondary battery
WO2026186896A1