Resin composition, film, film set, optical waveguide, optoelectric composite substrate, and electronic component

The resin composition and film with tailored properties address embeddability and thermal stability issues in opto-electrical composite substrates, enhancing optical waveguide performance by reducing voids and misalignment.

JP2024145148APending Publication Date: 2024-10-15SUMITOMO BAKELITE CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023057398
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Conventional opto-electrical composite substrates face challenges in achieving sufficient embeddability of optical waveguide cladding in vias and suffer from thermal contraction leading to misalignment and optical loss during high-temperature processes.

Method used

A resin composition and film with specific viscosity and modulus ranges are developed, incorporating polyimide resin and a compound with a cyclic ether structure, which enhance embeddability and suppress thermal shrinkage, ensuring improved optical waveguide performance.

Benefits of technology

The resin composition and film provide enhanced embeddability and thermal stability, reducing voids and misalignment, thereby improving optical waveguide performance and reducing optical loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145148000001_ABST
    Figure 2024145148000001_ABST
Patent Text Reader

Abstract

To provide a resin composition and a film which can yield an optical waveguide clad having improved embedding properties.SOLUTION: A resin composition is usable in an optical waveguide clad, wherein when a complex viscosity of a resin layer composed of the resin composition is measured by a melting viscoelasticity measurement test under the conditions of a measurement frequency of 10 rad / sec, a temperature range of 23°C to 200°C and a temperature rising speed of 3°C / min, a complex viscosity η* (10 rad / sec) at 100°C is 1.0×103 Pa s or more and 1.0×105 Pa s or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a film, a film set, an optical waveguide, an optical / electrical composite substrate, and an electronic component. [Background technology]

[0002] 2. Description of the Related Art In recent years, there has been a demand for components capable of realizing more advanced information communication, such as larger capacity information and faster information communication speeds, in information and communication devices. As one such component, an optical / electrical composite substrate has been considered.

[0003] An example of the optical / electrical composite substrate is one in which an optical waveguide is provided on a substrate. As optical waveguide technologies, for example, the technologies described in Patent Documents 1 to 3 can be mentioned.

[0004] Patent Document 1 describes an optical waveguide formed by laminating a core layer made of a polymer and a clad layer made of a polymer on a substrate, characterized in that the core layer is sandwiched in a direction perpendicular to the surface of the substrate between clad layers having a smaller refractive index than the clad layers that sandwich the core layer in a direction parallel to the surface of the substrate. According to the optical waveguide described in Patent Document 1, even if a polyimide having a large birefringence is used, an optical waveguide having a small PDL, which is easy to fabricate and has a low loss is provided, and further, it is described that the use of this waveguide can provide an optical integrated circuit and an optical module having excellent characteristics.

[0005] Patent Document 2 describes an opto-electrical hybrid board comprising a flexible circuit board in which electrical wiring having mounting pads is formed on the surface of an insulating layer, an element mounted on the mounting pad, and an optical waveguide laminated on the back surface of the insulating layer, wherein the flexible circuit board is a flexible double-sided circuit board in which electrical wiring is also formed on the back surface of the insulating layer, and a metallic reinforcing layer is formed by plating on at least the portion of the electrical wiring on the back surface that corresponds to the mounting pad, and the optical waveguide is in contact with the metallic reinforcing layer. According to the optical-electrical hybrid board described in Patent Document 2, a metallic reinforcing layer is adhered to an insulating layer of a flexible circuit board without an adhesive layer, and it is described that an optical-electrical hybrid board can be provided in which elements are properly mounted while suppressing deformation due to a pressure load when the elements are mounted by the metallic reinforcing layer.

[0006] Patent Document 2 describes a method of preparing a substrate in which copper foil 21 is formed on the front and back surfaces of an insulating layer 1 made of a resin such as polyimide, and forming through holes 1a and via holes 1b for an optical path in the substrate (see paragraph 0023 of Patent Document 2). It also describes a flexible double-sided circuit board E in which a metallic reinforcing layer M is formed (see paragraph 0028 of Patent Document 2). The flexible double-sided circuit board E includes the above substrate. Furthermore, Patent Document 2 describes that an undercladding layer 6 is formed on the back side of a flexible double-sided circuit board E in contact with a metal reinforcing layer M that covers the electrical wiring 2B on the back side, and describes that examples of a molding material for the undercladding layer 6 include photosensitive resins and thermosetting resins (see paragraph 0029 of Patent Document 2). According to Figures 4 to 6 of Patent Document 2, it can be seen that the molding material for the undercladding layer 6 is filled into a recess formed in the flexible double-sided circuit board E on which the metal reinforcing layer M is formed.

[0007] Patent Document 3 describes an optoelectronic wiring board that is formed by integrating a rigid section in which conductor circuits and insulating layers are laminated on both sides of a substrate with one or more bendable flex sections, wherein the rigid section is formed with external connection terminals for mounting optical elements and / or package substrates on which optical elements are mounted, and at least one of the flex sections is formed with optical wiring. According to the optoelectronic wiring board of Patent Document 3, it is described that large-volume information processing and high-speed information processing can be suitably performed without increasing the size of the wiring board.

[0008] Patent Document 3 describes that the rigid section has an optical signal transmitting region formed therein, and that the optical signal transmitting region is filled with a resin composition (see claims 4 and 5 of Patent Document 3). Furthermore, Patent Document 3 describes that the optical signal transmitting region is formed so as to penetrate all of the substrates and insulating layers that constitute the rigid section (see claim 6 of Patent Document 3).

[0009] Furthermore, Patent Document 3 describes a substrate 221 consisting of an optical waveguide film 250 and a surrounding resin layer (insulating layer) 221a, and describes that the resin layer 221a constitutes part of the optical signal transmitting regions 242a, 242b (see paragraph 0033 of Patent Document 3). [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2006-119659 A [Patent Document 2] JP 2014-238455 A [Patent Document 3] JP 2006-140233 A Summary of the Invention [Problem to be solved by the invention]

[0011] In conventional technology relating to optoelectronic composite substrates, there are known optoelectronic composite substrates in which recesses and through holes formed in a substrate are filled with a resin composition (see, in particular, Patent Documents 2 and 3).

[0012] An example of a manufacturing process for an optoelectronic composite substrate is a process for integrating a substrate having vias formed therein with a film for optical waveguide clad. In this process, the vias formed in the substrate must be embedded with the optical waveguide clad. In other words, resin compositions and films that can be used for optical waveguide clads are required to have properties that enable the optical waveguide clad to be sufficiently embedded in the vias (hereinafter, "embedding ability" refers to the property of the degree to which the optical waveguide clad can be embedded in the vias).

[0013] The present invention has been made in consideration of the above circumstances, and provides a resin composition and a film that are capable of producing an optical waveguide clad with improved embeddability. [Means for solving the problem]

[0014] According to the present invention, there are provided a resin composition, a film, a film set, an optical waveguide, an optical / electrical composite substrate, and an electronic component, as shown below.

[0015] [1] A resin composition that can be used for an optical waveguide clad, The complex viscosity of the resin layer made of the resin composition is measured by a melt viscoelasticity test under the conditions of a measurement frequency of 10 rad / sec, a temperature range of 23° C. to 200° C., and a heating rate of 3° C. / min. The complex viscosity η*(10 rad / sec) at 100° C. is 1.0×10 3 Pa·s or more 1.0×10 5 The resin composition has a viscosity of 0.01 Pa·s or less. [2] The resin composition according to the above item [1], wherein when a complex viscosity of a resin layer made of the resin composition is measured by a melt viscoelasticity test under conditions of a measurement frequency of 10 rad / sec, a temperature range of 23°C to 200°C, and a heating rate of 3°C / min, the temperature at which the complex viscosity η*(10 rad / sec) is a minimum is 70°C or higher and 180°C or lower. [3] The complex viscosity of the resin layer made of the resin composition is measured by a melt viscoelasticity test under the conditions of a measurement frequency of 100 rad / sec, a temperature range of 23° C. to 200° C., and a heating rate of 3° C. / min. The complex viscosity η*(100 rad / sec) at 100° C. is 0.1×10 2 Pa·s or more 5.0×10 4 The resin composition according to [1] or [2] above, having a viscosity of 0.01 Pa·s or less. [4] The complex viscosity of the resin layer made of the resin composition is measured by a melt viscoelasticity test under the conditions of a measurement frequency of 1 rad / sec, a temperature range of 23° C. to 200° C., and a heating rate of 3° C. / min. The complex viscosity η*(1 rad / sec) at 100° C. is 1.0×10 4 Pa·s or more 8.0×10 5 The resin composition according to any one of the above [1] to [3], having a viscosity of not more than Pa·s. [5] The resin composition according to any one of the above [1] to [4], wherein a cured product of the resin composition has a storage modulus E' at 200°C of 0.1 GPa or more and 3.0 GPa or less. [6] The resin composition according to any one of [1] to [5], wherein a cured product of the resin composition has a glass transition temperature of 150°C or higher and 400°C or lower, as calculated from the top peak of tan δ by a dynamic mechanical analysis (DMA). [7] The resin composition according to any one of the above [1] to [6], comprising a polyimide resin (A) and a compound (B) having a cyclic ether structure. [8] The resin composition according to [7] above, further comprising a curing agent (C). [9] A film that can be used for an optical waveguide clad, A resin layer is provided, The complex viscosity of the resin layer was measured by a melt viscoelasticity test under the conditions of a measurement frequency of 10 rad / sec, a temperature range of 23°C to 200°C, and a heating rate of 3°C / min. The complex viscosity η*(10 rad / sec) at 100°C was 1.0×10 3Pa·s or more 1.0×10 5 The film is below Pa·s.

[10] The film according to [9], wherein, when the complex viscosity of the resin layer is measured by a melt viscoelasticity test under conditions of a measurement frequency of 10 rad / sec, a temperature range of 23°C to 200°C, and a heating rate of 3°C / min, the temperature at which the complex viscosity η*(10 rad / sec) is a minimum is 70°C or higher and 180°C or lower.

[11] The complex viscosity of the resin layer is measured by a melt viscoelasticity test under the conditions of a measurement frequency of 100 rad / sec, a temperature range of 23°C to 200°C, and a heating rate of 3°C / min. The complex viscosity η*(100 rad / sec) at 100°C is 0.1×10 2 Pa·s or more 5.0×10 4 The film according to [9] or

[10] , wherein the elastic modulus is 0.01 Pa s or less.

[12] The complex viscosity of the resin layer was measured by a melt viscoelasticity test under the conditions of a measurement frequency of 1 rad / sec, a temperature range of 23°C to 200°C, and a heating rate of 3°C / min. The complex viscosity η*(1 rad / sec) at 100°C was 1.0×10 4 Pa·s or more 8.0×10 5 The film according to any one of the above [9] to

[11] , having a viscosity of not more than Pa·s.

[13] The film according to any one of the above [9] to

[12] , wherein a cured product obtained by curing the resin layer has a storage modulus E' at 200°C of 0.1 GPa or more and 3.0 GPa or less.

[14] The film according to any one of the above [9] to

[13] , wherein a glass transition temperature of a cured product obtained by curing the resin layer, calculated from a top peak of tan δ by a dynamic mechanical analyzer (DMA), is 150°C or higher and 400°C or lower.

[15] Further, the device includes a base film, The film according to any one of the above [9] to

[14] , wherein the resin layer is provided on the base film.

[16] The film according to

[15] above, wherein the resin constituting the base film contains at least one or more types selected from the group consisting of polyimide and polyethylene terephthalate.

[17] The film according to any one of the above [9] to

[16] , which is a dry film.

[18] A film set that can be used for an optical waveguide clad, comprising: A first film and a second film, A film set, wherein at least one of the first film and the second film is the film according to any one of [9] to

[17] above.

[19] An optical waveguide in which a first clad layer, a core layer, and a second clad layer are laminated in this order, An optical waveguide, wherein at least one of the first cladding layer and the second cladding layer contains the resin composition according to any one of [1] to [8] above.

[20] A substrate; An optical / electrical composite substrate comprising: the optical waveguide according to

[19] provided on the substrate. [twenty one] An electronic component comprising the optical / electrical composite substrate described in

[20] . Effect of the Invention

[0016] According to the present invention, it is possible to provide a resin composition and a film which are capable of producing an optical waveguide clad having improved embeddability. [Brief description of the drawings]

[0017] [Figure 1] 1 is a cross-sectional view showing a schematic example of a structure of an optical / electrical composite substrate according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, embodiments of the present invention will be described with reference to the drawings. Furthermore, a numerical range of "A to B" represents A or more and B or less unless otherwise specified.

[0019] 1 is a cross-sectional view showing a schematic example of the structure of an optoelectronic composite substrate according to the present embodiment, the drawing being a simplified view and not in accordance with the actual dimensional ratio. As shown in FIG. 1, the optical / electrical composite substrate 200 has an optical waveguide 100 provided on a substrate 110. The optical waveguide 100 has a first clad layer 20, a core layer 30, and a second clad layer 40 laminated in this order. A mirror 50 on the light-emitting element side and a mirror 60 on the light-receiving element side are formed on the optical waveguide 100. Vias 140 (140a, 140b) are formed on the substrate 110 (note that the vias 140 shown in FIG. 1 are embedded in the first clad layer 20). A light-emitting element 120 and a light-receiving element 130 are provided on the side of the substrate 110 opposite to the optical waveguide 100 side.

[0020] Providing the optical waveguide 100 on the substrate 110 includes, for example, a process of laminating the substrate 110 in which the vias 140 are formed and a film for forming the first cladding layer 20, and integrating them by heating and pressurizing. In the integration process, the vias 140 need to be embedded by the first cladding layer 20.

[0021] According to the study of the present inventors, it was found that with a conventional material for forming an optical waveguide clad, the optical waveguide clad cannot be sufficiently embedded in a via formed in a substrate, and a recess may be generated on the surface of the optical waveguide clad opposite to the substrate side (i.e., the core layer side of the optical waveguide clad) or a void may be generated in the via. It was also found that when the above-mentioned recess or void is generated in the optoelectronic composite substrate, an optical loss occurs at the interface of the recess or void. The present invention has been made in consideration of the above circumstances, and provides a resin composition and a film that can provide an optical waveguide clad with improved embeddability.

[0022] The propagation path of light in the photoelectric composite substrate 200 will be specifically described with reference to Fig. 1. The light emitted from the light emitting portion of the light emitting element 120 passes through via 140a formed in the substrate 110, enters the mirror 50 on the light emitting element side, and is transmitted through the core layer 30. Thereafter, it enters the mirror 60 on the light receiving element side, passes through via 140b formed in the substrate 110, and enters the light receiving element 130. The arrows in Fig. 1 are a schematic representation of the propagation of light.

[0023] When mounting an optoelectronic composite board on an electronic component, the process may include a step of exposing the optoelectronic composite board to high temperatures (e.g., 230°C to 270°C), such as a reflow soldering process. According to the study by the present inventors, it has been found that in a conventional optoelectronic composite board, the optical waveguide may be thermally shrunk when the optoelectronic composite board is exposed to high temperatures. It has been found that such thermal shrinkage of the optical waveguide may cause a positional deviation of the mirror. It has also been found that when the mirror is misaligned, light cannot propagate along the expected optical path, and normal light propagation is not possible. Furthermore, according to the present invention, it is possible to provide a resin composition and a film which are capable of producing an optical waveguide with suppressed thermal shrinkage.

[0024] [Resin composition] The resin composition of the present embodiment is a resin composition that can be used for an optical waveguide clad, and when the complex viscosity of a resin layer made of the resin composition is measured by a melt viscoelasticity test under the conditions of a measurement frequency of 10 rad / sec, a temperature range of 23° C. to 200° C., and a heating rate of 3° C. / min, the complex viscosity η*(10 rad / sec) at 100° C. is 1.0×10 3 Pa·s or more 1.0×10 5 It is less than Pa·s.

[0025] As described above, there is a demand for a resin composition that can provide an optical waveguide clad with improved embeddability. Here, the present inventors have found for the first time that embeddability can be improved by setting the complex viscosity η* (10 rad / sec) at 100° C. of a resin layer made of a resin composition within a specific range.

[0026] The complex viscosity η*(10 rad / sec) of the resin layer made of the resin composition of the present embodiment at 100° C. is preferably 2.0×10 3 Pa s or more, preferably 3.0×10 3 Pa s or more, more preferably 4.0×10 3 Pa s or more, more preferably 5.0×10 3 From the viewpoint of further improving embeddability, it is preferably 9.5×10 4 Pa s or less, preferably 9.3×10 4 Pa s or less, more preferably 9.0×10 4 Pa s or less, more preferably 8.8×10 4 It is less than Pa·s.

[0027] When the complex viscosity of a resin layer made of the resin composition of this embodiment is measured by a melt viscoelasticity test under conditions of a measurement frequency of 10 rad / sec, a temperature range of 23°C to 200°C, and a heating rate of 3°C / min, the temperature at which the complex viscosity η*(10 rad / sec) is minimum is preferably 70°C or higher, more preferably 80°C or higher, and even more preferably 90°C or higher, and from the viewpoint of further improving embeddability, is preferably 180°C or lower, more preferably 170°C or lower, and even more preferably 160°C or lower.

[0028] When the complex viscosity of the resin layer made of the resin composition of the present embodiment is measured by a melt viscoelasticity test under the conditions of a measurement frequency of 100 rad / sec, a temperature range of 23° C. to 200° C., and a heating rate of 3° C. / min, the complex viscosity η*(100 rad / sec) at 100° C. is preferably 0.1×10 2 Pa s or more, preferably 0.3×10 2 Pa s or more, more preferably 0.5×10 2 Pa s or more, more preferably 0.7×10 2From the viewpoint of further improving embeddability, it is preferably 5.0×10 4 Pa s or less, preferably 3.0×10 4 Pa s or less, more preferably 1.0×10 4 Pa s or less, more preferably 9.0×10 3 It is less than Pa·s.

[0029] When the complex viscosity of the resin layer made of the resin composition of the present embodiment is measured by a melt viscoelasticity test under the conditions of a measurement frequency of 1 rad / sec, a temperature range of 23° C. to 200° C., and a heating rate of 3° C. / min, the complex viscosity η*(1 rad / sec) at 100° C. is preferably 1.0×10 4 Pa s or more, preferably 3.0×10 4 Pa s or more, more preferably 4.0×10 4 Pa s or more, and preferably 8.0×10 5 Pa s or less, preferably 7.5×10 5 It is less than Pa·s.

[0030] Here, in the resin composition of this embodiment, a measurement sample for measuring the complex viscosity can be obtained, for example, by the method described in the Examples. When the resin composition is in a varnish form, for example, the varnish-like resin composition can be applied to a substrate film and dried to obtain a film-like resin composition, and then a measurement sample can be obtained by the method described in the examples.

[0031] The complex viscosity η* of the resin layer made of the resin composition of this embodiment can be adjusted to a desired numerical range, for example, by adjusting the type of resin constituting the resin composition, the weight average molecular weight (Mw) and glass transition temperature, the content ratio of the components of the resin composition, etc.

[0032] The storage modulus E' at 200°C of the cured product made of the resin composition of this embodiment is, from the viewpoint of further suppressing thermal shrinkage of the optical waveguide, preferably 0.1 GPa or more, more preferably 0.2 GPa or more, and even more preferably 0.3 GPa or more, and the upper limit is not particularly limited, but is, for example, 3.0 GPa or less.

[0033] The storage modulus E' at 200°C of the cured product made of the resin composition of this embodiment can be adjusted to a desired numerical range by, for example, adjusting the type of resin constituting the resin composition, the weight average molecular weight (Mw) and glass transition temperature, the content ratio of the components of the resin composition, etc.

[0034] The glass transition temperature (Tg) of the cured product made of the resin composition of the present embodiment is, from the viewpoint of further suppressing thermal shrinkage of the optical waveguide, preferably 150°C or higher, more preferably 160°C or higher, and even more preferably 180°C or higher, and the upper limit is not particularly limited, but is, for example, 400°C or lower. Here, the glass transition temperature (Tg) means the glass transition temperature calculated from the top peak of tan δ using a dynamic viscoelasticity measuring apparatus (DMA).

[0035] The storage modulus E' at 200° C. and the glass transition temperature (Tg) of the cured product made of the above-mentioned resin composition can be calculated by the method described in the Examples. Specifically, the cured product of the resin composition is heated from 30°C to 400°C using a dynamic viscoelasticity measuring device under conditions of a nitrogen atmosphere, a frequency of 1 Hz, tension mode, a sample distance of 1 cm, and a heating rate of 5°C / min, and the storage modulus E' and tan δ are measured against temperature. From the obtained storage modulus E', the storage modulus E' at 200°C of the cured product of the resin composition is calculated. In addition, the glass transition temperature (Tg) of the cured product of the resin composition is calculated from the top peak of the obtained tan δ. Here, the cured product made of the resin composition means a cured product in a state where the resin composition is completely cured (C stage). As a method for determining whether a resin composition is in a completely cured state (C stage), for example, there is a method of confirming whether the increase or decrease in the peak intensity derived from a functional group involved in the curing reaction (e.g., a CO group in a cyclic ether structure) is constant by Fourier transform infrared spectroscopy (FT-IR method). The method for curing the resin composition is not particularly limited, and examples thereof include a method of heating the resin composition, a method of irradiating the resin composition with light, and a method of irradiating the resin composition with light while heating it. Preferably, the resin composition is heated at 180°C for 2 hours in the atmosphere.

[0036] The shape of the resin composition of the present embodiment is not particularly limited, and examples thereof include a film, membrane, varnish, sheet, and the like.

[0037] The components of the resin composition of the present embodiment are not particularly limited, but preferably contain a polyimide resin (A) and a compound having a cyclic ether structure (B), and more preferably contain a polyimide resin (A), a compound having a cyclic ether structure (B), and a curing agent (C). Hereinafter, each of the preferable components of the resin composition of the present embodiment will be described.

[0038] <Polyimide resin (A)> The content of polyimide resin (A) in the resin composition of this embodiment, when the total content of the resin components in the resin composition is 100 parts by mass, is preferably 20 parts by mass or more, more preferably 23 parts by mass or more, even more preferably 25 parts by mass or more, and even more preferably 28 parts by mass or more, from the viewpoint of further improving embeddability, and is preferably 80 parts by mass or less, more preferably 75 parts by mass or less, even more preferably 70 parts by mass or less, and even more preferably 65 parts by mass or less, from the viewpoint of further improving embeddability.

[0039] The polyimide resin (A) of the present embodiment preferably contains an imide ring structure in the molecule from the viewpoint of suppressing voids due to volatile components. The present inventors believe that by containing an imide ring structure in the molecule, generation of volatile components (e.g., moisture, etc.) can be suppressed when the resin composition is cured, and therefore voids due to volatile components in vias can be suppressed.

[0040] The imidization rate of the polyimide resin (A) of the present embodiment is preferably 90% or more, more preferably 93% or more, even more preferably 95% or more, even more preferably 97% or more, even more preferably 98% or more, and even more preferably 99% or more. The imidization rate of polyimide resin (A) means the imidization rate expressed by {IM / (IM+AM)}×100(%), where IM is the number of moles of imide groups contained in polyimide resin (A) and AM is the number of moles of amide groups contained in polyimide resin (A). The imidization ratio can be determined, for example, from the area of ​​a peak corresponding to an amide group and the area of ​​a peak corresponding to an imide group in an NMR spectrum, etc. As another example, the imidization ratio can be determined from the area of ​​a peak corresponding to an amide group and the area of ​​a peak corresponding to an imide group in an infrared absorption spectrum, etc.

[0041] The polyimide resin (A) of the present embodiment preferably contains a fluorinated polyimide, which means a polyimide containing a fluorine atom. When the polyimide resin (A) of the present embodiment contains a fluorinated polyimide, the solubility in organic solvents is further improved, making it easier to obtain a varnish-like resin composition. From the viewpoint of further improving the solubility in organic solvents, the amount (mass ratio) of fluorine atoms in the fluorinated polyimide is preferably 1 mass % or more, more preferably 3 mass % or more, even more preferably 5 mass % or more, and is preferably 30 mass % or less, more preferably 28 mass % or less, even more preferably 25 mass % or less.

[0042] The fluorinated polyimide of the present embodiment preferably contains a structural unit represented by the following general formula (a).

[0043] [ka]

[0044] In general formula (a), X is a divalent organic group, Y is a tetravalent organic group, and at least one of X and Y has a fluorine atom.

[0045] In general formula (a), the divalent organic group of X and / or the tetravalent organic group of Y preferably contain an aromatic ring structure, more preferably a benzene ring structure, from the viewpoint of further suppressing the thermal shrinkage of the optical waveguide. In general formula (a), it is preferable that both the divalent organic group X and the tetravalent organic group Y are fluorine atom-containing groups, from the viewpoint of further improving solubility in organic solvents. In the general formula (a), the divalent organic group of X and / or the tetravalent organic group of Y preferably have a structure in which 2 to 6 benzene rings are bonded via a single bond or a divalent linking group. Examples of the divalent linking group include an alkylene group, a fluorinated alkylene group, and an ether group. The alkylene group and the fluorinated alkylene group may be linear or branched. In the general formula (a), the divalent organic group of X has 6 to 30 carbon atoms, for example. In the general formula (a), the tetravalent organic group for Y has 6 to 20 carbon atoms, for example. In the general formula (a), each of the two imide rings is preferably a five-membered ring.

[0046] The fluorinated polyimide of the present embodiment more preferably contains a structural unit represented by the following general formula (aa).

[0047] [ka]

[0048] In general formula (aa), Y' represents a single bond or an alkylene group, X has the same meaning as X in general formula (a), and at least one of X and Y' has a fluorine atom.

[0049] In the general formula (aa), the alkylene group of Y' may be linear or branched. It is preferable that some or all of the hydrogen atoms of the alkylene group of Y' are substituted with fluorine atoms. The number of carbon atoms of the alkylene group of Y' is preferably 1 to 6, more preferably 1 to 4, and further preferably 1 to 3. In general formula (aa), it is preferable that both X and Y' are fluorine atom-containing groups.

[0050] From the viewpoint of further improving the light propagation efficiency of the optical waveguide, the refractive index of the polyimide resin (A) of the present embodiment is preferably 1.58 or less, more preferably 1.56 or less, even more preferably 1.55 or less, and even more preferably 1.54 or less, and the lower limit is not particularly limited, but is, for example, 1.50 or more. The refractive index of the polyimide resin (A) refers to a refractive index measured using an Abbe refractometer under conditions of 23° C. and 589 nm.

[0051] The weight average molecular weight (Mw) of the polyimide resin (A) of the present embodiment is, from the viewpoint of further suppressing thermal shrinkage of the optical waveguide, preferably 5,000 or more, more preferably 7,000 or more, even more preferably 10,000 or more, even more preferably 30,000 or more, and even more preferably 40,000 or more, and from the viewpoint of further improving the solubility in organic solvents, is preferably 200,000 or less, more preferably 150,000 or less, even more preferably 130,000 or less, and even more preferably 110,000 or less. The weight average molecular weight can be determined by gel permeation chromatography (GPC) using polystyrene as a standard substance.

[0052] The polyimide resin (A) of the present embodiment can be obtained, for example, by (i) first synthesizing a polyamide by reacting (condensation polymerization) a diamine with an acid dianhydride, and then (ii) imidizing the polyamide (ring-closing reaction). Specific reaction conditions can be, for example, known conditions.

[0053] Examples of diamines used as raw materials in synthesizing the polyimide resin (A) of this embodiment include 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 3,4'-diaminodiphenyl ether (3,4'-ODA), 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl (TFMB), 3,3',5,5'-tetramethylbenzidine, and 2,3,5,6-tetramethyl-1,4-phenylenediamine. , 3,3'-diaminodiphenyl sulfone, 3,3'-dimethylbenzidine, 3,3'-bis(trifluoromethyl)benzidine, 2,2'-bis(p-aminophenyl)hexafluoropropane, bis(trifluoromethoxy)benzidine (TFMOB), 2,2'-bis(pentafluoroethoxy)benzidine (TFEOB), 2,2'-trifluoromethyl-4,4'-oxydianiline (OBABTF), 2-phenyl-2-trifluoromethyl-bis(p-aminophenyl)methane, 2-phenyl-2-trifluoromethyl-bis(p-aminophenyl)methane, bis(m-aminophenyl)methane, 2,2'-bis(2-heptafluoroisopropoxy-tetrafluoroethoxy)benzidine (DFPOB), 2,2-bis(m-aminophenyl)hexafluoropropane (6-FmDA), 2,2-bis(3-amino-4-methylphenyl)hexafluoropropane, 3,6-bis(trifluoromethyl)-1,4-diaminobenzene (2TFMPDA), 1-(3,5-diaminophenyl)-2,2-bis(trifluoromethyl)-3,3,4,4,5,5,5-heptafluoropentane, 3,5- Examples of such compounds include diaminobenzotrifluoride (3,5-DABTF), 3,5-diamino-5-(pentafluoroethyl)benzene, 3,5-diamino-5-(heptafluoropropyl)benzene, 2,2'-dimethylbenzidine (DMBZ), 2,2',6,6'-tetramethylbenzidine (TMBZ), 3,6-diamino-9,9-bis(trifluoromethyl)xanthene (6FCDAM), 3,6-diamino-9-trifluoromethyl-9-phenylxanthene (3FCDAM), and 3,6-diamino-9,9-diphenylxanthene. The diamines may be used alone or in combination of two or more.

[0054] Examples of acid dihydrates used as raw materials for synthesizing the polyimide resin (A) of this embodiment include 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride, 4,4'-oxydiphthalic dianhydride, pyromellitic dianhydride (PMDA), diphenylether-3,3',4,4'-tetracarboxylic dianhydride (ODPA), benzophenone-3,3',4,4'-tetracarboxylic dianhydride (BTDA), Examples of such compounds include biphenyl-3,3',4,4'-tetracarboxylic dianhydride (BPDA), diphenylsulfone-3,3',4,4'-tetracarboxylic dianhydride (DSDA), diphenylmethane-3,3',4,4'-tetracarboxylic dianhydride, 2,2-bis(3,4-phthalic anhydride)propane, and 2,2-bis(3,4-phthalic anhydride)-1,1,1,3,3,3-hexafluoropropane (6FDA). The acid dihydrate may be used alone or in combination of two or more kinds.

[0055] The polyimide resin (A) of the present embodiment may be a single polyimide resin, or may contain two or more polyimide resins.

[0056] <Compound (B) Having a Cyclic Ether Structure> The compound (B) having a cyclic ether structure in this embodiment preferably contains at least one or more types selected from the group consisting of epoxy resins and oxetane compounds, and more preferably contains one or more types of epoxy resins.

[0057] The content of the compound (B) having a cyclic ether structure contained in the resin composition of this embodiment, when the total content of the resin components in the resin composition is 100 parts by mass, is preferably 20 parts by mass or more, more preferably 25 parts by mass or more, even more preferably 30 parts by mass or more, and even more preferably 35 parts by mass or more, from the viewpoint of further improving embeddability, and is preferably 80 parts by mass or less, more preferably 75 parts by mass or less, from the viewpoint of further improving embeddability.

[0058] The compound (B) having a cyclic ether structure of this embodiment preferably contains an alicyclic structure in the molecule. Here, the compound (B) having a cyclic ether structure contains an alicyclic structure in the molecule means that it contains an alicyclic structure in addition to the cyclic ether structure. However, the alicyclic structure of this embodiment includes a condensed ring structure in which a cyclic ether and an aliphatic ring are condensed, and a spiro ring structure in which a cyclic ether and an aliphatic ring are bonded by a spiro bond atom. The number of ring members in the alicyclic structure is not particularly limited, but is preferably a 4- to 10-membered ring, more preferably a 4- to 8-membered ring, even more preferably a 5- or 6-membered ring, and even more preferably a 6-membered ring.

[0059] The compound (B) having a cyclic ether structure of this embodiment preferably contains two or more cyclic ether structures in the molecule, and more preferably contains two or three cyclic ether structures in the molecule.

[0060] The compound (B) having a cyclic ether structure of the present embodiment is preferably liquid at 23° C. from the viewpoint of ease of handling during production of the resin composition.

[0061] From the viewpoint of further improving the light propagation efficiency of the optical waveguide, the refractive index of the compound (B) having a cyclic ether structure of this embodiment is preferably 1.55 or less, more preferably 1.53 or less, and even more preferably 1.52 or less, and the lower limit is not particularly limited, but is, for example, 1.45 or more. The refractive index of the compound (B) having a cyclic ether structure means a refractive index measured using an Abbe refractometer under conditions of 23° C. and 589 nm.

[0062] The compound (B) having a cyclic ether structure in this embodiment may be a compound having one type of cyclic ether structure, or may contain compounds having two or more types of cyclic ether structures.

[0063] <Hardening agent (C)> As the curing agent (C) of the present embodiment, for example, a thermal polymerization initiator, a photopolymerization initiator, an amine compound, or the like can be used.

[0064] The content of the curing agent (C) in the resin composition of this embodiment, when the total content of the resin components in the resin composition is 100 parts by mass, is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, even more preferably 0.5 parts by mass or more, even more preferably 0.7 parts by mass or more, even more preferably 1.0 part by mass or more, and is preferably 10.0 parts by mass or less, more preferably 8.0 parts by mass or less, even more preferably 6.0 parts by mass or less, and even more preferably 5.5 parts by mass or less.

[0065] The curing agent (C) of the present embodiment preferably contains a cationic polymerization initiator. Examples of the cationic polymerization initiator include a thermal cationic polymerization initiator and a photo cationic polymerization initiator, and among these, a thermal cationic polymerization initiator is preferred. The thermal cationic polymerization initiator includes, for example, a sulfonium salt type polymerization initiator, an iodonium salt type polymerization initiator, and the like, and preferably includes a sulfonium salt type polymerization initiator. The photocationic polymerization initiator includes, for example, a sulfonium salt type polymerization initiator, an iodonium salt type polymerization initiator, and the like.

[0066] The curing agent (C) of the present embodiment preferably contains an imidazole compound. The imidazole compound means a compound containing an imidazole ring structure, for example, a compound in which hydrogen of imidazole is substituted with a hydrocarbon group or the like.

[0067] The curing agent (C) of the present embodiment may be a single curing agent, or may contain two or more curing agents.

[0068] <Surfactant (D)> From the viewpoint of further improving embeddability, the resin composition of the present embodiment preferably further contains a surfactant (D). The surfactant (D) includes, for example, a silicone-based surfactant, a fluorine-based surfactant, etc., and preferably includes a silicone-based surfactant. The surfactant (D) of the present embodiment may be a single surfactant, or may contain two or more surfactants.

[0069] The content of the surfactant (D) contained in the resin composition of this embodiment, when the total content of the resin components in the resin composition is 100 parts by mass, is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.07 parts by mass or more, and is preferably 3.0 parts by mass or less, more preferably 1.0 parts by mass or less, even more preferably 0.7 parts by mass or less, even more preferably 0.5 parts by mass or less, and even more preferably 0.3 parts by mass or less.

[0070] <Organic solvent (E)> The resin composition of the present embodiment may contain an organic solvent (E). When the resin composition of the present embodiment contains an organic solvent (E), it can be made into a varnish-like resin composition.

[0071] Examples of the organic solvent (E) in this embodiment include acetone, methyl ethyl ketone, toluene, propylene glycol monomethyl ether, propylene glycol methyl ethyl ether, propylene glycol dimethyl ether, propylene glycol 1-monomethyl ether 2-acetate, diethylene glycol ethyl methyl ether, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, benzyl alcohol, propylene carbonate, ethylene glycol diacetate, propylene glycol diacetate, propylene glycol monomethyl ether acetate, dipropylene glycol methyl-n-propyl ether, butyl acetate, γ-butyrolactone, methyl lactate, ethyl lactate, and butyl lactate. The organic solvent (E) in the present embodiment may be a single organic solvent, or may contain two or more organic solvents.

[0072] When the resin composition of the present embodiment contains an organic solvent (E), the concentration of all solids (non-volatile components) in the resin composition is preferably 10 mass % or more, more preferably 20 mass % or more, even more preferably 30 mass % or more, and even more preferably 35 mass % or more, from the viewpoint of appropriately controlling the viscosity of the resin composition, and is preferably 60 mass % or less, more preferably 55 mass % or less, and even more preferably 50 mass % or less, from the viewpoint of sufficiently dissolving each component in the resin composition.

[0073] <Other ingredients> The resin composition of the present embodiment may further contain, for example, a curing assistant, a leveling agent, a colorant, a storage stabilizer, a plasticizer, a filler, inorganic particles, a deterioration inhibitor, a wettability improver, an antistatic agent, etc. The content of the other components is an appropriate amount.

[0074] When the resin composition of the present embodiment contains a thermal cationic polymerization initiator, it may not contain a photosensitizer such as a photocationic polymerization initiator. When the resin composition of the present embodiment contains a thermal cationic polymerization initiator, the content of the photosensitizer in the resin composition of the present embodiment is not particularly limited, but when the total content of the resin components in the resin composition is 100 parts by mass, it may be, for example, less than 1.0 part by mass, less than 0.5 part by mass, less than 0.3 part by mass, less than 0.1 part by mass, or 0.0 part by mass.

[0075] The total content of the polyimide resin (A) and the compound (B) having a cyclic ether structure in the resin composition of this embodiment is, from the viewpoint of further improving embeddability, preferably 80 mass% or more, more preferably 85 mass% or more, even more preferably 90 mass% or more, even more preferably 95 mass% or more, even more preferably 98 mass% or more, and even more preferably 100 mass%, when the total content of the resin components in the resin composition is 100 mass%. The total content of the polyimide resin (A) and the compound (B) having a cyclic ether structure in the resin composition of this embodiment, when the total content of all components in the resin composition is 100 mass%, is preferably 10 mass% or more, more preferably 20 mass% or more, even more preferably 30 mass% or more, even more preferably 35 mass% or more, even more preferably 50 mass% or more, even more preferably 70 mass% or more, even more preferably 80 mass% or more, even more preferably 85 mass% or more, even more preferably 90 mass% or more, even more preferably 95 mass% or more, and the upper limit is not particularly limited, but is, for example, 99 mass% or less.

[0076] The total content of the polyimide resin (A), the compound having a cyclic ether structure (B), the curing agent (C), the surfactant (D), and the organic solvent (E) in the resin composition of this embodiment is, when the total content of all components in the resin composition is 100 mass%, preferably 50 mass% or more, more preferably 60 mass% or more, even more preferably 70 mass% or more, even more preferably 80 mass% or more, even more preferably 90 mass% or more, even more preferably 95 mass% or more, and even more preferably 100 mass%.

[0077] [Method of producing resin composition] The resin composition of the present embodiment can be obtained, for example, by mixing the respective components. The film-like resin composition of the present embodiment can be obtained, for example, by applying a varnish-like resin composition onto a substrate film and drying it.

[0078] [film] The film of the present embodiment is a film that can be used for an optical waveguide clad, and includes a resin layer. When the complex viscosity of the resin layer is measured by a melt viscoelasticity test under the conditions of a measurement frequency of 10 rad / sec, a temperature range of 23° C. to 200° C., and a heating rate of 3° C. / min, the complex viscosity η*(10 rad / sec) at 100° C. is 1.0×10 3 Pa·s or more 1.0×10 5 It is less than Pa·s.

[0079] As discussed above, there is a need for a film that can provide an optical waveguide cladding with improved embeddability. Here, the present inventors have found for the first time that the embeddability of the film is improved by setting the complex viscosity η* (10 rad / sec) at 100° C. of the resin layer within a specific range.

[0080] In the film of this embodiment, the complex viscosity η*(10 rad / sec) of the resin layer at 100° C. is preferably 2.0×10 3 Pa s or more, preferably 3.0×10 3 Pa s or more, more preferably 4.0×10 3 Pa s or more, more preferably 5.0×10 3 From the viewpoint of further improving embeddability, it is preferably 9.5×10 4 Pa s or less, preferably 9.3×10 4 Pa s or less, more preferably 9.0×10 4 Pa s or less, more preferably 8.8×10 4 It is less than Pa·s.

[0081] In the film of this embodiment, when the complex viscosity of the resin layer is measured by a melt viscoelasticity test under conditions of a measurement frequency of 10 rad / sec, a temperature range of 23°C to 200°C, and a heating rate of 3°C / min, the temperature at which the complex viscosity η*(10 rad / sec) is minimum is preferably 70°C or higher, more preferably 80°C or higher, and even more preferably 90°C or higher, and from the viewpoint of further improving embeddability, is preferably 180°C or lower, more preferably 170°C or lower, and even more preferably 160°C or lower.

[0082] In the film of this embodiment, when the complex viscosity of the resin layer is measured by a melt viscoelasticity test under the conditions of a measurement frequency of 100 rad / sec, a temperature range of 23° C. to 200° C., and a heating rate of 3° C. / min, the complex viscosity η*(100 rad / sec) at 100° C. is preferably 0.1×10 2 Pa s or more, preferably 0.3×10 2Pa s or more, more preferably 0.5×10 2 Pa s or more, more preferably 0.7×10 2 From the viewpoint of further improving embeddability, it is preferably 5.0×10 4 Pa s or less, preferably 3.0×10 4 Pa s or less, more preferably 1.0×10 4 Pa s or less, more preferably 9.0×10 3 It is less than Pa·s.

[0083] In the film of this embodiment, when the complex viscosity of the resin layer is measured by a melt viscoelasticity test under the conditions of a measurement frequency of 1 rad / sec, a temperature range of 23° C. to 200° C., and a heating rate of 3° C. / min, the complex viscosity η*(1 rad / sec) at 100° C. is preferably 1.0×10 4 Pa s or more, preferably 3.0×10 4 Pa s or more, more preferably 4.0×10 4 Pa s or more, and preferably 8.0×10 5 Pa s or less, preferably 7.5×10 5 It is less than Pa·s.

[0084] Here, in the film of this embodiment, a measurement sample for measuring the complex viscosity can be obtained, for example, by the method described in the Examples.

[0085] In the film of this embodiment, the complex viscosity η* of the resin layer can be adjusted to a desired numerical range, for example, by adjusting the type of resin constituting the resin layer, the weight average molecular weight (Mw) and glass transition temperature, the content ratio of the components of the resin layer, etc.

[0086] In the film of this embodiment, the storage modulus E' at 200°C of the cured product obtained by curing the resin layer is, from the viewpoint of further suppressing thermal shrinkage of the optical waveguide, preferably 0.1 GPa or more, more preferably 0.2 GPa or more, and even more preferably 0.3 GPa or more, and the upper limit is not particularly limited, but is, for example, 3.0 GPa or less.

[0087] In the film of this embodiment, the storage modulus E' at 200°C of the cured product obtained by curing the resin layer can be adjusted to a desired numerical range, for example, by adjusting the type of resin constituting the resin layer, the weight average molecular weight (Mw) and glass transition temperature, the content ratio of the components constituting the resin layer, etc.

[0088] In the film of the present embodiment, the glass transition temperature (Tg) of the cured product obtained by curing the resin layer is, from the viewpoint of further suppressing thermal shrinkage of the optical waveguide, preferably 150°C or higher, more preferably 160°C or higher, and even more preferably 180°C or higher, and the upper limit is not particularly limited, but is, for example, 400°C or lower. Here, the glass transition temperature (Tg) means the glass transition temperature calculated from the top peak of tan δ using a dynamic viscoelasticity measuring apparatus (DMA).

[0089] The storage modulus E' at 200° C. and the glass transition temperature (Tg) of the cured product obtained by curing the resin layer of the above-mentioned film can be calculated by the method described in the Examples. Specifically, the cured product obtained by curing the resin layer is heated from 30°C to 400°C using a dynamic viscoelasticity measuring device under conditions of a nitrogen atmosphere, a frequency of 1 Hz, tension mode, a sample distance of 1 cm, and a heating rate of 5°C / min, and the storage modulus E' and tan δ versus temperature are measured. From the obtained storage modulus E', the storage modulus E' at 200°C of the cured product obtained by curing the resin layer is calculated. In addition, the glass transition temperature (Tg) of the cured product obtained by curing the resin layer is calculated from the top peak of the obtained tan δ. Here, the cured product obtained by curing the resin layer means a cured product in a state where the resin composition constituting the resin layer is completely cured (C stage). As a method for determining whether a resin composition is in a completely cured state (C stage), for example, there is a method of confirming whether the increase or decrease in the peak intensity derived from a functional group involved in the curing reaction (e.g., a CO group in a cyclic ether structure) is constant by Fourier transform infrared spectroscopy (FT-IR method). The method for curing the resin layer is not particularly limited, and examples thereof include a method of heating the resin layer, a method of irradiating the resin layer with light, and a method of irradiating the resin layer with light while heating. Preferably, the resin layer is heated at 180°C for 2 hours in air.

[0090] In the film of the present embodiment, the resin layer is preferably formed from the resin composition of the present embodiment.

[0091] From the viewpoint of further improving embeddability, the thickness of the resin layer in this embodiment is preferably 1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, even more preferably 15 μm or more, and even more preferably 20 μm or more, and from the viewpoint of further improving the light propagation efficiency of the optical waveguide, the thickness is preferably 150 μm or less, more preferably 100 μm or less, even more preferably 50 μm or less, even more preferably 40 μm or less, and even more preferably 30 μm or less.

[0092] The film of this embodiment is preferably a dry film.

[0093] From the viewpoint of further improving the handleability of the film, the thickness of the film of this embodiment is preferably 10 μm or more, more preferably 30 μm or more, even more preferably 50 μm or more, even more preferably 80 μm or more, even more preferably 100 μm or more, and is preferably 500 μm or less, even more preferably 300 μm or less, even more preferably 200 μm or less, even more preferably 150 μm or less, even more preferably 130 μm or less.

[0094] The film of the present embodiment preferably further includes a base film, and a resin layer is provided on the base film. The base film may be, for example, a resin film. The resin constituting the base film is not particularly limited, but it is preferable that the base film contains at least one or more types selected from the group consisting of polyimide and polyethylene terephthalate.

[0095] From the viewpoint of further improving the handleability of the film, the thickness of the base film in this embodiment is preferably 10 μm or more, more preferably 15 μm or more, even more preferably 20 μm or more, preferably 30 μm or more, and is preferably 100 μm or less, more preferably 80 μm or less, even more preferably 60 μm or less, even more preferably 40 μm or less.

[0096] The substrate film of the present embodiment may be subjected to a surface treatment such as an antistatic treatment or a release treatment.

[0097] The film of the present embodiment may further include a cover film. The cover film is preferably provided so as to be in direct contact with the resin layer. When the film of the present embodiment includes a base film, the cover film is preferably provided on the surface of the resin layer opposite to the base film. The cover film is not particularly limited, but for example, an OPP cover film can be used.

[0098] The film of the present embodiment can be obtained, for example, by applying the varnish-like resin composition of the present embodiment onto a substrate film and drying it. Examples of the application method include a direct application method using various coater devices such as a pin coater, a die coater, a comma coater, and a curtain coater, and a printing method such as screen printing.

[0099] [Film set] The film set of this embodiment includes a first film and a second film, and at least one of the first film and the second film is the film of this embodiment. In the film set of this embodiment, both the first film and the second film are preferably the film of this embodiment.

[0100] [Optical waveguide] The optical waveguide of this embodiment will be described with reference to FIG. The optical waveguide 100 of this embodiment is an optical waveguide in which a first clad layer 20, a core layer 30, and a second clad layer 40 are laminated in this order, and at least one of the first clad layer 20 and the second clad layer 40 contains the resin composition of this embodiment. In the optical waveguide of this embodiment, both the first cladding layer 20 and the second cladding layer 40 preferably contain the resin composition of this embodiment.

[0101] When the optical waveguide 100 is provided on a substrate 110, it is preferable that the first cladding layer 20 be on the substrate 110 side. When the first cladding layer 20 faces the substrate 110, the preferred thicknesses of the first cladding layer 20 and the second cladding layer 40 are as follows. From the viewpoint of further improving embeddability, the thickness of the first cladding layer 20 is preferably 1 μm or more, more preferably 3 μm or more, even more preferably 5 μm or more, even more preferably 8 μm or more, even more preferably 10 μm or more, even more preferably 15 μm or more, and even more preferably 20 μm or more, and from the viewpoint of further improving the light propagation efficiency of the optical waveguide, the thickness is preferably 150 μm or less, more preferably 100 μm or less, even more preferably 70 μm or less, even more preferably 50 μm or less, even more preferably 40 μm or less, and even more preferably 30 μm or less. From the viewpoint of further suppressing thermal shrinkage of the optical waveguide, the thickness of the second cladding layer 40 is preferably 1 μm or more, more preferably 3 μm or more, even more preferably 5 μm or more, and even more preferably 8 μm or more, and is preferably 150 μm or less, more preferably 100 μm or less, even more preferably 70 μm or less, even more preferably 50 μm or less, even more preferably 40 μm or less, even more preferably 30 μm or less, and even more preferably 20 μm or less.

[0102] The material for forming the core layer 30 is not particularly limited, but it is formed from, for example, a resin composition. The resin for forming the core layer 30 may be, for example, a resin used for the core of a known optical waveguide, but preferably contains a cyclic olefin resin, and more preferably contains a norbornene resin. The resin composition for forming the core layer 30 may contain an antioxidant, a photoacid generator, and the like.

[0103] The thickness of the core layer 30 is preferably 1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, even more preferably 20 μm or more, even more preferably 30 μm or more, and preferably 100 μm or less, more preferably 80 μm or less, even more preferably 60 μm or less, even more preferably 50 μm or less.

[0104] A waveguide pattern may be formed in the core layer 30. Methods for forming the waveguide pattern include, for example, an exposure method, an etching method, a replication method, and the like.

[0105] The optical waveguide 100 may have a mirror formed thereon, and may have a mirror 50 on the light-emitting element side and a mirror 60 on the light-receiving element side. The mirror may be formed, for example, by forming an inclined surface by laser processing or the like.

[0106] In addition to the first cladding layer 20, the core layer 30, and the second cladding layer 40, the optical waveguide 100 may include other layers as long as the excellent performance of the optical waveguide 100 is not adversely affected.

[0107] [Optical / electrical composite circuit board] The optical and electrical composite substrate of this embodiment will be described with reference to FIG. The optical / electrical composite substrate 200 includes a substrate 110 and an optical waveguide 100 provided on the substrate 110 .

[0108] Examples of the substrate 110 include a printed circuit board and a flexible substrate, and a flexible substrate is preferable. The substrate 110 may have vias 140 formed therein.

[0109] The optical / electrical composite substrate 200 may include a light emitting element 120, a light receiving element 130, and the like.

[0110] The optical-electrical composite substrate 200 is obtained, for example, by (i) forming a first clad layer 20 on a substrate 110, (ii) forming a core layer 30 on the first clad layer 20, and (iii) forming a second clad layer 40 on the core layer 30. Examples of methods for forming each layer include methods in which films for forming each layer are laminated in order by roll lamination, vacuum roll lamination, flat plate lamination, vacuum flat plate lamination, atmospheric pressing, vacuum pressing, etc.

[0111] [Electronic components] The electronic component of this embodiment includes the optical / electrical composite substrate of this embodiment. Examples of the electronic components of this embodiment include electronic components in electronic devices such as mobile phones, game machines, router devices, WDM devices, personal computers, televisions, and home servers.

[0112] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. Furthermore, the present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES

[0113] The present embodiment will be described in detail below based on examples and comparative examples. Note that the present embodiment is not limited to the descriptions of these examples.

[0114] [Raw materials] First, the raw materials used in the examples and comparative examples will be described.

[0115] <Synthesis of polyimide resin> (Synthesis of polyimide resin (A-1)) 67.3g (0.210 mol) of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 97.7g (0.220 mol) of 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride, and 495g of dimethylacetamide were charged into a 3L glass separable flask equipped with a stirrer and agitator blade, and dissolved by stirring. The mixture was further stirred at room temperature for 12 hours under a nitrogen stream to carry out a polymerization reaction, yielding a polyamic acid solution.

[0116] After adding 16 g of pyridine to the obtained polyamic acid solution, 82 g of acetic anhydride was added dropwise at room temperature. The liquid temperature was then kept at 20 to 100° C. and the mixture was stirred for 24 hours to carry out an imidization reaction, thereby obtaining a polyimide solution.

[0117] The obtained polyimide solution was stirred in a 5L container and poured into 1,000g of methanol to precipitate the polyimide resin. The solid polyimide resin was then filtered using a suction filter and washed with 1,000g of methanol. The solid polyimide resin was then dried at 100°C for 24 hours using a vacuum dryer and then dried at 200°C for 3 hours to obtain a powdered polyimide resin (A-1). The weight average molecular weight (Mw) of the polyimide resin (A-1) measured by GPC was 51,000. 1 H-NMR was measured, and the imidization rate was calculated from the quantitative value of the amide peak relative to the peak of the aromatic ring of the polyimide, and the imidization rate was found to be 99% or more. Polyimide resin (A-1) was dissolved in propylene glycol monomethyl ether acetate to a solid content of 25%, and then coated with an applicator to a film thickness of 30 μm, and dried in an oven at 100° C. for 10 minutes to obtain a polyimide coating film. The refractive index of the obtained coating film was measured under conditions of 23° C. and 589 nm using an Abbe refractometer (manufactured by Atago Co., Ltd., product name: NAR-1T SOLID), and the refractive index of the polyimide was 1.54.

[0118] (Synthesis of polyimide resin (A-2)) In the synthesis of polyimide resin (A-1), except that the amount of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl was 68.9 g (0.215 mol), polymer synthesis was carried out in the same manner as in the synthesis of polyimide resin (A-1), to obtain polyimide resin (A-2). The weight average molecular weight (Mw) of the polyimide resin (A-2) measured by GPC was 101,000, the imidization rate of the polyimide resin (A-2) measured by NMR was 99% or more, and the refractive index of the polyimide resin (A-2) measured by an Abbe refractometer at 23°C and 589 nm was 1.54.

[0119] (Synthesis of polyimide resin (A-3)) In the synthesis of polyimide resin (A-1), 57.6 g (0.180 mol) of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl and 15.6 g (0.030 mol) of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane were used instead of 67.3 g (0.210 mol) of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, and polymer synthesis was performed in the same manner as in the synthesis of polyimide resin (A-1), to obtain polyimide resin (A-3). The weight average molecular weight (Mw) of the polyimide resin (A-3) measured by GPC was 48,000, the imidization rate of the polyimide resin (A-3) measured by NMR was 99% or more, and the refractive index of the polyimide resin (A-3) measured by an Abbe refractometer at 23°C and 589 nm was 1.55.

[0120] (Synthesis of polyimide resin (A-4)) In the synthesis of polyimide resin (A-1), except that 88.85 g (0.200 mol) of 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride and 6.20 g (0.020 mol) of 4,4'-oxydiphthalic dianhydride were used instead of 97.7 g (0.220 mol) of 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride, polymer synthesis was performed in the same manner as in the synthesis of polyimide resin (A-1), to obtain polyimide resin (A-4). The weight average molecular weight (Mw) of the polyimide resin (A-4) measured by GPC was 49,000, the imidization rate of the polyimide resin (A-4) measured by NMR was 99% or more, and the refractive index of the polyimide resin (A-4) measured by an Abbe refractometer at 23°C and 589 nm was 1.55.

[0121] Details of the raw materials for each component in Tables 1 and 2 are as follows:

[0122] <Polymer (A)> (A-1) Polyimide resin synthesized above (Mw = 51,000, imidization rate 99% or more, refractive index n = 1.54) (A-2) Polyimide resin synthesized above (Mw = 101,000, imidization rate 99% or more, refractive index n = 1.54) (A-3) Polyimide resin synthesized above (Mw=48,000, imidization rate 99% or more, refractive index n=1.55) (A-4) Polyimide resin synthesized above (Mw=49,000, imidization rate 99% or more, refractive index n=1.55) (A-5) Rubber-based elastomer (manufactured by Kuraray Co., Ltd., product name: Septon Q1250) (Mw = 100,000, refractive index n = 1.50) (for comparison)

[0123] [ka]

[0124] <Compound (B) Having a Cyclic Ether Structure> (B-1) Celloxide 2021P (manufactured by Daicel Corporation, epoxy resin having an alicyclic structure, liquid at 23°C, refractive index 1.51) (B-2) EHPE-3150 (manufactured by Daicel Corporation, epoxy resin having an alicyclic structure, solid at 23°C, refractive index 1.51) (B-3) Epicoat YX-8000 (manufactured by Mitsubishi Chemical Corporation, epoxy resin with an alicyclic structure, liquid at 23°C, refractive index 1.51) (B-4) Denacol EX-321L (Nagase ChemteX Corporation, aliphatic epoxy resin, liquid at 23°C, refractive index 1.50) (B-5)OXT-221 (manufactured by Toagosei Co., Ltd., oxetane compound, liquid at 23°C, refractive index 1.50)

[0125] [ka]

[0126] <Hardening agent (C)> (C-1) San-Aid SI-110 (manufactured by Sanshin Chemical Industry Co., Ltd., thermal cationic polymerization initiator) (C-2) San-Aid SI-150 (manufactured by Sanshin Chemical Industry Co., Ltd., thermal cationic polymerization initiator) (C-3) San-Aid SI-B3 (manufactured by Sanshin Chemical Industry Co., Ltd., thermal cationic polymerization initiator) (C-4) Curezol C11z (manufactured by Shikoku Kasei Co., Ltd., an imidazole compound)

[0127] <Surfactant (D)> (D-1) BYK-333 (BYK Japan Co., Ltd., silicone surfactant) (D-2) BYK-361 (manufactured by BYK Japan Co., Ltd., acrylic polymer surfactant) (for comparison)

[0128] <Organic solvent (E)> (E-1) Propylene glycol monomethyl ether acetate (E-2) Propylene glycol monomethyl ether (E-3) Toluene

[0129] [Examples 1 to 9, Comparative Examples 1 and 2, and Reference Example 2] (Preparation of resin composition) The raw materials mixed according to Tables 1 and 2 were stirred at room temperature until the raw materials were completely dissolved to obtain a solution. The solution was then filtered through a PTFE filter having a pore size of 0.2 μm to obtain varnish-like resin compositions of Examples 1 to 9, Comparative Examples 1 and 2, and Reference Example 2, respectively.

[0130] (Film Creation) The resin compositions of Examples 1 to 9, Comparative Examples 1 and 2, and Reference Example 2 obtained by preparing the above resin compositions were applied to a 38 μm thick antistatically treated polyethylene terephthalate substrate (manufactured by Nippa Corporation, product name: PET38×1-TR1-ASQ) using an applicator so that the thickness after drying would be the thickness of the resin layer described in Tables 1 and 2. The resulting material was then dried at 100° C. for 10 minutes, and finally an OPP cover film (manufactured by Oji F-Tex Corporation, product name: E201F-50 μm) was attached to the surface of the resin layer formed by the resin composition to prepare a film, thereby obtaining the films of Examples 1 to 9 and Comparative Examples 1 and 2. It should be noted that the resin composition of Reference Example 2 was unable to form a film.

[0131] [Reference example 1] In the same manner as in the above-mentioned Examples 1 to 9, Comparative Examples 1 and 2, and Reference Example 2 (Preparation of Resin Compositions), a varnish-like resin composition of Reference Example 1 formulated according to Table 2 was obtained. The varnish-like resin composition of Reference Example 1 was applied to a 25 μm-thick polyimide substrate (manufactured by UBE Corporation, product name: Upilex 25S) using an applicator so that the film thickness after drying would be 10 μm. The film was then dried at 160° C. for 10 minutes, and finally an OPP cover film (manufactured by Oji F-Tex Corporation, product name: E201F-50 μm) was attached to the surface of the resin layer formed by the resin composition to obtain the film of Reference Example 1.

[0132] [Examples 10 to 18 and Comparative Example 3] (Synthesis of polymer for forming core layer) In a glove box filled with dry nitrogen, with both moisture and oxygen concentrations controlled to 1 ppm or less, 7.2 g (40.1 mmol) of hexylnorbornene (HxNB) and 12.9 g (40.1 mmol) of diphenylmethylnorbornene methoxysilane were weighed into a 500 mL vial, 60 g of dehydrated toluene and 11 g of ethyl acetate were added, and the vial was covered with a silicone sealer and sealed at the top. Next, 1.56 g (3.2 mmol) of Ni catalyst and 10 mL of dehydrated toluene were weighed into a 100 mL vial, a stirrer tip was inserted and the vial was sealed, and the Ni catalyst was thoroughly stirred to completely dissolve, obtaining a Ni catalyst solution. 1 mL of the Ni catalyst solution was accurately weighed with a syringe and quantitatively injected into the vial in which the above two types of norbornene were dissolved, and stirred at room temperature for 1 hour, whereupon a significant increase in viscosity was confirmed. At this point, the stopper was removed, 60 g of tetrahydrofuran (THF) was added and stirred to obtain a reaction solution. 9.5 g of acetic anhydride, 18 g of hydrogen peroxide (concentration 30%), and 30 g of ion-exchanged water were added to a 100 mL beaker and stirred to prepare an aqueous solution of peracetic acid. Next, the entire amount of the aqueous solution of peracetic acid was added to the reaction solution and stirred for 12 hours to carry out the reduction treatment of Ni. Next, the reaction solution after the treatment was transferred to a separatory funnel, and after removing the lower aqueous layer, 100 mL of a 30% aqueous solution of isopropyl alcohol was added and vigorously stirred. After leaving it to stand and completely separating into two layers, the aqueous layer was removed. After repeating this water washing process three times in total, the oil layer was dropped into a large excess of acetone to reprecipitate the produced polymer, which was separated from the filtrate by filtration and then heated and dried for 12 hours in a vacuum dryer set at 60°C to obtain a polymer for forming the core layer.

[0133] The molecular weight of the core layer-forming polymer was measured by GPC and found to be Mw = 100,000 and Mn = 40,000. The molar ratio of each structural unit in the core layer-forming polymer was identified by NMR measurement and found to be 50 mol% for hexylnorbornene structural units and 50 mol% for diphenylmethylnorbornene methoxysilane structural units.

[0134] (Preparation of resin composition for forming core layer) 10 g of the purified core layer-forming polymer was weighed into a 100 mL glass container, and 30 g of methylcyclohexane, 0.01 g of a hindered phenol-based antioxidant (manufactured by BASF, product name: Irganox1076), 2.4 g of an oxetane compound (manufactured by Toa Gosei Co., Ltd., product name: OXT-212), 0.8 g of Celloxide 2021P (manufactured by Daicel Corporation), and 0.03 g of a photoacid generator (manufactured by San-Apro Co., Ltd., product name: CPI-310B) were added thereto and dissolved uniformly. The mixture was then filtered through a 0.2 μm PTFE filter to obtain a resin composition for forming a core layer.

[0135] (Creation of the core layer) The obtained core layer-forming resin composition was applied to a release-treated PET film using an applicator so that the film thickness after drying would be 40 μm. After application, the film was placed in a 45° C. dryer for 5 minutes to completely remove the solvent and form a coating. The obtained coating was exposed to light at an exposure dose of 100 mJ / cm using a direct imaging exposure machine (manufactured by SCREEN Co., Ltd., product name: LS-9000). 2The film was irradiated with ultraviolet light of 1000 u.s., creating 20 lines and spaces with a length of 9 cm and a width of 50 μm. It was then placed in an oven at 150°C for 30 minutes. When it was removed from the oven, it was confirmed that a clear waveguide pattern (multiple cores) with a rectangular cross section had appeared on the film.

[0136] (Preparation of photoelectric composite substrate) A double-sided copper-clad laminate was placed on a stainless steel plate, and the first clad layer, core layer, and second clad layer were laminated in this order using a vacuum laminator in the combinations shown in Table 3 to obtain a laminate. At this time, the PET film and OPP cover film of the substrate were removed at appropriate times so that the various clads and the core were in contact, and the dry film of the polyimide substrate was used as it was as the substrate for the outermost layer. In other words, the layer structure of the obtained laminate was "double-sided copper-clad laminate / first clad layer / core layer / second clad layer / polyimide substrate". The obtained laminate was heat-treated in an oven at 160°C for 2 hours to obtain the photoelectric composite substrates of Examples 10 to 18 and Comparative Example 3.

[0137] [evaluation] The evaluation methods for the examples and comparative examples are described below.

[0138] <Measurement of complex viscosity η* of resin layer> The films of Examples 1 to 9 and Comparative Examples 1 and 2 were laminated in a laminator under the conditions of temperature: 30°C, pressure: 1.0 MPa, and time: 120 seconds so that the thickness of the resin layer formed by the resin composition was 100 μm, to obtain a sample for complex viscosity measurement. More specifically, two films were laminated to prepare two films with a resin layer thickness of 50 μm, and then the two films with a resin layer thickness of 50 μm were laminated to obtain a sample with a resin layer thickness of 100 μm. When obtaining the sample for complex viscosity measurement, the PET film and OPP cover film of the substrate were appropriately removed. The melt viscoelasticity of the sample for complex viscosity measurement was measured using a viscoelasticity measuring device (Anton Paar Japan, product name: MCH302) under three frequency conditions of 1 rad / sec, 10 rad / sec, and 100 rad / sec, while changing the temperature from 23°C to 200°C at a heating rate of 3°C / min. From the results obtained, the complex viscosity η* [Pa s] at 100°C at each frequency and the temperature [°C] at which the complex viscosity η* at a frequency of 10 rad / sec is minimum were calculated.

[0139] <Measurement of storage modulus E' and glass transition temperature (Tg) of cured product> After removing the OPP cover film from the films of Examples 1 to 9 and Comparative Examples 1 and 2, two sheets were laminated so that the resin layers formed from the resin composition faced each other, and the laminate was laminated under the conditions of temperature: 100°C, pressure: 0.5 MPa, and time: 2 minutes. Furthermore, the laminate was cured in an oven in the atmosphere at 180°C for 2 hours, and then the substrates on both sides were peeled off to obtain a sample for DMA measurement. The obtained DMA measurement sample was heated from 30°C to 400°C under nitrogen atmosphere, at a frequency of 1Hz, in tension mode, with a sample distance of 1cm, and at a heating rate of 5°C / min, using a dynamic viscoelasticity measuring device (manufactured by TA, product name: Q800), to measure the storage modulus E' and tan δ versus temperature. From the obtained storage modulus E', the storage modulus E' [GPa] at 200°C of the cured product was read. In addition, from the top peak of the obtained tan δ, the glass transition temperature (Tg) [°C] of the cured product was read.

[0140] <Embeddability evaluation> A 50 μm thick double-sided copper-clad laminate (CCL) with a 100 μm diameter via hole was prepared. The OPP cover film of each of the films in Examples 1 to 9 and Comparative Examples 1 and 2 was peeled off, and the film was attached to the CCL so that the resin layer formed from the resin composition was on the CCL side. Lamination was then performed using a laminator under the conditions of temperature: 100° C., pressure: 5.0 MPa, and time: 2 minutes. The via holes of the obtained substrate were observed under a microscope, and samples that were filled without voids were rated as A, samples that were filled with some voids but had some voids were rated as B, and samples that were not filled were rated as C.

[0141] <Optical loss evaluation> Both sides of the optoelectronic composite substrates of Examples 10 to 18 and Comparative Example 3 were cut by dicing so that the length of the pattern portion was 7 cm, to obtain samples for evaluating optical loss. The propagation loss of the samples for optical loss evaluation was evaluated in accordance with 4.6.2.1 Cutback Method of "Test Method for Polymer Optical Waveguides (JPCA-PE02-05-01S-2008)". Note that light with a wavelength of 850 nm was used for the measurements. From the results, samples with a propagation loss of less than 1 dB were rated as A, samples with a propagation loss of 1 dB to 3 dB were rated as B, and samples with a propagation loss of more than 3 dB were rated as C.

[0142] <Mirror angle change rate evaluation> On the line and space of the photoelectric composite substrate of Examples 10 to 18 and Comparative Example 3, a mirror was processed from the polyimide substrate side with an excimer laser (wavelength 193 nm, manufactured by OPTEC, product name: ProMaster) at a laser intensity of 7 mJ, a laser oscillation frequency of 250 Hz, an opening of the stainless steel mask for cutting the laser light of 1 mm x 1 mm, a moving speed of the processing table of 45 μm / s, and a moving distance of the processing table of 150 μm, so that the angle was about 45 degrees. The length of the obtained mirror was measured with a laser microscope to calculate the mirror angle (angle A) after processing. Next, the mirror-processed optical waveguide sample was treated three times at a maximum temperature of 250 ° C. in an N2 reflow device, and the mirror angle (angle B) was measured again. The change rate of the mirror angle before and after reflow was calculated from the following formula, and samples with a change rate of < 1% were evaluated as A, samples with a change rate of 1 to 3% as B, and samples with a change rate of more than 3% as C. Mirror angle change rate [%] = [(angle A - angle B) / angle A] x 100

[0143] The evaluation results for Examples 1 to 9 and Comparative Examples 1 and 2 are shown in Tables 1 and 2, respectively. The evaluation results for Examples 10 to 18 and Comparative Example 3 are shown in Table 3, respectively. In the tables, "-" next to the evaluation results means that the results were not measured.

[0144] [Table 1]

[0145] [Table 2]

[0146] [Table 3]

[0147] As can be seen from Tables 1 and 2, the embeddability of all of the films of the examples was evaluated as good. That is, it can be seen that the embeddability is improved according to the resin composition and film of the present embodiment. Furthermore, it was found from Table 3 that the optical / electrical composite substrates of the examples had small mirror angle deformation ratios and could suppress thermal shrinkage. In other words, it can be understood that the resin composition and film of the present embodiment can suppress thermal shrinkage of the optical waveguide. [Explanation of symbols]

[0148] 20 First cladding layer 30 Core Layer 40 Second Cladding Layer 50 Light emitting element side mirror 60 Mirror on the light receiving element side 100 optical waveguide 110 Substrate 120 Light emitting element 130 Photodetector 140a, 140b vias 200 Photoelectric composite board

Claims

1. A resin composition that can be used for an optical waveguide clad, The resin layer made of the resin composition has a complex viscosity of 1.0×10 at 100° C., as measured by a melt viscoelasticity test under the conditions of a measurement frequency of 10 rad / sec, a temperature range of 23° C. to 200° C., and a temperature rise rate of 3° C. / min. 3 Pa・s or more 1.0×10 5 The resin composition has a viscosity of 0.1 Pa·s or less.

2. The resin layer made of the resin composition has a complex viscosity measured by a melt viscoelasticity test under the conditions of a measurement frequency of 10 rad / sec, a temperature range of 23°C to 200°C, and a heating rate of 3°C / min. The temperature at which the complex viscosity η* (10 rad / sec) is minimum is 70°C or higher and 180°C or lower.

3. The resin layer made of the resin composition has a complex viscosity of 0.1×10 or less at 100° C. when measured by a melt viscoelasticity test under the conditions of a measurement frequency of 100 rad / sec, a temperature range of 23° C. to 200° C., and a heating rate of 3° C. / min. 2 Pa・s or more 5.0×10 4 The resin composition according to claim 1 or 2, having a viscosity of Pa·s or less.

4. The resin layer made of the resin composition has a complex viscosity of 1.0×10 at 100° C., as measured by a melt viscoelasticity test under the conditions of a measurement frequency of 1 rad / sec, a temperature range of 23° C. to 200° C., and a temperature rise rate of 3° C. / min. 4 Pa・s or more 8.0×10 5 The resin composition according to claim 1 or 2, having a viscosity of Pa·s or less.

5. 3. The resin composition according to claim 1, wherein a cured product of the resin composition has a storage modulus E' at 200°C of 0.1 GPa or more and 3.0 GPa or less.

6. The resin composition according to claim 1 or 2, wherein a glass transition temperature of a cured product of the resin composition calculated from a top peak of tan δ using a dynamic mechanical analyzer (DMA) is 150° C. or higher and 400° C. or lower.

7. The resin composition according to claim 1 or 2, comprising a polyimide resin (A) and a compound (B) having a cyclic ether structure.

8. The resin composition according to claim 7, further comprising a curing agent (C).

9. A film that can be used for an optical waveguide clad, A resin layer is provided, The complex viscosity of the resin layer was measured by a melt viscoelasticity test under the conditions of a measurement frequency of 10 rad / sec, a temperature range of 23° C. to 200° C., and a temperature rise rate of 3° C. / min. The complex viscosity η* (10 rad / sec) at 100° C. was 1.0×10 3 Pa・s or more 1.0×10 5 A film having a viscosity of less than Pa·s.

10. 10. The film according to claim 9, wherein, when the complex viscosity of the resin layer is measured by a melt viscoelasticity test under conditions of a measurement frequency of 10 rad / sec, a temperature range of 23°C to 200°C, and a heating rate of 3°C / min, the temperature at which the complex viscosity η* (10 rad / sec) is minimum is 70°C or higher and 180°C or lower.

11. The complex viscosity of the resin layer was measured by a melt viscoelasticity test under the conditions of a measurement frequency of 100 rad / sec, a temperature range of 23° C. to 200° C., and a temperature rise rate of 3° C. / min. The complex viscosity η* (100 rad / sec) at 100° C. was less than 0.1×10 2 Pa・s or more 5.0×10 4 The film according to claim 9 or 10, having a viscosity of not more than Pa·s.

12. The complex viscosity of the resin layer was measured by a melt viscoelasticity test under the conditions of a measurement frequency of 1 rad / sec, a temperature range of 23° C. to 200° C., and a temperature rise rate of 3° C. / min. The complex viscosity η* (1 rad / sec) at 100° C. was 1.0×10 4 Pa・s or more 8.0×10 5 The film according to claim 9 or 10, having a viscosity of not more than Pa·s.

13. 11. The film according to claim 9, wherein a cured product obtained by curing the resin layer has a storage modulus E' at 200°C of 0.1 GPa or more and 3.0 GPa or less.

14. The film according to claim 9 or 10, wherein the glass transition temperature of a cured product obtained by curing the resin layer is 150° C. or higher and 400° C. or lower, as calculated from a top peak of tan δ using a dynamic mechanical analyzer (DMA).

15. Further, the device includes a base film, The film according to claim 9 or 10, wherein the resin layer is provided on the base film.

16. The film according to claim 15, wherein the resin constituting the base film comprises at least one or more selected from the group consisting of polyimide and polyethylene terephthalate.

17. The film of claim 9 or 10, wherein the film is a dry film.

18. A film set that can be used for an optical waveguide clad, comprising: A first film and a second film, A film set, wherein at least one of the first film and the second film is the film according to claim 9 or 10.

19. An optical waveguide in which a first clad layer, a core layer, and a second clad layer are laminated in this order, An optical waveguide, wherein at least one of the first cladding layer and the second cladding layer comprises the resin composition according to claim 1 .

20. A substrate; An optical / electrical composite substrate comprising: the optical waveguide according to claim 19 provided on the substrate.

21. An electronic component comprising the optical / electrical composite substrate according to claim 20.

Citation Information

Patent Citations

  • Polymer optical waveguide and method of manufacturing the same

    JP2006119659A

  • Optical and electrical wiring board and device for optical communication

    JP2006140233A

  • Photo-electric hybrid substrate

    JP2014238455A