Resin composition, film, film set, optical waveguide, optoelectric composite substrate, and electronic component

The resin composition for opto-electrical composite substrates addresses propagation loss by using polyimide resin and cyclic ether compounds to enhance core layer formation and minimize acid migration, resulting in improved light propagation efficiency and reduced defects.

JP2024145149APending Publication Date: 2024-10-15SUMITOMO BAKELITE CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023057402
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing opto-electrical composite substrates suffer from propagation loss due to incomplete formation of the core layer patterns and the presence of acids from monomers and acid generators between cladding and core layers.

Method used

A resin composition comprising polyimide resin, a compound with a cyclic ether structure, and a photopolymerization initiator, specifically designed to suppress propagation loss by ensuring neat core layer patterns and minimizing acid migration, with a refractive index optimized for efficient light propagation.

Benefits of technology

The resin composition effectively reduces propagation loss in opto-electrical composite substrates by improving core layer formation and minimizing thermal shrinkage, enhancing light propagation efficiency and reducing defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145149000001_ABST
    Figure 2024145149000001_ABST
Patent Text Reader

Abstract

To provide a resin composition which can suppress propagation loss in an optoelectric composite substrate.SOLUTION: A resin composition, which is usable in an optical waveguide clad, contains a polyimide resin (A), a compound (B) having a cyclic ether structure, and a photopolymerization initiator (C).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a film, a film set, an optical waveguide, an optical / electrical composite substrate, and an electronic component. [Background technology]

[0002] 2. Description of the Related Art In recent years, there has been a demand for components capable of realizing more advanced information communication, such as larger capacity information and faster information communication speeds, in information and communication devices. As one such component, an optical / electrical composite substrate has been considered.

[0003] An example of the optical / electrical composite substrate is one in which an optical waveguide is provided on a substrate. As optical waveguide technologies, for example, the technologies described in Patent Documents 1 to 3 can be mentioned.

[0004] Patent Document 1 describes a flexible optical waveguide having a lower clad layer, a core layer formed on the lower clad layer, and an upper clad layer formed on the lower clad layer and the core layer so as to embed the core layer, wherein at least one of the lower clad layer, the core layer and the upper clad layer is composed of an epoxy film formed using an epoxy resin composition containing a polyglycidyl compound having a polyalkylene glycol chain and at least two glycidyl groups. According to the flexible optical waveguide described in Patent Document 1, it is described that a flexible optical waveguide that is excellent in flexibility and resistant to bending can be provided, even though it is made of epoxy resin.

[0005] Patent Document 2 describes an opto-electrical hybrid board comprising a flexible circuit board in which electrical wiring having mounting pads is formed on the surface of an insulating layer, an element mounted on the mounting pad, and an optical waveguide laminated on the back surface of the insulating layer, wherein the flexible circuit board is a flexible double-sided circuit board in which electrical wiring is also formed on the back surface of the insulating layer, and a metallic reinforcing layer is formed by plating on at least the portion of the electrical wiring on the back surface that corresponds to the mounting pad, and the optical waveguide is in contact with the metallic reinforcing layer. According to the optical-electrical hybrid board described in Patent Document 2, a metallic reinforcing layer is adhered to an insulating layer of a flexible circuit board without an adhesive layer, and it is described that an optical-electrical hybrid board can be provided in which elements are properly mounted while suppressing deformation due to a pressure load when the elements are mounted by the metallic reinforcing layer.

[0006] Patent Document 2 describes a method of preparing a substrate in which copper foil 21 is formed on the front and back surfaces of an insulating layer 1 made of a resin such as polyimide, and forming through holes 1a and via holes 1b for an optical path in the substrate (see paragraph 0023 of Patent Document 2). It also describes a flexible double-sided circuit board E in which a metallic reinforcing layer M is formed (see paragraph 0028 of Patent Document 2). The flexible double-sided circuit board E includes the above substrate. Furthermore, Patent Document 2 describes that an undercladding layer 6 is formed on the back side of a flexible double-sided circuit board E in contact with a metal reinforcing layer M that covers the electrical wiring 2B on the back side, and describes that examples of a molding material for the undercladding layer 6 include photosensitive resins and thermosetting resins (see paragraph 0029 of Patent Document 2). According to Figures 4 to 6 of Patent Document 2, it can be seen that the molding material for the undercladding layer 6 is filled into a recess formed in the flexible double-sided circuit board E on which the metal reinforcing layer M is formed.

[0007] Patent Document 3 describes an optoelectronic wiring board that is formed by integrating a rigid section in which conductor circuits and insulating layers are laminated on both sides of a substrate with one or more bendable flex sections, wherein the rigid section is formed with external connection terminals for mounting optical elements and / or package substrates on which optical elements are mounted, and at least one of the flex sections is formed with optical wiring. According to the optoelectronic wiring board of Patent Document 3, it is described that large-volume information processing and high-speed information processing can be suitably performed without increasing the size of the wiring board.

[0008] Patent Document 3 describes that the rigid section has an optical signal transmitting region formed therein, and that the optical signal transmitting region is filled with a resin composition (see claims 4 and 5 of Patent Document 3). Furthermore, Patent Document 3 describes that the optical signal transmitting region is formed so as to penetrate all of the substrates and insulating layers that constitute the rigid section (see claim 6 of Patent Document 3).

[0009] Furthermore, Patent Document 3 describes a substrate 221 consisting of an optical waveguide film 250 and a surrounding resin layer (insulating layer) 221a, and describes that the resin layer 221a constitutes part of the optical signal transmitting regions 242a, 242b (see paragraph 0033 of Patent Document 3). [Prior art documents] [Patent documents]

[0010] [Patent Document 1] International Publication No. 2008 / 053888 [Patent Document 2] JP 2014-238455 A [Patent Document 3] JP 2006-140233 A Summary of the Invention [Problem to be solved by the invention]

[0011] One of the characteristics required for an optoelectronic composite substrate is the suppression of propagation loss.

[0012] The present invention provides a resin composition capable of suppressing the propagation loss in an optoelectronic composite substrate. [Means for solving the problem]

[0013] According to the present invention, there are provided a resin composition, a film, a film set, an optical waveguide, an optical / electrical composite substrate, and an electronic component, as shown below.

[0014] [1] A resin composition that can be used for an optical waveguide clad, A resin composition comprising a polyimide resin (A), a compound having a cyclic ether structure (B), and a photopolymerization initiator (C). [2] The resin composition according to [1], wherein the content of the photopolymerization initiator (C) contained in the resin composition is 0.01 parts by mass or more and 5.0 parts by mass or less, when the total content of the resin components in the resin composition is 100 parts by mass. [3] The resin composition according to the above [1] or [2], wherein the photopolymerization initiator (C) contains a photocationic polymerization initiator. [4] The resin composition according to [3] above, wherein the photocationic polymerization initiator includes a sulfonium salt type polymerization initiator. [5] The resin composition according to any one of the above [1] to [4], wherein the content of the polyimide resin (A) in the resin composition is 20 parts by mass or more and 80 parts by mass or less, when the total content of resin components in the resin composition is 100 parts by mass. [6] The resin composition according to any one of the above [1] to [5], wherein the polyimide resin (A) contains an imide ring structure in the molecule. [7] The resin composition according to any one of the above [1] to [6], wherein the polyimide resin (A) has an imidization rate of 90% or more. [8] The resin composition according to any one of the above [1] to [7], wherein the polyimide resin (A) contains a fluorinated polyimide. [9] The resin composition according to [8] above, wherein the fluorinated polyimide contains a structural unit represented by the following general formula (a): [ka] In general formula (a), X is a divalent organic group, Y is a tetravalent organic group, and at least one of X and Y has a fluorine atom.

[10] The resin composition according to any one of the above [1] to [9], wherein the polyimide resin (A) has a refractive index of 1.50 or more and 1.58 or less.

[11] The resin composition according to any one of the items [1] to

[10] , wherein the content of the compound (B) having a cyclic ether structure is 20 parts by mass or more and 80 parts by mass or less, when the total content of the resin components in the resin composition is 100 parts by mass.

[12] The resin composition according to any one of the above [1] to

[11] , wherein the compound (B) having a cyclic ether structure includes at least one or more compounds selected from the group consisting of epoxy resins and oxetane compounds.

[13] The resin composition according to

[12] , wherein the compound (B) having a cyclic ether structure includes an epoxy resin.

[14] The resin composition according to any one of the above [1] to

[13] , wherein the compound (B) having a cyclic ether structure contains an alicyclic structure in the molecule.

[15] The resin composition according to any one of the above [1] to

[14] , wherein the compound (B) having a cyclic ether structure contains two or more cyclic ether structures in the molecule.

[16] The resin composition according to any one of the above [1] to

[15] , wherein the compound (B) having a cyclic ether structure is liquid at 23°C.

[17] The resin composition according to any one of the above [1] to

[16] , wherein the refractive index of the compound (B) having a cyclic ether structure is 1.45 or more and 1.55 or less.

[18] A film that can be used for an optical waveguide clad, A film comprising a resin layer formed from the resin composition according to any one of the above [1] to

[17] .

[19] Further, the device includes a base film, The film according to

[18] , wherein the resin layer is provided on the base film.

[20] The film according to

[19] above, wherein the resin constituting the base film contains at least one or more types selected from the group consisting of polyimide and polyethylene terephthalate. [twenty one] The film according to any one of the above

[18] to

[20] , which is a dry film. [twenty two] The film according to any one of the above

[18] to

[21] , which is a film from which an optical waveguide can be manufactured by a sequential lamination process. [twenty three] A film set that can be used for an optical waveguide clad, comprising: A first film and a second film, A film set, wherein at least one of the first film and the second film is the film according to any one of

[18] to

[22] above. [twenty four] An optical waveguide in which a first clad layer, a core layer, and a second clad layer are laminated in this order, An optical waveguide, wherein at least one of the first cladding layer and the second cladding layer contains the resin composition according to any one of [1] to

[17] above. [twenty five] The resin composition for forming the core layer contains a photopolymerization initiator, The optical waveguide according to

[24] , wherein the photopolymerization initiator contained in the resin composition for forming the core layer has the same chemical structure as the photopolymerization initiator (C) contained in the resin composition that can be used for the optical waveguide clad.

[26] A substrate; An optical / electrical composite substrate comprising: an optical waveguide according to

[24] or

[25] provided on the substrate.

[27] An electronic component comprising the optical / electrical composite substrate according to

[26] . Effect of the Invention

[0015] According to the present invention, it is possible to provide a resin composition capable of suppressing the propagation loss in an optoelectronic composite substrate. [Brief description of the drawings]

[0016] [Figure 1] 1 is a cross-sectional view showing a schematic example of a structure of an optical / electrical composite substrate according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, embodiments of the present invention will be described with reference to the drawings. Furthermore, a numerical range of "A to B" means A or more and B or less unless otherwise specified.

[0018] 1 is a cross-sectional view showing a schematic example of the structure of an optoelectronic composite substrate according to the present embodiment, the drawing being a simplified view and not in accordance with the actual dimensional ratio. 1, an optical / electrical composite substrate 200 has an optical waveguide 100 provided on a substrate 110. The optical waveguide 100 has a first cladding layer 20, a core layer 30, and a second cladding layer 40 laminated in this order. The core layer 30 is patterned, and has a first core portion 35 and a second core portion 36. Here, the first core portion 35 is a core layer that is a light propagation path, and the second core portion 36 is a core layer that is not a light propagation path.

[0019] According to the study of the present inventors, it was found that in the conventional photoelectric composite substrate, the core layer pattern may not be formed neatly. Specifically, the core layer pattern not being formed neatly means, for example, that the interface between the first core portion 35 and the second core portion 36 is blurred. According to the study of the present inventors, it was found that propagation loss in the optical / electrical composite substrate may occur if the core layer pattern is not formed neatly.

[0020] Furthermore, according to the inventors' investigations, it is believed that in conventional optoelectronic composite substrates, acid derived from the monomer and / or acid generator contained in the cladding layer and / or core layer migrates between the cladding layer and core layer, and as a result, the pattern of the core layer is not formed neatly. That is, the present inventors consider that one of the reasons why the core layer pattern is not formed neatly is that the composition of the resin composition for forming the cladding layer has an effect.

[0021] The present invention has been made in consideration of the above circumstances, and provides a resin composition capable of suppressing the propagation loss in an optoelectronic composite substrate.

[0022] [Resin composition] The resin composition of the present embodiment is a resin composition that can be used for an optical waveguide clad, and contains a polyimide resin (A), a compound having a cyclic ether structure (B), and a photopolymerization initiator (C).

[0023] From the viewpoint of further improving the optical propagation efficiency of the optical waveguide, the refractive index of the resin composition of this embodiment is preferably 1.58 or less, more preferably 1.56 or less, even more preferably 1.55 or less, and even more preferably 1.54 or less, and the lower limit is not particularly limited, but is, for example, 1.50 or more. The refractive index of a resin composition means the refractive index measured for a resin film made of the resin composition using an Abbe refractometer under conditions of 23° C. and 589 nm. The resin film made of the resin composition can be produced, for example, by applying the resin composition onto a substrate film and drying it.

[0024] The glass transition temperature (Tg) of the cured product made of the resin composition of this embodiment is, from the viewpoint of further suppressing the thermal shrinkage of the optical waveguide and further suppressing the propagation loss of the photoelectric composite substrate, preferably 150°C or higher, more preferably 160°C or higher, and even more preferably 180°C or higher, and the upper limit is not particularly limited, but is, for example, 400°C or lower. The glass transition temperature (Tg) of the cured product of the resin composition means the glass transition temperature calculated from the top peak of tan δ by a dynamic viscoelasticity measuring device (DMA) of the cured product of the resin composition. More specifically, the cured product of the resin composition is heated from 30°C to 400°C under nitrogen atmosphere, frequency of 1Hz, tension mode, sample distance of 1cm, and heating rate of 5°C / min using a dynamic viscoelasticity measuring device, and the storage modulus and tan δ against temperature are measured, and the glass transition temperature (Tg) of the cured product of the resin composition is calculated from the top peak of tan δ. Here, the cured product made of the resin composition means a cured product in a state where the resin composition is completely cured (C stage). As a method for determining whether a resin composition is in a completely cured state (C stage), for example, there is a method of confirming whether the increase or decrease in the peak intensity derived from a functional group involved in the curing reaction (e.g., a CO group in a cyclic ether structure) is constant by Fourier transform infrared spectroscopy (FT-IR method). The method for curing the resin composition is not particularly limited, and examples thereof include a method of irradiating the resin composition with light, a method of irradiating the resin composition with light while heating it, and a method of irradiating the resin composition with light and then heating it.

[0025] The shape of the resin composition of the present embodiment is not particularly limited, and examples thereof include a film, membrane, varnish, sheet, and the like.

[0026] Hereinafter, each of the components of the resin composition of the present embodiment will be described.

[0027] <Polyimide resin (A)> The resin composition of the present embodiment contains a polyimide resin (A). The content of polyimide resin (A) in the resin composition of this embodiment, when the total content of the resin components in the resin composition is 100 parts by mass, is preferably 20 parts by mass or more, more preferably 23 parts by mass or more, even more preferably 25 parts by mass or more, and even more preferably 28 parts by mass or more, from the viewpoint of further suppressing the propagation loss of the optical-electrical composite substrate, and is preferably 80 parts by mass or less, more preferably 75 parts by mass or less, even more preferably 70 parts by mass or less, and even more preferably 65 parts by mass or less, from the viewpoint of further suppressing the propagation loss of the optical-electrical composite substrate.

[0028] The polyimide resin (A) of the present embodiment preferably contains an imide ring structure in the molecule from the viewpoint of suppressing voids due to volatile components. By containing an imide ring structure in the molecule, it is possible to suppress the generation of volatile components (e.g., moisture, etc.) when the resin composition is cured. If voids due to volatile components can be suppressed, the propagation loss of the photoelectric composite substrate can be further suppressed.

[0029] The imidization rate of the polyimide resin (A) of the present embodiment is preferably 90% or more, more preferably 93% or more, even more preferably 95% or more, even more preferably 97% or more, even more preferably 98% or more, and even more preferably 99% or more. The imidization rate of polyimide resin (A) means the imidization rate expressed by {IM / (IM+AM)}×100(%), where IM is the number of moles of imide groups contained in polyimide resin (A) and AM is the number of moles of amide groups contained in polyimide resin (A). The imidization ratio can be determined, for example, from the area of ​​a peak corresponding to an amide group and the area of ​​a peak corresponding to an imide group in an NMR spectrum, etc. As another example, the imidization ratio can be determined from the area of ​​a peak corresponding to an amide group and the area of ​​a peak corresponding to an imide group in an infrared absorption spectrum, etc.

[0030] The polyimide resin (A) of the present embodiment preferably contains a fluorinated polyimide, which means a polyimide containing a fluorine atom. When the polyimide resin (A) of the present embodiment contains a fluorinated polyimide, the solubility in organic solvents is further improved, making it easier to obtain a varnish-like resin composition. From the viewpoint of further improving the solubility in organic solvents, the amount (mass ratio) of fluorine atoms in the fluorinated polyimide is preferably 1 mass % or more, more preferably 3 mass % or more, even more preferably 5 mass % or more, and is preferably 30 mass % or less, more preferably 28 mass % or less, even more preferably 25 mass % or less.

[0031] The fluorinated polyimide of the present embodiment preferably contains a structural unit represented by the following general formula (a).

[0032] [ka]

[0033] In general formula (a), X is a divalent organic group, Y is a tetravalent organic group, and at least one of X and Y has a fluorine atom.

[0034] In general formula (a), the divalent organic group of X and / or the tetravalent organic group of Y preferably contain an aromatic ring structure, more preferably a benzene ring structure, from the viewpoint of further suppressing the thermal shrinkage of the optical waveguide. In general formula (a), it is preferable that both the divalent organic group X and the tetravalent organic group Y are fluorine atom-containing groups, from the viewpoint of further improving solubility in organic solvents. In the general formula (a), the divalent organic group of X and / or the tetravalent organic group of Y preferably have a structure in which 2 to 6 benzene rings are bonded via a single bond or a divalent linking group. Examples of the divalent linking group include an alkylene group, a fluorinated alkylene group, and an ether group. The alkylene group and the fluorinated alkylene group may be linear or branched. In the general formula (a), the divalent organic group of X has 6 to 30 carbon atoms, for example. In the general formula (a), the tetravalent organic group for Y has 6 to 20 carbon atoms, for example. In the general formula (a), each of the two imide rings is preferably a five-membered ring.

[0035] The fluorinated polyimide of the present embodiment more preferably contains a structural unit represented by the following general formula (aa).

[0036] [ka]

[0037] In general formula (aa), Y' represents a single bond or an alkylene group, X has the same meaning as X in general formula (a), and at least one of X and Y' has a fluorine atom.

[0038] In the general formula (aa), the alkylene group of Y' may be linear or branched. It is preferable that some or all of the hydrogen atoms of the alkylene group of Y' are substituted with fluorine atoms. The number of carbon atoms of the alkylene group of Y' is preferably 1 to 6, more preferably 1 to 4, and further preferably 1 to 3. In general formula (aa), it is preferable that both X and Y' are fluorine atom-containing groups.

[0039] From the viewpoint of further improving the light propagation efficiency of the optical waveguide, the refractive index of the polyimide resin (A) of the present embodiment is preferably 1.58 or less, more preferably 1.56 or less, even more preferably 1.55 or less, and even more preferably 1.54 or less, and the lower limit is not particularly limited, but is, for example, 1.50 or more. The refractive index of the polyimide resin (A) refers to a refractive index measured using an Abbe refractometer under conditions of 23° C. and 589 nm.

[0040] The weight average molecular weight (Mw) of the polyimide resin (A) of the present embodiment is, from the viewpoint of further suppressing thermal shrinkage of the optical waveguide, preferably 5,000 or more, more preferably 7,000 or more, even more preferably 10,000 or more, even more preferably 30,000 or more, and even more preferably 40,000 or more, and from the viewpoint of further improving the solubility in organic solvents, is preferably 200,000 or less, more preferably 150,000 or less, even more preferably 130,000 or less, and even more preferably 110,000 or less. The weight average molecular weight can be determined by gel permeation chromatography (GPC) using polystyrene as a standard substance.

[0041] The polyimide resin (A) of the present embodiment can be obtained, for example, by (i) first synthesizing a polyamide by reacting (condensation polymerization) a diamine with an acid dianhydride, and then (ii) imidizing the polyamide (ring-closing reaction). Specific reaction conditions can be, for example, known conditions.

[0042] Examples of diamines used as raw materials in synthesizing the polyimide resin (A) of this embodiment include 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 3,4'-diaminodiphenyl ether (3,4'-ODA), 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl (TFMB), 3,3',5,5'-tetramethylbenzidine, and 2,3,5,6-tetramethyl-1,4-phenylenediamine. , 3,3'-diaminodiphenyl sulfone, 3,3'-dimethylbenzidine, 3,3'-bis(trifluoromethyl)benzidine, 2,2'-bis(p-aminophenyl)hexafluoropropane, bis(trifluoromethoxy)benzidine (TFMOB), 2,2'-bis(pentafluoroethoxy)benzidine (TFEOB), 2,2'-trifluoromethyl-4,4'-oxydianiline (OBABTF), 2-phenyl-2-trifluoromethyl-bis(p-aminophenyl)methane, 2-phenyl-2-trifluoromethyl-bis(p-aminophenyl)methane, bis(m-aminophenyl)methane, 2,2'-bis(2-heptafluoroisopropoxy-tetrafluoroethoxy)benzidine (DFPOB), 2,2-bis(m-aminophenyl)hexafluoropropane (6-FmDA), 2,2-bis(3-amino-4-methylphenyl)hexafluoropropane, 3,6-bis(trifluoromethyl)-1,4-diaminobenzene (2TFMPDA), 1-(3,5-diaminophenyl)-2,2-bis(trifluoromethyl)-3,3,4,4,5,5,5-heptafluoropentane, 3,5- Examples of such compounds include diaminobenzotrifluoride (3,5-DABTF), 3,5-diamino-5-(pentafluoroethyl)benzene, 3,5-diamino-5-(heptafluoropropyl)benzene, 2,2'-dimethylbenzidine (DMBZ), 2,2',6,6'-tetramethylbenzidine (TMBZ), 3,6-diamino-9,9-bis(trifluoromethyl)xanthene (6FCDAM), 3,6-diamino-9-trifluoromethyl-9-phenylxanthene (3FCDAM), and 3,6-diamino-9,9-diphenylxanthene. The diamines may be used alone or in combination of two or more.

[0043] Examples of acid dihydrates used as raw materials for synthesizing the polyimide resin (A) of this embodiment include 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride, 4,4'-oxydiphthalic dianhydride, pyromellitic dianhydride (PMDA), diphenylether-3,3',4,4'-tetracarboxylic dianhydride (ODPA), benzophenone-3,3',4,4'-tetracarboxylic dianhydride (BTDA), Examples of such compounds include biphenyl-3,3',4,4'-tetracarboxylic dianhydride (BPDA), diphenylsulfone-3,3',4,4'-tetracarboxylic dianhydride (DSDA), diphenylmethane-3,3',4,4'-tetracarboxylic dianhydride, 2,2-bis(3,4-phthalic anhydride)propane, and 2,2-bis(3,4-phthalic anhydride)-1,1,1,3,3,3-hexafluoropropane (6FDA). The acid dihydrate may be used alone or in combination of two or more kinds.

[0044] The polyimide resin (A) of the present embodiment may be a single polyimide resin, or may contain two or more polyimide resins.

[0045] <Compound (B) Having a Cyclic Ether Structure> The resin composition of the present embodiment contains a compound (B) having a cyclic ether structure. The compound (B) having a cyclic ether structure in this embodiment preferably contains at least one or more types selected from the group consisting of epoxy resins and oxetane compounds, and more preferably contains one or more types of epoxy resins.

[0046] The content of the compound (B) having a cyclic ether structure contained in the resin composition of this embodiment, when the total content of the resin components in the resin composition is 100 parts by mass, is preferably 20 parts by mass or more, more preferably 25 parts by mass or more, even more preferably 30 parts by mass or more, and even more preferably 35 parts by mass or more, from the viewpoint of further suppressing the propagation loss of the optical-electrical composite substrate, and is preferably 80 parts by mass or less, more preferably 75 parts by mass or less, from the viewpoint of further suppressing the propagation loss of the optical-electrical composite substrate.

[0047] The compound (B) having a cyclic ether structure of this embodiment preferably contains an alicyclic structure in the molecule. Here, the compound (B) having a cyclic ether structure contains an alicyclic structure in the molecule means that it contains an alicyclic structure in addition to the cyclic ether structure. However, the alicyclic structure of this embodiment includes a condensed ring structure in which a cyclic ether and an aliphatic ring are condensed, and a spiro ring structure in which a cyclic ether and an aliphatic ring are bonded by a spiro bond atom. The number of ring members in the alicyclic structure is not particularly limited, but is preferably a 4- to 10-membered ring, more preferably a 4- to 8-membered ring, even more preferably a 5- or 6-membered ring, and even more preferably a 6-membered ring.

[0048] The compound (B) having a cyclic ether structure of this embodiment preferably contains two or more cyclic ether structures in the molecule, and more preferably contains two or three cyclic ether structures in the molecule.

[0049] The compound (B) having a cyclic ether structure of the present embodiment is preferably liquid at 23° C. from the viewpoint of ease of handling during production of the resin composition.

[0050] From the viewpoint of further improving the light propagation efficiency of the optical waveguide, the refractive index of the compound (B) having a cyclic ether structure of this embodiment is preferably 1.55 or less, more preferably 1.53 or less, and even more preferably 1.52 or less, and the lower limit is not particularly limited, but is, for example, 1.45 or more. The refractive index of the compound (B) having a cyclic ether structure means a refractive index measured using an Abbe refractometer under conditions of 23° C. and 589 nm.

[0051] The compound (B) having a cyclic ether structure in this embodiment may be a compound having one type of cyclic ether structure, or may contain compounds having two or more types of cyclic ether structures.

[0052] <Photopolymerization initiator (C)> The resin composition of the present embodiment contains a photopolymerization initiator (C). The photopolymerization initiator (C) of the present embodiment is not particularly limited, and a photocationic polymerization initiator, a photoradical polymerization initiator, or the like can be used.

[0053] The photopolymerization initiator (C) of this embodiment preferably contains a cationic photopolymerization initiator. The photocationic polymerization initiator includes, for example, a sulfonium salt type polymerization initiator and an iodonium salt type polymerization initiator, preferably a sulfonium salt type polymerization initiator, more preferably a triarylsulfonium salt type polymerization initiator, and further preferably a triphenylsulfonium salt type polymerization initiator.

[0054] The anion site of the cationic photopolymerization initiator of the present embodiment preferably contains a fluorine atom.

[0055] The anion moiety of the cationic photopolymerization initiator of this embodiment preferably contains an aryl group. The aryl group is, for example, an aryl group having 6 to 14 carbon atoms (not including the number of carbon atoms of the following substituents), in which some of the hydrogen atoms in the aryl group are replaced with an alkyl group having 1 to 18 carbon atoms, an alkyl group having 1 to 8 carbon atoms substituted with a halogen atom, an alkenyl group having 2 to 18 carbon atoms, an alkynyl group having 2 to 18 carbon atoms, an aryl group having 6 to 14 carbon atoms, a nitro group, a hydroxyl group, a cyano group, -OR 1 an alkoxy group or an aryloxy group represented by the formula: 2 An acyl group represented by CO-, R 3 Acyloxy group represented by COO-, -SR4 an alkylthio group or an arylthio group represented by the formula -NR 5 R 6 or a halogen atom. Also, R 1 ~R 4 is an alkyl group having 1 to 8 carbon atoms or an aryl group having 6 to 14 carbon atoms, R 5 and R 6 is a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or an aryl group having 6 to 14 carbon atoms. The aryl group is preferably one in which some of the hydrogen atoms in the aryl group have been substituted with fluorine atoms.

[0056] The content of the photopolymerization initiator (C) contained in the resin composition of this embodiment, when the total content of the resin components in the resin composition is 100 parts by mass, is, from the viewpoint of further suppressing the propagation loss of the photoelectric composite substrate, preferably 0.01 parts by mass or more, more preferably 0.03 parts by mass or more, even more preferably 0.05 parts by mass or more, and even more preferably 0.07 parts by mass or more, and is preferably 5.00 parts by mass or less, more preferably 3.00 parts by mass or less, even more preferably 1.00 parts by mass or less, even more preferably 0.50 parts by mass or less, even more preferably 0.30 parts by mass or less, even more preferably 0.20 parts by mass or less, and even more preferably 0.17 parts by mass or less.

[0057] The photopolymerization initiator (C) of this embodiment may be a single photopolymerization initiator, or may contain two or more photopolymerization initiators.

[0058] <Surfactant (D)> The resin composition of the present embodiment may further contain a surfactant (D) from the viewpoint of further improving the leveling property. The surfactant (D) includes, for example, a silicone-based surfactant, a fluorine-based surfactant, etc., and preferably includes a silicone-based surfactant. The surfactant (D) of the present embodiment may be a single surfactant, or may contain two or more surfactants.

[0059] The content of the surfactant (D) contained in the resin composition of this embodiment, when the total content of the resin components in the resin composition is 100 parts by mass, is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.07 parts by mass or more, and is preferably 3.0 parts by mass or less, more preferably 1.0 parts by mass or less, even more preferably 0.7 parts by mass or less, even more preferably 0.5 parts by mass or less, and even more preferably 0.3 parts by mass or less.

[0060] <Organic solvent (E)> The resin composition of the present embodiment may contain an organic solvent (E). When the resin composition of the present embodiment contains an organic solvent (E), it can be made into a varnish-like resin composition.

[0061] Examples of the organic solvent (E) in this embodiment include acetone, methyl ethyl ketone, methyl amyl ketone, toluene, propylene glycol monomethyl ether, propylene glycol methyl ethyl ether, propylene glycol dimethyl ether, propylene glycol 1-monomethyl ether 2-acetate, diethylene glycol ethyl methyl ether, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, benzyl alcohol, propylene carbonate, ethylene glycol diacetate, propylene glycol diacetate, propylene glycol monomethyl ether acetate, dipropylene glycol methyl-n-propyl ether, butyl acetate, γ-butyrolactone, methyl lactate, ethyl lactate, and butyl lactate. The organic solvent (E) in the present embodiment may be a single organic solvent, or may contain two or more organic solvents.

[0062] When the resin composition of the present embodiment contains an organic solvent (E), the concentration of all solids (non-volatile components) in the resin composition is preferably 10 mass % or more, more preferably 20 mass % or more, even more preferably 30 mass % or more, and even more preferably 35 mass % or more, from the viewpoint of appropriately controlling the viscosity of the resin composition, and is preferably 60 mass % or less, more preferably 55 mass % or less, and even more preferably 50 mass % or less, from the viewpoint of sufficiently dissolving each component in the resin composition.

[0063] <Other ingredients> The resin composition of the present embodiment may further contain, for example, a curing assistant, a leveling agent, a colorant, a storage stabilizer, a plasticizer, a filler, inorganic particles, a deterioration inhibitor, a wettability improver, an antistatic agent, etc. The content of the other components is an appropriate amount.

[0064] The total content of the polyimide resin (A), the compound (B) having a cyclic ether structure, and the photopolymerization initiator (C) in the resin composition of this embodiment, when the total content of all components in the resin composition is 100 mass%, is preferably 10 mass% or more, more preferably 20 mass% or more, even more preferably 30 mass% or more, even more preferably 35 mass% or more, even more preferably 50 mass% or more, even more preferably 70 mass% or more, even more preferably 80 mass% or more, even more preferably 85 mass% or more, even more preferably 90 mass% or more, even more preferably 95 mass% or more, even more preferably 97 mass% or more, even more preferably 99 mass% or more, and the upper limit is not particularly limited, but is, for example, 100 mass% or less.

[0065] The total content of the polyimide resin (A), the compound having a cyclic ether structure (B), the photopolymerization initiator (C), the surfactant (D) and the organic solvent (E) in the resin composition of this embodiment is preferably 50 mass% or more, more preferably 60 mass% or more, even more preferably 70 mass% or more, even more preferably 80 mass% or more, even more preferably 90 mass% or more, even more preferably 95 mass% or more, and even more preferably 100 mass%, when the total content of all components in the resin composition is 100 mass%.

[0066] [Method of producing resin composition] The resin composition of the present embodiment can be obtained, for example, by mixing the respective components. The film-like resin composition of the present embodiment can be obtained, for example, by applying a varnish-like resin composition onto a substrate film and drying it.

[0067] [Resin film] The resin film of the present embodiment is a resin film made of the resin composition of the present embodiment. The resin film of the present embodiment includes not only a resin film alone but also a resin film formed on a substrate film.

[0068] The light transmittance of the resin film of this embodiment at a wavelength of 850 nm is preferably 80% or more, more preferably 85% or more, even more preferably 90% or more, even more preferably 95% or more, and even more preferably 98% or more, from the viewpoint of further improving the light propagation efficiency of the optical waveguide. The light transmittance at a wavelength of 850 nm can be measured by an ultraviolet-visible spectrophotometer.

[0069] The thickness of the resin film in this embodiment is preferably 1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, even more preferably 15 μm or more, and even more preferably 20 μm or more, and from the viewpoint of further improving the light propagation efficiency of the optical waveguide, it is preferably 150 μm or less, more preferably 100 μm or less, even more preferably 40 μm or less, and even more preferably 30 μm or less.

[0070] The resin film of the present embodiment can be obtained by a known method for forming a coating film using, for example, the varnish-like resin composition of the present embodiment as a raw material.

[0071] [film] The film of the present embodiment includes a resin layer formed from the resin composition of the present embodiment. The film of this embodiment is preferably a dry film.

[0072] The film of the present embodiment is preferably a film that allows the optical waveguide to be manufactured by a sequential lamination process.

[0073] Here, the sequential lamination process will be described with reference to Fig. 1. The sequential lamination process of this embodiment refers to a manufacturing process for an optical waveguide in which at least the following steps (i) and (ii) are carried out in this order. Step (i): Forming the core layer 30 on the first clad layer 20 Step (ii): After step (ii), a step of forming a second clad layer 40 on the core layer 30 That is, the sequential lamination process is a process in which the first cladding layer 20, the core layer 30, and the second cladding layer 40 are laminated in order to form an optical waveguide. The sequential lamination process may appropriately include other steps in addition to the steps (i) and (ii), such as a step of forming a first clad layer 20 on the substrate 110 before the step (i) and a step of forming a pattern on the core layer 30.

[0074] The film of this embodiment may be a film for forming the first cladding layer 20, or a film for forming the second cladding layer 40.

[0075] From the viewpoint of further improving the handleability of the film, the thickness of the film of this embodiment is preferably 10 μm or more, more preferably 30 μm or more, even more preferably 50 μm or more, even more preferably 80 μm or more, even more preferably 100 μm or more, and is preferably 250 μm or less, more preferably 200 μm or less, even more preferably 150 μm or less, even more preferably 130 μm or less.

[0076] The thickness of the resin layer in this embodiment is preferably 1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, even more preferably 15 μm or more, and even more preferably 20 μm or more, and from the viewpoint of further improving the light propagation efficiency of the optical waveguide, it is preferably 150 μm or less, more preferably 100 μm or less, even more preferably 40 μm or less, and even more preferably 30 μm or less.

[0077] The film of the present embodiment preferably further includes a base film, and a resin layer is provided on the base film. The base film may be, for example, a resin film. The resin constituting the base film is not particularly limited, but it is preferable that the base film contains at least one or more types selected from the group consisting of polyimide and polyethylene terephthalate.

[0078] From the viewpoint of further improving the handleability of the film, the thickness of the base film in this embodiment is preferably 10 μm or more, more preferably 15 μm or more, even more preferably 20 μm or more, and is preferably 100 μm or less, more preferably 80 μm or less, even more preferably 60 μm or less, even more preferably 40 μm or less.

[0079] The substrate film of the present embodiment may be subjected to a surface treatment such as an antistatic treatment or a release treatment.

[0080] The film of the present embodiment may further include a cover film. The cover film is preferably provided so as to be in direct contact with the resin layer. When the film of the present embodiment includes a base film, the cover film is preferably provided on the surface of the resin layer opposite to the base film. The cover film is not particularly limited, but for example, an OPP cover film can be used.

[0081] The film of the present embodiment can be obtained, for example, by applying the varnish-like resin composition of the present embodiment onto a substrate film and drying it. Examples of the application method include a direct application method using various coater devices such as a pin coater, a die coater, a comma coater, and a curtain coater, and a printing method such as screen printing.

[0082] [Film set] The film set of this embodiment includes a first film and a second film, and at least one of the first film and the second film is the film of this embodiment. In the film set of this embodiment, both the first film and the second film may be the film of this embodiment.

[0083] [Optical waveguide] The optical waveguide of this embodiment will be described with reference to FIG. The optical waveguide 100 of this embodiment is an optical waveguide in which a first clad layer 20, a core layer 30, and a second clad layer 40 are laminated in this order, and at least one of the first clad layer 20 and the second clad layer 40 contains the resin composition of this embodiment. In the optical waveguide of this embodiment, both the first cladding layer 20 and the second cladding layer 40 may contain the resin composition of this embodiment.

[0084] When the optical waveguide 100 is provided on a substrate 110, it is preferable that the first cladding layer 20 be on the substrate 110 side. When the first cladding layer 20 faces the substrate 110, the preferred thicknesses of the first cladding layer 20 and the second cladding layer 40 are as follows. The thickness of the first cladding layer 20 is preferably 1 μm or more, more preferably 3 μm or more, even more preferably 5 μm or more, even more preferably 8 μm or more, even more preferably 10 μm or more, even more preferably 15 μm or more, and even more preferably 20 μm or more, and from the viewpoint of further improving the optical propagation efficiency of the optical waveguide, it is preferably 150 μm or less, more preferably 100 μm or less, even more preferably 70 μm or less, even more preferably 50 μm or less, even more preferably 40 μm or less, and even more preferably 30 μm or less. The thickness of the second cladding layer 40 is, from the viewpoint of further suppressing thermal shrinkage of the optical waveguide and further suppressing propagation loss of the optical-electrical composite substrate, preferably 1 μm or more, more preferably 3 μm or more, even more preferably 5 μm or more, even more preferably 8 μm or more, and is preferably 150 μm or less, more preferably 100 μm or less, even more preferably 70 μm or less, even more preferably 50 μm or less, even more preferably 40 μm or less, even more preferably 30 μm or less, even more preferably 20 μm or less.

[0085] The material for forming the core layer 30 is not particularly limited, but it is formed from, for example, a resin composition. The resin for forming the core layer 30 may be, for example, a resin used for the core of a known optical waveguide, but preferably contains a cyclic olefin resin, and more preferably contains a norbornene resin.

[0086] The resin composition for forming the core layer 30 preferably contains a photopolymerization initiator, and more preferably the photopolymerization initiator contained in the resin composition for forming the core layer 30 has the same chemical structure as the photopolymerization initiator (C) contained in the resin composition that can be used for the optical waveguide clad. The inventors consider that when the photopolymerization initiator contained in the resin composition for forming the core layer 30 has the same chemical structure as the photopolymerization initiator (C) contained in the resin composition that can be used for the optical waveguide clad, the acid derived from the photopolymerization initiator can be further inhibited from migrating between the clad layer and the core layer, and the propagation loss of the obtained optical-electrical composite substrate can be further suppressed.

[0087] The core layer 30 may contain components such as an antioxidant as appropriate.

[0088] The thickness of the core layer 30 is preferably 1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, even more preferably 20 μm or more, even more preferably 30 μm or more, and preferably 100 μm or less, more preferably 80 μm or less, even more preferably 60 μm or less, even more preferably 50 μm or less.

[0089] A waveguide pattern may be formed in the core layer 30. That is, a first core portion 35 and a second core portion 36 may be formed. Examples of a method for forming a waveguide pattern include an exposure method, an etching method, and a replication method.

[0090] A mirror may be formed on the optical waveguide 100, and a mirror on the light-emitting element side and a mirror on the light-receiving element side may be formed. As a method for forming the mirror, for example, a method for forming an inclined surface by laser processing or the like can be mentioned.

[0091] In addition to the first cladding layer 20, the core layer 30, and the second cladding layer 40, the optical waveguide 100 may include other layers as long as the excellent performance of the optical waveguide 100 is not adversely affected.

[0092] [Optical / electrical composite circuit board] The optical and electrical composite substrate of this embodiment will be described with reference to FIG. The optical / electrical composite substrate 200 includes a substrate 110 and an optical waveguide 100 provided on the substrate 110 .

[0093] Examples of the substrate 110 include a printed circuit board and a flexible substrate, and the like. A flexible substrate is preferable, and a flexible double-sided copper-clad laminate is more preferable. The substrate 110 may have a through hole.

[0094] The optical / electrical composite substrate 200 may include a light receiving element, a light emitting element, and the like.

[0095] The optical-electrical composite substrate 200 is obtained, for example, by (i) forming a first clad layer 20 on a substrate 110, (ii) forming a core layer 30 on the first clad layer 20, and (iii) forming a second clad layer 40 on the core layer 30. Examples of methods for forming each layer include methods in which films for forming each layer are laminated in order by roll lamination, vacuum roll lamination, flat plate lamination, vacuum flat plate lamination, atmospheric pressing, vacuum pressing, etc.

[0096] [Electronic components] The electronic component of this embodiment includes the optical / electrical composite substrate of this embodiment. Examples of the electronic components of this embodiment include electronic components in electronic devices such as mobile phones, game machines, router devices, WDM devices, personal computers, televisions, and home servers.

[0097] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. Furthermore, the present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES

[0098] The present embodiment will be described in detail below based on examples and comparative examples. Note that the present embodiment is not limited to the descriptions of these examples.

[0099] [Raw materials] First, the raw materials used in the examples and comparative examples will be described.

[0100] (Synthesis of polyimide resin (A-1)) 67.3g (0.210 mol) of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 97.7g (0.220 mol) of 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride, and 495g of dimethylacetamide were charged into a 3L glass separable flask equipped with a stirrer and agitator blade, and dissolved by stirring. The mixture was further stirred at room temperature for 12 hours under a nitrogen stream to carry out a polymerization reaction, yielding a polyamic acid solution.

[0101] After adding 16 g of pyridine to the obtained polyamic acid solution, 82 g of acetic anhydride was added dropwise at room temperature. The liquid temperature was then kept at 20 to 100° C. and the mixture was stirred for 24 hours to carry out an imidization reaction, thereby obtaining a polyimide solution.

[0102] The obtained polyimide solution was stirred in a 5L container and poured into 1,000g of methanol to precipitate the polyimide resin. The solid polyimide resin was then filtered using a suction filter and washed with 1,000g of methanol. The solid polyimide resin was then dried at 100°C for 24 hours using a vacuum dryer and then dried at 200°C for 3 hours to obtain a powdered polyimide resin (A-1). The weight average molecular weight (Mw) of the polyimide resin (A-1) measured by GPC was 51,000. 1 H-NMR was measured, and the imidization rate was calculated from the quantitative value of the amide peak relative to the peak of the aromatic ring of the polyimide, and the imidization rate was found to be 99% or more. Polyimide resin (A-1) was dissolved in propylene glycol monomethyl ether acetate to a solid content of 25%, and then coated with an applicator to a film thickness of 30 μm, and dried in an oven at 100° C. for 10 minutes to obtain a polyimide coating film. The refractive index of the obtained coating film was measured under conditions of 23° C. and 589 nm using an Abbe refractometer (manufactured by Atago Co., Ltd., product name: NAR-1T SOLID), and the refractive index of the polyimide was 1.54.

[0103] Details of the raw materials for each component in Table 1 are as follows:

[0104] <Polyimide resin (A)> (A-1) Polyimide resin synthesized above (Mw = 51,000, imidization rate 99% or more, refractive index n = 1.54)

[0105] [ka]

[0106] <Compound (B) Having a Cyclic Ether Structure> (B-1) Celloxide 2021P (manufactured by Daicel Corporation, epoxy resin having an alicyclic structure, liquid at 23°C, refractive index 1.51)

[0107] [ka]

[0108] <Photopolymerization initiator (C)> (C-1) CPI-310B (San-Apro Co., Ltd., photocationic polymerization initiator, triarylsulfonium salt) (C-2) CPI-310FG (San-Apro Co., Ltd., photocationic polymerization initiator, triarylsulfonium salt)

[0109] <Surfactant (D)> (D-1) BYK-333 (BYK Japan Co., Ltd., silicone surfactant)

[0110] <Organic solvent (E)> (E-1) Propylene glycol monomethyl ether acetate (E-2) Propylene glycol monomethyl ether

[0111] <Thermal polymerization initiator (F)> (F-1) San-Aid SI-110 (manufactured by Sanshin Chemical Industry Co., Ltd., thermal cationic polymerization initiator) (F-2) San-Aid SI-150 (manufactured by Sanshin Chemical Industry Co., Ltd., thermal cationic polymerization initiator)

[0112] [Creating film for forming core layer] (Synthesis of polymer for forming core layer) In a glove box filled with dry nitrogen, with both moisture and oxygen concentrations controlled to 1 ppm or less, 7.2 g (40.1 mmol) of hexylnorbornene (HxNB) and 12.9 g (40.1 mmol) of diphenylmethylnorbornene methoxysilane were weighed into a 500 mL vial, 60 g of dehydrated toluene and 11 g of ethyl acetate were added, and the vial was covered with a silicone sealer and sealed at the top. Next, 1.56 g (3.2 mmol) of Ni catalyst and 10 mL of dehydrated toluene were weighed into a 100 mL vial, a stirrer tip was inserted and the vial was sealed, and the Ni catalyst was thoroughly stirred to completely dissolve, obtaining a Ni catalyst solution. 1 mL of the Ni catalyst solution was accurately weighed with a syringe and quantitatively injected into the vial in which the above two types of norbornene were dissolved, and stirred at room temperature for 1 hour, whereupon a significant increase in viscosity was confirmed. At this point, the stopper was removed, 60 g of tetrahydrofuran (THF) was added and stirred to obtain a reaction solution. 9.5 g of acetic anhydride, 18 g of hydrogen peroxide (concentration 30%), and 30 g of ion-exchanged water were added to a 100 mL beaker and stirred to prepare an aqueous solution of peracetic acid. Next, the entire amount of the aqueous solution of peracetic acid was added to the reaction solution and stirred for 12 hours to carry out the reduction treatment of Ni. Next, the reaction solution after the treatment was transferred to a separatory funnel, and after removing the lower aqueous layer, 100 mL of a 30% aqueous solution of isopropyl alcohol was added and vigorously stirred. After leaving it to stand and completely separating into two layers, the aqueous layer was removed. After repeating this water washing process three times in total, the oil layer was dropped into a large excess of acetone to reprecipitate the produced polymer, which was separated from the filtrate by filtration and then heated and dried for 12 hours in a vacuum dryer set at 60°C to obtain a polymer for forming the core layer.

[0113] The molecular weight of the core layer-forming polymer was measured by GPC and found to be Mw = 100,000 and Mn = 40,000. The molar ratio of each structural unit in the core layer-forming polymer was identified by NMR measurement and found to be 50 mol% for hexylnorbornene structural units and 50 mol% for diphenylmethylnorbornene methoxysilane structural units.

[0114] (Preparation of resin composition for forming core layer) 10 g of the purified polymer for forming the core layer was weighed into a 100 mL glass container, and 3 g of methylcyclohexane, 27 g of toluene, 2.4 g of Aron Oxetane (manufactured by Toagosei Co., Ltd., product name: OXT-213), 0.8 g of Celloxide 2021P (manufactured by Daicel Corporation, epoxy resin), 0.4 g of Celloxide 2000 (manufactured by Daicel Corporation, epoxy resin), 0.5 g of CPI-310B (manufactured by San-Apro Co., Ltd., photopolymerization reaction product), and 100 g of ethyl cyclohexane (manufactured by San-Apro Co., Ltd., photopolymerization reaction product) were added to the container. 0.06 g of a cationic polymerization initiator, 0.003 g of Curezol C11z (manufactured by Shikoku Kasei Corporation, an imidazole-based compound), 0.1 g of Irgafox168 (manufactured by BASF, a phosphorus-based antioxidant), and 0.025 g of Irganox1076 (manufactured by BASF, a hindered phenol-based antioxidant) were added and dissolved uniformly, and then the mixture was filtered through a 0.2 μm PTFE filter to obtain a resin composition for forming a core layer.

[0115] (Creating a film for forming a core layer) The obtained core layer forming resin composition was applied to a release-treated PET substrate using an applicator so that the film thickness after drying would be 40 μm. After application, the substrate was placed in a 45° C. dryer for 5 minutes to completely remove the solvent, and then an OPP cover film (manufactured by Oji F-Tex Co., Ltd., product name: E201F-50 μm) was attached to the surface of the resin layer formed by the resin composition to obtain a core layer forming film.

[0116] [Creation of film for forming second cladding layer] (Preparation of Resin Composition for Forming Second Clad Layer) 300.6 parts by mass of toluene, 91.7 parts by mass of Septon Q1250 (Kuraray Co., Ltd., rubber-based elastomer), 2.8 parts by mass of BYK-361N (BYK Japan Co., Ltd., acrylic polymer-based surfactant), 2.8 parts by mass of X-12-1281C (Shin-Etsu Chemical Co., Ltd., silane coupling agent), and 2.8 parts by mass of Curesol C11z (Shikoku Kasei Co., Ltd., imidazole-based compound) were stirred at room temperature until each raw material was completely dissolved, to obtain a solution. Then, the solution was filtered through a PTFE filter with a pore size of 0.2 μm to obtain a resin composition for forming a second clad layer.

[0117] (Preparation of film for forming second cladding layer) The resin composition for forming the second clad layer was applied as a varnish using an applicator onto a 25 μm thick polyimide substrate (manufactured by UBE Corporation, product name: Upilex 25S) so that the film thickness after drying would be 10 μm. The film was then dried at 160°C for 10 minutes, and finally an OPP cover film (manufactured by Oji F-Tex Corporation, product name: E201F-50 μm) was attached to the surface of the resin layer formed by the resin composition to obtain a film for forming a second clad layer.

[0118] [Examples 1 to 7 and Comparative Example 1] (Preparation of resin composition) The raw materials mixed according to Table 1 were stirred at room temperature until the raw materials were completely dissolved to obtain a solution. The solution was then filtered through a PTFE filter having a pore size of 0.2 μm to obtain varnish-like resin compositions of Examples 1 to 7 and Comparative Example 1, respectively.

[0119] (Film Creation) A varnish was applied using an applicator onto a 38 μm thick antistatic treated polyethylene terephthalate substrate (manufactured by Nippa Corporation, product name: PET38×1-TR1-ASQ, hereafter referred to as PET substrate) so that the dried thickness would be 25 μm, and then dried at 100° C. for 10 minutes. Finally, an OPP cover film (manufactured by Oji F-Tex Corporation, product name: E201F-50 μm) was attached to the surface of the resin layer formed by the resin composition to create a film, thereby obtaining the films of Examples 1 to 7 and Comparative Example 1, respectively.

[0120] (Step of laminating the substrate and the first clad layer) A double-sided copper-clad laminate was placed on a stainless steel plate as a substrate. The OPP cover film of the films of Examples 1 to 7 and Comparative Example 1 was peeled off, and the double-sided copper-clad laminate and the films of Examples 1 to 7 and Comparative Example 1 were overlapped with each other so that the surface of the double-sided copper-clad laminate opposite to the stainless steel plate was in contact with the resin layer of the films of Examples 1 to 7 and Comparative Example 1. Next, the double-sided copper-clad laminate and the films of Examples 1 to 7 and Comparative Example 1 were laminated using a vacuum laminator (manufactured by Nikko Materials Co., Ltd., product name: CVP-300) under conditions of temperature: 140°C, pressure: 0.5 MPa, and time: 120 seconds, to obtain laminates with a layer structure of "double-sided copper-clad laminate / first clad layer / PET substrate". The PET substrate in the laminate was the PET substrate derived from the films of Examples 1 to 7 and Comparative Example 1.

[0121] (Step of Heating the First Clad Layer) The laminates having a layer structure of "double-sided copper-clad laminate / first clad layer / PET substrate" in Examples 1 to 7 were placed in a 140° C. oven for 30 minutes. In Comparative Example 1, the step of heating the first cladding layer was not carried out.

[0122] (Step of photocuring the first cladding layer) After the process of heating the first clad layer, the PET substrate surface of the laminate having the layer structure of "double-sided copper-clad laminate / first clad layer / PET substrate" in Examples 1 to 7 was irradiated with light under the conditions shown in Table 1 using a direct imaging exposure machine (manufactured by SCREEN Co., Ltd., product name: LS-9000), and after light irradiation, the first clad layer was photo-cured by placing the laminate in a 160°C oven for 30 minutes. In Comparative Example 1, the step of photocuring the first cladding layer was not carried out.

[0123] The PET substrate of the laminate having the layer structure of "double-sided copper-clad laminate / first clad layer / PET substrate" in Examples 1 to 7 and Comparative Example 1 was peeled off, and the laminate and the film for forming a core layer were superimposed so that the first clad layer of the laminate and the core layer of the film for forming a core layer were in contact with each other. At this time, the OPP cover film of the film for forming a core layer was peeled off. Next, the laminate and the film for forming a core layer were laminated using a vacuum laminator (manufactured by Nikko Materials Co., Ltd., product name: CVP-300) under the conditions of temperature: 60°C, pressure: 0.5 MPa, and time: 30 seconds to obtain a laminate of "double-sided copper-clad laminate / first clad layer / core layer / PET substrate". The PET substrate in the laminate is a PET substrate derived from the film for forming a core layer. In Examples 1 to 7, the step of laminating the core layer was carried out after the step of photocuring the first cladding layer.

[0124] (Process for forming a pattern on the core layer) The PET substrate was peeled off from the laminate having the layer structure of "double-sided copper-clad laminate / first clad layer / core layer / PET substrate" in Examples 1 to 7 and Comparative Example 1, and 20 lines and spaces, each 9 cm long and 50 μm wide, were created on the core layer using a direct imaging exposure machine (manufactured by SCREEN Co., Ltd., product name: LS-9000). The product was then placed in an oven at 150° C. for 30 minutes. When the product was removed from the oven, it was confirmed that a clear waveguide pattern (multiple core portions) with a rectangular cross section appeared on the coating.

[0125] (Step of laminating the second clad layer) After the process of forming a pattern on the core layer, the laminate and the film for forming a second clad layer were superimposed so that the core layer of the laminate having the layer structure of "double-sided copper-clad laminate / first clad layer / core layer" of Examples 1 to 7 and Comparative Example 1 and the second clad layer of the film for forming a second clad layer were in contact with each other. At this time, the OPP cover film of the film for forming a second clad layer was peeled off. Next, the laminate and the film for forming a second clad layer were laminated using a vacuum laminator (manufactured by Nikko Materials Co., Ltd., product name: CVP-300) under the conditions of temperature: 140°C, pressure: 0.5 MPa, and time: 210 seconds to obtain laminates having the layer structure of "double-sided copper-clad laminate / first clad layer / core layer / second clad layer / polyimide substrate". The polyimide substrate in the laminate is a polyimide substrate derived from the film for forming a second clad layer. In Examples 1-7, the obtained laminate was used as the optical / electrical composite substrate in Examples 1-7. In Comparative Example 1, the obtained laminate was heat-treated in an oven at 160° C. for 2 hours to obtain the optoelectronic composite substrate in Comparative Example 1.

[0126] [evaluation] The evaluation methods for the examples and comparative examples are described below.

[0127] <Optical loss evaluation> Both sides of the photoelectric composite substrates obtained in Examples 1 to 7 and Comparative Example 1 were cut by dicing so that the length of the pattern portion was 7 cm, to obtain samples for evaluating optical loss. The propagation loss [dB] of the sample for optical loss evaluation was evaluated in accordance with 4.6.2.1 Cutback method of "Test method for polymer optical waveguide (JPCA-PE02-05-01S-2008)". Note that light with a wavelength of 850 nm was used for the measurement. The results of the optical loss evaluation are shown in Table 1.

[0128] <Film appearance evaluation> (Creating a laminate) The OPP cover film was peeled off from the films of Examples 1 to 7 and Comparative Example 1, and the films of Examples 1 to 7 and Comparative Example 1 were overlapped with the PET film so that the resin layer of the films of Examples 1 to 7 and Comparative Example 1 was in contact with the PET film. Next, the films of Examples 1 to 7 and Comparative Example 1 were laminated with the PET film using a vacuum laminator (manufactured by Nikko Materials Co., Ltd., product name: CVP-300) under conditions of temperature: 140°C, pressure: 0.5 MPa, and time: 120 seconds to obtain laminates. The layer structure of the laminate was "PET film / resin layer for cladding layer / PET substrate derived from the films of Examples 1 to 7 and Comparative Example 1."

[0129] (Laminate Processing) The laminates of the films of Examples 1 to 7 and the PET film were placed in an oven at 140° C. for 30 minutes, and then irradiated with light under the conditions shown in Table 1. After the light irradiation, the laminates were placed in an oven at 160° C. for 30 minutes to obtain samples for appearance evaluation. The above-mentioned treatment of the laminate is a treatment that assumes a step of heating the first cladding layer and a step of photocuring the first cladding layer. In Comparative Example 1, the laminate was not treated and was used as a sample for evaluating appearance.

[0130] The resin layer for the cladding layer was observed using an optical measuring microscope (manufactured by Mitutoyo Corporation, product name: MF-UA1730THD) for the samples for appearance evaluation of Examples 1 to 7 and Comparative Example 1. The observation results were evaluated according to the following criteria. A (Good): No defects (grains of about 5 μm in size) observed B (bad): Defects (grains of about 5 μm in size) are observed. The results of the appearance evaluation are shown in Table 1.

[0131] [Table 1]

[0132] It can be seen from Table 1 that the optical / electrical composite substrate using the resin composition of the example in the cladding layer has a suppressed propagation loss compared to the optical / electrical composite substrate of the comparative example. That is, the resin composition of the present embodiment can suppress the propagation loss of the optical / electrical composite substrate.

[0133] Furthermore, the films of the examples had good results in the appearance evaluation. The present inventors believe that because the films of the examples had good appearance evaluation, it is possible to suppress the propagation loss of the photoelectric composite substrate. [Explanation of symbols]

[0134] 20 First cladding layer 30 Core Layer 35 First Core 36 Second Core 40 Second Cladding Layer 100 optical waveguide 110 Substrate 200 Photoelectric composite board

Claims

1. A resin composition that can be used for an optical waveguide clad, A resin composition comprising a polyimide resin (A), a compound having a cyclic ether structure (B), and a photopolymerization initiator (C).

2. 2. The resin composition according to claim 1, wherein the content of the photopolymerization initiator (C) contained in the resin composition is 0.01 parts by mass or more and 5.0 parts by mass or less when the total content of the resin components in the resin composition is 100 parts by mass.

3. The resin composition according to claim 1 or 2, wherein the photopolymerization initiator (C) includes a photocationic polymerization initiator.

4. The resin composition according to claim 3 , wherein the photocationic polymerization initiator comprises a sulfonium salt type polymerization initiator.

5. 3. The resin composition according to claim 1, wherein a content of the polyimide resin (A) contained in the resin composition is 20 parts by mass or more and 80 parts by mass or less when a total content of resin components in the resin composition is 100 parts by mass.

6. The resin composition according to claim 1 or 2, wherein the polyimide resin (A) contains an imide ring structure in the molecule.

7. The resin composition according to claim 1 or 2, wherein the polyimide resin (A) has an imidization rate of 90% or more.

8. The resin composition according to claim 1 or 2, wherein the polyimide resin (A) comprises a fluorinated polyimide.

9. The resin composition according to claim 8 , wherein the fluorinated polyimide contains a structural unit represented by the following general formula (a): [Formula 1] In general formula (a), X is a divalent organic group, Y is a tetravalent organic group, and at least one of X and Y has a fluorine atom.

10. The resin composition according to claim 1 or 2, wherein the polyimide resin (A) has a refractive index of 1.50 or more and 1.58 or less.

11. The resin composition according to claim 1 or 2, wherein the content of the compound (B) having a cyclic ether structure is 20 parts by mass or more and 80 parts by mass or less when the total content of the resin components in the resin composition is 100 parts by mass.

12. The resin composition according to claim 1 or 2, wherein the compound (B) having a cyclic ether structure includes at least one or more compounds selected from the group consisting of epoxy resins and oxetane compounds.

13. The resin composition according to claim 12, wherein the compound (B) having a cyclic ether structure includes an epoxy resin.

14. The resin composition according to claim 1 or 2, wherein the compound (B) having a cyclic ether structure contains an alicyclic structure in the molecule.

15. The resin composition according to claim 1 or 2, wherein the compound (B) having a cyclic ether structure contains two or more cyclic ether structures in the molecule.

16. The resin composition according to claim 1 or 2, wherein the compound (B) having a cyclic ether structure is liquid at 23°C.

17. The resin composition according to claim 1 or 2, wherein the compound (B) having a cyclic ether structure has a refractive index of 1.45 or more and 1.55 or less.

18. A film that can be used for an optical waveguide clad, A film comprising a resin layer formed from the resin composition according to claim 1 or 2.

19. Further, the device includes a base film, The film according to claim 18 , wherein the resin layer is provided on the base film.

20. The film according to claim 19, wherein the resin constituting the base film comprises at least one or more selected from the group consisting of polyimide and polyethylene terephthalate.

21. 20. The film of claim 18, wherein the film is a dry film.

22. 20. The film of claim 18, which is a film capable of producing optical waveguides by a layer-by-layer process.

23. A film set that can be used for an optical waveguide clad, comprising: A first film and a second film, 20. A film set, wherein at least one of the first film and the second film is the film of claim 18.

24. An optical waveguide in which a first clad layer, a core layer, and a second clad layer are laminated in this order, An optical waveguide, wherein at least one of the first cladding layer and the second cladding layer comprises the resin composition according to claim 1 .

25. The resin composition for forming the core layer contains a photopolymerization initiator, The optical waveguide according to claim 24, wherein a photopolymerization initiator contained in a resin composition for forming the core layer has the same chemical structure as a photopolymerization initiator (C) contained in a resin composition that can be used for an optical waveguide clad.

26. A substrate; An optical / electrical composite substrate comprising: the optical waveguide according to claim 24 provided on the substrate.

27. An electronic component comprising the optical / electrical composite substrate according to claim 26.

Citation Information

Patent Citations

  • Optical and electrical wiring board and device for optical communication

    JP2006140233A

  • Photo-electric hybrid substrate

    JP2014238455A

  • Flexible optical waveguide, method for producing the same, and epoxy resin composition for flexible optical waveguide

    WO2008053888A1