Three-dimensional cross-linked gel polymer electrolyte as well as preparation method and application thereof
By using three-dimensional crosslinked gel polymer electrolyte in lithium-ion batteries, epoxy group grafting and in-situ coupling chemical reactions, the problem of initiator affecting performance is solved, and higher cycle stability and safety are achieved It is suitable for high-voltage lithium metal batteries.
Patent Information
- Application Number
- CN202411018709.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
During the preparation of lithium-ion batteries, adding initiators will affect the rate performance, cycle performance and high and low temperature performance of lithium-ion batteries. Common organic liquid electrolytes are prone to leakage of electrolytes, increasing safety hazards.
By grafting the epoxy groups onto the surface of inorganic nanoparticles, a three-dimensional crosslinked gel polymer electrolyte is formed by in situ coupling chemical reaction, using lithium tetrafluoroborate and lithium fluorine-containing salts as electrolyte salts, and cyclic ether monomers are carried out The in situ polymerization catalyzed by cations forms a polymer network with strong chemical interactions, avoiding the use of initiators.
Achieve more uniform dispersion of inorganic nanoparticles in lithium metal batteries, improve ion transportability, thermal stability, processability and interface contact, significantly inhibit the formation and growth of lithium dendrites, and improve the cyclic stability of the battery and Security.
Smart Images

Figure CN118970164A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries, and specifically relates to a three-dimensional cross-linked gel polymer electrolyte and a preparation method and application thereof. Background Art
[0002] Lithium metal anode materials have a high theoretical capacity (3680 mAh g -1 ) and low electrochemical potential (-3.04V vs. standard hydrogen electrode potential) have received extensive attention in recent years. However, the side reactions between common organic liquid electrolytes (LE) and lithium metal anodes lead to unstable solid electrolyte interfaces (SEI) and lithium dendrites, which severely limit the cycling stability of lithium metal batteries. In addition, there are more free phases in LE, which easily cause electrolyte leakage, thereby exacerbating the safety hazards of lithium batteries. In recent years, gel electrolytes (mixtures of polymer matrix and liquid solution, referred to as GPEs) have become the focus of research. They have a higher voltage window than LE, stronger mechanical properties, and better ionic conductivity than all-solid electrolytes. Secondly, GPEs can effectively avoid the safety risks caused by electrolyte leakage due to their reduced free mobile phase. More importantly, GPEs can be prepared by in-situ polymerization, which is highly compatible with the current state-of-the-art lithium-ion battery manufacturing industry. The in-situ polymerization method ensures that the electrode is fully wetted by LE before and after polymerization, which largely avoids the high interfacial resistance in batteries using traditional solid electrolytes. Therefore, lithium metal batteries containing polymer electrolytes obtained based on in-situ curing are considered to be highly promising next-generation energy storage devices.
[0003] The invention patent with application publication number CN115799625A discloses a polymer solid electrolyte, a solid battery and a preparation method thereof. The preparation method of the polymer solid electrolyte comprises the following steps: Step 1, dispersing grafted nano-silicon dioxide and lithium salt in polymer monomers to form a basic solution; Step 2, introducing an initiator into the basic solution to make the grafted nano-silicon dioxide and the polymer monomers in situ polymerize and solidify to form a solid electrolyte. Initiators are added during the preparation of the polymer solid electrolyte, and the initiators may react with the lithium metal negative electrode, affecting the rate performance, high and low temperature performance and cycle performance of the lithium-ion battery. Summary of the invention
[0004] The purpose of the present invention is to provide a three-dimensional cross-linked gel polymer electrolyte to solve the technical problem of adding an initiator during the preparation of the electrolyte, thereby affecting the performance of a lithium ion battery.
[0005] The second object of the present invention is to provide a method for preparing a three-dimensional cross-linked gel polymer electrolyte.
[0006] The third object of the present invention is to provide an application of a three-dimensional cross-linked gel polymer electrolyte.
[0007] In order to achieve the above purpose, the technical solution adopted by the present invention is:
[0008] A method for preparing a three-dimensional cross-linked gel polymer electrolyte comprises the following steps:
[0009] S1: Grafting epoxy groups onto the surface of inorganic nanoparticles to obtain inorganic nanoparticle modified products;
[0010] S2: adding the modified inorganic nanoparticles, mixed lithium salts and cyclic ether monomers into a solvent to obtain an ether-based precursor solution, and allowing the ether-based precursor solution to stand to obtain the product.
[0011] Furthermore, the mixed lithium salt is a mixed lithium salt of lithium tetrafluoroborate and a fluorine-containing lithium salt, and the mass ratio of the lithium tetrafluoroborate to the fluorine-containing lithium salt is 1:1-6, preferably 1:1-3.
[0012] Furthermore, the fluorine-containing lithium salt is one or more of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, and lithium bis(fluorosulfonyl)imide.
[0013] Furthermore, the standing in S2 is standing at room temperature for 12 to 36 hours.
[0014] Furthermore, the mass fraction of the inorganic nanoparticle modification in the solvent is 1-10%, preferably 4-8%; the mass fraction of the mixed lithium salt in the solvent is 5-20%, preferably 6-12%; the mass fraction of the cyclic ether monomer in the solvent is 10-50%, preferably 20-30%.
[0015] Furthermore, the preparation method of the inorganic nanoparticle modification is: using an in-situ coupling chemical reaction to graft the epoxy groups on the silane coupling agent onto the surface of the inorganic nanoparticles; the silane coupling agent is γ-(2,3-epoxypropoxy)propyltrimethoxysilane, and the inorganic nanoparticles are one or more of nano-titanium dioxide, nano-silicon dioxide, nano-zinc oxide, and nano-aluminum oxide, preferably nano-titanium dioxide and nano-silicon dioxide.
[0016] Furthermore, the cyclic ether monomer is one or more of epichlorohydrin, dioxolane, glycidyl phenyl ether, cyclopropyl phenyl sulfide, cyclohexyl sulfide, glycidyl methyl ether, and tetrahydrofuran, preferably epichlorohydrin, dioxolane, glycidyl phenyl ether, and cyclopropyl phenyl sulfide.
[0017] Furthermore, the solvent is one or more of ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol methylene ether, tetrahydropyran, and epichlorohydrin, preferably ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and tetrahydropyran.
[0018] A three-dimensional cross-linked gel polymer electrolyte is prepared by using the above-mentioned method for preparing the three-dimensional cross-linked gel polymer electrolyte.
[0019] Application of a three-dimensional cross-linked gel polymer electrolyte in lithium metal batteries.
[0020] Beneficial effects of the present invention:
[0021] The present invention grafts the epoxy groups on the silane coupling agent onto the surface of the inorganic nanoparticles through an in-situ coupling chemical reaction to achieve modification of the inorganic nanoparticles. The inorganic nanoparticle modifier is used as the particle hybridization center, lithium tetrafluoroborate and fluorine-containing lithium salt are used as electrolyte salts, and the cyclic ether compound is used as a monomer for cationic catalytic in-situ polymerization. The entire process is carried out inside the lithium metal battery. In this process, the epoxy groups grafted onto the surface of the inorganic nanoparticles can realize the transformation from the traditional weak physical contact between the organic / inorganic components to a strong chemical interaction, so that the inorganic nanoparticles are more evenly dispersed, thereby combining the advantages of the cyclic ether monomer, such as good processability, interface contact and electrode compatibility, with the advantages of the inorganic nanoparticle modifier, such as excellent ion transport, thermal stability, etc., so that the prepared three-dimensional cross-linked gel polymer electrolyte has excellent ion transport, thermal stability, good processability, interface contact and electrode compatibility compared with traditional commercial electrolytes.
[0022] The three-dimensional cross-linked gel polymer electrolyte generated by the invention is composed of polyether, and the three-dimensional cross-linked gel polymer electrolyte has excellent flexibility, high ion conductivity and is highly compatible with the lithium negative electrode.
[0023] The denser and more efficient three-dimensional cross-linked polymer network in the three-dimensional cross-linked gel polymer electrolyte prepared by the present invention has a higher solvent absorption capacity and better oxidation stability, and is suitable for the construction of a high-voltage lithium metal battery system. In addition, the strong interaction between the three-dimensional cross-linked polymer network of the three-dimensional cross-linked gel polymer electrolyte of the present invention and the solvent can reduce the Li + The desolvation barrier is favorable for Li + The uniform deposition of Li has a significant inhibitory effect on the formation and growth of lithium dendrites.
[0024] The fluorine-containing lithium salt used in the present invention has high oxidation stability and can be applied to high-voltage positive electrode material systems. Lithium tetrafluoroborate not only has good thermal stability, but also can improve the ion conductivity of the electrolyte. Lithium tetrafluoroborate is easily reduced to boron trifluoride on the surface of alkali metals. Boron trifluoride can be used as an initiator to catalyze the in-situ ring-opening polymerization of cyclic ether monomers, thereby avoiding the introduction of excess monomers.
[0025]
[0026] The process of in-situ ring-opening polymerization of cyclic ether monomers initiated by boron trifluoride formed by decomposition of lithium tetrafluoroborate can be carried out at room temperature without adding other initiators, which can significantly improve the defects caused by high-temperature free radical polymerization. The preparation method of the three-dimensional cross-linked gel polymer electrolyte is highly compatible with the preparation method of industrial lithium-ion batteries, and is expected to realize the commercialization of lithium metal batteries.
[0027] The three-dimensional cross-linked gel polymer electrolyte prepared by the present invention can greatly inhibit the irreversible interface change of the oxide positive electrode material and can effectively inhibit the side reaction of the three-dimensional cross-linked gel polymer electrolyte at the positive electrode interface. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 Graph showing the cycle performance of the lithium metal battery of Example 1 and a reference lithium metal battery;
[0029] Figure 2 Graph showing the cycle performance of the lithium metal battery of Example 2 and a reference lithium metal battery;
[0030] Figure 3 Graph showing the cycle performance of the lithium metal battery of Example 3 and a reference lithium metal battery;
[0031] Figure 4 Graph showing the cycle performance of the lithium metal battery of Comparative Example 1 and the reference lithium metal battery;
[0032] Figure 5 It is a cycle performance diagram of the lithium metal battery of Comparative Example 2 and the reference lithium metal battery. DETAILED DESCRIPTION
[0033] The present invention will be further described below in conjunction with the embodiments of the present invention and the accompanying drawings.
[0034] Example 1
[0035] The preparation method of the three-dimensional cross-linked gel polymer electrolyte of Example 1 comprises the following steps:
[0036] S1: Add 1g of nano-titanium dioxide to 10g of deionized water and disperse by ultrasonic for 0.5h to obtain a uniform and stable suspension. First, add 6g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane to the suspension, then add 10g of anhydrous ethanol, and mix by ultrasonic to obtain a mixed solution. The mixed solution is reacted in a constant temperature bath at 100℃ for 4h, and then centrifuged and vacuum dried to obtain γ-titanium dioxide;
[0037] S2: 0.4 g of γ-titanium dioxide, 0.5 g of lithium tetrafluoroborate, 0.5 g of lithium bis(trifluoromethanesulfonyl imide) and 2 g of 1,2-pentane were added to 10 g of ethylene glycol dimethyl ether in sequence, and the mixture was stirred thoroughly until the γ-titanium dioxide, lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl imide) and 1,2-pentane were completely dissolved to obtain an ether-based precursor solution. The ether-based precursor solution was allowed to stand at room temperature for 24 h to obtain a three-dimensional cross-linked gel polymer electrolyte.
[0038] The ether-based precursor solution in Example 1 is assembled together with a high-nickel positive electrode, a lithium metal negative electrode, a separator, a gasket and a spring and left at room temperature for 24 hours to obtain a lithium metal battery containing the three-dimensional cross-linked gel polymer electrolyte of Example 1.
[0039] Preparation method of reference electrolyte: add lithium bis(trifluoromethanesulfonyl imide) to ethylene carbonate solvent, stir thoroughly until lithium bis(trifluoromethanesulfonyl imide) is completely dissolved, and prepare lithium bis(trifluoromethanesulfonyl imide-ethylene carbonate solution with a concentration of 1 mol / L to obtain reference electrolyte.
[0040] The reference electrolyte is assembled together with a high-nickel positive electrode, a lithium metal negative electrode, a separator, a gasket and a spring to prepare a reference lithium metal battery.
[0041] Example 2
[0042] The preparation method of the three-dimensional cross-linked gel polymer electrolyte of Example 2 comprises the following steps:
[0043] S1: Add 1g of nano-silicon dioxide to 10g of deionized water and disperse by ultrasonic for 0.5h to obtain a uniform and stable suspension. First add 6g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane to the suspension, then add 10g of anhydrous ethanol, and mix by ultrasonic to obtain a mixed solution. The mixed solution is reacted in a constant temperature bath at 100℃ for 4h, centrifuged, and vacuum dried to obtain γ-silicon dioxide;
[0044] S2: 0.5 g of γ-silicon dioxide, 0.3 g of lithium tetrafluoroborate, 0.7 g of lithium bis(fluorosulfonyl)imide and 3 g of epichlorohydrin are added to 10 g of ethylene glycol diethyl ether in sequence, and stirred thoroughly until the γ-silicon dioxide, lithium tetrafluoroborate, lithium bis(fluorosulfonyl)imide and epichlorohydrin are completely dissolved to obtain an ether-based precursor solution. The ether-based precursor solution is allowed to stand at room temperature for 24 hours to obtain a three-dimensional cross-linked gel polymer electrolyte.
[0045] The ether-based precursor solution of Example 2 was assembled together with a high-nickel positive electrode, a lithium metal negative electrode, a separator, a gasket and a spring and left at room temperature for 24 hours to obtain a lithium metal battery containing a three-dimensional cross-linked gel polymer electrolyte.
[0046] Reference electrolyte: Add lithium bis(fluorosulfonyl)imide to diethyl carbonate solvent, stir thoroughly until the lithium bis(fluorosulfonyl)imide is completely dissolved, and prepare a lithium bis(fluorosulfonyl)imide-diethyl carbonate solution with a concentration of 1 mol / L to obtain a reference electrolyte.
[0047] The reference electrolyte is assembled together with a high-nickel positive electrode, a lithium metal negative electrode, a separator, a gasket and a spring to prepare a reference lithium metal battery.
[0048] Example 3
[0049] The preparation method of the three-dimensional cross-linked gel polymer electrolyte of Example 3 comprises the following steps:
[0050] S1: Add 1g of nano zinc oxide to 10g of deionized water and disperse by ultrasonic for 0.5h to obtain a uniform and stable suspension. First add 6g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane to the suspension, then add 10g of anhydrous ethanol, and mix by ultrasonic to obtain a mixed solution. The obtained mixed solution is reacted in a constant temperature bath at 100℃ for 4h, centrifuged, and vacuum dried to obtain γ-zinc oxide;
[0051] S2: 0.6 g of γ-zinc oxide, 0.6 g of lithium tetrafluoroborate, 0.6 g of lithium hexafluorophosphate and 2.5 g of glycidyl phenyl ether are added to 10 g of tetrahydropyran in sequence, and stirred until γ-zinc oxide, lithium tetrafluoroborate, lithium hexafluorophosphate and glycidyl phenyl ether are completely dissolved to obtain an ether-based precursor solution. The ether-based precursor solution is allowed to stand at room temperature for 24 hours to obtain a three-dimensional cross-linked gel polymer electrolyte.
[0052] The ether-based precursor solution of Example 3 was assembled together with a high-nickel positive electrode, a lithium metal negative electrode, a separator, a gasket and a spring and left at room temperature for 24 hours to obtain a lithium metal battery containing a three-dimensional cross-linked gel polymer electrolyte.
[0053] Reference electrolyte: Add lithium hexafluorophosphate to dimethyl carbonate solvent, stir thoroughly until the lithium hexafluorophosphate is completely dissolved, and prepare a lithium hexafluorophosphate-dimethyl carbonate solution with a concentration of 1 mol / L to obtain the reference electrolyte.
[0054] The reference electrolyte is assembled together with a high-nickel positive electrode, a lithium metal negative electrode, a separator, a gasket and a spring to prepare a reference lithium metal battery.
[0055] Comparative Example 1
[0056] The preparation method of the three-dimensional cross-linked gel polymer electrolyte of Comparative Example 1 comprises the following steps:
[0057] S1: Add 1g of nano-silicon dioxide to 10g of deionized water and disperse by ultrasonic for 0.5h to obtain a uniform and stable suspension. First, add 6g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane to the suspension, then add 10g of anhydrous ethanol, and mix by ultrasonic to obtain a mixed solution. The obtained mixed solution is continuously reacted in a 100℃ constant temperature bath for 4h, centrifuged and vacuum dried to obtain γ-silicon dioxide;
[0058] S2: 0.08 g of γ-silicon dioxide, 0.7 g of lithium tetrafluoroborate, 0.05 g of lithium hexafluorophosphate, 0.05 g of lithium bis(fluorosulfonyl)imide, 0.5 g of cyclopropylphenyl sulfide, 1.5 g of cyclohexyl sulfide, and 0.8 g of glycidyl methyl ether are sequentially added to 10 g of dioxolane, and the mixture is stirred until the γ-silicon dioxide, lithium tetrafluoroborate, lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, cyclopropylphenyl sulfide, cyclohexyl sulfide, and glycidyl methyl ether are completely dissolved to obtain an ether-based precursor solution. The ether-based precursor solution is allowed to stand at room temperature for 24 h to obtain a three-dimensional cross-linked gel polymer electrolyte.
[0059] The ether-based precursor solution is assembled together with a high-nickel positive electrode, a lithium metal negative electrode, a separator, a gasket and a spring and left at room temperature for 24 hours to obtain a lithium metal battery containing a three-dimensional cross-linked gel polymer electrolyte.
[0060] Reference electrolyte: Add 0.8 g lithium hexafluorophosphate and 0.05 g lithium bis(fluorosulfonyl)imide into ethyl methyl carbonate solvent, stir thoroughly until lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide are completely dissolved, and prepare a lithium hexafluorophosphate-lithium bis(fluorosulfonyl)imide-ethyl methyl carbonate solution with a concentration of 1 mol / L to obtain the reference electrolyte.
[0061] The reference electrolyte is assembled together with a high-nickel positive electrode, a lithium metal negative electrode, a separator, a gasket and a spring to prepare a reference lithium metal battery.
[0062] Comparative Example 2
[0063] The preparation method of the three-dimensional cross-linked gel polymer electrolyte of Comparative Example 2 comprises the following steps:
[0064] S1: preparing γ-silicon dioxide and γ-titanium dioxide, the preparation method of γ-silicon dioxide and γ-titanium dioxide is the same as the preparation method of γ-silicon dioxide and γ-titanium dioxide in Example 1 and Example 2;
[0065] S2: 1 g of γ-silicon dioxide, 1 g of γ-titanium dioxide, 0.9 g of lithium tetrafluoroborate, 0.1 g of lithium hexafluorophosphate, 0.6 g of cyclohexyl sulfide, and 2.3 g of glycidyl methyl ether are added in sequence to a mixed solvent of 5 g of dioxolane and 5 g of ethylene glycol dimethyl ether, and the mixture is stirred until the γ-silicon dioxide, γ-titanium dioxide, lithium tetrafluoroborate, lithium hexafluorophosphate, cyclohexyl sulfide, and glycidyl methyl ether are completely dissolved to obtain an ether-based precursor solution. The ether-based precursor solution is allowed to stand at room temperature for 24 h to obtain a three-dimensional cross-linked gel polymer electrolyte.
[0066] The ether-based precursor solution is assembled together with a high-nickel positive electrode, a lithium metal negative electrode, a separator, a gasket and a spring and left at room temperature for 24 hours to obtain a lithium metal battery containing a three-dimensional cross-linked gel polymer electrolyte.
[0067] Reference electrolyte: Add lithium hexafluorophosphate to a mixed solvent of ethyl methyl carbonate and ethylene carbonate, stir thoroughly until the lithium hexafluorophosphate is completely dissolved, and prepare a lithium hexafluorophosphate-ethyl methyl carbonate / ethylene carbonate solution with a concentration of 1 mol / L to obtain a reference electrolyte.
[0068] The reference electrolyte is assembled together with a high-nickel positive electrode, a lithium metal negative electrode, a separator, a gasket and a spring to prepare a reference lithium metal battery.
[0069] from Figure 1 It can be seen that the capacity retention rate of the lithium metal battery of Example 1 after 400 cycles at a rate of 1.5C is 93.97%, which is much higher than the capacity retention rate of the reference lithium metal battery of 86.23%. Figure 2 It can be seen that the capacity retention rate of the lithium metal battery of Example 2 after 400 cycles at a rate of 1.5C is 94.78%, which is much higher than the capacity retention rate of the reference lithium metal battery of 84.26%. Figure 3 It can be seen that the capacity retention rate of the lithium metal battery of Example 3 after 400 cycles at a rate of 1.5C is 89.26%, which is much higher than the capacity retention rate of the reference lithium metal battery of 84.85%; this is mainly because compared with the reference lithium metal battery, the three-dimensional cross-linked gel polymer electrolyte of the present invention has higher solvent absorption capacity and better oxidation stability, and has good interface compatibility with high nickel and high voltage positive electrodes. In addition, the strong interaction between the cross-linked polymer network and the solvent reduces the Li + The desolvation barrier is favorable for Li +The uniform deposition of lithium dendrites can effectively inhibit the formation and growth of lithium dendrites. Therefore, the lithium metal battery using the in-situ prepared three-dimensional cross-linked gel polymer electrolyte has remarkable cycle performance at a high charge and discharge rate of 1.5C.
[0070] from Figure 4 It can be seen that the capacity retention rate of the lithium metal battery of Comparative Example 1 after 400 cycles at a rate of 1.5C is 75.21%, which is much lower than the capacity retention rate of the reference lithium metal battery of 85.17%. Figure 5 It can be seen that the capacity retention rate of the lithium metal battery in Comparative Example 2 after 400 cycles at a rate of 1.5C is 77.19%, which is much lower than the capacity retention rate of the reference lithium metal battery of 82.24%. This shows that when the mass of the inorganic nanoparticle modifier is less than 1% of the total mass of the cyclic ether monomer or greater than 10% of the total mass of the cyclic ether monomer, the prepared three-dimensional cross-linked gel polymer electrolyte has a lower solvent absorption capacity and weaker oxidation stability, thereby deteriorating the compatibility with the high-nickel, high-voltage positive electrode interface. In addition, the strong interaction between the cross-linked polymer network and the solvent is weakened, which will increase the Li + The desolvation energy barrier weakens the ability to inhibit the growth of lithium dendrites, resulting in a significant decrease in the cycle performance of lithium metal batteries.
Claims
1. A method for preparing a three-dimensional cross-linked gel polymer electrolyte, characterized in that: The following steps are involved: S1: Grafting epoxy groups onto the surface of inorganic nanoparticles to obtain inorganic nanoparticle modified products; S2: adding the modified inorganic nanoparticles, mixed lithium salts and cyclic ether monomers into a solvent to obtain an ether-based precursor solution, and allowing the ether-based precursor solution to stand to obtain the product.
2. The method for preparing a three-dimensional cross-linked gel polymer electrolyte according to claim 1, characterized in that: The mixed lithium salt is a mixed lithium salt of lithium tetrafluoroborate and a fluorine-containing lithium salt, and the mass ratio of the lithium tetrafluoroborate to the fluorine-containing lithium salt is 1:1-6.
3. The method for preparing a three-dimensional cross-linked gel polymer electrolyte according to claim 2, characterized in that: The fluorine-containing lithium salt is one or more of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, and lithium bis(fluorosulfonyl)imide.
4. The method for preparing a three-dimensional cross-linked gel polymer electrolyte according to claim 1, characterized in that: The standing in S2 is standing at room temperature for 12 to 36 hours.
5. The method for preparing a three-dimensional cross-linked gel polymer electrolyte according to claim 1, characterized in that: The mass fraction of the inorganic nanoparticle modification in the solvent is 1-10%; the mass fraction of the mixed lithium salt in the solvent is 5-20%; and the mass fraction of the cyclic ether monomer in the solvent is 10-50%.
6. The method for preparing a three-dimensional cross-linked gel polymer electrolyte according to claim 1, characterized in that: The preparation method of the inorganic nanoparticle modification is: using an in-situ coupling chemical reaction to graft the epoxy groups on the silane coupling agent onto the surface of the inorganic nanoparticle; the silane coupling agent is γ-(2,3-epoxypropoxy)propyltrimethoxysilane, and the inorganic nanoparticle is one or more of nano titanium dioxide, nano silicon dioxide, nano zinc oxide, and nano aluminum oxide.
7. The method for preparing a three-dimensional cross-linked gel polymer electrolyte according to claim 1, characterized in that: The cyclic ether monomer is one or more of epichlorohydrin, dioxolane, glycidyl phenyl ether, cyclopropyl phenyl sulfide, cyclohexyl sulfide, glycidyl methyl ether and tetrahydrofuran.
8. The method for preparing a three-dimensional cross-linked gel polymer electrolyte according to claim 1, characterized in that: The solvent is one or more of ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol methylene ether, tetrahydropyran, and epichlorohydrin.
9. A three-dimensional cross-linked gel polymer electrolyte, characterized in that: The three-dimensional cross-linked gel polymer electrolyte is prepared by the preparation method of any one of claims 1 to 8.
10. Use of the three-dimensional cross-linked gel polymer electrolyte as claimed in claim 9 in a lithium metal battery.
Citation Information
Cited By
Composite polymer electrolyte based on surface organic modified lithium titanium aluminum phosphate as well as preparation method and application of composite polymer electrolyte
CN119875141A